Photosensitive resin composition, cured film, and semiconductor device

The photosensitive resin composition combines polyimide and polybenzoxazole precursors with thermally crosslinkable compounds and photosensitizers to achieve high heat resistance, sensitivity, and resolution, addressing the limitations of existing technologies for power devices.

JP2024154449APending Publication Date: 2024-10-31TORAY INDUSTRIES INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023068255
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing photosensitive resin compositions for power devices struggle to balance high heat resistance with high sensitivity and resolution, as well as adequate adhesion and chemical resistance, particularly under high temperature and humidity conditions.

Method used

A photosensitive resin composition comprising polyimide, polybenzoxazole, or their precursors, combined with a compound having one or more thermally crosslinkable groups, and a photosensitizer, such as a photoacid generator, to enhance heat resistance and sensitivity while maintaining pattern resolution.

Benefits of technology

The composition achieves high heat resistance, sensitivity, and resolution, with a 5% weight loss temperature above 470°C, and improved adhesion to copper, suitable for power devices under harsh conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154449000037
    Figure 2024154449000037
  • Figure 2024154449000001
    Figure 2024154449000001
  • Figure 2024154449000002
    Figure 2024154449000002
Patent Text Reader

Abstract

To provide a photosensitive resin composition which achieves both high heat resistance and high resolution.SOLUTION: The photosensitive resin composition contains: (A) one or more resins selected from the group consisting of a polyimide, a polyimide precursor, a polybenzoxazole, a polybenzoxazole precursor, and copolymers thereof; (B) a photosensitizer; and (C) a thermal crosslinking group-containing compound. The thermal crosslinking group-containing compound (C) contains (C1) a compound containing one thermal crosslinking group and (C2) a compound containing four or more thermal crosslinking groups.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition, a cured film, and a semiconductor device. [Background technology]

[0002] Polyimide resins, which have excellent heat resistance and mechanical properties, are widely used for the surface protection films of power devices. As power devices become more highly functional, such as withstanding higher voltages, operating at higher frequencies, and at higher temperatures, there are increasing demands for the protection films that remain on the devices as permanent films, in terms of withstanding voltage, volume resistivity, chemical resistance, reliability, and durability.

[0003] For example, various resistances are required, such as sufficient voltage resistance to withstand high voltages, volume resistivity equivalent to that at room temperature even under high temperature and humidity conditions, high volume resistivity that is maintained even after a pressure cooker test, high humidity and heat resistance, etc. Furthermore, strong acid and base aqueous solutions are used to form electrodes for power devices that handle large amounts of electricity, so the protective film also needs to have excellent acid and base resistance.

[0004] As highly reliable resin compositions suitable for such power device devices, there have been proposed a highly heat-resistant resin composition containing a polyamic acid ester of a specific structure with a low linear expansion coefficient (see Patent Document 1), a polybenzoxazole precursor resin composition of a specific structure which has high withstand voltage and high volume resistivity and chemical resistance under high temperature and high humidity conditions, and which maintains these performance properties over a long period of time (see Patent Document 2), a negative-type photosensitive resin composition in which a polyfunctional (meth)acrylate and a low-molecular-weight imide compound having a molecular weight of less than 1000 are applied to a polyamic acid or polybenzoxazole precursor which is a polyimide precursor (see Patent Document 3), and a negative-type photosensitive resin composition containing a polyimide precursor of a specific structure containing two or more polymerizable groups selected from the group consisting of an acid-polymerizable group, a base-polymerizable group, and a radical-polymerizable group, and a specific amount of a photopolymerization initiator (see Patent Document 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2014-15507 A [Patent Document 2] JP 2016-23226 A [Patent Document 3] JP 2017-219850 A [Patent Document 4] JP 2020-24374 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the 5% weight loss temperature of the cured film after 400 hours of pressure cooker testing, which is an index of heat resistance, is low in the technologies described in Patent Documents 1 and 2, and it cannot be said that the technology has sufficient high-temperature reliability for use in power devices. In addition, although the technologies described in Patent Documents 3 and 4 have high high-temperature resistance and adhesion to copper, they have low resolution due to their negative photosensitivity, and it cannot be said that they combine high heat resistance with high resolution.

[0007] In order to solve the above problems, an object of the present invention is to provide a photosensitive resin composition that has both high heat resistance and high sensitivity. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention has the following configuration. That is, the photosensitive resin composition of the present invention is a photosensitive resin composition containing (A) one or more resins selected from the group consisting of polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, and copolymers thereof, (B) a photosensitizer, and (C) a compound having a thermal crosslinking group, wherein the (C) compound having a thermal crosslinking group contains (C1) a compound having one thermal crosslinking group and (C2) a compound having four or more thermal crosslinking groups. Effect of the Invention

[0009] According to the photosensitive resin composition of the present invention, a photosensitive resin composition having both high heat resistance and high sensitivity can be obtained. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view of a semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In the present invention, it has been newly discovered that the combined use of a compound containing one thermal crosslinking group and a compound containing four or more thermal crosslinking groups improves heat resistance and sensitivity, and further, it has been discovered that higher heat resistance can be achieved by specifying the content thereof.

[0012] The photosensitive resin composition of the present invention is a photosensitive resin composition containing (A) one or more resins selected from the group consisting of polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, and copolymers thereof (hereinafter referred to as (A) resin), (B) a photosensitizer, and (C) a compound having a thermal crosslinking group, wherein the (C) compound having a thermal crosslinking group contains (C1) a compound having one thermal crosslinking group and (C2) a compound having four or more thermal crosslinking groups.

[0013] By coexisting the compound having a thermal crosslinking group (C) with the resin (A), the compatibility of the photosensitive resin composition is maintained while crosslinking with the resin or other additive components, and the heat resistance and chemical resistance of the film after thermal curing can be further improved. In addition, by using the compound having a thermal crosslinking group (C), the compound having a thermal crosslinking group (C) reacts with the polymer during thermal curing and is added to the polymer, so that decomposition and vaporization due to heat do not occur in the subsequent process. By using a compound having one thermal crosslinking group (C1), it is possible to reduce the shrinkage of the film during curing and suppress wrinkles that occur in the pattern after curing. By using the compound having four or more thermal crosslinking groups (C2), which crosslinks polymers to improve heat resistance, in combination, it is possible to improve the 5% weight loss temperature after curing, and obtain high heat resistance.

[0014] Here, the 5% weight loss temperature is defined as the temperature at which the weight of the cured film at 200°C is reduced by 5% when the cured film is heated from room temperature to 200°C at 10°C / min using a DTG-60 manufactured by Shimadzu Corporation, heat-treated at 200°C for 10 minutes, and then heated to 500°C at 10°C / min. The 5% weight loss temperature is preferably 470 to 500°C, and the high heat resistance required for power devices can be achieved. The 5% weight loss temperature is more preferably 480 to 500°C.

[0015] In this application, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0016] (C) The compound having a thermal crosslinking group refers to a compound having at least one thermally reactive functional group in the molecule, such as an alkoxymethyl group, a methylol group, an epoxy group, or an oxetanyl group.

[0017] The compound (C1) having one thermal crosslinking group is not particularly limited as long as it has an alkoxymethyl group, a methylol group, an epoxy group, or an oxetanyl group in the molecule, but is preferably a compound having a phenolic hydroxyl group and having one group selected from a methylol group and an alkoxymethyl group, and examples of the compound have the structure shown below.

[0018] [ka]

[0019] A more preferred example is the structure shown in the following general formula (1).

[0020] [ka]

[0021] In the above general formula (1), R 10 R represents an organic group having 1 to 20 carbon atoms, and is preferably an alkyl group having 1 to 4 carbon atoms. If the number of carbon atoms is 20 or less, the shrinkage rate during curing is small, which is preferable. 11 represents an organic group having 1 to 20 carbon atoms and having at least one functional group selected from an alkyl group, a vinyl group, an ester group, an amide group, an ethynyl group, a phenoxy group, a sulfone group, a thioether group, a phenyl group, a fluoroalkyl group, and a ketone group, a fluorine atom, or an alkoxy group having 1 to 20 carbon atoms. y represents an integer of 0 to 4. In order to reduce the shrinkage rate during curing, y is preferably 0 to 1, and more preferably 0. z represents an integer of 1 to 5, with the proviso that y+z≦5.

[0022] Among the compounds represented by the general formula (1), more preferred examples include the following compounds, but are not limited to these.

[0023] [ka]

[0024] The content of the compound (C1) containing one thermal crosslinking group is preferably 0.5 to 40 parts by weight, more preferably 5 to 30 parts by weight, based on 100 parts by weight of the resin (A). By containing the compound in this range, good alkali solubility can be obtained. In addition, the compound (C2) containing four or more thermal crosslinking groups is not particularly limited as long as it has four or more thermally reactive functional groups, such as an alkoxymethyl group, a methylol group, an epoxy group, or an oxetanyl group, in the molecule, but is preferably a compound having a phenolic hydroxyl group and containing four to six groups selected from a methylol group and an alkoxymethyl group, and examples of the compounds include, but are not limited to, the following compounds:

[0025] [ka]

[0026] As the (C2) compound containing four or more thermal crosslinking groups, specific examples of the alkoxymethyl group-containing compound containing a urea-based organic group are shown below, but the compound is not limited to these.

[0027] [ka]

[0028] Preferred examples of compounds having four or more alkoxymethyl groups or methylol groups include well-known compounds such as HMOM-TPPHBA (all trade names, manufactured by Honshu Chemical Industry Co., Ltd.), NIKALAC MX-270, and MW-100LM (all trade names, manufactured by Sanwa Chemical Co., Ltd.).

[0029] Examples of compounds having an epoxy group or an oxetanyl group include known compounds such as "EPOLITE" (registered trademark) 40E, "EPOLITE" 100E, "EPOLITE" 200E (all trade names, manufactured by Kyoeisha Chemical Co., Ltd.), VG3101L (trade name, manufactured by Printec Co., Ltd.), "TEPIC" (registered trademark) S, "TEPIC" G, "TEPIC" P (all trade names, manufactured by Nissan Chemical Industries, Ltd.), OXT-121, OXT-221, OX-SQ-H, OXT-191, PNOX-1009, RSOX (all trade names, manufactured by Toagosei Co., Ltd.).

[0030] The content of the (C2) compound having 4 or more thermal crosslinking groups is preferably 3 to 40 parts by weight, more preferably 5 to 20 parts by weight, based on 100 parts by weight of the (A) resin. Within this range, the crosslinking density is high, the mechanical properties, heat resistance, and chemical resistance are improved, and the occurrence of wrinkles after curing can be suppressed.

[0031] The photosensitive resin composition of the present invention also contains (B) a photosensitizer (hereinafter, sometimes referred to as component (B)).

[0032] When the photosensitive resin composition containing the resin (A) further contains a photosensitizer (B), the resin composition is imparted with photosensitivity, and a fine opening pattern can be formed. (B) The photosensitizer is a compound whose chemical structure changes in response to ultraviolet light. Examples of the photosensitizer include a photoacid generator, a photobase generator, and a photopolymerization initiator.

[0033] From the viewpoint of fine processability, the photosensitive resin composition containing the (A) resin and the (B) photosensitizer preferably has positive photosensitivity.

[0034] Among the above-mentioned (B) photosensitizers, photoacid generators are preferred. By using a photoacid generator, an acid is generated in the light-irradiated portion of the photosensitive resin composition, and the solubility of the light-irradiated portion in an alkaline developer is increased, so that a positive pattern in which the light-irradiated portion dissolves can be obtained. Examples of photoacid generators include quinone diazide compounds, sulfonium salts, phosphonium salts, diazonium salts, and iodonium salts. Furthermore, a sensitizer or the like can be included as necessary.

[0035] As the quinone diazide compound, a compound in which a sulfonic acid of naphthoquinone diazide is bonded to a compound having a phenolic hydroxyl group by ester bonding is preferred. As the compound having a phenolic hydroxyl group used here, a known compound may be used, and a compound in which 4-naphthoquinone diazide sulfonic acid or 5-naphthoquinone diazide sulfonic acid is introduced by ester bonding can be exemplified as a preferred example, but other compounds can also be used.

[0036] It is preferable that 50 mol % or more of the functional groups of the compound having a phenolic hydroxyl group are substituted with a quinone diazide sulfonyl group. By using a quinone diazide compound substituted with 50 mol % or more, the affinity of the quinone diazide compound to an alkaline aqueous solution is reduced. As a result, the solubility of the resin composition in an alkaline aqueous solution of the unexposed portion is greatly reduced. Furthermore, the quinone diazide sulfonyl group is converted to an indene carboxylic acid by exposure, and a high dissolution rate of the photosensitive resin composition in an alkaline aqueous solution of the exposed portion can be obtained. That is, as a result, the dissolution rate ratio of the exposed portion and the unexposed portion of the composition can be increased, and a pattern with high resolution can be obtained.

[0037] By containing such a quinone diazide compound, it is possible to obtain a resin composition having positive photosensitivity that is sensitive to the i-line (365 nm), h-line (405 nm), and g-line (436 nm) of a general mercury lamp, or to a broad band including these rays. The photosensitizer (B) may be contained alone or in combination of two or more kinds.

[0038] Examples of the quinone diazide sulfonyl group include a 5-naphthoquinone diazide sulfonyl group, a 4-naphthoquinone diazide sulfonyl group, and a group containing a 4-naphthoquinone diazide sulfonyl group and a 5-naphthoquinone diazide sulfonyl group in the same molecule.

[0039] The quinone diazide compound can be synthesized by a known method through an esterification reaction between a compound having a phenolic hydroxyl group and a quinone diazide sulfonic acid compound. The use of the quinone diazide compound improves the resolution, sensitivity, and film remaining rate.

[0040] The molecular weight of the (B) photosensitizer is preferably 2500 or less, more preferably 1600 or less. If the molecular weight is 2500 or less, the quinone diazide compound can be sufficiently thermally decomposed in the heat treatment after the pattern formation, and a cured film having excellent heat resistance, mechanical properties, and adhesiveness can be obtained. On the other hand, the molecular weight is preferably 800 or more, more preferably 900 or more.

[0041] The content of the (B) photosensitizer is preferably 1 to 100 parts by weight, and more preferably 5 to 30 parts by weight, per 100 parts by weight of the (A) resin component. Within this range, photosensitivity can be imparted while maintaining the heat resistance, chemical resistance, and mechanical properties of the film after heat treatment.

[0042] It is preferred that the photosensitizer having a 4-naphthoquinone diazide sulfonyl group (hereinafter, abbreviated as compound (B1)) contains a compound represented by formula (2), and the photosensitizer having a 5-naphthoquinone diazide sulfonyl group (hereinafter, abbreviated as compound (B2)) contains a compound represented by formula (3).

[0043] [ka]

[0044] [ka]

[0045] Specific examples of the compound represented by formula (2) include 4CPA-15, 4CPA-20, 4CPA-80 (all trade names, manufactured by Daito Chemistry Co., Ltd.), TP4-250, HA4-170 (all trade names, manufactured by Toyo Gosei Co., Ltd.), and the like.

[0046] Specific examples of the compound represented by formula (3) include TP5-250, TP5-280, HA5-170 (all trade names, manufactured by Toyo Gosei Co., Ltd.), STP-525, STP-528 (all trade names, manufactured by Sanbo Chemical Laboratory Co., Ltd.), and the like.

[0047] The photosensitive resin composition according to the present invention also contains a resin (A).

[0048] (A) Explain resin.

[0049] The polyimide is not particularly limited as long as it has an imide ring. The polyimide precursor is not particularly limited as long as it has a structure that becomes a polyimide having an imide ring by dehydration ring closure, and can contain polyamic acid, polyamic acid ester, etc. The polybenzoxazole is not particularly limited as long as it has an oxazole ring. The polybenzoxazole precursor is not particularly limited as long as it has a structure that becomes a polybenzoxazole having a benzoxazole ring by dehydration ring closure, and can contain polyhydroxyamide, etc. From the viewpoint of heat resistance, polyimide and polyimide precursor are preferred. By forming a cyclic structure, heat resistance and solvent resistance are dramatically improved. Furthermore, from the viewpoint of alkali solubility, polyimide precursors are more preferred.

[0050] Polyimide has a structural unit represented by general formula (4), polyimide precursor and polybenzoxazole precursor have a structural unit represented by the following general formula (5), and polybenzoxazole has a structural unit represented by general formula (6).

[0051] The (A) resin may contain two or more of these, or may contain a resin copolymerized with a structural unit represented by general formula (4), a structural unit represented by general formula (5), and a structural unit represented by general formula (6).

[0052] [ka]

[0053] In the general formula (4), V represents a tetravalent to decavalent organic group having 4 to 40 carbon atoms, and W represents a divalent to octavalent organic group having 4 to 40 carbon atoms. a and b each independently represent an integer of 0 to 6, and in order to impart alkali solubility, it is preferable that a+b>0. R 1 and R 2 represents a group selected from the group consisting of a hydroxyl group, a carboxyl group, a sulfonic acid group, and a thiol group, and a plurality of R 1 and R 2 may be the same or different.

[0054] [ka]

[0055] In the general formula (5), X and Y each independently represent a divalent to octavalent organic group having 4 to 40 carbon atoms. 3 and R 4 each independently represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. c and d each independently represent an integer of 0 to 4, and c+d>0. e and f each independently represent the number of carboxyl groups or ester groups, and each independently represent an integer of 0 to 2, preferably 1 or 2. From the viewpoints of solubility in an alkaline developer and solution stability of the resulting photosensitive resin composition, R contained in general formula (5) 3 and R 4 Of these, it is preferable that 10 mol % to 90 mol % are hydrogen atoms. 3 and R 4Each of the groups independently contains at least one monovalent hydrocarbon group having 1 to 16 carbon atoms, and the rest are more preferably hydrogen atoms.

[0056] X has an aromatic group, e≧2, and has a carboxy group or a carboxy ester group at the ortho position of the aromatic amide group, and forms an imide ring by dehydration ring closure.

[0057] In the case of a polybenzoxazole precursor, X in general formula (5) has an aromatic group, d>0, and has a hydroxyl group at the ortho position of the aromatic amide group, and forms a benzoxazole ring by dehydration ring closure.

[0058] [ka]

[0059] In formula (6), T represents a divalent organic group having 4 to 40 carbon atoms, and U represents a tetravalent organic group having 4 to 40 carbon atoms.

[0060] The weight average molecular weight of the resin of the present invention is preferably 3,000 to 200,000. In this range, the resin has a suitable solubility in an alkaline developer, so that a high contrast between exposed and unexposed areas can be obtained and a desired pattern can be formed. From the viewpoint of the solubility of the resin in an alkaline developer, the weight average molecular weight is more preferably 100,000 or less, and more preferably 50,000 or less. Also, from the viewpoint of improving elongation, the weight average molecular weight is preferably 10,000 or more. Here, the molecular weight can be measured by gel permeation chromatography (GPC) and converted from a standard polystyrene calibration curve.

[0061] The (A) resin may have other structural units in addition to the structural units represented by general formula (4), general formula (5) or general formula (6). Examples of the other structural units include, but are not limited to, cardo structures and siloxane structures. In this case, it is preferable that the structural units represented by general formula (4), general formula (5) or general formula (6) are the main structural units. Here, the main structural units refer to structural units represented by general formula (4), general formula (5) or general formula (6) that account for 50 mol% or more of the total number of structural units in the (A) resin, more preferably 70 mol% or more, and even more preferably 90 mol% or more.

[0062] In the general formula (4) above, V-(R 1 ) a In the above general formula (5), (OH) c -X-(COOR 3 ) e represents a residue of an acid dianhydride, and T in the above general formula (6) represents a residue of a dicarboxylic acid. V is a tetravalent to decavalent organic group having 4 to 40 carbon atoms, and among these, an organic group having 4 to 40 carbon atoms containing an aromatic ring or a cyclic aliphatic group is preferred. X is a divalent to octavalent organic group having 4 to 40 carbon atoms, and T is a divalent organic group having 4 to 40 carbon atoms, and among these, an organic group having 4 to 40 carbon atoms containing an aromatic ring or a cyclic aliphatic group is preferred.

[0063] Examples of the acid residues constituting the (A) resin include dicarboxylic acid residues such as aromatic dicarboxylic acids, such as terephthalic acid, isophthalic acid, diphenyl ether dicarboxylic acid, naphthalenedicarboxylic acid, and bis(carboxyphenyl)propane, and aliphatic dicarboxylic acids, such as cyclohexane dicarboxylic acid and adipic acid. Examples of trivalent acid residues include tricarboxylic acids, such as trimellitic acid and trimesic acid. The tetravalent acid residues are pyromellitic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, 2,2',3,3'-biphenyltetracarboxylic acid, 3,3',4,4'-diphenylethertetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 2,2',3,3'-benzophenonetetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)propane, 2,2-bis(2,3-dicarboxyphenyl)propane, 1,1-bis(3,4-dicarboxyphenyl)ethane, 1,1-bis(2,3-dicarboxyphenyl)ethane, bis(3,4-dicarboxyphenyl)methane, bis(2,3-dicarboxyphenyl)methane, bis( 3,4-dicarboxyphenyl)ether, 1,2,5,6-naphthalenetetracarboxylic acid, 9,9-bis(3,4-dicarboxyphenyl)fluorene, 9,9-bis{4-(3,4-dicarboxyphenoxy)phenyl}fluorene, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,5,6-pyridinetetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, and aromatic tetracarboxylic acids having the structures shown below, butanetetracarboxylic acid, cyclobutanetetracarboxylic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, etc. can be mentioned, but are not limited thereto. As the acid residue constituting the (A) resin, two or more of these may be used, but it is preferable that the tetracarboxylic acid residue is contained in the acid residue contained in the (A) resin at 1 to 40 mol %.In terms of solubility in an alkaline developer and photosensitivity, it is preferred that the acid residues contained in the resin (A) are 50 mol % or more of acid residues having a hydroxyl group.

[0064] The acid component constituting the acid residue preferably has an aromatic ring from the viewpoint of heat resistance, and more preferably is a trivalent or tetravalent organic group having 6 to 30 carbon atoms as shown below.

[0065] [ka]

[0066] In the formula, R 17 R represents an oxygen atom, C(CF3)2, or C(CH3)2. 18 and R 19 represents a hydrogen atom or a hydroxyl group.

[0067] It is preferable that the (A) resin contains fluorine atoms, because when the resin is developed with an alkaline aqueous solution, water repellency is imparted to the interface of the film, and the developer is prevented from seeping in from the interface. The fluorine atom content per 100 parts by weight of the (A) resin is preferably 10 parts by weight or more in order to obtain a sufficient effect of preventing seepage from the interface, and is preferably 20 parts by weight or less in terms of solubility in an alkaline aqueous solution.

[0068] (A) Acids constituting the resin and diamine residues having fluorine base paper include 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, 2,2',3,3'-biphenyltetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 2,2',3,3'-benzophenonetetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)propane, 2,2-bis(2,3-dicarboxyphenyl)propane, 1,1-bis(3,4-dicarboxyphenyl)ethane, 1,1-bis(2,3 ... Preferred are bis(3,4-dicarboxyphenyl)ethane, bis(3,4-dicarboxyphenyl)methane, bis(2,3-dicarboxyphenyl)methane, bis(3,4-dicarboxyphenyl)sulfone dianhydride, bis(3,4-dicarboxyphenyl)ether, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, 3,3',4,4'-diphenylsulfonetetracarboxylic acid, 9,9-bis(3,4-dicarboxyphenyl)fluorene acid, 9,9-bis{4-(3,4-dicarboxyphenoxy)phenyl}fluorene acid, and the structures shown below.

[0069] [ka]

[0070] In the formula, R 17 R represents an oxygen atom, C(CF3)2, or C(CH3)2. 18 and R 19 represents a hydrogen atom or a hydroxyl group.

[0071] W-(R 2 ) b (OH) in the above general formula (5) d -Y-(COOR 4 ) f In the above general formula (6), U represents a residue of a diamine. W, Y and U are divalent to tetravalent organic groups having 4 to 40 carbon atoms, and among these, organic groups having 4 to 40 carbon atoms and containing an aromatic ring or a cyclic aliphatic group are preferred.

[0072] Specific examples of diamine residues include hydroxyl group-containing diamines such as bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(3-amino-4-hydroxyphenyl)sulfone, bis(3-amino-4-hydroxyphenyl)propane, bis(3-amino-4-hydroxyphenyl)methylene, bis(3-amino-4-hydroxyphenyl)ether, bis(3-amino-4-hydroxy)biphenyl, and bis(3-amino-4-hydroxyphenyl)fluorene; and 3-sulfonic acid-4,4'-diaminodiphenyl ether. Sulfonic acid-containing diamines, thiol group-containing diamines such as dimercaptophenylenediamine, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl methane, 4,4'-diaminodiphenyl methane, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 1,4-bis(4-aminophenoxy)benzene, benzine, m-phenylenediamine, p-phenylenediamine, 1, 5-Naphthalenediamine, 2,6-Naphthalenediamine, bis(4-aminophenoxyphenyl)sulfone, bis(3-aminophenoxyphenyl)sulfone, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl}ether, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-diethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-diethyl-4,4'-diaminobiphenyl, 2,2',3 aromatic diamine residues such as 3,3',4,4'-tetramethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, and compounds in which some of the hydrogen atoms in these aromatic rings have been substituted with alkyl groups or fluoroalkyl groups having 1 to 10 carbon atoms, halogen atoms, and the like; 2,4-diamino-1,3,5-triazine (guanamine), 2,4-diamino-6-methyl-1,3,5-triazine (acetoguanamine), 2,4-diamino-6-phenyl-1,3,Examples of the diamine residue include those having a nitrogen-containing heteroaromatic ring such as 5-triazine (benzoguanamine), silicone diamines such as 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(p-aminophenyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(p-aminophenethyl)-1,1,3,3-tetramethyldisiloxane, and 1,7-bis(p-aminophenyl)-1,1,3,3,5,5,7,7-octamethyltetrasiloxane, alicyclic diamine residues such as cyclohexyldiamine and methylenebiscyclohexylamine, and diamine residues having the structure shown below. Two or more of these diamine residues may be used, but from the viewpoint of solubility in an alkaline developer, it is preferable that the diamine residues having a hydroxyl group account for 60 mol % or more of the diamine residues contained in the (A) resin, out of 100 mol % of the diamine residues contained in the resin.

[0073] [ka]

[0074] In the formula, R 20 is an oxygen atom, C(CF3)2, C(CH3)2, R 21 ~R 24 respectively represent a hydrogen atom or a hydroxyl group.

[0075] Among these, from the viewpoint of improving the alkali developability and the transmittance of the (A) resin and its cured film, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl methane, 4,4'-diaminodiphenyl methane, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, m-phenylenediamine, p-phenylenediamine, 1,4-bis(4-aminophenoxy)benzene, 9,9-bis(4-aminophenyl)fluorene, and diamines having the structures shown below are preferred.

[0076] [ka]

[0077] In the formula, R 20 R represents an oxygen atom, C(CF3)2, or C(CH3)2. 21 ~R 22 respectively represent a hydrogen atom or a hydroxyl group.

[0078] Particularly preferred are 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 1,4-bis(4-aminophenoxy)benzene, and diamines having the structures shown below.

[0079] [ka]

[0080] In the formula, R 20 R represents an oxygen atom, C(CF3)2, or C(CH3)2. 21 ~R 22 respectively represent a hydrogen atom or a hydroxyl group.

[0081] These diamines can be used as they are, or as diisocyanate compounds or trimethylsilylated diamines obtained by reacting the diamines with phosgene.

[0082] Diamine residues having an aliphatic polysiloxane structure may be copolymerized within a range that does not reduce heat resistance. By copolymerizing diamine residues having an aliphatic polysiloxane structure, adhesion to a substrate can be improved. Specifically, as the diamine component, bis(3-aminopropyl)tetramethyldisiloxane, bis(p-aminophenyl)octamethylpentasiloxane, etc., copolymerized at 1 to 15 mol % of the total diamine residues, etc., can be mentioned. Copolymerization within this range is preferable in terms of improving adhesion to a substrate such as a silicon wafer and not reducing solubility in an alkaline solution.

[0083] (A) The end of the resin can be reacted with a terminal blocking agent. By blocking the end of the polymer with a monoamine having a functional group selected from the group consisting of a hydroxyl group, a carboxyl group, a sulfonic acid group, and a thiol group, the dissolution rate of the resin in an alkaline aqueous solution can be adjusted to a preferred range. In addition, by blocking the end of the polymer with an acid anhydride, an acid chloride, or a monocarboxylic acid, the dissolution rate of the resin in an alkaline aqueous solution can be adjusted to a preferred range.

[0084] Monoamines used as end-capping agents include 5-amino-8-hydroxyquinoline, 1-hydroxy-7-aminonaphthalene, 1-hydroxy-6-aminonaphthalene, 1-hydroxy-5-aminonaphthalene, 1-hydroxy-4-aminonaphthalene, 2-hydroxy-7-aminonaphthalene, 2-hydroxy-6-aminonaphthalene, 2-hydroxy-5-aminonaphthalene, 1-carboxy-7-aminonaphthalene, 1-carboxy-6-aminonaphthalene, 1-carboxy-5-aminonaphthalene, 2-carboxy-7-aminonaphthalene, Preferred are 2-carboxy-6-aminonaphthalene, 2-carboxy-5-aminonaphthalene, 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, 2-aminobenzenesulfonic acid, 3-aminobenzenesulfonic acid, 4-aminobenzenesulfonic acid, 3-amino-4,6-dihydroxypyrimidine, 2-aminophenol, 3-aminophenol, 4-aminophenol, 2-aminothiophenol, 3-aminothiophenol, 4-aminothiophenol, etc. These may be used alone or in combination of two or more to cap the ends of the resin.

[0085] Examples of acid anhydrides include phthalic anhydride, maleic anhydride, nadic acid, cyclohexanedicarboxylic anhydride, 3-hydroxyphthalic anhydride, and other acid anhydrides, 3-carboxyphenol, 4-carboxyphenol, 3-carboxythiophenol, 4-carboxythiophenol, 1-hydroxy-7-carboxynaphthalene, 1-hydroxy-6-carboxynaphthalene, 1-hydroxy-5-carboxynaphthalene, 1-mercapto-7-carboxynaphthalene, 1-mercapto-6-carboxynaphthalene, 1-mercapto-5-carboxynaphthalene, 3-carboxybenzenesulfonic acid, 4-carboxybenzenesulfonic acid, and other acid anhydrides. Preferred are monocarboxylic acids such as benzenesulfonic acid, monoacid chloride compounds in which the carboxyl groups of these are acid chlorides, monoacid chloride compounds in which only the monocarboxyl groups of dicarboxylic acids such as terephthalic acid, phthalic acid, maleic acid, cyclohexanedicarboxylic acid, 1,5-dicarboxynaphthalene, 1,6-dicarboxynaphthalene, 1,7-dicarboxynaphthalene, and 2,6-dicarboxynaphthalene are acid chlorides, and active ester compounds obtained by reacting a monoacid chloride compound with N-hydroxybenzotriazole or N-hydroxy-5-norbornene-2,3-dicarboximide. These may be used alone or in combination of two or more.

[0086] The proportion of monoamine used in the end-capping agent is preferably 2 to 50 mol %, more preferably 2 to 25 mol %, based on the total amine components in the resin. The proportion of acid anhydride, acid chloride, and monocarboxylic acid is preferably 2 to 50 mol %, more preferably 2 to 25 mol %, based on the total acid components in the resin.

[0087] The end-capping agent introduced into the polymer can be easily detected by the following method. For example, the polymer into which the end-capping agent has been introduced is dissolved in an acidic solution, decomposed into the amine component and the acid anhydride component, which are the structural units of the polymer, and the end-capping agent can be easily detected by measuring the components by gas chromatography (GC) or NMR. Separately, the polymer into which the end-capping agent has been introduced can be directly measured by pyrolysis gas chromatography (PGC) or infrared spectroscopy, and 13It can also be detected by measuring C-NMR spectroscopy.

[0088] The (A) resin preferably has a weight average molecular weight of 10,000 or more and 100,000 or less. If the weight average molecular weight is 10,000 or more, the mechanical properties of the cured film after curing can be improved. More preferably, the weight average molecular weight is 20,000 or more. On the other hand, if the weight average molecular weight is 100,000 or less, the developability with various developers can be improved, and if the weight average molecular weight is 50,000 or less, the developability with an alkaline solution can be improved, which is preferable.

[0089] The weight average molecular weight (Mw) can be confirmed using gel permeation chromatography (GPC). For example, it can be measured using N-methyl-2-pyrrolidone (hereinafter sometimes abbreviated as NMP) as the developing solvent and calculated in terms of polystyrene.

[0090] The (A) resin is synthesized by a known method. When the (A) resin is a polyimide precursor, that is, a polyamic acid or a polyamic acid ester, the (A) resin can be synthesized by, for example, reacting a tetracarboxylic dianhydride with a diamine compound at low temperature, obtaining a diester from a tetracarboxylic dianhydride with an alcohol and then reacting it with an amine in the presence of a condensing agent, obtaining a diester from a tetracarboxylic dianhydride with an alcohol and then converting the remaining dicarboxylic acid into an acid chloride and reacting it with an amine, or the like.

[0091] In the case of polyhydroxyamide, which is a precursor of polybenzoxazole, it can be produced by condensation reaction of bisaminophenol compound with dicarboxylic acid. Specifically, there is a method of reacting a dehydration condensation agent such as dicyclohexylcarbodiimide (DCC) with an acid and adding a bisaminophenol compound to the reaction, or a method of dropping a solution of dicarboxylic acid dichloride into a solution of a bisaminophenol compound to which a tertiary amine such as pyridine has been added.

[0092] In the case of a polyimide, it can be obtained by dehydrating and ring-closing the polyamic acid or polyamic acid ester obtained by the above-mentioned method through heating or a chemical treatment with an acid or base.

[0093] Polybenzoxazole can be obtained by dehydrating and ring-closing the polybenzoxazole precursor (polyhydroxyamide) obtained by the above-mentioned method through heating or a chemical treatment with an acid or base.

[0094] After polymerization using the above method, it is desirable to put the polymer into a large amount of water or a mixture of methanol and water, precipitate it, filter it, dry it, and isolate it. This precipitation process removes unreacted monomers and oligomer components such as dimers and trimers, improving the film properties after thermal curing.

[0095] The content of the (A) resin is preferably 20 to 60% by weight, and more preferably 25 to 40% by weight, based on 100% by weight of the photosensitive resin composition. By setting the content within the above range, it is possible to obtain a viscosity suitable for spin coating.

[0096] In the present invention, when the content of the (C1) compound is CW1 (parts by weight) and the content of the (C2) compound is CW2 (parts by weight) relative to 100 parts by weight of the (A) resin, it is preferable that 1.0≦CW1 / CW2≦3.0. If CW1 / CW2 is 1.0 or more, high heat resistance can be obtained, and if CW1 / CW2 is 3.0 or less, the occurrence of wrinkles after curing can be suppressed.

[0097] Preferably, 1.5≦CW1 / CW2≦2.5, more preferably, 1.7≦CW1 / CW2≦2.2, and further preferably, 1.9≦CW1 / CW2≦2.1.

[0098] In the present invention, the thermal crosslinking group of the compound (C1) is a methylol group or an alkoxymethyl group, It is preferable that the four thermal crosslinking groups of the compound (C2) are each independently a methylol group or an alkoxymethyl group. This allows both alkaline developability and improved crosslink density to be achieved. It is further preferable that the compound (C2) contains a phenolic hydroxyl group in the molecule in order to improve the alkaline developability, i.e., the sensitivity.

[0099] In the present invention, it is preferable that the (B) photosensitizer contains (B1) a 1,2-naphthoquinone-2-diazide-4-sulfonic acid ester compound and (B2) a 1,2-naphthoquinone-2-diazide-5-sulfonic acid ester compound, and when the content of the (B1) compound is BW1 (parts by weight) and the content of the (B2) compound is BW2 (parts by weight) relative to 100 parts by weight of the resin (A), 1.0≦BW1 / BW2≦4.0.

[0100] For broadband light, which is mainly used as an exposure light source, a highly sensitive photosensitive resin composition is required to improve the throughput of the manufacturing process. Therefore, it is necessary to improve the absorption in all regions of g-line, h-line, and i-line. However, (B1) 1,2-naphthoquinone-2-diazide-4-sulfonic acid ester compound becomes colored when reacted with i-line, so light does not pass through to the bottom and the solubility of the light-irradiated part in alkaline aqueous solution does not increase. (B2) 1,2-naphthoquinone-2-diazide-5-sulfonic acid ester compound is irradiated with g-line and the photobleaching effect increases the transmittance of i-line, and when the mixing ratio is 1.0≦BW1 / BW2≦4.0, (B-1) 1,2-naphthoquinone-2-diazide-4-sulfonic acid ester compound reacts to the bottom, resulting in higher sensitivity. Preferably, 1.5≦BW1 / BW2≦3.0, more preferably, 1.8≦BW1 / BW2≦2.7, and further preferably, 2≦BW1 / BW2≦2.5.

[0101] In the present invention, when the content of the photosensitizer (B) is BW (parts by weight) and the content of the compound having a thermal crosslinking group (C) is CW (parts by weight) relative to 100 parts by weight of the resin (A), it is preferable that 0.5≦BW / CW≦1.0. If BW / CW is 0.5 or more, high sensitivity is obtained, and if BW / CW is 1.0 or less, high heat resistance is obtained. This allows both high sensitivity and high heat resistance to be achieved. Preferably, 0.6≦BW / CW≦0.9, and more preferably, 0.7≦BW / CW≦0.8.

[0102] In the present invention, it is preferable to further contain (D) an antioxidant. The inclusion of an antioxidant can suppress deterioration of the cured film in the post-curing process, suppress yellowing and deterioration of mechanical properties such as elongation, and improve heat resistance. The antioxidant has a rust-preventing effect on metal materials, suppressing oxidation of metal materials and improving adhesion to copper in particular, which is preferable.

[0103] In the present invention, the (D) antioxidant preferably has a hindered phenol structure. When the development is possible with an alkaline aqueous solution, the hindered phenol compound acts as a dissolution promoter and also has a residue suppressing effect. (D) The antioxidant is preferably a hindered phenol-based antioxidant or a hindered amine-based antioxidant, and most preferably a hindered phenol-based antioxidant. The number of phenol groups or amino groups in one molecule is preferably 2 or more, more preferably 4 or more, because the antioxidant effect is easily obtained.

[0104] Examples of the hindered phenol-based antioxidant include, but are not limited to, the following structures:

[0105] [ka]

[0106] [ka]

[0107] [ka]

[0108] [ka]

[0109] [ka]

[0110] Examples of the hindered amine compound include bis(1,2,2,6,6-pentamethyl-4-piperidyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butyl malonate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, methyl-1,2,2,6,6-pentamethyl-4-piperidylsebacate, 1,2,2,6,6-pentamethyl-4-piperidylmethacrylate, and 2,2,6,6-tetramethyl 4-piperidyl methacrylate, reaction product of decanedioic acid bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl) ester with 1,1-dimethylethyl hydroperoxide and octane, tetrakis(1,2,2,6,6-pentamethyl-4-pyridyl)butane-1,2,3,4-tetracarboxylate or tetrakis(2,2,6,6-tetramethyl-4-pyridyl)butane-1,2,3,4-tetracarboxylate.

[0111] The amount of the (D) antioxidant added is preferably 0.1 to 10.0 parts by weight, more preferably 0.3 to 5.0 parts by weight, per 100 parts by weight of the (A) resin component. When the content of the antioxidant is within this range, the developability and the effect of suppressing discoloration due to curing can be appropriately maintained. In addition, the adhesion to copper can be improved.

[0112] The photosensitive resin composition of the present invention preferably contains a solvent. This allows the photosensitive resin composition to be in a varnish state, improving the coatability.

[0113] The solvent may be a polar aprotic solvent such as γ-butyrolactone, ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, tetrahydrofuran, and dioxane, acetone, methyl ethyl ketone, etc. Ketones such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, esters such as ethyl 2-hydroxy-2-methylpropionate, 3-methoxypropionate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, ethyl acetate, n-propyl acetate, i-propyl acetate, n-butyl acetate, i-butyl acetate, n-pentyl formate, i-pentyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, i-propyl butyrate,Solvents such as n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl 2-oxobutanoate, and other esters, and aromatic hydrocarbons such as toluene and xylene can be contained alone or in combination.

[0114] The content of the solvent is not particularly limited, but is preferably 50 to 2000 parts by weight, and more preferably 100 to 1500 parts by weight, per 100 parts by weight of the (A) resin component.

[0115] The photosensitive resin composition containing the (A) resin may contain, as necessary, other components such as a radical polymerizable compound, a compound having a phenolic hydroxyl group, an adhesion improver, an adhesion improver, a surfactant, etc. In addition, in order to enhance adhesion to the substrate, a silane compound can be contained in the resin composition of the present invention within a range that does not impair storage stability. By containing a silane compound, adhesion to the underlying substrate is improved. Specific examples of the silane compound include trimethoxyaminopropylsilane, trimethoxyepoxysilane, trimethoxyvinylsilane, trimethoxythiolpropylsilane, p-styryltrimethoxysilane, α-methylstyryldimethylmethoxysilane, p-styryltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-ethyl-[(triethoxysilylpropoxy)methyl]oxetane, N-phenylaminopropyltrimethoxysilane, vinyltriethoxysilane, m-acetylaminophenyltrimethoxysilane, etc., but are not limited thereto. The content of the silane coupling agent is preferably 0.01 to 5 parts by weight based on 100 parts by weight of the (A) resin.

[0116] Next, a method for producing the photosensitive resin composition of the present invention will be described. For example, the method includes a method in which (A) resin, (B) photosensitizer, (C) compound having a thermal crosslinking group, (D) antioxidant, radical polymerizable compound, solvent, compound having a phenolic hydroxyl group, adhesion improver, adhesive improver, surfactant, etc. are placed in a glass flask or a stainless steel container and stirred and dissolved with a mechanical stirrer, a method in which they are dissolved with ultrasonic waves, and a method in which they are stirred and dissolved with a planetary stirring and defoaming device.

[0117] The solid component concentration of the photosensitive resin composition is preferably 10 to 50 parts by weight when the total components including the solvent are taken as 100 parts by weight. At this solid component concentration, the viscosity is in the range of 500 to 3000 mPa·s, which makes it easy to obtain a desired film thickness with excellent coatability. Here, the solid component concentration refers to the concentration of components other than the solvent.

[0118] The photosensitive resin composition thus obtained is preferably filtered using a filter to remove dust and particles. Filter materials include polypropylene (PP), polyethylene (PE), nylon (NY), polytetrafluoroethylene (PTFE), etc., with polyethylene and nylon being preferred. To ensure the removal of foreign matter, it is preferred to filter using a filter made of such a material with a pore size of 0.1 μm to 5 μm.

[0119] Next, a method for forming a cured film using the resin composition of the present invention will be described. In the present invention, when a photosensitive resin composition is applied onto a substrate, a film in which solvent remains immediately after application is defined as a coated film, a film obtained by drying the coated film is defined as a dried film, a film obtained by exposing the dried film to actinic rays such as ultraviolet light or visible light and then developing it with a solvent is defined as a developed film, and a film obtained by heating and curing the dried film or developed film is defined as a cured film.

[0120] First, the resin composition of the present invention is applied to a substrate to obtain a coating film. Examples of substrates include, but are not limited to, silicon wafers, metal-sputtered silicon wafers, ceramics, gallium arsenide, organic circuit boards, inorganic circuit boards, composite substrates of silicon wafers and sealing resins such as epoxy resins, sealing resin substrates, and substrates on which circuit components are arranged. Examples of organic circuit boards include glass substrate copper-clad laminates such as glass cloth-epoxy copper-clad laminates, composite copper-clad laminates such as glass nonwoven cloth-epoxy copper-clad laminates, temporary carrier substrates, heat-resistant thermoplastic substrates such as polyetherimide resin substrates, polyetherketone resin substrates, and polysulfone resin substrates, and flexible substrates such as polyester copper-clad film substrates and polyimide copper-clad film substrates. Examples of inorganic circuit boards include ceramic substrates such as glass substrates, alumina substrates, aluminum nitride substrates, and silicon carbide substrates, and metal substrates such as aluminum-based substrates and iron-based substrates. Examples of materials constituting the circuit include conductors containing metals such as silver, gold, and copper, resistors containing inorganic oxides, low dielectrics containing glass-based materials and / or resins, high dielectrics containing resins and high-dielectric-constant inorganic particles, and insulators containing glass-based materials.

[0121] Examples of the coating method include spin coating using a spinner, spray coating, roll coating, screen printing, blade coater, die coater, calendar coater, meniscus coater, bar coater, roll coater, comma roll coater, gravure coater, screen coater, slit die coater, etc. The coating thickness varies depending on the coating method, the solid component concentration of the composition, the viscosity, etc., but the coating is usually performed so that the film thickness after drying is 0.1 to 150 μm.

[0122] In order to enhance the adhesion between a substrate such as a silicon wafer and a resin composition, the substrate may be pretreated with the above-mentioned silane coupling agent. For example, a solution in which a silane coupling agent is dissolved in a solvent such as isopropanol, ethanol, methanol, water, tetrahydrofuran, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, ethyl lactate, or diethyl adipate at 0.5 to 20% by weight is used for surface treatment by spin coating, immersion, spray coating, steam treatment, or the like. In some cases, a heat treatment up to 50°C to 300°C is then performed to promote the reaction between the substrate and the silane coupling agent.

[0123] Next, the substrate is dried to obtain a dry film, which is preferably dried at a temperature in the range of 50° C. to 150° C. for one minute to several hours using an oven, a hot plate, infrared rays, etc.

[0124] This resin film may be irradiated with actinic radiation through a mask having a desired pattern, and then exposed and developed to form a pattern. Actinic radiation used for exposure includes ultraviolet rays, visible light, electron beams, X-rays, etc., but in the present invention, it is preferable to use i-rays (365 nm), h-rays (405 nm), and g-rays (436 nm) from a mercury lamp.

[0125] After exposure, a developed film is obtained using a developer, which is preferably a solution of an alkaline compound such as tetramethylammonium hydroxide, diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, or hexamethylenediamine.

[0126] In the present invention, it is particularly preferable to use an alkaline aqueous solution as the developer, since after the alkaline development step, minute surface roughness and uniform in-plane wettability are improved, and a pattern with excellent dimensional uniformity can be formed.

[0127] In some cases, polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, γ-butyrolactone, and dimethylacrylamide, alcohols such as methanol, ethanol, and isopropanol, esters such as ethyl lactate and propylene glycol monomethyl ether acetate, and ketones such as cyclopentanone, cyclohexanone, isobutyl ketone, and methyl isobutyl ketone may be added to the alkaline solution alone or in combination. Development can be performed by spraying the above-mentioned developer on the coating surface, immersing the substrate in the developer, applying ultrasonic waves while immersing the substrate in the developer, or spraying the developer while rotating the substrate. After development, it is preferable to perform a rinsing treatment with water. Here, alcohols such as ethanol and isopropyl alcohol, esters such as ethyl lactate and propylene glycol monomethyl ether acetate, etc. may be added to water to perform a rinsing treatment.

[0128] The developed film is heated to proceed with a thermal crosslinking reaction, thereby curing the resin film to obtain a cured film. Crosslinking can improve heat resistance and chemical resistance. The heat treatment method can be selected from a method of gradually increasing the temperature, and a method of continuously increasing the temperature by selecting a certain temperature range for 5 minutes to 5 hours. An example of the former is a method of heat treatment at 130°C and 200°C for 30 minutes each. An example of the latter is a method of linearly increasing the temperature from room temperature to 400°C over 2 hours. The heat treatment conditions in the present invention are in a nitrogen atmosphere, and the maximum curing temperature is preferably 200°C to 400°C, more preferably 250°C to 390°C, and most preferably 320°C to 380°C.

[0129] Furthermore, the method for producing a cured film of the present invention preferably includes a step of subjecting the cured film obtained by the heat treatment to a dry etching treatment. By subjecting the cured film to the dry etching step, minute surface roughness on the cured film can be improved, and the adhesion to the barrier metal can be improved by the anchor effect.

[0130] The dry etching step of the present invention includes plasma etching and reactive ion etching. Reactive ion etching is preferred because it enables highly anisotropic etching in the cured film and provides a high anchor effect. The reactive gas used in dry etching is not particularly limited, and reactive gases such as tetrafluoromethane, trifluoromethane, oxygen, nitrogen, tetrachloromethane, carbon monoxide, and carbon dioxide are used alone or in a mixture of two or more. Inert gases such as helium and argon may also be mixed. Among these, it is preferable that the reactive gas contains oxygen, since it can improve the surface energy of the cured film and improve the adhesion with the barrier metal. In addition, the plasma output during plasma etching is preferably 200 W or more and 1500 W or less, and the pressure is preferably 5 to 80 Pa.

[0131] The amount of film loss of the cured film etched in the dry etching step is preferably 0.1 to 0.5 μm.

[0132] The semiconductor device of the present invention is a semiconductor device having a cured film. One embodiment relates to a semiconductor device having a cured film formed using the photosensitive resin composition of the above embodiment.

[0133] The components of a semiconductor device generally include a semiconductor element and a sealing member (sealing layer). The semiconductor element is typically made of inorganic materials such as a semiconductor chip (Si, SiC, GaN), Cu, Ni plating, Ag plating, Au plating, Au / Pd / Ni plating, solder, sintered silver, sintered copper, Al wire, Au wire, and ceramic substrate (alumina, alumina zirconia, aluminum nitride, silicon nitride). The sealing layer is typically made of an organic material such as a resin. Hereinafter, a sealing layer made of resin is referred to as a resin sealing layer.

[0134] In the semiconductor device, the adhesion between the components can be easily improved by forming a cured film using the photosensitive resin composition of the above embodiment as a primer layer between each component. More specifically, for example, by forming a cured film of the photosensitive resin composition between the resin sealing layer and the substrate, or between the resin sealing layer and the semiconductor element, the adhesion between each component can be ensured, and peeling during cycle testing can be prevented. From this viewpoint, in one embodiment, the semiconductor device has a substrate, a semiconductor element mounted on the substrate, a primer layer provided on at least the semiconductor element mounting surface of the substrate, and a resin sealing layer provided on the primer layer, and the primer layer is preferably composed of a cured film formed using the photosensitive resin composition of the above embodiment. The substrate may be a lead frame composed of a die pad on which a semiconductor element is mounted and a lead, and the electrode pad of the semiconductor element and the lead of the lead frame are electrically connected via a wire.

[0135] In one embodiment, the photosensitive resin composition can be suitably used as a constituent material of a power semiconductor device using the silicon carbide (SiC) substrate or the gallium nitride (GaN) substrate. When the photosensitive resin composition is used to constitute a power semiconductor device, a decrease in adhesion between the components during a heat cycle test can be easily suppressed.

[0136] A typical structure of the semiconductor device of the above embodiment will be specifically described below with reference to FIG. 1. FIG. 1 is a schematic cross-sectional view showing one embodiment of a semiconductor device. The semiconductor device shown in FIG. 1 has a die pad 1a, a semiconductor element 2, a primer layer 3, leads 1b, wires 4, and a resin sealing layer 5, and the primer layer 3 is formed from the photosensitive resin composition of the above embodiment. As shown in FIG. 1, the primer layer 3 formed from the photosensitive resin composition is provided on the semiconductor element mounting surface (the surface of the die pad 1a on which the leads 1b and the semiconductor element 2 are mounted) of the substrate in contact with the resin sealing layer 5, and this makes it possible to easily increase the adhesion between the respective members.

[0137] In one embodiment, a method for manufacturing a semiconductor device includes at least a step of applying the photosensitive resin composition of the above embodiment to a surface of a substrate carrying a semiconductor element and drying the composition to form a primer layer, and a step of forming a resin sealing layer on the primer layer.

[0138] In the above embodiment, the primer layer is formed using the photosensitive resin composition of the above embodiment. From the viewpoint of workability, it is preferable to use a photosensitive resin composition containing (A) resin as the resin component. The primer layer can be obtained by applying the photosensitive resin composition to a predetermined location and drying the coating. By imparting the photosensitivity as described in the present invention, it becomes possible to form a pattern of the primer layer. The method of pattern formation is as described above.

[0139] The material of the lead frame, which is composed of a die pad on which a semiconductor element is mounted and a lead, is not particularly limited and can be selected from materials well known in the art. From the viewpoint of application to a power semiconductor device, the die pad material is preferably at least one selected from the group consisting of Ni and Cu. In addition, the one selected from the group consisting of Ni and Cu may have Ag plating on its surface. The lead material of the lead frame is preferably selected from the group consisting of Ni and Cu.

[0140] The material of the semiconductor element is not particularly limited, and may be, for example, a silicon wafer, a silicon carbide wafer, or the like.

[0141] The resin sealing layer may be formed using a sealing material known in the art. For example, the resin sealing material may be a liquid or solid epoxy-based resin composition. The resin sealing layer may be formed by transfer molding using the resin sealing material.

[0142] In another embodiment, the method for manufacturing a semiconductor device includes, for example, a step of applying and drying the photosensitive resin composition of the above embodiment to a semiconductor substrate on which a plurality of wirings of the same structure are formed to form a cured film, and a step of forming rewiring on the photosensitive resin layer that is electrically connected to the electrodes on the semiconductor substrate, as necessary. In addition to the above steps, a step of forming a cured film on the rewiring or on the resin layer using the photosensitive resin composition of the above embodiment may be included as necessary. Furthermore, in addition to the above steps, a step of forming an external electrode terminal on the cured film, as necessary, and then a step of dicing may be included as necessary.

[0143] The method of applying the photosensitive resin layer (primer layer) is not particularly limited, but is preferably spin coating, spray coating, or dispense coating. The method of drying the resin layer can be performed by a method known in the art. The resin composition of the above embodiment is also excellent in properties such as sputtering resistance, plating resistance, and alkali resistance required in the process of forming rewiring. Therefore, the photosensitive resin composition of the above embodiment can be suitably used as a material for any semiconductor device without being limited to the configuration of the semiconductor device described above. EXAMPLES

[0144] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. The photosensitive resin compositions in the examples were evaluated by the following methods.

[0145] (1) Sensitivity assessment <Preparation of Photosensitive Resin Composition Film> A photosensitive resin composition (hereinafter referred to as varnish) was applied onto an 8-inch silicon wafer so that the film thickness after pre-baking would be 15 μm, and a photosensitive resin film (dried film) was obtained by drying for 3 minutes at 120° C. using a hot plate (ACT8 coating and developing apparatus manufactured by Tokyo Electron Ltd.).

[0146] <How to measure film thickness> Using Lambda Ace manufactured by Dainippon Screen Mfg. Co., Ltd., the dried film and developed film were measured at a refractive index of 1.629, and the cured film was measured at a refractive index of 1.773.

[0147] <Exposure> A reticle with square patterns of 20 μm, 40, 60, 80, 100, and 150 μm was set on an exposure machine (Nikon i-line stepper NSR-2005i9C), and the dried film was exposed to i-line at an intensity of 365 nm with varying exposure times.

[0148] <Development> Using a Tokyo Electron Ltd. ACT8 developing device, a 2.38% by weight aqueous solution of tetramethylammonium hydroxide was sprayed onto the exposed film for 10 seconds at 50 rpm. After this, the film was left to stand for 120 seconds at 0 rpm, rinsed with water at 400 rpm, and dried by shaking at 3000 rpm for 10 seconds. The evaluation criteria were the optimum exposure time (hereinafter referred to as EOP) at which a 20 μm pattern was formed using a pattern with a mask size of 20 μm after the above development. The EOP was 800 mJ / cm 2 The following are very good (A): 800mJ / cm 2 Super 1000mJ / cm 2 The following are good (B), 1000mJ / cm 2 Super 1200mJ / cm 2 The following are acceptable (C): 1200mJ / cm 2 Those exceeding this limit were rated as defective (D).

[0149] (2) Evaluation of pattern wrinkles after heat curing <Heat curing treatment> The developed film prepared by the method (1) above was placed in an inert oven CLH-21CD-S manufactured by Koyo Thermo Systems Co., Ltd. at room temperature, and then heated to 350° C. at a rate of 3.5° C. / min with an oxygen concentration of 20 ppm or less, and heat-treated at 350° C. for 1 hour. When the temperature reached 50° C. or less, the wafer was removed and a heat-resistant resin film (cured film) was prepared.

[0150] <Wrinkle evaluation> The corners of the patterns of the cured film obtained were observed using an optical microscope. The evaluation criteria were as follows: square pattern with one side of more than 100 μm and no wrinkles was good (A), square pattern with one side of more than 100 μm, wrinkles, and square pattern with one side of more than 80 μm to 100 μm and no wrinkles was acceptable (B), and square pattern with one side of more than 80 μm, wrinkles, and square pattern with one side of 80 μm or less, no wrinkles was unacceptable (C).

[0151] (3) Heat resistance evaluation <Preparation of cured film> <Weight loss temperature evaluation after high temperature and humidity> A dried film of the varnish was obtained on an 8-inch silicon substrate under the above-mentioned (1) conditions, and then a cured film was obtained by heat treatment under the above-mentioned (2) conditions. The obtained cured film was placed in a Tabai Espec HAST CHAMBER (EHS-211MD) and treated for 400 hours under conditions of 121°C, 100% humidity, and 2 atm as a PCT test (pressure cooker test). The wafer was removed and immersed in 45% by weight hydrofluoric acid for 5 minutes to peel the cured film from the wafer. The peeled film was cut into pieces of about 20 mg, and heated from room temperature to 200°C at 10°C / min using a Shimadzu Corporation DTG-60, treated at 200°C for 10 minutes, and then heated to 500°C at 10°C / min. The temperature at which the weight was reduced by 5% from the weight after treatment at 200°C was determined. Those with a 5% weight loss temperature of 480°C or higher were rated as extremely good (A), those with a 5% weight loss temperature of 470°C or higher but less than 480°C were rated as good (B), those with a 5% weight loss temperature of 460°C or higher but less than 470°C were rated as fair (C), and those with a 5% weight loss temperature of less than 460°C were rated as poor (D).

[0152] (Synthesis Example 1) Synthesis of hydroxyl group-containing diamine compound (a) 18.3 g (0.05 mol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (product name BAHF, manufactured by Central Glass Co., Ltd.) was dissolved in 100 mL of acetone and 17.4 g (0.3 mol) of propylene oxide, and cooled to -15°C. A solution of 20.4 g (0.11 mol) of 3-nitrobenzoyl chloride dissolved in 100 mL of acetone was added dropwise to the solution. After the addition was completed, the mixture was reacted at -15°C for 4 hours, and then returned to room temperature. The precipitated white solid was filtered and dried in vacuum at 50°C.

[0153] 30 g of the solid was placed in a 300 mL stainless steel autoclave and dispersed in 250 mL of methyl cellosolve, and 2 g of 5% palladium-carbon was added. Hydrogen was introduced into the autoclave using a balloon, and the reduction reaction was carried out at room temperature. After about 2 hours, the reaction was terminated when it was confirmed that the balloon was no longer deflating. After the reaction was completed, the palladium compound catalyst was removed by filtration, and the mixture was concentrated using a rotary evaporator to obtain a hydroxyl group-containing diamine compound (a) represented by the following formula.

[0154] [ka]

[0155] (Synthesis Example 2) Synthesis of hydroxyl-containing acid anhydride (b) Under a dry nitrogen stream, 18.3 g (0.05 mol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (BAHF) and 34.2 g (0.3 mol) of allyl glycidyl ether were dissolved in 100 g of gamma butyrolactone (GBL) and cooled to -15°C. 22.1 g (0.11 mol) of trimellitic anhydride chloride dissolved in 50 g of GBL was added dropwise so that the temperature of the reaction solution did not exceed 0°C. After the dropwise addition, the reaction was carried out at 0°C for 4 hours. The solution was concentrated using a rotary evaporator and poured into 1 L of toluene to obtain a hydroxyl-containing acid anhydride (b) represented by the following formula.

[0156] [ka]

[0157] (Synthesis Example 3) (A) Synthesis of Resin (A-1) Under a dry nitrogen stream, 13.6 g (0.0225 mol) of the hydroxyl group-containing diamine (a) obtained in Synthesis Example 1 was dissolved in 50 g of NMP. 17.5 g (0.025 mol) of the hydroxyl group-containing acid anhydride (b) obtained in Synthesis Example 2 was added together with 30 g of pyridine, and the mixture was reacted at 40°C for 2 hours. Then, 0.58 g (0.005 mol) of 4-aminophenylacetylene was added as a terminal blocking agent, and the mixture was reacted at 40°C for another hour. After the reaction was completed, the solution was poured into 2 L of water, and the precipitate of the polymer solid was collected by filtration. The polymer solid was dried in a vacuum dryer at 80°C for 72 hours to obtain a polyimide precursor (A) resin (A-1). The weight average molecular weight of the obtained polymer was measured by GPC, and it was confirmed to be in the range of 10,000 to 50,000.

[0158] (Synthesis Example 4) (A) Synthesis of Resin (A-2) Under a dry nitrogen stream, 15.13 g (0.040 mol) of the hydroxyl group-containing diamine compound (a) obtained in Synthesis Example 1 and 1.24 g (0.005 mol) of 1,3-bis(3-aminopropyl)tetramethyldisiloxane (SiDA) were dissolved in 50 g of N-methyl-2-pyrrolidone (NMP). 15.51 g (0.05 mol) of 3,3',4,4'-diphenylethertetracarboxylic anhydride (ODPA, manufactured by Manac Co., Ltd.) was added together with 21 g of NMP, and the mixture was reacted at 20°C for 1 hour, and then at 50°C for 2 hours. After that, a solution obtained by diluting 14.7 g (0.1 mol) of N,N-dimethylformamide diethyl acetal with 15 g of NMP was added dropwise over 10 minutes. After the dropwise addition, the mixture was stirred at 40°C for 3 hours. After the reaction was completed, the solution was poured into 2 L of water, and the precipitate of the polymer solid was collected by filtration. The polymer solid was dried in a vacuum dryer at 80°C for 72 hours to obtain a polyimide precursor (A) resin (A-2). The weight average molecular weight of the obtained (A) resin (A-2) was measured by GPC and confirmed to be in the range of n = 10 to 100,000.

[0159] (Synthesis Example 5) Synthesis of phenolic resin Under a dry nitrogen stream, 70.2g (0.65 mol) of m-cresol, 37.8g (0.35 mol) of p-cresol, 75.5g of 37% by weight formaldehyde aqueous solution (0.93 mol of formaldehyde), 0.63g (0.005 mol) of oxalic acid dihydrate, and 264g of methyl isobutyl ketone were charged, and then the flask was immersed in an oil bath, and the reaction solution was refluxed while polycondensation reaction was carried out for 4 hours. The temperature of the oil bath was then raised over 3 hours, and the pressure in the flask was then reduced to 30-50mmHg, the volatile matter was removed, and the dissolved resin was cooled to room temperature to obtain a phenolic resin. The weight average molecular weight was 3,500 from GPC.

[0160] (Synthesis Example 6) (B1) Synthesis of 1,2-naphthoquinone-2-diazide-4-sulfonic acid ester compound (B1-1) Under a dry nitrogen stream, 21.22 g (0.05 mol) of TrisP-PA (trade name, manufactured by Honshu Chemical Industry Co., Ltd.), 26.86 g (0.10 mol) of 4-naphthoquinone diazide sulfonyl chloride, and 13.43 g (0.05 mol) of 4-naphthoquinone diazide sulfonyl chloride were dissolved in 50 g of 1,4-dioxane and brought to room temperature. 15.18 g of triethylamine mixed with 50 g of 1,4-dioxane was added dropwise so that the temperature in the system did not exceed 35°C. After the dropwise addition, the mixture was stirred at 30°C for 2 hours. The triethylamine salt was filtered, and the filtrate was poured into water. The precipitate was then collected by filtration. The precipitate was dried in a vacuum dryer to obtain (B1) 1,2-naphthoquinone-2-diazide-4-sulfonic acid ester compound (B1-1) represented by the following formula.

[0161] [ka]

[0162] (Synthesis Example 7) (B2) Synthesis of 1,2-naphthoquinone-2-diazide-5-sulfonic acid ester compound (B2-1) Under a dry nitrogen stream, 15.31 g (0.05 mol) of TrisP-HAP (trade name, manufactured by Honshu Chemical Industry Co., Ltd.) and 40.28 g (0.15 mol) of 5-naphthoquinone diazide sulfonyl acid chloride were dissolved in 450 g of 1,4-dioxane and cooled to room temperature, and the same procedure as in Synthesis Example 2 was repeated to obtain 1,2-naphthoquinone-2-diazide-5-sulfonic acid ester compound (B2-2) represented by the following formula (B2).

[0163] [ka]

[0164] Other compounds having a thermal crosslinking group and antioxidants used in each of the Examples and Comparative Examples are shown below. (C1) Compound having one thermal crosslinking group; Denacol EX-145 (trade name, manufactured by Nagase ChemteX Corporation)

[0165] [ka]

[0166] (C1) Compound having one thermal crosslinking group; MOM-26X (trade name, manufactured by Honshu Chemical Industry Co., Ltd.)

[0167] [ka]

[0168] (C1) Compound having one thermal crosslinking group; 4MOM-P (trade name, manufactured by Honshu Chemical Industry Co., Ltd.)

[0169] [ka]

[0170] (C2) Compound having four or more thermal crosslinking groups; HMOM-TPPHBA (trade name, manufactured by Honshu Chemical Industry Co., Ltd.)

[0171] [ka]

[0172] (C2) Compound having four or more thermal crosslinking groups; NIKALAC MX-270 (trade name, manufactured by Sanwa Chemical Co., Ltd.)

[0173] [ka]

[0174] (C2) Compound having four or more thermal crosslinking groups; NIKALAC MW-100LM (product name, manufactured by Sanwa Chemical Co., Ltd.)

[0175] [ka]

[0176] (C2) Compound having four or more thermal crosslinking groups; TML-BPA (trade name, manufactured by Honshu Chemical Industry Co., Ltd.)

[0177] [ka]

[0178] (D) Antioxidant; “Irgafas” 168 (trade name, manufactured by BASF Japan Ltd.)

[0179] [ka]

[0180] Antioxidant; “Irganox” 245 (product name: manufactured by BASF Japan Ltd.)

[0181] [ka]

[0182] Example 1 100.0 g of the resin (A-1) (A) obtained in Synthesis Example 3, 15.0 g of the 1,2-naphthoquinone-2-diazide-4-sulfonic acid ester compound (B1-1) (B1) obtained in Synthesis Example 6, 24.5 g of DENACOL EX-145 (trade name) as a compound having one thermal crosslinking group (C1), and 7.0 g of HMOM-TPPHBA (trade name) as a compound having four or more thermal crosslinking groups (C2) were weighed out, and 250.0 g of γ-butyrolactone (GBL) was added as a solvent to dissolve the mixture, followed by filtering through a 0.5 μm polytetrafluoroethylene filter (manufactured by Sumitomo Electric Industries, Ltd.) to obtain a photosensitive resin composition (varnish).

[0183] (Examples 2 to 24) A varnish was obtained in the same manner as in Example 1.

[0184] (Comparative Examples 1 to 3) A varnish was obtained in the same manner as in Example 1.

[0185] The types and amounts of (A) resin, (B) photosensitizer, (C) compound having a thermal crosslinking group, and (D) antioxidant of the varnish, and the curing temperature of the photosensitive resin composition are shown in Table 1. The amounts of each component are listed below the numbered columns in Table 1. The solvent used in all Examples and Comparative Examples was 250.0 g of gamma-butyrolactone (GBL).

[0186] [Table 1-1]

[0187] [Table 1-2]

[0188] Using this varnish, the sensitivity, pattern wrinkles after thermal curing, and heat resistance were evaluated by the methods described above. The substrate used to evaluate the sensitivity was an 8-inch silicon wafer. The evaluation results are shown in Table 2.

[0189] [Table 2] [Industrial Applicability]

[0190] INDUSTRIAL APPLICABILITY The resin composition according to the present invention has high heat resistance and can be suitably used, for example, as a semiconductor insulating film, a TFT-LCD insulating film, an electrode protective film, or a substrate material in the manufacture of flexible displays such as organic EL. [Explanation of symbols]

[0191] 1a: Die pad 1b: Lead 1:1a (die pad) + 1b (lead) 2: Semiconductor elements 3: Primer layer 4: Wire 5: Resin sealing layer

Claims

1. A photosensitive resin composition comprising: (A) one or more resins selected from the group consisting of polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, and copolymers thereof; (B) a photosensitizer; and (C) a compound having a thermal crosslinking group, The photosensitive resin composition, wherein the compound (C) having a thermal crosslinking group contains (C1) a compound having one thermal crosslinking group and (C2) a compound having four or more thermal crosslinking groups.

2. 2. The photosensitive resin composition according to claim 1, wherein, when the content of the (C1) compound is CW1 (parts by weight) and the content of the (C2) compound is CW2 (parts by weight) relative to 100 parts by weight of the (A) resin, 1.0≦CW1 / CW2≦3.

0.

3. the thermal crosslinking group of the compound (C1) is a methylol group or an alkoxymethyl group, The photosensitive resin composition according to claim 1 or 2, wherein the four or more thermal crosslinking groups of the compound (C2) are each independently a methylol group or an alkoxymethyl group.

4. the (B) photosensitizer contains (B1) a 1,2-naphthoquinone-2-diazide-4-sulfonic acid ester compound and (B2) a 1,2-naphthoquinone-2-diazide-5-sulfonic acid ester compound; 3. The photosensitive resin composition according to claim 1, wherein, when the content of the (B1) compound is BW1 (parts by weight) and the content of the (B2) compound is BW2 (parts by weight) relative to 100 parts by weight of the (A) resin, 1.0≦BW1 / BW2≦4.

0.

5. 3. The photosensitive resin composition according to claim 1, wherein, when the content of the photosensitizer (B) is BW (parts by weight) and the content of the compound (C) is CW (parts by weight) relative to 100 parts by weight of the resin (A), 0.5≦BW / CW≦1.

0.

6. The photosensitive resin composition according to claim 1 or 2, further comprising (D) an antioxidant.

7. The photosensitive resin composition according to claim 6 , wherein the antioxidant (D) has a hindered phenol structure.

8. A cured film obtained by curing the photosensitive resin composition according to claim 1 or 2.

9. A semiconductor device comprising the cured film according to claim 8.

Citation Information

Patent Citations

  • Resin composition, method of producing patterned resin film, polymer and semiconductor device

    JP2014015507A

  • Protective film for power semiconductor element, and method for forming the same

    JP2016023226A

  • Photosensitive resin composition

    JP2017219850A

  • Photosensitive resin composition, and method for producing cured relief pattern

    JP2020024374A