Aluminum alloy material with superior intergranular corrosion resistance and covering material

By controlling Ti concentration layers in aluminum alloys through rolling processes to achieve a 40 mV potential difference, the material achieves high strength and intergranular corrosion resistance, addressing the limitations of existing methods in aluminum alloys.

JP2024154853APending Publication Date: 2024-10-31MA ALUMINUM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023069007
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing aluminum alloy materials face challenges in achieving both high strength and intergranular corrosion resistance, particularly when using recycled materials or undergoing processes like brazing, as existing methods for suppressing intergranular corrosion are not universally applicable and can increase costs or have limited effectiveness.

Method used

The aluminum alloy material is designed with controlled Ti concentrations through rolling processes, forming layers with specific potential differences to prevent intergranular corrosion, independent of alloy composition, by ensuring a potential difference of 40 mV or less between Ti-concentrated and depleted regions.

Benefits of technology

This approach effectively suppresses intergranular corrosion, allowing for high strength and corrosion resistance without composition adjustments or surface films, applicable to various aluminum alloys including Al-Cu, Al-Mn, Al-Si, and Al-Mg-Si alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154853000001_ABST
    Figure 2024154853000001_ABST
Patent Text Reader

Abstract

To improve the intergranular corrosion resistance of an aluminum alloy material.SOLUTION: An aluminum alloy material includes a solute element-depleted layer adjacent to the grain boundaries, and contains 0.05-0.5 mass% of Ti, wherein, within the crystal, Ti concentration gradient layers that extend in the rolling direction and have varying Ti concentrations are distributed in a layered manner in the plate thickness direction. The Ti concentration gradient layers have a pitch interval of 100 μm or less. The potential difference between the pitting potential in regions within the crystal grains with relatively low Ti concentration and the pitting potential in regions within the solute element-depleted layer with relatively low Ti concentration is 40 mV or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aluminum alloy material and a coating material having excellent resistance to intergranular corrosion. [Background technology]

[0002] Aluminum alloy materials used in structural components, automobile body materials, and heat exchangers for automobiles and air conditioners are required to be highly corrosion resistant as well as strong. In recent years, there has been a growing demand for thinner and smaller parts in order to reduce the amount of aluminum used per part in order to realize a sustainable society, and aluminum alloy materials are desired to have even higher strength. Furthermore, there are studies on increasing the use of recycled materials with the aim of reducing the use of virgin metals, but the content of various impurity elements in the material increases, reducing corrosion resistance, so it is essential to study technologies to improve corrosion resistance.

[0003] Precipitation strengthening by aging is an effective method for increasing the strength of aluminum alloy materials. However, aging not only improves strength, but also induces grain boundary precipitation, forming a solid solution element depleted layer near the grain boundary, which dissolves preferentially when exposed to a corrosive environment, causing intergranular corrosion. Intergranular corrosion is the most undesirable form of corrosion for materials that require material strength and airtightness, because even a small amount of corrosion can cause deep corrosion in the material and relatively quickly turn into a through hole. For this reason, aging conditions are selected that suppress intergranular corrosion at the expense of some strength, and the balance between high strength and high corrosion resistance has not been fully achieved. Even if aging heat treatment is not performed, for example, when brazing heat treatment is performed during the manufacture of a heat exchanger, intergranular corrosion occurs. As a countermeasure for such a case, a method of suppressing intergranular corrosion by appropriately controlling the alloy composition has been proposed (for example, Patent Document 1). Also, a method has been proposed in which a hydrated oxide film is formed on the surface of a material to suppress intergranular corrosion (Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-75378 A [Patent Document 2] JP 2001-20081 A [Patent Document 3] JP 2008-255457 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the technology of adjusting the alloy composition proposed as a method of suppressing intergranular corrosion is not universal because it depends on the alloy composition, and there are cases where countermeasures cannot be taken. For example, when trying to increase the utilization rate of recycled materials, it is a challenge to develop a universal technology to prevent intergranular corrosion because they contain various impurity elements. In addition, the method of forming a film on the surface of the material has problems such as limited applications and increased manufacturing costs. Also, a method of improving corrosion resistance by adding Ti to the composition is known (Patent Document 3). When Ti-added materials are rolled, layers with different Ti concentrations are formed. When Ti dissolves in Al, the potential becomes noble, and potential-concentration layers corresponding to Ti-concentration layers are formed. Since low-concentration layers corrode preferentially compared to high-concentration layers, the corrosion form is layered, and as a result, it is believed that the progression of corrosion in the thickness direction is hindered. However, this Ti-rich layer is indifferent to grain boundaries and intragranular regions, and is distributed across multiple crystal grains, so sufficient corrosion resistance to intergranular corrosion is not obtained.

[0006] The present invention has been made against the background of the above circumstances, and has an object to provide an aluminum alloy material having sufficient resistance to intergranular corrosion without requiring adjustment of the composition or formation of a coating on the surface, and a coating material using the alloy material. [Means for solving the problem]

[0007] As described above, layers with different Ti concentrations are formed by subjecting Ti-added materials to an appropriate rolling process. Here, the potential difference due to the Ti-rich layer is in competition with the potential difference between the pitting potential of the low Ti concentration region within the crystal grain and the low Ti concentration region in the solid solution element depleted layer near the grain boundary. In this case, intergranular corrosion can be suppressed by controlling the potential difference between the pitting potential of the low Ti concentration region within the crystal grain and the low Ti concentration region in the solid solution element depleted layer near the grain boundary to 40 mV or less. The technology of the present invention can overcome the trade-off between high strength and intergranular corrosion. Furthermore, since the technology of the present invention does not depend on the alloy composition, it can be generally effective for any intergranular corrosion that is preferentially dissolved by the solute element depleted layer.

[0008] That is, a first embodiment of the aluminum alloy material excellent in intergranular corrosion resistance according to the present invention is an aluminum alloy material having a solid solution element depleted layer, containing 0.05 to 0.5 mass% of Ti, and having Ti-shape layers extending along the rolling direction and having different Ti concentrations distributed in a layered manner in the sheet thickness direction within the crystal, The pitch interval of the Ti-rich layers is 100 μm or less, and the potential difference between the pitting potential of the layer region having a relatively low Ti concentration within the crystal grain and the pitting potential of the solid solution element depleted layer having a relatively low Ti concentration is 40 mV or less.

[0009] Another aspect of the invention of the aluminum alloy material excellent in intergranular corrosion resistance is the invention of the above aspect, wherein the aluminum alloy material is any one of an Al-Cu based alloy, an Al-Mn based alloy, an Al-Si based alloy, an Al-Mg-Si based alloy, and an Al-Mg-Si-Cu based alloy.

[0010] The present invention provides an aluminum alloy material having excellent intergranular corrosion resistance in accordance with the above-mentioned embodiment, wherein the aluminum alloy material has an alloy composition selected from the group consisting of a JIS A2000 series alloy, an A3000 series alloy, an A4000 series alloy, and an A6000 series alloy.

[0011] In still another embodiment of the invention of the aluminum alloy material having excellent intergranular corrosion resistance, in the above-mentioned embodiment of the invention, the Ti concentration in the relatively high-concentration layer in the Ti-rich layer is 0.3 mass% or more, and the Ti concentration in the relatively low-concentration region in the solid solution element depleted layer is less than 0.1 mass%.

[0012] In a first embodiment of the invention, the aluminum alloy material described in the above embodiment is used as a core material, and one or more layers of aluminum or aluminum alloy skin material are laminated to one or both sides of the core material.

[0013] Another embodiment of the coating material comprises one or more layers of skin material bonded to one or both sides of an aluminum or aluminum alloy core material, and at least one layer of the skin material is made of the aluminum alloy material described above.

[0014] The contents stipulated in the present invention will be explained below. Contains 0.05 to 0.5 mass% Ti Ti forms layers of different Ti concentrations through a peritectic reaction during casting and a subsequent appropriate rolling process. Below the lower limit, the light and dark layers are distributed coarsely, and sufficient effect cannot be obtained. Above the upper limit, coarse intermetallic compounds (crystallized products) are formed during casting, reducing rollability. For the same reason, it is preferable to set the lower limit at 0.08% and the upper limit at 0.3%.

[0015] The pitch interval in the thickness direction of the layers with high and low Ti concentrations is 100 μm or less If the pitch interval of the Ti-tinned layers is too large, they will not be able to cross the grains sufficiently, and the effect of suppressing intergranular corrosion will not be obtained. Therefore, the pitch interval must be controlled to 100 μm or less.

[0016] The difference between the pitting potential of the region with low Ti concentration within the crystal grain (excluding the solute element depleted layer near the grain boundary) and the pitting potential of the region with low Ti concentration in the solute element depleted layer near the grain boundary is 40 mV or less. Corrosion at the grain boundaries can be suppressed by controlling the potential difference between the pitting potential of the region with low Ti concentration within the crystal grain (excluding the solute element depleted layer near the grain boundary) and the pitting potential of the region with low Ti concentration in the solute element depleted layer near the grain boundary to 40 mV or less. If this potential difference exceeds 40 mV, the effect of the Ti-rich layer in suppressing intergranular corrosion cannot be obtained. Therefore, the potential difference must be controlled to 40 mV or less. The solute-element-depleted zone near the grain boundary refers to a region about 500 nm wide on either side of the grain boundary where the amount of solute elements other than Ti is reduced compared to the center of the grain.

[0017] Aluminum alloy material The aluminum alloy material has a solute element depleted layer formed therein and has the property of preferential dissolution of the solute element depleted layer, and can be applied to a wide range of alloys containing Ti. Examples of alloys used in this type of alloy material include Al-Cu alloys, Al-Mn alloys, Al-Si alloys, Al-Mg-Si alloys, and Al-Mg-Si-Cu alloys, and in terms of JIS numbers, JIS A2000 series alloys, A3000 series alloys, A4000 series alloys, and A6000 series alloys.

[0018] Ti concentration For example, in the Ti-rich layer, the high concentration layer has a Ti content of 0.3 mass % or more, and the low concentration layer has a Ti content of less than 0.1 mass %. Effect of the Invention

[0019] According to the present invention, the potential difference between a solute element depleted layer having a high Ti concentration and a matrix having a low Ti concentration is reduced, thereby making it possible to suppress preferential dissolution of the solute element depleted layer along the grain boundaries, and to obtain an aluminum alloy material having excellent intergranular corrosion resistance. [Brief description of the drawings]

[0020] [Figure 1] 1 shows a conceptual diagram of a crystal structure in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] An embodiment of the present invention will be described below. The alloy compositions used are Al-Cu alloys, Al-Mn alloys, Al-Si alloys, Al-Mg-Si alloys, Al-Mg-Si-Cu alloys, or JIS A2000 series alloys, A3000 series alloys, A4000 series alloys, and A6000 series alloys, and these alloy compositions contain 0.05 to 0.5 mass % Ti. The Al-Cu alloy contains Cu: 0.5-6.0%, and may further contain, as desired, Si: 0.01-1.5%, Fe: 0.01-1.5%, Mn: 0.05-2.0%, Mg: 0.05-2.0%, and 0.5% or less of one or more of Zr, Cr, Sr, V, and Zn. The Al-Mn alloy contains 0.5-2.5% Mn, and may further contain, as desired, 0.05-2.0% Si, 0.01-1.5% Fe, 0.05-2.0% Cu, 0.01-2.0% Mg, 0.05-8.0% Zn, and 0.5% or less of one or more of Zr, Cr, Sr, and V. The Al-Si alloy contains 0.5-12.5% ​​Si, and may further contain, as desired, 0.01-0.7% Mn, 0.01-1.5% Fe, 0.1-3.5% Cu, 0.01-1.0% Mg, 0.05-5.0% Zn, and 0.5% or less of one or more of Zr, Cr, Sr, and V. The Al-Mg-Si alloy contains 0.5-2.0% Mg and 0.1-2.0% Si, and may further contain, as desired, 0.01-1.2% Mn, 0.01-1.5% Fe, 0.05-5.0% Zn, and 0.5% or less of one or more of Zr, Cr, Sr, and V. The Al-Mg-Si-Cu alloy contains 0.5-2.0% Mg, 0.1-2.0% Si, 0.05-1.0% Cu, and may further contain, as desired, 0.01-1.2% Mn, 0.01-1.5% Fe, 0.05-5.0% Zn, and 0.5% or less of one or more of Zr, Cr, Sr, and V. Each of the above alloys may contain 0.05 to 0.5 mass % Ti, with the balance being Al and unavoidable impurities.

[0022] The alloy undergoes the steps of casting ⇒ homogenization ⇒ facing ⇒ soaking ⇒ hot rolling ⇒ cold rolling, and further undergoes intermediate annealing and final annealing as necessary.

[0023] During casting, it is desirable to set the cooling rate to 0.2°C / sec or more and less than 25°C / sec. If the cooling rate during casting is less than 0.2°C / sec, the Al3Ti will be coarse and sparsely distributed, resulting in an unsatisfactory pitch interval between the Ti-rich layers. If the cooling rate is more than 25°C / sec, the cooling rate is too fast and the peritectic reaction will not proceed sufficiently, making it impossible to form a layer with a high Ti concentration.

[0024] The homogenization treatment is not limited to specific conditions, but may be performed, for example, at 400 to 500° C. for 1 to 10 hours. The reason for this is to eliminate distortion that occurs during cooling and to homogenize the distribution of elements that diffuse quickly.

[0025] The soaking can be carried out, for example, at 450 to 530° C. for one hour or more. The metal heat treatment is carried out in preparation for hot rolling.

[0026] The hot rolling and cold rolling can be carried out by conventional methods.

[0027] Intermediate annealing Intermediate annealing can be performed during the cold rolling, for example, at 200 to 450° C. for 1 to 10 hours. Intermediate annealing is performed to soften the material to ensure rollability and to adjust the reduction rate in the final rolling.

[0028] Final annealing After the cold rolling, final annealing can be performed. For example, the final annealing is performed at 200 to 450° C. for 1 to 10 hours. The final annealing is performed for the purpose of controlling mechanical properties.

[0029] [Aging process] If necessary, aging treatment is performed to improve the material strength. The aging treatment may be performed after cold rolling and then solution treatment, or may be performed without solution treatment. The aging treatment is suitably performed under conditions of, for example, 180 to 450° C. and 1 to 1000 minutes. The solution treatment is carried out, for example, at 300 to 580° C. for 1 to 180 minutes, and then water-cooled.

[0030] The relationship between the aging conditions and the potential difference cannot be specified in general because the conditions differ for each alloy. Since aging promotes grain boundary precipitation and forms a solute element depleted layer near the grain boundary, it is necessary to control the aging conditions so that the potential difference between the pitting potential of the region with low Ti concentration within the crystal grain and the pitting potential of the region with low Ti concentration in the solute element depleted layer near the grain boundary does not exceed 40 mV.

[0031] [Brazing heat treatment] If necessary, a brazing heat treatment is performed. The brazing heat treatment may be performed after cold rolling or after recrystallization annealing. In addition, after the brazing heat treatment, an aging treatment may be performed to improve the material strength. The relationship between the cooling rate and potential difference during brazing cannot be specified in general because the conditions differ for each alloy. Brazing heat treatment can form a metal structure similar to solution treatment at high temperatures, but if the cooling rate is slow after that, grain boundary precipitation is promoted and a solid solution element depleted layer is formed near the grain boundaries, so it is necessary to control the cooling rate so that the potential difference between the pitting potential of the area with low Ti concentration within the crystal grains and the pitting potential of the area with low Ti concentration in the solid solution element depleted layer near the grain boundaries does not exceed 40 mV. The brazing conditions can be, for example, to hold at 590 to 610°C for 1 to 600 seconds, and then control the cooling rate to 150°C at 5 to 200°C / min.

[0032] Total heat input ΣDt when heat treatment is performed on material after rolling is completed Total heat input ΣDt<25.0×10 -10 When heat treatment is applied to the material after rolling, there are processes such as temper annealing, aging heat treatment, and brazing heat treatment, but if the heat input in these processes is excessive, Ti will diffuse and the concentration difference between the Ti-shape layers will not be maintained. In addition, the concentration difference will become small and the pitch interval between the Ti-shape layers will not be able to be maintained. For the same reason, ΣDt<25.0×10 -10 It is preferable that ΣDt<15.0×10 -10 It is. Here, ΣDt means that t is the heat treatment time (s), which is the time from room temperature to the target temperature and then cooling to 100°C. Also, D is the diffusion coefficient of Zn (cm 2 / s) is used to calculate the D is calculated using the following formula: In D=D0exp(-Q / RT), D0: 1.77×10 -1 (cm 2 / s) Q: 118(kJ / mol) R: 8.3145(J / Kmol) T: Temperature (K)

[0033] In the produced aluminum alloy, as shown in FIG. 1, a low Ti concentration layer 2 having a relatively low Ti concentration and a high Ti concentration layer 3 having a relatively high Ti concentration are formed in the crystal 1 along the rolling direction. The pitch interval t between the low Ti concentration layer 2 and the high Ti concentration layer 3 is 100 μm or less. The pitch interval can be determined, for example, by the distance between the ends of one of the adjacent high Ti concentration layers 3, 3. The pitch between the layers is achieved by adding an appropriate amount of Ti and appropriately controlling the cooling rate during casting and the total heat input ΣDt when the material after rolling is subjected to heat treatment. The high Ti concentration layer 3 has a Ti content of 0.3 mass% or more, and the low Ti concentration layer 2 has a Ti content of less than 0.1 mass%.

[0034] In the crystal 1, a solute element depleted layer 4 containing Si, Cu, Mg, Mn, and the like, except for Ti, is formed along the grain boundary 1A. The elements depleted in the solute element depleted layer 4 depend on the composition. In the Ti low concentration layer 2, the potential E M In the case where the Ti-rich layer 3 has a potential change amount ΔE Ti Add E M +ΔE Ti As a result, the Ti high concentration layer 3 becomes relatively more noble than the Ti low concentration layer 2, and the Ti low concentration layer 2 corrodes preferentially. In the solute element depleted layer 4, a region where Ti is present at a high concentration and a region where Ti is present at a low concentration are present so as to straddle each other. Therefore, in the solute element depleted layer 4, in the region where the Ti concentration is relatively low, the potential E I In the region where the Ti concentration is relatively high, the potential change due to Ti solid solution ΔE Ti Add E I +ΔE Ti In this embodiment, E M and E I The potential difference between E and E is 40mV or less. M and E I The potential difference is achieved by appropriately controlling the aging conditions when aging treatment is performed, the cooling rate after brazing heat treatment when brazing heat treatment is performed for each alloy type, and the total heat input ΣDt when heat treatment is performed on the material after rolling.

[0035] The obtained alloy can be widely used as a material having excellent resistance to intergranular corrosion.

[0036] In the above embodiment, the aluminum alloy material of the present invention has been described as a single material. However, the aluminum alloy material may be used as a bare material, or may be used as a constituent material of a multi-layer material. In the multi-layer material, the above-mentioned aluminum alloy material may be used as a core material and / or a skin material.

[0037] When the aluminum alloy material is used as the core material, the skin material can have one or more layers of aluminum or aluminum alloy. The material of the skin material may be the aluminum alloy material of the present invention, or other aluminum or aluminum alloys may be used, and the material used for the skin material is not limited to a specific one.

[0038] When the aluminum alloy material is used as a skin material, aluminum or an aluminum alloy is used as a core material. The material of the core material may be the aluminum alloy material of the present invention, or other aluminum or aluminum alloys, and the material used for the core material is not limited to a specific one. The skin material may be one layer or two or more layers, and when two or more layers are provided, the material of the other skin material may be the aluminum alloy material of the present invention, or other aluminum or aluminum alloys, and the other materials used for the skin material are not limited to a specific one. In the previous or present paragraph, when the skin material has two or more layers, the compositions of the skin materials may be the same or different.

[0039] The multi-layered material can be manufactured through normal procedures and is not limited to a specific method. In this process, the cooling rate during casting, the total heat input ΣDt when heat treating the material after rolling, etc. are appropriately controlled to ensure the pitch interval of the Ti-rich layers and the potential difference between the pitting potential of the layer area with a relatively low Ti concentration in the crystal grain and the pitting potential of the solid solution element depleted layer with a relatively low Ti concentration. EXAMPLES

[0040] The aluminum alloy shown in Table 1 (the balance being Al and unavoidable impurities) was cast, homogenized, hot-rolled, and cold-rolled to a plate thickness of 0.3 mm. Then, final annealing, solution treatment, aging treatment, and brazing treatment were performed. Casting was performed at the casting cooling rate shown in Table 1, homogenization treatment was performed at 520°C for 5 hours, soaking treatment was performed at 480°C for 2 hours, and solution treatment, aging treatment, and brazing were performed under the conditions shown in Table 1 to obtain the test materials. For the obtained test materials, the pitch interval between the Ti-tinned and Ti-tinned layers and the potential difference of the pitting corrosion potential were measured.

[0041] -Pitch interval of Ti-shaded layers After filling the cross section of the material with resin, it was polished with emery and buffed to a mirror surface, and then element concentration surface analysis was performed from the cross section direction using FE-EPMA (electron emission type electron probe microanalyzer, JEOL: JXA-8530F). 2 The pitch was defined as the distance between one end of adjacent Ti-rich layers.

[0042] The potential difference between the pitting potential of the region with low Ti concentration within the crystal and the pitting potential of the region with low Ti concentration in the solid solution element depleted layer near the grain boundary The sample was cut to 15 x 50 mm, and the masked test material, leaving an exposed area of ​​10 x 10 mm, was etched in a 5% NaOH aqueous solution at 50°C for 30 seconds, rinsed with pure water, and then desmutted in a HNO3 aqueous solution at room temperature for 60 seconds. The material was washed again with pure water, and then used as the electrolyte a 5% NaCl aqueous solution with a pH adjusted to 3 with acetic acid at room temperature, and after sufficient degassing with high-purity nitrogen gas, the anodic polarization measurement was carried out. The anodic polarization measurement was carried out by measuring the natural immersion potential for 290 seconds, and then measuring the potential from that potential at a potential sweep rate of 0.1 mV / s until the anodic current reached 20 mA / cm. 2 A potential sweep was performed until flow occurred.

[0043] After that, the samples that had undergone polarization measurement were etched for 5 seconds in a 5% NaOH solution at 50°C, washed with pure water, and desmutted for 10 seconds in a HNO3 solution at room temperature, and then the anodic polarization measurement was carried out again under the same conditions. Here, the pitting potential is defined as the potential at which the current value increases sharply in response to the potential sweep.

[0044] The pitting potential obtained in the first polarization measurement is defined as the pitting potential of the region with low Ti concentration in the solid solution element depleted layer near the grain boundary, and the pitting potential obtained in the second polarization measurement is defined as the pitting potential of the region with low Ti concentration within the crystal, and the potential difference between them can be calculated. Note that Ag / AgCl was used as the reference electrode.

[0045] -Evaluation of intergranular corrosion resistance The sample was cut to 15 x 70 mm, and masked leaving an exposed area of ​​10 x 20 mm. - +100ppmSO4 2- Electric charge of 1mA / cm in aqueous solution 2 An anodic dissolution test was carried out with an electrical charge of ×5 hours. After the anodic dissolution test, the samples were immersed in a boiled phosphoric acid chromic acid mixed solution for 10 minutes to remove the corrosion products, and then the corroded areas were filled with resin and emery polished and buffed to a mirror finish. The cross sections were then observed with an optical microscope to confirm the state of dissolution at the grain boundaries and within the grains, and the intergranular corrosion properties were evaluated. Those in which the grain boundary dissolution was predominant were marked with ×, those in which the grain boundaries and within the grains were dissolved to the same extent were marked with 〇, and those in which the intragranular dissolution was predominant were marked with 〇〇.

[0046] [Table 1] [Explanation of symbols]

[0047] 1 crystal 1A grain boundary 2 Ti low concentration layer 3 Ti high concentration layer 4. Solute element depleted zone t Pitch interval

Claims

1. An aluminum alloy material having a solute element depleted layer adjacent to a grain boundary, containing 0.05 to 0.5 mass % Ti, and having Ti-shape layers extending along a rolling direction and having different Ti concentrations distributed in a layered manner in a sheet thickness direction within a crystal, An aluminum alloy material having excellent resistance to intergranular corrosion, wherein the pitch interval of the Ti-shape layers is 100 μm or less, and the potential difference between the pitting potential of a region of the layer having a relatively low Ti concentration within a crystal grain and the pitting potential of a region of the solid solution element depleted layer having a relatively low Ti concentration is 40 mV or less.

2. 2. The aluminum alloy material having excellent intergranular corrosion resistance according to claim 1, wherein the aluminum alloy material is any one of an Al-Cu alloy, an Al-Mn alloy, an Al-Si alloy, an Al-Mg-Si alloy, and an Al-Mg-Si-Cu alloy.

3. 2. The aluminum alloy material according to claim 1, wherein the aluminum alloy material has an alloy composition selected from the group consisting of a JIS A2000 series alloy, an A3000 series alloy, an A4000 series alloy and an A6000 series alloy.

4. The Ti concentration of the relatively high concentration layer in the Ti-shape layer is 0.3 mass% or more, and the Ti concentration of the relatively low concentration region in the Ti-shape layer is less than 0.1 mass%. The aluminum alloy material having excellent intergranular corrosion resistance according to any one of claims 1 to 3.

5. A multi-layer material comprising the aluminum alloy material according to any one of claims 1 to 3 as a core material, and one or more layers of aluminum or aluminum alloy skin material laminated to one or both sides of the core material.

6. 5. A multi-layer material comprising the aluminum alloy material according to claim 4 as a core material, and one or more layers of aluminum or aluminum alloy skin material laminated to one or both sides of the core material.

7. A multilayer material comprising one or more layers of skin material laminated to one or both sides of an aluminum or aluminum alloy core material, at least one layer of the skin material being made of the aluminum alloy material according to any one of claims 1 to 3.

8. 5. A multi-layer material comprising one or more layers of skin material laminated to one or both sides of an aluminum or aluminum alloy core material, at least one layer of said skin material being made of the aluminum alloy material according to claim 4.

Citation Information

Patent Citations

  • Reinforcing member for transport excellent in integranular corrosion resistance

    JP2001020081A

  • Aluminum alloy piping material for heat exchanger, and its manufacturing method

    JP2008255457A

  • Aluminum alloy material having excellent intergranular corrosion resistance

    JP2017075378A