Carbon fiber and manufacturing method of carbon fiber-reinforced resin composition
By chemically decomposing and controlling resin residue in CFRP prepreg using an acidic solution, the method addresses the limitations of existing recycling methods, producing high-quality cut fibers for resin composites with equivalent mechanical properties to virgin carbon fibers, enhancing recycling efficiency and reducing waste.
Patent Information
- Application Number
- JP2024065870
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-30
AI Technical Summary
Existing methods for recycling carbon fibers from carbon fiber reinforced resin (CFRP) waste result in fibers with reduced mechanical strength and limited applications due to high manufacturing costs, residual resin issues, and poor feedability, making them unsuitable for high-quality cut fibers used in composite materials.
A method involving chemical decomposition of the base material resin in CFRP prepreg using an acidic aqueous solution, followed by controlled heating to produce cut fibers with specific resin residue content, bulk density, and mechanical strength comparable to virgin carbon fibers, ensuring stable feedability.
The method enables the production of high-performance cut fibers with mechanical properties equivalent to virgin carbon fibers, suitable for various applications in resin composites, reducing waste and environmental impact while maintaining product quality.
Smart Images

Figure 2024154397000006 
Figure 2024154397000007 
Figure 2024154397000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon fiber and a carbon fiber reinforced resin composition. More specifically, the present invention relates to a recycled carbon fiber and a manufacturing method thereof suitable for addition when obtaining a resin composite for injection molding, extrusion molding, press molding, etc., and a recycled carbon fiber reinforced resin composition and a manufacturing method thereof. [Background technology]
[0002] Carbon fiber has been attracting attention as a lightweight and high-strength material, and is used as carbon fiber composite materials, which are materials compounded with binders such as thermoplastic resins and thermosetting resins. Carbon fiber reinforced plastic (CFRP), a composite of carbon fiber and resin, is widely used in aircraft and automobile materials, sports goods, etc., and is expected to expand in the future as it leads to improved fuel efficiency through weight reduction. However, at the same time, the disposal of surplus materials and waste materials from the process has become an issue.
[0003] If carbon fibers from CFRP waste materials discharged as surplus materials from aircraft component manufacturers and carbon fiber manufacturers could be recycled at low cost with the same quality as virgin carbon fibers, it is expected that the market will expand in various fields where they have not been used until now, and the amount of waste materials that are landfilled or incinerated will decrease, which will also reduce the environmental burden. For this reason, there have been many reports on manufacturing methods for recycled carbon fibers that isolate and recover carbon fibers from CFRP waste materials, and new research is also being conducted. However, recycled carbon fibers are not widely used, even though they are cheaper than virgin (new) carbon fibers. One of the reasons for this is that, although there are various reasons, their quality is unknown and they are difficult to use.
[0004] Carbon fiber recycling methods are broadly divided into a method in which CFRP is heated and fired to thermally decompose the base resin, and a dissolution method in which the base resin is dissolved or chemically decomposed with chemicals. In the thermal decomposition method described in Patent Document 1, the base resin is decomposed by supplying superheated steam and firing at a high temperature of 400°C or higher in a heating furnace, but in this method, the carbon fiber deteriorates due to the heat treatment, and it is described in Example 1 that the mechanical strength of the recycled carbon fiber is only 80% of that of virgin carbon fiber.
[0005] As a dissolution method, there is a normal pressure dissolution method (Patent Document 2) in which the base resin is dissolved at 200°C. There is no resin residue, and the mechanical strength of the obtained recycled carbon fiber is high, but the manufacturing cost is high and it has not been put to practical use. Other dissolution (solvent) methods that have been reported include a method using persulfuric acid generated by electrolysis (Patent Document 3) and a method in which the base resin is dissolved with sulfuric acid or phosphoric acid heated to a high temperature (Patent Documents 4-5). These dissolution methods generally produce recycled carbon fibers with high mechanical strength, but because the base resin of the CFRP is completely removed, only cotton-like or wool-like fibers are obtained, which has the disadvantage of limiting applications.
[0006] The applicant of the present application also developed a manufacturing method in which uncured prepregs, which are discarded in large quantities from aircraft component manufacturers and carbon fiber manufacturers, are used as raw materials to chemically decompose the base epoxy resin with nitric acid, and then the base resin is removed with an alkaline aqueous solution, resulting in an invention (Patent Document 6) in which strength equal to or greater than that of virgin carbon fiber is obtained. However, as with other dissolution methods, only cotton-like or wool-like fibers are obtained, and the use of the resulting fiber is limited to nonwoven fabrics and the like.
[0007] Carbon fiber products include short fibers of around 6 mm called cut fiber or chopped strands, which are used in large quantities to improve the strength of thermoplastic resins. Cut fiber is produced by bundling continuous carbon fibers with a bundling agent and then cutting them to a certain length. The cut fiber obtained from continuous fibers is sufficiently bundling so there is no fraying of the fibers, and when it is mixed with thermoplastic resin in an extruder or fed into a feeder called a side feeder, it is fed stably and smoothly without clogging.
[0008] On the other hand, in the case of recycled carbon fiber, the carbon fiber recycled by the dissolution (solvent) method is in a cotton-like state, so cut fibers cannot be obtained, and cut fibers have mainly been supplied by manufacturers using the pyrolysis method. However, cut fibers obtained by the pyrolysis method are recycled at high temperatures of 400 to 600°C, which significantly reduces the strength of the carbon fibers contained therein. In addition, it is necessary to leave the base resin in order to maintain the cohesion, but the base resin is carbonized at high temperatures and has weak cohesion, and the obtained cut fibers have fraying and a significant decrease in bulk density, which is an indicator of side feedability. Furthermore, 15 to 20% of the carbonized base resin remains, so satisfactory quality is not obtained. Against this background, there was a strong demand for high-quality cut fibers made by the dissolution (solvent) method. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2013-064219 A (Patent 5347056) [Patent Document 2] JP 2005-255835 A (Patent 4686991) [Patent Document 3] Patent Application No. 2016-062004 (Patent 6669354) [Patent Document 4] JP 2020-050704 A [Patent Document 5] Patent Publication No. 2022-102186 [Patent Document 6] JP 2023-040186 A Summary of the Invention [Problem to be solved by the invention]
[0010] Therefore, the object of the present invention is to provide cut fibers made of recycled carbon fibers at low cost without deteriorating the carbon fibers from carbon fiber reinforced plastics (CFRP). In order to avoid confusion, the terms recycled carbon fiber and cut fiber are defined below.
[0011] recycled carbon fiber; Carbon fibers recovered from CFRP using various recycled carbon manufacturing methods. Depending on the manufacturing method, the performance of the carbon fibers and the amount of remaining resin in the base material (resin residue amount) vary, but they can be used as cut fibers as they are. This does not mean that it can be used.
[0012] Cut fiber; Recycled carbon fiber used when making resin composites by extrusion molding, etc. Generally, it is cut to a length of 3 to 12 mm, but 6 mm is the most common. When manufacturing recycled carbon fiber, part of the base resin is often left as a binder, but a separate binder may also be used to strengthen the binding. It is necessary that it does not get stuck or clogged in the feed machine or feed pipe. [Means for solving the problem]
[0013] After much investigation, the inventors discovered a method in which the base resin of uncured CFRP prepreg is chemically decomposed using an acidic aqueous solution containing nitric acid to reduce its molecular weight, then heated and melted for use as a binding agent, and the remaining base resin is further removed by heating at a higher temperature to produce high-performance cut fibers, thereby completing the present invention.
[0014] The present invention is as follows. [1] The cut fibers are made from an uncured prepreg of a carbon fiber reinforced resin composition, and the composition contains recycled carbon fibers obtained from the uncured prepreg, and satisfies the following conditions (1) to (4): (1) The content of the residue of the base material resin component excluding the carbon fiber (hereinafter referred to as the resin residue) is in the range of 2% by mass to 12% by mass; (2) When 6 mm long, the bulk density is 0.15 g / cc or more; (3) The average molecular weight of the resin residue excluding the carbon fiber is in the range of 280 to 500; (4) The tensile strength of the carbon fiber retains 95% or more of the tensile strength of the original carbon fiber (virgin carbon fiber) contained in the uncured prepreg, and the tensile modulus of elasticity retains 90% or more of the original carbon fiber. [2] A method for producing bundled carbon fibers, comprising: step (1) of stirring uncured prepreg in an acidic aqueous solution containing nitric acid at a concentration in the range of 1 to 10 M to dissolve a portion of the resin content of the uncured prepreg and obtain a partially fibrous product (hereinafter referred to as cut fiber-like product); and step (2) of heating and baking the cut fiber-like product obtained in step (1) to dissolve a portion of the resin content of the cut fiber-like product and obtain carbon fibers. [3] The method for producing bundled carbon fibers described in [2], in which uncured prepreg cut into fiber lengths of less than 50 mm in step (1) described in [2] is stirred in a reaction tank containing an acidic aqueous solution with a unidirectional rotation or swirling liquid flow, and reacted in a stirring region with a stirring Reynolds number of 1000 or more to obtain a cut fiber-like material, is obtained. [4] A method for producing bundled carbon fibers as described in [2], in which uncured prepregs of 50 mm or more are moved in a certain direction within a pipe containing an acidic aqueous solution, or an acidic aqueous solution is made to flow in a certain direction counter to the fixed uncured prepregs, and reacted at a flow rate in a cylinder with a Reynolds number of 10 or more to obtain cut fibers. [5] The method for producing bundled carbon fibers according to any one of [2] to [4], wherein in step (2) described in [1], the cut fiber-like material obtained in step (1) is subjected to a first-stage heat treatment in the range of 120 to 300°C to volatilize and melt the chemically decomposed resin residue to bundle the recycled carbon fibers, and then is subjected to a second-stage heat treatment in the range of 380 to 520°C to further reduce the amount of the chemically decomposed resin residue, thereby obtaining cut fibers. [6] A method for producing a carbon fiber reinforced resin composition, comprising: obtaining cut fibers or bundled carbon fibers by the method according to any one of [1] to [5]; and producing a carbon fiber reinforced resin composition using the obtained cut fibers or bundled carbon fibers. [7] The carbon fiber reinforced resin composition is a resin composition containing carbon fiber and a thermoplastic resin and / or a thermosetting resin, and is a carbon fiber reinforced resin composition consisting of 5 to 95 mass% of (A) carbon fiber and 5 to 95 mass% of (B) thermoplastic resin and / or thermosetting resin, where the total amount of (A) recycled carbon fiber and (B) thermoplastic resin and / or thermosetting resin is 100 mass%, in accordance with the manufacturing method described in [6]. [8] The manufacturing method according to [7], wherein the thermoplastic resin is at least one selected from the group consisting of polyolefin resins, polyamide resins, styrene resins, polycarbonate resins, polyester resins, polyphenylene ether resins, polyphenylene sulfide resins, polyacetal resins, acrylic resins, and polyvinyl chloride resins. [9] The manufacturing method according to [7], wherein the thermosetting resin is at least one selected from the group consisting of epoxy resins, phenolic resins, melamine resins, urea resins, diallyl phthalate resins, and unsaturated polyester resins. Effect of the Invention
[0015] According to the present invention, by using high-performance cut fibers of recycled carbon fibers having properties not previously available, it is possible to obtain a resin composition having excellent mechanical properties at low cost. [Brief description of the drawings]
[0016] [Figure 1] Photographs of cut recycled carbon fiber fibers obtained by the present invention (left) and cut virgin carbon fiber fibers (Toray Industries, TV014-006 (base carbon fiber T700)) (right) are shown. [Diagram 2] The photographs of the cut fiber-like material obtained by the present invention after the nitric acid reaction are shown in Fig. 1. The right photo is an enlarged photograph of the same. [Diagram 3] The diagram below shows how to use cut fiber for injection molding. The cut fiber is fed into the twin-screw extruder midway (side feed). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] [Cut fiber made from recycled carbon fibers] The cut fiber of the present invention is produced, for example, by the production method of the present invention described below, and satisfies the following conditions (1) to (4). (1) The content of the residue of the base material resin component excluding the carbon fiber (hereinafter referred to as the resin residue) is in the range of 2% by mass to 12% by mass; (2) When 6 mm long, the bulk density is 0.15 g / cc or more; (3) The average molecular weight of the resin residue excluding the carbon fiber is in the range of 280 to 500; (4) The tensile strength of the carbon fiber retains 95% or more of the tensile strength of the original carbon fiber (virgin carbon fiber) contained in the uncured prepreg, and the tensile modulus of elasticity retains 90% or more of the original carbon fiber.
[0018] In the present invention, the residue of the base resin component in the raw material uncured prepreg is used as a binder to maintain the bond, but this residue is a resin obtained by chemically decomposing the epoxy resin in an acidic aqueous solution containing nitric acid, and is different from the carbonized resin residue generated by the thermal decomposition method. The amount of resin residue affects the degree of bonding, and also affects the mechanical strength when added to a thermoplastic resin or a thermosetting resin to obtain a composite material.
[0019] When carbon fiber is mixed with a thermoplastic resin, a resin processing machine such as a twin-screw extruder is used, and carbon fiber is supplied from the middle of the processing machine by an automatic feeder or the like. If the bundling is weak, the bundling will come loose during feeding, causing a problem of clogging the feeder. If the amount of resin residue is less than 2%, the carbon fiber cannot be sufficiently bound, so the bundling will come loose and clog the feeder. On the other hand, if the amount of resin residue exceeds 12% by weight, the strength will decrease when made into a resin composite material, and the desired strength will not be obtained. The amount of resin residue is preferably 3% by weight to 10% by weight, more preferably 4% by weight to 8% by weight. In addition, within these ranges of the amount of resin residue, commercially available binders and surface treatment agents can be used in appropriate amounts according to the purpose.
[0020] For the same reason, the bulk density affects the feeding properties of carbon fibers. If the bulk density is low, the feeding speed decreases and the feeding machine is clogged. The bulk density depends on the fiber length and the diameter of the carbon fibers, but based on recycled carbon fibers obtained by cutting prepregs to a length of 6 mm, the bulk density must be 0.15 g / cc or more. If the bulk density is less than 0.15 g / cc, not only cannot be fed stably, but when a wood composite is made, the mechanical strength is insufficient or varies. The preferred range of bulk density is 0.20 g / cc or more, more preferably 0.25 g / cc or more.
[0021] In this invention, the base resin of CFRP is chemically decomposed with an acidic aqueous solution containing nitric acid, and the resin residue is used to bind the CFRP. The main components of the decomposed resin are nitrophenols, in which nitro groups derived from nitric acid are added to the aromatic rings of epoxy resin, but the low molecular weight components include dinitrophenol (molecular weight 184), trinitrophenol (also known as picric acid: molecular weight 229), and trinitroaniline (also known as picramide: molecular weight 228), which cannot be effectively used for binding and must be thoroughly removed in a later process due to their strong acidity.
[0022] These low molecular weight components remain dissolved or precipitated in the acidic aqueous solution, but the remaining decomposition products remain attached to the carbon fiber surface. When these are dissolved in an organic solvent such as N-methylpyrrolidone and the solution is analyzed by high performance liquid chromatography or mass spectrometry, many peaks are observed. Among these, peaks with a molecular weight of less than 280 are volatile components and are partially vaporized by heating at 220°C or less, while decomposition products with a molecular weight of 280 to 500 are difficult to vaporize at 220°C or more, but show adhesiveness when heated, so they can be used as binding materials and can be removed by thermal decomposition at 400°C or more. In addition, if there is a large amount of resin residue components with a molecular weight of 500 or more, it becomes difficult to unravel the binding when kneaded with a thermoplastic resin, so the average molecular weight of the resin residue components is appropriate to be 280 to 500.
[0023] Various properties of recycled carbon fibers are often required to be equivalent to those of virgin carbon fibers. Although the properties required of carbon fibers vary widely depending on the application, the basic property of carbon fibers is mechanical strength. In the present invention, recycled carbon fibers having higher mechanical strength than recycled carbon fibers obtained by competing methods such as pyrolysis are obtained, but the recycled carbon fibers in the cut fibers are also required to have appropriate strength in order to be applicable to various applications.
[0024] The manufacturing method of the present invention provides recycled carbon fibers having high strength, but in order to be considered almost equivalent to virgin products and to be reused, it is necessary that the tensile strength of the recycled carbon fiber monofilament is 95% or more of the tensile strength of the original virgin carbon fiber monofilament (single fiber) contained in the raw material uncured prepreg, and the tensile modulus is 90% or more of the tensile modulus of the original carbon fiber monofilament. If the tensile strength of the recycled carbon fiber monofilament is less than 95% of the tensile strength of the original carbon fiber monofilament, the cut fiber containing resin residues and the like is not considered to have the same performance as the cut fiber made of virgin carbon fiber. Similarly, if the tensile modulus of the recycled carbon fiber is 90% or less of the tensile modulus of the original virgin carbon fiber, it is not considered to have the same performance as the virgin cut fiber, and replacement or reuse becomes difficult. The preferred tensile strength of the recycled carbon fiber monofilament is 97% or more, more preferably 99% or more, and the preferred tensile modulus is 93% or more, more preferably 95% or more.
[0025] [Method of manufacturing cut fibers made from recycled carbon fibers] The cut fiber manufacturing method of the present invention uses uncured prepreg of CFRP as a raw material and includes step (1) of stirring the uncured prepreg in an acidic aqueous solution containing nitric acid to dissolve at least a portion of the resin content of the CFRP to obtain a cut fiber-like material, and step (2) of heating and baking the cut fiber-like material obtained in step (1) to remove a portion of the resin content of the cut fiber-like material to obtain carbon fibers.
[0026] Process (1) The uncured CFRP prepreg is stirred in an acidic aqueous solution to dissolve at least a portion of the resin content of the CFRP. Uncured CFRP prepreg is waste material or defective products generated during the manufacturing process of CFRP products, which are usually incinerated or landfilled.
[0027] The shape and dimensions of the CFRP to be subjected to step (1) are not particularly limited, but from the viewpoints of obtaining cut fibers, ease of dissolving the resin content of the CFRP, and ease of stirring and moving in the solution, it is preferable to cut the CFRP to a certain size or less in advance. However, if the size is made too small, the size (length) of the carbon fibers contained therein will be reduced, so it is preferable to appropriately determine the size taking into consideration the size of the carbon fibers to be recovered. In practice, a length of 3 mm to 25 mm is often used, but it is not intended to be limited to this range.
[0028] The acidic aqueous solution used in step (1) contains nitric acid at a concentration in the range of 1 to 10 M, and can also contain inorganic acids such as sulfuric acid, hydrochloric acid, and phosphoric acid, organic acids such as formic acid, acetic acid, and citric acid, and water-soluble peroxides such as hydrogen peroxide and organic hydroperoxides. The acidic aqueous solution can be appropriately selected taking into consideration the type of CFRP to be treated and the treatment conditions (mainly the treatment temperature and time).
[0029] Uncured prepreg cut into pieces less than 50 mm is stirred in a reaction tank containing an acidic aqueous solution. Cut fibers of a desirable shape can be obtained by stirring in the transition region or turbulent region where the stirring Reynolds number is 1000 or more. In addition, stirring conditions that produce a high rotation speed and a rotating flow (swirling flow) are preferred because they result in uniform cut fiber shapes. The shape and diameter of the blades used for stirring are appropriately selected depending on the stirring conditions. The stirring Reynolds number is defined by the following formula.
[0030]
number
[0031] Uncured prepreg cut to a length of 50 mm or more tends to get tangled around the agitator blades when agitated, so it is treated by circulating it in a cylindrical pipe of an appropriate size containing an acidic aqueous solution, or by fixing it in the pipe and running the acidic aqueous solution through it. Treating it at a flow rate that results in an in-cylinder Reynolds number of 10 or more will yield cut fiber-like products of a desirable shape. The in-cylinder Reynolds number is defined by the following formula:
[0032]
number
[0033] The temperature of the acidic aqueous solution can be in the range of 40 to 100°C, and is preferably in the range of 50 to 95°C, and more preferably in the range of 60 to 90°C, because this is particularly effective in terms of resin solubility.
[0034] The base epoxy resin of the uncured CFRP prepreg is chemically decomposed in an acidic aqueous solution in a short time, and becomes a low molecular weight material. In step (1), it is preferable to chemically decompose the base resin of the uncured prepreg by stirring in the acidic aqueous solution until a part of the uncured prepreg becomes a cut fiber-like material as shown in Figure 1. If the stirring conditions and the reaction conditions of the acidic aqueous solution are appropriate, the base resin of the uncured CFRP prepreg becomes sticky as it chemically decomposes, and the CFRP sticks to itself and grows into a cut fiber-like material. In addition, part of it dissolves into the acidic aqueous solution as it chemically decomposes. If the base resin of the CFRP is chemically decomposed, cut fibers can be obtained by heat treatment in step (2).
[0035] The amount of the resin that is partially chemically decomposed and eluted into the acidic aqueous solution in step (1) can be, for example, in the range of 2 to 98, preferably in the range of 3 to 95, and more preferably in the range of 5 to 95, when the mass of the CFRP before immersion is taken as 100. The remainder remains on the carbon fiber surface as a resin residue. Since the resin residue contains an acidic aqueous solution or an acidic resin component that has been chemically decomposed, it is preferable to wash the resin with water and then neutralize the resin at an appropriate concentration using an alkaline aqueous solution or a basic aqueous solution before proceeding to step (2). The basic aqueous solution is an aqueous solution with a pH (hydrogen ion exponent) of more than 7.
[0036] The alkaline aqueous solution used for neutralization may be, for example, an alkali such as hydroxide, carbonate, hydrogen carbonate, sulfate, sulfite, or nitrate of an alkali metal, or an alkali earth metal such as hydroxide, carbonate, hydrogen carbonate, sulfate, sulfite, or nitrate. The base of the basic aqueous solution may be, for example, an amine compound, an alkyl acid salt containing an aliphatic alkyl acid structure or an aromatic structure, or a salt containing a polyhydric alcohol alkylene oxide compound. Examples of the alkali metal include lithium, sodium, or potassium, and examples of the alkaline earth metal include beryllium, magnesium, or calcium. Examples of the base used in the basic aqueous solution may include amines such as ammonia, monomethylamine, diethylamine, monoethanolamine, or diethanolamine. Examples of the carboxylic acid having an aliphatic alkyl group structure include lauric acid, myristic acid, palmitic acid, stearic acid, or oleic acid, and examples of the alkyl acid containing an aromatic structure include dodecylbenzenesulfonic acid. Examples of the polyhydric alcohol alkylene oxide compound include polyoxyethylene alkyl ether and polyoxypropylene ether. These are appropriately selected taking into consideration solubility in water, ease of availability, and the like.
[0037] The concentration of these alkaline or basic aqueous solutions can be appropriately determined taking into consideration the properties of the compound to be dissolved, as well as the dissolution temperature and dissolution time, and is used at, for example, 0.01% by weight to 10% by weight.
[0038] Process (2) After washing the cut fiber-like material obtained in step (1), the cut fiber is heated and baked in two stages in step (2) to obtain cut fibers. The first stage of heating is performed at a temperature in the range of 120 to 300°C to remove remaining moisture and volatile components. At this time, the low-melting-point resin residue contained in the cut fiber-like material binds the carbon fibers. The second stage of heating is performed at a temperature in the range of 350°C or higher and 520°C or lower, and the baking time is in the range of 15 to 120 minutes. If the baking temperature is less than 350°C, the amount of resin residue cannot be reduced to the desired amount, and if the baking is performed at 520°C or higher, the carbon fiber deteriorates and the strength decreases. If the baking time is less than 15 minutes, the amount of resin residue cannot be reduced to the desired amount, and if the baking is performed for 120 minutes or more, the carbon fiber deteriorates and the strength decreases. The baking temperature and baking time are applied in combination so that the amount of resin residue and the single yarn strength reach the desired values.
[0039] For the heating and calcining of the cut fiber-like material, a batch type hot air drying oven, a continuous type hot air dryer, a batch type rotary kiln, a continuous type rotary kiln, etc. may be used, and a combination of these may also be used.
[0040] The cut fibers of the recycled carbon fibers obtained in steps (1) and (2) are washed and dried as necessary, and then recovered. A dehydrator such as a centrifuge is used to dehydrate the washed cut fibers. A pressure press, a screw press, a belt press, a pressure filter, etc. are used under conditions that do not destroy the shape of the cut fibers. These machines can be used alone or in combination.
[0041] The cut fibers of recycled carbon fibers produced by the method of the present invention can be added to thermoplastic resins to form pellets or sheets, and can be added to thermosetting resins to obtain press-molded products. They can also be dispersed in adhesives, pressure sensitive adhesives, inks, paints, etc. and applied to them.
[0042] [Method of producing carbon fiber reinforced resin composition] The method for producing a carbon fiber reinforced resin composition of the present invention includes a step of producing carbon fibers by the above-described method of the present invention, and a step of producing a carbon fiber reinforced resin composition using the obtained carbon fibers.
[0043] The process for producing cut fibers of recycled carbon fibers is as described above. Furthermore, the cut fibers obtained here are used to produce a carbon fiber reinforced resin composition. The carbon fiber reinforced resin composition using cut fibers can be produced by any known method, such as a method of kneading the cut fibers with resin using a single-screw or twin-screw extruder, a plastomill, a pressure kneader, or the like to produce pellets for injection molding, or a method of kneading the resin with the cut fibers and then molding them into a sheet using a sheet extruder, a press, or the like.
[0044] The cut fibers produced by the method of the present invention can be further bound by using a commercially available bundling material. Depending on the type of resin to be composited, the bundling material may be a polyurethane, epoxy, epoxyurethane, modified acrylic, modified olefin, phenol, special resin, or water-soluble polymer. Examples of water-soluble polymers include oxazoline polymers and pyrrolidone polymers.
[0045] The carbon fiber reinforced resin composition produced may be, for example, a resin composition containing carbon fiber and a thermoplastic resin and / or a thermosetting resin, and may be a carbon fiber reinforced resin composition consisting of 5 to 95 mass % of (A) carbon fiber and 5 to 95 mass % of (B) thermoplastic resin and / or thermosetting resin, where the total amount of (A) carbon fiber and (B) thermoplastic resin and / or thermosetting resin is 100 mass %.
[0046] The cut fibers obtained in the present invention have excellent mechanical strength due to the above-mentioned manufacturing method of the present invention, and furthermore, the inventors have found that a carbon fiber reinforced resin composition obtained using the cut fibers of the present invention has sufficient mechanical strength for practical use and can be used as an excellent structural material. That is, it has been found that by mixing the cut fibers of the present invention with a thermoplastic resin and / or a thermosetting resin, a carbon fiber reinforced resin composition that has excellent mechanical strength and practical properties and is suitable for various applications and structural materials can be obtained.
[0047] A preferred embodiment of the carbon fiber reinforced resin composition of the present invention is a carbon fiber reinforced thermoplastic resin composition, and the carbon fiber reinforced thermoplastic resin composition is, for example, a thermoplastic resin that is at least one thermoplastic resin selected from the group consisting of polypropylene resin, polyamide resin, styrene resin, polycarbonate resin, polyester resin, polyphenylene ether resin, polyphenylene sulfide resin, polyacetal resin, acrylic resin, and vinyl chloride resin.
[0048] Representative examples of polyolefin resins include homopolymers or copolymers of α-olefins such as ethylene, propylene, butene-1, 3-methylbutene-1, 3-methylpentene-1, 4-methylpentene-1, etc., or copolymers of these with unsaturated monomers copolymerizable therewith. Representative examples include polyethylenes such as high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear low-density polyethylene, ultra-high molecular weight polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, ethylene-octene-1 copolymer, etc., ethylenes such as atactic polypropylene, syndiotactic polypropylene, isotactic polypropylene, propylene-ethylene block copolymer or random copolymer, polymethylpentene-1, etc.
[0049] The polyamide resin is not particularly limited as long as it has an amide bond in the repeating structure of the polymer. The polyamide resin is preferably a thermoplastic polyamide resin, and examples of the polyamide resin include homopolyamides and copolyamides obtained by polymerizing monomers such as lactams, aminocarboxylic acids, and / or diamines and dicarboxylic acids, and mixtures thereof. Specific examples include polycaproamide (nylon 6), polyhexamethylene adipamide (nylon 66), polytetramethylene adipamide (nylon 46), polyhexamethylene sebacamide (nylon 610), polyhexamethylene dodecamide (nylon 612), polyundecamethylene adipamide (nylon 116), polybis(4-aminocyclohexyl)methandecamide (nylon PACM12), polybis(3-methyl-4-aminocyclohexyl)methandecamide (nylon dimethyl PACM12), polynonamethylene terephthalamide (nylon 9T), polydecamethylene terephthalamide (nylon 10T), polyundecamethylene terephthalamide (nylon 11T), polyunde Examples of the thermoplastic polyamide resin include camethylene hexahydroterephthalamide (nylon 11T(H)), polyundecamide (nylon 11), polydodecamide (nylon 12), polytrimethylhexamethylene terephthalamide (nylon TMDT), polyhexamethylene terephthalamide (nylon 6T), polyhexamethylene isophthalamide (nylon 6I), polymetaxylylene adipamide (nylon MXD6), and copolymers and mixtures thereof. Among them, from the viewpoint of moldability and surface appearance, nylon 6, nylon 66, nylon MXD6, nylon 9T, nylon 10T, and copolymer polyamides thereof are preferred, nylon 9T, nylon 10T, and nylon MXD6 are more preferred, and nylon 9T is particularly preferred. Furthermore, it is practically preferable to use these thermoplastic polyamide resins as a mixture depending on the required properties such as impact resistance and moldability.
[0050] Examples of polycarbonate resins include 4,4-dihydroxydiarylalkane polycarbonates, etc. Specific examples include bisphenol A polycarbonate (PC), modified bisphenol A polycarbonate, and flame-retardant bisphenol A polycarbonate.
[0051] Examples of the styrene-based resin include homopolymers of styrene, α-methylstyrene, etc., copolymers thereof, and copolymers of these with unsaturated monomers that can be copolymerized with these. Specific examples include general-purpose polystyrene (GPPS), high impact polystyrene (HIPS), heat-resistant polystyrene (for example, α-methylstyrene polymer or copolymer), acrylonitrile-butadiene-styrene copolymer (ABS), acrylonitrile-butadiene-styrene-α-methylstyrene copolymer (α-methylstyrene-based heat-resistant ABS), acrylonitrile-butadiene-styrene-phenylmaleimide copolymer (phenylmaleimide-based heat-resistant ABS), acrylonitrile-styrene copolymer (AS), acrylonitrile 50-chlorinated polystyrene-styrene copolymer (ACS), acrylonitrile-ethylene propylene rubber-styrene copolymer (AES), acrylic rubber-acrylonitrile-styrene copolymer (AAS), syndiotactic polystyrene (SPS), etc. The styrene-based resin may also be a polymer blend.
[0052] Examples of polyester resins include those obtained by polycondensation of aromatic dicarboxylic acids with alkylene glycols such as ethylene glycol, propylene glycol, butylene glycol, etc. Specific examples include polyethylene terephthalate (PET), polypropylene terephthalate (PPT), polybutylene terephthalate (PBT), etc.
[0053] Examples of polyphenylene ether resins (PPE) include homopolymers such as poly(2,6-dimethyl-1,4-phenylene) ether and poly(2-methyl-6-ethyl-1,4-phenylene) ether, and these may also be modified with a styrene-based resin.
[0054] Polyphenylene sulfide resin is a highly heat-resistant crystalline polymer with a structure in which benzene and sulfur are alternately bonded, and is often mixed with fillers such as glass fiber, carbon fiber, silica, and talc rather than being used alone.
[0055] Examples of polyacetal resins (POM) include homopolymer polyoxymethylene and formaldehyde-ethylene oxide copolymers obtained from trioxane and ethylene oxide.
[0056] Examples of acrylic resins include homopolymers of methacrylic acid esters and acrylic acid esters, copolymers thereof, and copolymers of these with other copolymerizable unsaturated monomers. Examples of methacrylic acid ester and acrylic acid ester monomers include methacrylic acid, methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, and butyl acrylate. A representative example is methacrylic resin (PMMA). These thermoplastic resins may be used alone or in combination of two or more kinds.
[0057] Examples of polyvinyl chloride resins include vinyl chloride homopolymers and copolymers of vinyl chloride and unsaturated monomers copolymerizable therewith. Specific examples include vinyl chloride-acrylic acid ester copolymers, vinyl chloride-methacrylic acid ester copolymers, vinyl chloride-ethylene copolymers, vinyl chloride-propylene copolymers, vinyl chloride-vinyl acetate copolymers, vinyl chloride-vinylidene chloride copolymers, etc. Also usable are polyvinyl chloride resins that have been chlorinated to increase the chlorine content.
[0058] Another embodiment of the carbon fiber reinforced resin composition of the present invention is a carbon fiber reinforced thermosetting resin composition, and the thermosetting resin may be, for example, at least one selected from the group consisting of epoxy resin, phenol resin, melamine resin, urea resin, diallyl phthalate resin, and unsaturated polyester resin. The carbon fiber of the present invention disperses well in water, and by papermaking (papermaking) at an appropriate concentration, a wet nonwoven fabric, specifically a thin carbon fiber sheet or carbon fiber paper, can be obtained. The obtained carbon fiber nonwoven fabric is mixed with or impregnated with a thermosetting resin before curing, and then cured by heat or the like, to obtain a carbon fiber reinforced thermosetting resin composition having excellent mechanical properties not previously available.
[0059] In addition to the thermoplastic resin, the carbon fiber reinforced resin composition of the present invention may contain, depending on the intended use, fillers such as glass fiber, silica, and talc, and various flame retardants such as phosphorus compounds, bromine compounds, antimony compounds, metal oxides, and nitrogen compounds. In addition to these additives, various additives such as flow improvers for molten resins, moldability improvers, impact resistance improvers such as rubber-based fillers and thermoplastic elastomers, and matte materials that impart a matte effect to the surface, which are added to ordinary thermoplastic resin compositions, may be added in appropriate amounts. EXAMPLES
[0060] The present invention will be described in more detail below with reference to examples. However, the examples are merely illustrative of the present invention and are not intended to limit the present invention.
[0061] Example 1
[0062] Process (1) 120 kg of concentrated nitric acid diluted to 6M was placed in a 300 L stainless steel reaction vessel, the jacket temperature of the reaction vessel was heated to 60-70 ° C, and 10 parts by mass of uncured prepreg containing 65% Toray T700 cut into 6 mm lengths was added to 100 parts by mass of nitric acid while stirring. While keeping the temperature inside the reaction vessel at 70-80 ° C, stirring was performed for 1 hour with a constant swirling flow at a rotation speed of 300 rpm using a propeller stirring blade with a diameter of 25 cm. The reactant was removed from the nitric acid and immediately put into water to obtain recycled carbon fiber in the form of cut fibers in which part of the epoxy resin had dissolved. The stirring Reynolds number was about 240,000.
[0063] Process (2) Next, the cut fiber-like recycled carbon fiber was washed with hot water at 40°C, and then mixed with a 0.5% by weight aqueous sodium hydroxide solution and a 0.5% by weight aqueous monoethanolamine solution in a weight ratio of 1:1, and neutralized by stirring at 40°C for 30 minutes. After that, it was dehydrated in a centrifugal dehydrator, heated at 140°C for 1 hour (first stage heating), and then further heated at 450°C for 60 minutes (second stage heating) to obtain cut fiber a-1. Cut fibers a-2 to a-5 were obtained by changing the conditions of steps (1) and (2) in the same manner as cut fiber a-1.
[0064] For the obtained cut fibers, a weighed sample was heated and baked at 530°C for 1 hour, and the weight of the remaining carbon fiber alone and the weight of the original sample were weighed. The difference between the weights was used to calculate the amount of resin residue in the cut fibers according to the following formula. Resin residue amount = resin amount in cut fiber ÷ (carbon fiber amount + resin amount in cut fiber)
[0065] In addition, 100 cc of cut fibers was filled into a 100 cc graduated cylinder, and the resulting weight was divided by 100 to determine the bulk density. The average molecular weight of the resin residue was determined based on a chart obtained by high performance liquid chromatography manufactured by Waters.
[0066] The tensile strength and tensile modulus of the single yarn were measured as follows. In step (1) of the acidic aqueous solution process, 15 cm long uncured prepreg was reacted together with uncured prepreg waste material broken into 6 mm lengths, and the resin residue adhering to the obtained yarn was completely removed with N-methylpyrrolidone, an organic solvent, and the yarn was measured using a Shimadzu EZ-L testing machine in accordance with JIS-R7606 (carbon fiber - single fiber tensile property test method). The cross-sectional area of each carbon fiber was determined by polishing the cross section of the carbon fiber and processing the image using a white light confocal microscope.
[0067] The physical properties of the cut fibers a-1 to a-5 and the conditions of steps (1) and (2) are shown in Table 1. Of these, a-5 is a product obtained by treating the recycled carbon fiber with an aqueous solution of N-vinyloxazoline as a surface treatment agent so that the amount of the solution adhered to the recycled carbon fiber was 2%.
[0068] [Table 1]
[0069] As can be seen from Table 1, the cut fiber obtained by the manufacturing method claimed in the present invention has the same bulk density, mechanical strength, and feedability as the original carbon fiber, T700 cut fiber (shown in Table 2).
[0070] Comparative Example
[0071] As in Example 1, the physical properties of cut fibers b-1 to b-4 obtained by changing the production conditions in steps (1) and (2), cut fiber (b-5) obtained by heating and sintering an uncured prepreg containing T700, and cut fiber (b-6) made of T700 virgin carbon fiber corresponding to the carbon fiber contained in the uncured prepreg, as well as the results of steps (1) and (2) are shown in Table 2.
[0072] [Table 2]
[0073] In Table 2, for b-1, the second heat treatment temperature in step (2) is lower than the range of claim 5, and as a result, the resin residue of the cut fibers falls outside the range of the claims. In b-2, the second heat treatment temperature in step (2) is higher than the range of claim 5, and as a result, the amount of resin residue, bulk density, tensile strength and tensile modulus of the single fiber of the obtained cut fiber are outside the range of the present invention. Also, the feedability is poor. In b-3, the stirring conditions in the acidic aqueous solution in step (1) are outside the scope of the present invention, and under these conditions the reaction product obtained blocks and becomes lumpy, making it impossible to obtain cut fibers of a good shape. In addition, the acidic aqueous solution does not penetrate into the inside of the blocked product produced. As a result, the amount of resin residue in the obtained product is outside the scope of claim 1 of the present invention in terms of bulk density, and the feedability is poor. In b-4, the first-stage heat treatment temperature in step (2) is lower than the scope of claim 5 of the present invention, so the average molecular weight of the resin residue remaining in the cut fibers is outside the scope of claim 1, and the amount of resin residue is outside the scope of claim 1.
[0074] The a-1 to a-5 and cut fibers of T700 virgin carbon fiber obtained in Example 1, and the b-1 to b-6 obtained in Comparative Example were blended with each thermoplastic resin and kneaded in a twin-screw extruder to prepare pellets. The pellets obtained were molded in an injection molding machine to prepare test pieces, and the tensile strength, tensile modulus, flexural strength, and flexural modulus were measured.
[0075] The twin-screw extruder used for kneading was a co-rotating twin-screw extruder ZE40A (φ=42, L / D=38) manufactured by Berstorff, and the side feeder used was a gravimetric weighing single-screw feeder KS60 manufactured by K-Tron. The results are shown in Table 3.
[0076] [Table 3]
[0077] The cut fibers obtained according to the present invention exhibited feedability equivalent to that of virgin carbon fibers, and thermoplastic resin compositions prepared using these exhibited mechanical properties equivalent to that of virgin carbon fibers.
[0078] In this method, the base resin of CFRP can be decomposed into smaller molecules by chemical decomposition, and these can be melted and effectively used as a binder, making it possible to obtain cut fibers using the dissolution method. In addition, the base resin (resin residue) that has been decomposed into smaller molecules can be removed at a lower temperature than in the thermal decomposition method, so there is less damage to the carbon fiber and the quality is equivalent to that of virgin products. It is now possible to obtain cut fibers. [Industrial Applicability]
[0079] The present invention is useful in the technical field relating to carbon fiber reinforced resin compositions.
Claims
1. The present invention relates to a cut fiber composition that uses an uncured prepreg of a carbon fiber reinforced resin composition as a raw material, the cut fiber composition containing recycled carbon fibers obtained from the uncured prepreg satisfies the following conditions (1) to (4): (1) The content of the residue of the base resin component excluding the carbon fiber (hereinafter referred to as the resin residue) is in the range of 2% by mass to 12% by mass; (2) A bulk density of 0.15 g / cc or more when 6 mm long; (3) The average molecular weight of the resin residue excluding the carbon fiber is in the range of 280 to 500; (4) The tensile strength of the carbon fiber retains 95% or more of the tensile strength of the original carbon fiber (virgin carbon fiber) contained in the uncured prepreg, and the tensile modulus of elasticity retains 90% or more of the original carbon fiber.
2. The method for producing bundled carbon fibers includes the steps of: (1) immersing an uncured prepreg in an acidic aqueous solution containing nitric acid at a concentration in the range of 1 to 10 M, thereby dissolving a portion of the resin content of the uncured prepreg to obtain a cut fiber-like product (hereinafter referred to as a cut fiber-like product); and (2) heat-treating the cut fiber-like product obtained in the step (1) to remove a portion of the resin content of the cut fiber-like product to obtain carbon fibers.
3. 3. The method for producing bundled carbon fibers according to claim 2, wherein in step (1), the uncured prepreg cut into fiber lengths of less than 50 mm is agitated in a reaction tank containing an acidic aqueous solution with a unidirectional rotation or swirling liquid flow, and reacted in a stirring region having a stirring Reynolds number of 1000 or more, to obtain a cut fiber-like material.
4. 3. The method for producing bundled carbon fibers according to claim 2, wherein in step (1), uncured prepreg having a fiber length of 50 mm or more is moved in a fixed direction in a pipe containing an acidic aqueous solution, or an acidic aqueous solution is caused to flow in a fixed direction counter to the uncured prepreg fixed in the pipe, and a cut fiber-like material is obtained by reacting the uncured prepreg at a flow rate in the tube having a Reynolds number of 10 or more.
5. The method for producing bundled carbon fibers according to claim 2, wherein in step (2), the cut fiber-like material obtained in step (1) is subjected to a first-stage heat treatment in the range of 120°C to 300°C to volatilize and melt the chemically decomposed resin residue to bundle the recycled carbon fibers, and then is subjected to a second-stage heat treatment in the range of 380°C to 520°C to further reduce the amount of the chemically decomposed resin residue, thereby obtaining cut fibers.
6. 3. A method for producing a carbon fiber reinforced resin composition, comprising the steps of obtaining cut fibers or bundled carbon fibers by the method according to claim 1 or 2, and producing a carbon fiber reinforced resin composition using the obtained cut fibers or bundled carbon fibers.
7. The carbon fiber reinforced resin composition is a resin composition containing carbon fiber and a thermoplastic resin and / or a thermosetting resin, and is a carbon fiber reinforced resin composition consisting of 5 to 95 mass% of (A) carbon fiber and 5 to 95 mass% of (B) thermoplastic resin and / or thermosetting resin, where the total amount of (A) recycled carbon fiber and (B) thermoplastic resin and / or thermosetting resin is 100 mass%. The production method according to claim 6.
8. The method according to claim 7, wherein the thermoplastic resin is at least one selected from the group consisting of polyolefin resins, polyamide resins, styrene resins, polycarbonate resins, polyester resins, polyphenylene ether resins, polyphenylene sulfide resins, polyacetal resins, acrylic resins, and vinyl chloride resins.
9. 8. The method according to claim 7, wherein the thermosetting resin is at least one selected from the group consisting of epoxy resins, phenolic resins, melamine resins, urea resins, diallyl phthalate resins, and unsaturated polyester resins.
Citation Information
Patent Citations
Heat conveyor
JP1978047056A
Method for separating carbon material / acid anhydride-cured epoxy resin composite
JP2005255835A
Apparatus for producing recycled carbon fiber and method for producing recycled carbon fiber
JP2013064219A
Inspection device, and wave surface aberration correction method
JP2016062004A
Carbon fiber collection method
JP2020050704A
Cited By
Decomposition solution and method for decomposing epoxy resin
JP2025092389A
Decomposition solution and method for decomposing epoxy resin
JP7873709B2
Recycled carbon fiber, carbon fiber roving, woven fabric, prepreg, and method for producing recycled carbon fiber