Polyglycolic acid-containing resin composition and film containing the same
A polyglycolic acid-containing resin composition with ethylene-(meth)acrylic and ethylene-based terpolymer improves PGA's processability and biodegradability, achieving films with reduced gas permeability and enhanced durability for eco-friendly applications.
Patent Information
- Application Number
- JP2024061945
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-08
- Publication Date
- 2024-10-30
AI Technical Summary
Polyglycolic acid (PGA) resin has high melting point and low melt strength, making film processing difficult due to ease of decomposition by heat and moisture, while also requiring improved biodegradability, gas barrier properties, and durability.
A polyglycolic acid-containing resin composition comprising PGA, an ethylene-(meth)acrylic polymer, and an ethylene-based terpolymer, with specific weight ratios and processing conditions to enhance molecular weight, impact resistance, and processability, thereby improving biodegradability and gas barrier properties.
The composition achieves reduced gas permeability, increased molecular weight, and improved processability, allowing for the production of films with enhanced durability and biodegradability, suitable for various applications including biodegradable packaging and eco-friendly products.
Smart Images

Figure 2024154381000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a polyglycolic acid-containing resin composition and a film containing the same. [Background technology]
[0002] Biodegradable resins are decomposed by other organic organisms such as bacteria and microorganisms, and as environmental regulations have been strengthened due to the worsening environmental pollution caused by conventional difficult-to-decompose polymers, demand for them as alternative materials to difficult-to-decompose resins is increasing. Recently, they have been used in a variety of fields, including the packaging materials industry, electronics industry, automobile industry, building materials industry, marine industry, stationery industry, and pulp and paper industry.
[0003] Examples of biodegradable resins include poly(glycolic acid) (PGA), poly(butylene succinate) (PBS), polyhydroxyalkanoate (PHA), polylactic acid (PLA), etc. Among them, PGA is a synthetic resin produced by polymerizing glycolic acid, and has excellent biodegradability and, as a resin with a linear structure, has excellent gas barrier properties.
[0004] In addition, PGA resin has ester bonds inside, high crystallinity, and excellent mechanical strength and brittleness. For this reason, there are attempts to develop barrier films using PGA resin that have high gas barrier properties, excellent biodegradability, and excellent durability.
[0005] However, PGA resin has a high melting point and low melt strength, and is easily decomposed by heat and moisture, making it difficult to process into a conventional film.
[0006] Therefore, it is necessary to develop a resin that is easy to process into a film while improving biodegradability, gas barrier properties, and durability by compounding or blending PGA resin with other polymers. Summary of the Invention [Problem to be solved by the invention]
[0007] One object of the present disclosure is to provide a polyglycolic acid-containing resin composition that provides improved barrier properties.
[0008] One object of the present disclosure is to provide a film formed from the resin composition and having improved barrier properties. [Means for solving the problem]
[0009] A polyglycolic acid-containing resin composition according to an exemplary embodiment may include poly(glycolic acid), an ethylene-(meth)acrylic polymer, and an ethylene-based terpolymer.
[0010] In some embodiments, the ethylene-(meth)acrylic polymer can include a copolymer of ethylene and an alkyl (meth)acrylate monomer.
[0011] In some embodiments, the ethylene-(meth)acrylic polymer can include a copolymer of ethylene and (meth)acrylic acid.
[0012] In some embodiments, the ethylene-based terpolymer may include a copolymer of ethylene, glycidyl methacrylate, and an alkyl acrylate.
[0013] In some embodiments, the content of the polyglycolic acid may be 60% by weight to 98% by weight based on the total weight of the polyglycolic acid-containing resin composition.
[0014] In some embodiments, the content of the ethylene-(meth)acrylic polymer may be 1% by weight to 39% by weight based on the total weight of the polyglycolic acid-containing resin composition.
[0015] In some embodiments, the content of the ethylene-based terpolymer may be 1% by weight to 39% by weight based on the total weight of the polyglycolic acid-containing resin composition.
[0016] In some embodiments, the polyglycolic acid content may be greater than the sum of the ethylene-(meth)acrylic polymer content and the ethylene terpolymer content.
[0017] In some embodiments, the polyglycolic acid-containing resin composition may have a melt viscosity of 200 Pa·s to 10,000 Pa·s, measured under conditions of a temperature of 230° C., a strain of 5%, and a frequency of 0.1 Hz.
[0018] In some embodiments, the polyglycolic acid-containing resin composition may have a melt flow index of 1 g / 10 min to 200 g / 10 min measured under conditions of a temperature of 230° C. and a load of 2.16 kg.
[0019] A film according to an exemplary embodiment may be formed from the polyglycolic acid-containing resin composition.
[0020] In some embodiments, the film may have a thickness of from 50 μm to 250 μm.
[0021] In some embodiments, the film has an oxygen transmission rate of 200 g / m2 or less, measured at a relative humidity of 50% and a temperature of 25° C. 2 ·days or less is acceptable.
[0022] In some embodiments, the oxygen permeability of the film can satisfy Equation 1: [Formula 1] OTR(PGA-Poly)<0.1(x OTR(PGA)+(1-x) OTR(Poly))
[0023] In the above formula 1, OTR(PGA-Poly) is the oxygen permeability of a film formed from the polyglycolic acid-containing resin composition, OTR(PGA) is the oxygen permeability of a film containing only polyglycolic acid, OTR(Poly) is the oxygen permeability of a film containing a resin containing only an ethylene-(meth)acrylic polymer or an ethylene terpolymer, and x is 0.6≦x<1. Effect of the Invention
[0024] The polyglycolic acid-containing resin composition according to the exemplary embodiment may include poly(glycolic acid, PGA), an ethylene-(meth)acrylic polymer, and an ethylene-based terpolymer, which increases the molecular weight of the polyglycolic acid-containing resin composition, thereby improving impact resistance, and decreases the melt flow index, thereby improving processability.
[0025] The polyglycolic acid-containing resin composition can contain PGA in a predetermined content, which can improve the biodegradability and gas barrier properties of a film containing the polyglycolic acid-containing resin composition while improving the processability.
[0026] The film according to the exemplary embodiment may include the polyglycolic acid-containing resin composition, which may complicate the gas permeation path inside the film and reduce the gas permeability.
[0027] The polyglycolic acid-containing resin composition and film of the present disclosure can be widely applied in the field of green technology such as biodegradable resins, biodegradable food packaging films, biodegradable sanitary products, and other biodegradable plastics in which the biodegradable composition is used. The polyglycolic acid-containing resin composition and film of the present disclosure can suppress land pollution, water pollution, air pollution, etc., and can be used as a material for disposable items that are eco-friendly. [Brief description of the drawings]
[0028] [Figure 1] FIG. 1 is a graph showing measured and estimated oxygen permeability of films according to an exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] According to an exemplary embodiment, there is provided a polyglycolic acid-containing resin composition including poly(glycolic acid) (PGA), an ethylene-(meth)acrylic polymer, and an ethylene-based terpolymer, and a film including the polyglycolic acid-containing resin composition.
[0030] Hereinafter, embodiments of the present disclosure will be described in more detail with reference to the accompanying drawings. However, these embodiments are merely illustrative of the present disclosure and are not intended to limit the present disclosure.
[0031] According to an exemplary embodiment, the polyglycolic acid-containing resin composition can include PGA, an ethylene-(meth)acrylic polymer, and an ethylene-based terpolymer.
[0032] The PGA is a biodegradable polymer having a linear structure with ester bonds, and can have high biodegradability. In addition, due to hydrogen bonds between PGA polymers, it can have high crystallinity. This can improve the gas barrier properties of the polyglycolic acid-containing resin composition.
[0033] The carboxyl group or acrylate group of the ethylene-(meth)acrylic polymer can form hydrogen bonds or electrostatic interactions with the carboxyl group and / or hydroxyl group formed by decomposition of the ester group located in the middle of the polymer chain of the PGA or the carboxyl group and / or hydroxyl group located at the end of the chain, thereby improving the mechanical strength and impact strength of the polyglycolic acid-containing resin composition.
[0034] The ethylene-based terpolymer is a copolymer of three basic monomers including a monomer derived from ethylene. The ethylene-based terpolymer can be crosslinked with the carboxyl group and / or hydroxyl group at the end of the PGA. The ethylene-based terpolymer can also be crosslinked with the carboxyl group and / or hydroxyl group formed by decomposition of the ester group located in the middle of the polymer chain of the PGA. This can increase the molecular weight of the polyglycolic acid-containing resin composition and improve its melt strength and durability.
[0035] In some embodiments, the ethylene-(meth)acrylic polymer can include at least one of a copolymer of ethylene and an alkyl (meth)acrylate monomer (EA) and a copolymer of ethylene and (meth)acrylic acid (EAA).
[0036] For example, EA or EAA can be used alone as the ethylene-(meth)acrylic polymer. For example, EA and EAA can be used together as the ethylene-(meth)acrylic polymer.
[0037] The acrylate group of the EA or the carboxyl group of the EAA can form hydrogen bonds or electrostatic interactions with the carboxyl and / or hydroxyl groups formed by decomposition of the ester group located in the middle of the polymer chain of the PGA or the carboxyl and / or hydroxyl groups located at the ends of the chain, thereby improving the mechanical strength and impact strength of the polyglycolic acid-containing resin composition.
[0038] In one embodiment, the content of the ethylene monomer derived units in the total weight of the EA is not limited, but may be, for example, 50% by weight to 90% by weight, 55% by weight to 85% by weight, or 60% by weight to 80% by weight. The content of the alkyl (meth)acrylate monomer derived units in the total weight of the EA is not limited, but may be, for example, 10% by weight to 50% by weight, 15% by weight to 45% by weight, or 20% by weight to 40% by weight.
[0039] In one embodiment, the content of units derived from an ethylene monomer in the total weight of the EAA is not limited, but may be, for example, 70% by weight to 99% by weight, 73% by weight to 95% by weight, or 78% by weight to 90% by weight. The content of units derived from a (meth)acrylic acid monomer in the total weight of the EAA is not limited, but may be, for example, 1% by weight to 30% by weight, 5% by weight to 27% by weight, or 10% by weight to 22% by weight.
[0040] In some embodiments, the ethylene-based terpolymer can include a copolymer of ethylene, glycidyl methacrylate, and an alkyl acrylate (EAG).
[0041] The EAG is an ethylene-based polymer containing a glycidyl group, and the glycidyl group of the EAG is contained in the polyglycolic acid-containing resin composition and can be crosslinked with at least one of the PGA and the ethylene-(meth)acrylic polymer.
[0042] This allows the polyglycolic acid-containing resin composition to be elongated and the polymer structure to be made complex, thereby improving the melt strength and durability of the polyglycolic acid-containing resin composition and improving the processability.
[0043] In one embodiment, the content of units derived from an ethylene monomer in the total weight of the EAG is not limited, but may be, for example, 48% by weight to 90% by weight, 52% by weight to 85% by weight, or 55% by weight to 80% by weight.
[0044] In one embodiment, the content of units derived from a glycidyl methacrylate monomer in the total weight of the EAG is not limited, and may be, for example, 1% by weight to 30% by weight, 3% by weight to 25% by weight, or 5% by weight to 20% by weight.
[0045] In one embodiment, the content of units derived from alkyl acrylate monomers in the total weight of the EAG is not limited, but may be, for example, 8% by weight to 50% by weight, 12% by weight to 45% by weight, or 15% by weight to 45% by weight.
[0046] In some embodiments, the PGA may be 60% to 98% by weight, 60% to 93% by weight, 60% to 88% by weight, or 65% to 85% by weight based on the total weight of the polyglycolic acid-containing resin composition.
[0047] In the above range, PGA can be distributed throughout the entire region of the polyglycolic acid-containing resin composition. This allows the polyglycolic acid-containing resin composition to have improved melt strength, durability and processability while maintaining low gas permeability. In addition, PGA can improve the biodegradability of the polyglycolic acid-containing resin composition.
[0048] In some embodiments, the ethylene-(meth)acrylic polymer may be 1 wt % to 39 wt %, 5 wt % to 38 wt %, 7 wt % to 30 wt %, or 8 wt % to 20 wt % based on the total weight of the polyglycolic acid-containing resin composition.
[0049] In one embodiment, when EA and EAA are used together as the ethylene-(meth)acrylic polymer, the content of EA and EAA may be 1% by weight or more, respectively, based on the total weight of the polyglycolic acid-containing resin composition. For example, the content of EA and the content of EAA may be 1% by weight to 39% by weight, 10% by weight to 39% by weight, 10% by weight to 35% by weight, or 10% by weight to 20% by weight, respectively, based on the total weight of the polyglycolic acid-containing resin composition.
[0050] When EA and EAA are used together as the ethylene-(meth)acrylic polymer, the total content of EA and EAA may be 2 wt % to 39 wt %, 10 wt % to 39 wt %, 10 wt % to 35 wt %, or 10 wt % to 30 wt % based on the total weight of the polyglycolic acid-containing resin composition.
[0051] In the above range, PGA can be uniformly distributed in the polyglycolic acid-containing resin composition while preventing a decrease in gas barrier properties due to an increase in the ethylene-(meth)acrylic polymer and a decrease in the PGA. This can improve the durability of the polyglycolic acid-containing resin composition and prevent the polymer structure from collapsing due to the high biodegradability of the polyglycolic acid-containing resin composition. Therefore, the structural stability of the polyglycolic acid-containing resin composition can be improved.
[0052] In some embodiments, the content of the ethylene-based terpolymer (e.g., EAG) may be 1 wt % to 39 wt %, 1 wt % to 38 wt %, 2 wt % to 35 wt %, 2 wt % to 33 wt %, 5 wt % to 33 wt %, or 7 wt % to 27 wt %, based on the total weight of the polyglycolic acid-containing resin composition.
[0053] Within this range, the ethylene-based terpolymer (e.g., EAG) can be crosslinked with the PGA and the ethylene-(meth)acrylic acid polymer, which can further improve the melt strength and processability of the polyglycolic acid-containing resin composition.
[0054] In one embodiment, the sum of the content of the ethylene-(meth)acrylic polymer and the content of the ethylene terpolymer may be 2 wt % to 40 wt %, 3 wt % to 40 wt %, 10 wt % to 40 wt %, or 10 wt % to 35 wt % based on the total weight of the polyglycolic acid-containing resin composition.
[0055] Within the above range, the content of PGA contained in the polyglycolic acid-containing resin composition can be 60% by weight or more, 65% by weight or more, or 80% by weight or more, which can reduce gas permeability and improve processability without reducing the biodegradability of the polyglycolic acid-containing resin composition.
[0056] In some embodiments, the content of the PGA may be greater than the sum of the content of the ethylene-(meth)acrylic polymer and the content of the ethylene-based terpolymer, thereby improving the biodegradability and gas barrier properties of the polyglycolic acid-containing resin composition while improving its durability.
[0057] As described above, the melt viscosity and melt flow index can be adjusted by adjusting the contents of PGA, ethylene-(meth)acrylic polymer, and ethylene terpolymer contained in the polyglycolic acid-containing resin composition.
[0058] In some embodiments, the melt viscosity of the polyglycolic acid-containing resin composition may be 50 Pa·s to 10,000 Pa·s, 100 Pa·s to 10,000 Pa·s, 200 Pa·s to 10,000 Pa·s, 200 Pa·s to 8,000 Pa·s, or 200 Pa·s to 6,000 Pa·s.
[0059] The melt viscosity was measured on a test piece prepared by pressing the polyglycolic acid-containing resin composition to a thickness of 2 mm at a temperature of 230° C. under conditions of strain of 5% and frequency of 0.1 Hz.
[0060] In one embodiment, the melt flow index of the polyglycolic acid-containing resin composition may be 1 g / 10 min to 200 g / 10 min, 1 g / 10 min to 100 g / 10 min, or 2 g / 10 min to 50 g / 10 min.
[0061] The melt flow index was measured and calculated under conditions of a temperature of 230° C. and a load of 2.16 kg in accordance with ASTM D1238.
[0062] By maintaining the melt viscosity and melt flow index within the above ranges, the polyglycolic acid-containing resin composition can have improved flexibility compared to PGA. This can improve processability in processes such as foaming-expansion molding, injection molding, compression molding, casting filming process, and inflation film process. This can improve processability of the polyglycolic acid-containing resin composition into a film.
[0063] The polyglycolic acid-containing resin composition can be formed by drying and kneading a mixture of PGA, an ethylene-(meth)acrylic polymer, and an ethylene terpolymer.
[0064] In an exemplary embodiment, the PGA, the ethylene-(meth)acrylic polymer and the ethylene terpolymer can be charged to a Hopper Dryer.
[0065] The PGA can be dried by being placed in a hopper dryer maintained at a temperature condition of, for example, 60°C to 100°C, 70°C to 90°C, or 75°C to 85°C.
[0066] When EA is used as the ethylene-(meth)acrylic polymer, it can be dried, for example, by being placed in a hopper dryer maintained at a temperature of 30° C. to 70° C., 40° C. to 60° C., or 45° C. to 55° C. When EAA is used as the ethylene-(meth)acrylic polymer, it can be dried, for example, by being placed in a hopper dryer maintained at a temperature of 20° C. to 60° C., 30° C. to 50° C., or 35° C. to 45° C.
[0067] The ethylene-based terpolymer (eg, EAG) can be dried by being loaded into a hopper dryer maintained at a temperature condition of, for example, 20°C to 60°C, 30°C to 50°C, or 35°C to 45°C.
[0068] The PGA, ethylene-(meth)acrylic polymer, and ethylene-based terpolymer can be dried for, for example, 10 hours to 14 hours, 11 hours to 13 hours, or 11 hours 30 minutes to 12 hours 30 minutes. Within the above range, the PGA, ethylene-(meth)acrylic polymer, and ethylene-based terpolymer can be sufficiently dried. This can suppress side reactions in the kneading process of the PGA, ethylene-(meth)acrylic polymer, and ethylene-based terpolymer.
[0069] The dried PGA, ethylene-(meth)acrylic polymer, and ethylene terpolymer can be placed in a chamber of an internal mixer, which can be maintained at a temperature of, for example, 220°C to 260°C, 225°C to 250°C, or 230°C to 240°C.
[0070] When the dried PGA, ethylene-(meth)acrylic polymer, and ethylene terpolymer are charged into an internal mixer, the rotor in the internal mixer can rotate at, for example, 10 rpm to 70 rpm, 20 rpm to 60 rpm, or 30 rpm to 50 rpm.
[0071] Within the above range, kneading can be started without the PGA, ethylene-(meth)acrylic polymer, and ethylene terpolymer agglomerating together.
[0072] After the addition of the dried PGA, ethylene-(meth)acrylic polymer, and ethylene terpolymer is completed, the rotor speed can be maintained at, for example, 60 rpm to 100 rpm, 70 rpm to 90 rpm, or 75 rpm to 85 rpm while kneading. The kneading can be performed for, for example, 1 minute to 5 minutes, 2 minutes to 4 minutes, or 2 minutes 30 seconds to 3 minutes 30 seconds.
[0073] Within this range, the PGA, ethylene-(meth)acrylic polymer, and ethylene terpolymer can be uniformly distributed and kneading can be completed.
[0074] The kneaded product obtained as described above can be recovered to obtain a polyglycolic acid-containing resin composition.
[0075] Although the above kneading step is described as being performed using an internal mixer, the means for the kneading step is not limited to an internal mixer. For example, the dried PGA, ethylene-(meth)acrylic polymer, and ethylene terpolymer may be fed into a single-screw extruder or a twin-screw extruder, and melted and kneaded to complete the kneading. The kneaded resin composition discharged from the outlet of the single-screw extruder or twin-screw extruder can be cut with a pelletizer to obtain a polyglycolic acid-containing resin composition in the form of pellets.
[0076] According to an exemplary embodiment, the film may include the polyglycolic acid-containing resin composition described above, which may reduce the gas permeability of the film and improve its biodegradability and durability.
[0077] In some embodiments, the thickness of the film may be 50 μm to 250 μm, 100 μm to 200 μm, or 120 μm to 180 μm, which is sufficient to reduce the gas permeability through the film.
[0078] In one embodiment, the oxygen permeability of the film is 200 g / m 2 ·day or less, 100g / m 2 ·day or less, or 30g / m 2 The lower limit of the oxygen permeability of the film is not limited, but for example, the oxygen permeability of the film may be 0.3 g / m 2 ·day or more, 1g / m 2 ·day or more, 2g / m 2 ·day or more, 5g / m 2 day or more, or 10g / m 2 · days or more is acceptable.
[0079] The oxygen permeability may be measured under conditions of relative humidity: 50% and temperature: 25°C.
[0080] Within this range, when the film is used as a barrier film, the barrier properties against gases (for example, oxygen) are improved, and products inside the barrier film can be sufficiently protected.
[0081] When the PGA contained in the polyglycolic acid-containing resin composition is contained in an amount of 60% by weight or more based on the total weight of the polyglycolic acid-containing resin composition, the PGA can be uniformly distributed throughout the entire region of the polyglycolic acid-containing resin composition, and the high gas barrier property of the PGA can thereby be maintained at a high level in the film containing the polyglycolic acid-containing resin composition.
[0082] Therefore, the polyglycolic acid-containing resin composition contains 60% by weight or more of the PGA based on the total weight of the polyglycolic acid-containing resin composition, and the oxygen permeability of the polyglycolic acid-containing resin composition can be kept low. For example, the oxygen permeability of the polyglycolic acid-containing resin composition can be made lower than the arithmetic average value of the oxygen permeability of each of the polymer components contained in the polyglycolic acid-containing resin composition.
[0083] In some embodiments, the oxygen permeability of the film can satisfy Equation 1:
[0084] [Formula 1] OTR(PGA-Poly)<0.1(x OTR(PGA)+(1-x) OTR(Poly))
[0085] In the above formula 1, OTR(PGA-Poly) is the oxygen permeability of a film formed from the polyglycolic acid-containing resin composition, OTR(PGA) is the oxygen permeability of a film containing only polyglycolic acid, OTR(Poly) is the oxygen permeability of a film containing a resin containing only an ethylene-(meth)acrylic polymer or an ethylene terpolymer, and x is 0.6≦x<1.
[0086] The film can be used as a barrier film for packaging materials for various products, such as food packaging materials and battery packaging materials.
[0087] The aforementioned films can be produced from polyglycolic acid-containing resin compositions.
[0088] According to an exemplary embodiment, the polyglycolic acid-containing resin composition can be compressed by a press to produce a film.
[0089] In some embodiments, the press can be maintained at 200° C. to 260° C., 210° C. to 250° C., 220° C. to 240° C., or 225° C. to 235° C. The above ranges allow for forming and deforming a film comprising the polyglycolic acid-containing resin composition.
[0090] In some embodiments, the polyglycolic acid-containing resin composition can be compressed to a pressure of 10 MPa to 30 MPa, 15 MPa to 25 MPa, or 18 MPa to 22 MPa for 1 minute to 3 minutes, or 1 minute 30 seconds to 2 minutes 30 seconds.
[0091] In the above range, the film can be manufactured to the above thickness, which reduces the oxygen permeability and allows the film to be manufactured to a small thickness.
[0092] Although the above-mentioned film production is performed by applying pressure by a press, the film production method is not limited thereto. For example, the polyglycolic acid-containing resin composition melted in an extruder can be extruded through a chill roll in a t-die and cooled to produce a film (for example, a cast film production method). For example, the polyglycolic acid-containing resin composition can be cooled by contacting air with an air ring in a ring-shaped die (for example, a spiral die) to produce a film (for example, a blown film production method).
[0093] Below, preferred examples are presented to aid in understanding the present invention. However, these examples are merely illustrative of the present invention and do not limit the scope of the appended claims. It will be apparent to those skilled in the art that various changes and modifications to the examples are possible within the scope of the scope and technical spirit of the present invention, and it is natural that such changes and modifications also fall within the scope of the appended claims. EXAMPLES
[0094] Examples and Comparative Examples Example 1 (1) Preparation of raw materials for polyglycolic acid-containing resin composition Poly(glycolic acid, PGA) was dried in a hopper dryer set at 80° C. for 12 hours to prepare dried PGA.
[0095] A copolymer of ethylene and acrylic acid (EAA) as an ethylene-(meth)acrylic polymer was dried for 12 hours in a hopper dryer set at 50° C. to prepare dried EAA. The contents of units derived from ethylene monomers and units derived from (meth)acrylic acid monomers in the total weight of the EAA were 90.5 wt % and 9.5 wt %, respectively.
[0096] A terpolymer of ethylene, glycidyl methacrylate, and methyl acrylate (EAG) was dried for 12 hours in a hopper dryer set at 40° C. to prepare dried EAG. The contents of units derived from ethylene monomer, units derived from glycidyl methacrylate monomer, and units derived from methyl acrylate monomer in the total weight of the EAG were 68 wt%, 8 wt%, and 24 wt%, respectively.
[0097] As the hopper dryer, a Mitsui hot air dryer was used.
[0098] (2) Production of polyglycolic acid-containing resin composition The dried PGA, dried EAA and dried EAG were placed in the chamber of an internal mixer at 80 wt%, 10 wt% and 10 wt%, respectively. The temperature in the chamber of the internal mixer was maintained at 230° C. and the rotor of the internal mixer rotated at a speed of 40 rpm.
[0099] Thereafter, the rotor speed was increased to 80 rpm and kneading was continued for 3 minutes, after which a kneaded product, a polyglycolic acid-containing resin composition, was produced and collected.
[0100] As the internal mixer, a Brabender Measuring Mixer W50 was used.
[0101] (3) Film manufacturing The polyglycolic acid-containing resin composition was pressed at a pressure of 20 MPa for 2 minutes using a press set at 230° C. to produce a film.
[0102] Examples 2 to 14 and Comparative Examples 1 to 5 An ethylene and acrylate copolymer (EA) as an ethylene-(meth)acrylic polymer was dried for 12 hours in a hopper dryer set at 40° C. to prepare dried EA. The contents of units derived from ethylene monomer and units derived from methyl acrylate monomer in the total weight of the EA were 71 wt % and 29 wt %, respectively.
[0103] The polyglycolic acid-containing resin compositions and films of Examples 2 to 14 and Comparative Examples 1 to 5 were produced in the same manner as in Example 1, except that the type of PGA used and the weight ratios of the dried PGA, the dried ethylene-(meth)acrylic polymer, and the dried EAG charged into the chamber of the internal mixer were adjusted as shown in Table 1 below.
[0104] [Table 1]
[0105] The types of PGAs shown in Table 1 are as follows: Types of PGA A: Polyglycolic acid having a number average molecular weight (Mn) of 35,000 to 45,000 and a weight average molecular weight (Mw) of 80,000 to 95,000 as measured by gel permeation chromatography (GPC). B: Polyglycolic acid having a number average molecular weight (Mn) of 70,000 to 80,000 and a weight average molecular weight (Mw) of 160,000 to 180,000 as measured by gel permeation chromatography (GPC).
[0106] The gel permeation chromatography was carried out by dissolving polyglycolic acid in hexafluoroisopropyl alcohol (HFIP), filtering the solution through a polytetrafluoroethylene (PTFE) filter, and injecting the solution into EcoSEC HLC-8320 GPC manufactured by Tosoh Corporation for measurement. Polymethyl methacrylate was used as a standard substance.
[0107] Experimental Example 1 FIG. 1 is a graph showing the measured and estimated oxygen permeabilities of films depending on the total EA content and EAG content contained in a polyglycolic acid-containing resin composition, and the total EAA content and EAG content contained in a polyglycolic acid-containing resin composition.
[0108] The estimated oxygen permeability is the arithmetic average of the oxygen permeability of PGA, and the oxygen permeability of EA, EAA and EAG contained in the polyglycolic acid-containing resin composition, calculated by weight ratio.
[0109] The measured oxygen permeability indicates a value obtained by measuring the oxygen permeability of a film containing the polyglycolic acid-containing resin composition.
[0110] As the measured value of oxygen permeability of the film containing the polyglycolic acid-containing resin composition containing PGA, EA and EAG, the measured values of Example 3, Example 7 and Example 12 were used.
[0111] As the measurement value of the oxygen permeability of the film containing the polyglycolic acid-containing resin composition containing PGA, EAA and EAG, the measurement values of Example 1, Example 4, Example 8, Example 10 and Example 13 were used.
[0112] Referring to FIG. 1, it was calculated that the estimated oxygen permeability of the films increased linearly with the sum of the EA and EAG contents, or the sum of the EAA and EAG contents.
[0113] However, the measured oxygen permeability of the film remained low when the total content of EA and EAG or the total content of EAA and EAG was 40 wt% or less (PGA was 60 wt% or more), and it was measured that the oxygen permeability increased in proportion to the content when the total content of EA and EAG or the total content of EAA and EAG exceeded 40 wt%.
[0114] Experimental Example 2 (1) Measurement of melt viscosity The polyglycolic acid-containing resin compositions prepared in the above examples and comparative examples were pressed to a thickness of 2 mm at a temperature of 230° C., and the melt viscosity was measured using a viscometer (TA ARES).
[0115] The viscosity meter was set under the following conditions: temperature: 230° C., strain: 5%, and frequency: 0.1 Hz to 400 Hz, and the viscosity value measured at a frequency of 0.1 Hz was taken as the melt viscosity.
[0116] (2) Measurement of Melt Flow Index The melt flow index of each of the polyglycolic acid-containing resin compositions produced in the above-mentioned Examples and Comparative Examples was measured at a temperature of 230° C. under a load of 2.16 kg in accordance with ASTM D1238.
[0117] (3) Measurement of oxygen permeability The films prepared in the above examples and comparative examples were attached to an oxygen permeability meter (MOCON OX TRANS model 2 / 61) to measure the oxygen permeability.
[0118] The oxygen transmission rate was measured at a relative humidity of 50% and a temperature of 25° C. for 12 hours, and then the value at which the transmission rate stabilized was measured.
[0119] The upper limit of the oxygen permeability measurement is 1,200 g / m 2 The oxygen permeability of the film which could not be measured exceeding the upper limit was expressed as "Ultra".
[0120] The evaluation results are shown in Table 2 below.
[0121] [Table 2]
[0122] Referring to Table 2, the film according to the embodiment has a thickness of 200 g / m 2 The oxygen permeability was less than 1000 times that of the control.
[0123] In Examples 6 to 9, in which the PGA content was reduced to 60 wt %, the oxygen permeability increased.
[0124] In Examples 12 and 13, where the PGA content was reduced to less than 60 wt%, the oxygen permeability increased.
[0125] In Example 14, where the molecular weight of the PGA was increased, the melt viscosity increased and the melt flow index decreased.
[0126] In Comparative Example 1, in which only PGA was used, the melt viscosity of the polyglycolic acid-containing resin composition decreased and the melt flow index increased.
[0127] In Comparative Example 2, in which only EA was used, the oxygen permeability was 200 g / m 2 ·day has passed.
[0128] In Comparative Example 3, in which only EAA was used, the oxygen permeability was 200 g / m 2 ·day has passed.
[0129] In Comparative Example 4, in which only EAG was used, the oxygen permeability was 1,200 g / m 2 ·day has passed.
Claims
1. A polyglycolic acid-containing resin composition comprising poly(glycolic acid), an ethylene-(meth)acrylic polymer, and an ethylene-based terpolymer.
2. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the ethylene-(meth)acrylic polymer comprises a copolymer of ethylene and an alkyl (meth)acrylate monomer.
3. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the ethylene-(meth)acrylic polymer comprises a copolymer of ethylene and (meth)acrylic acid.
4. 2. The polyglycolic acid-containing resin composition of claim 1, wherein the ethylene-based terpolymer comprises a copolymer of ethylene, glycidyl methacrylate, and an alkyl acrylate.
5. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the content of the polyglycolic acid is 60% by weight to 98% by weight based on the total weight of the polyglycolic acid-containing resin composition.
6. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the content of the ethylene-(meth)acrylic polymer is 1% by weight to 39% by weight based on the total weight of the polyglycolic acid-containing resin composition.
7. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the content of the ethylene-based terpolymer is 1% by weight to 39% by weight based on the total weight of the polyglycolic acid-containing resin composition.
8. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the content of the polyglycolic acid is greater than the sum of the content of the ethylene-(meth)acrylic polymer and the content of the ethylene terpolymer.
9. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the polyglycolic acid-containing resin composition has a melt viscosity of 200 Pa·s to 10,000 Pa·s measured under conditions of a temperature of 230° C., a strain of 5%, and a frequency of 0.1 Hz.
10. The polyglycolic acid-containing resin composition according to claim 1, wherein the polyglycolic acid-containing resin composition has a melt flow index of 1 g / 10 min to 200 g / 10 min measured under conditions of a temperature of 230° C. and a load of 2.16 kg.
11. A film formed from the polyglycolic acid-containing resin composition according to claim 1.
12. The film of claim 11, wherein the thickness of the film is from 50 μm to 250 μm.
13. The film has an oxygen transmission rate of 200 g / m2 measured at a relative humidity of 50% and a temperature of 25° C. 2 13. The film of claim 12, wherein the film has a viscosity of 0.05 to 1.0 s.
14. The film according to claim 11, wherein the oxygen permeability of the film satisfies the following formula 1: [Formula 1] OTR(PGA-Poly)<0.1(x・OTR(PGA)+(1-x)・OTR(Poly)) (In formula 1, OTR(PGA-Poly) is the oxygen permeability of a film formed from the polyglycolic acid-containing resin composition, OTR(PGA) is the oxygen permeability of a film containing only polyglycolic acid, OTR(Poly) is the oxygen permeability of a film containing a resin containing only an ethylene-(meth)acrylic polymer or an ethylene terpolymer, and x is 0.6≦x<1.)