Optical sensor and manufacturing method for optical sensor
The optical sensor addresses the issue of large dark currents in graphene-based sensors by employing a nanocarbon layer with controlled conductivity regions and electrodes, achieving reduced dark current and enhanced sensitivity.
Patent Information
- Application Number
- JP2023069068
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional optical sensors using photoconductors containing graphene suffer from large dark currents, hindering sensitivity improvements.
The optical sensor incorporates a nanocarbon material layer with distinct regions of different conductivity types, modulated by specific electrodes and films, and applies electric fields to enhance carrier concentration, functioning as a pn junction photodiode to reduce dark current.
This configuration effectively suppresses dark current and enhances sensitivity by aligning conductivity types without causing dielectric breakdown, improving overall performance.
Smart Images

Figure 2024154869000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to optical sensors and methods for manufacturing optical sensors. [Background technology]
[0002] Graphene, a two-dimensional layered material, has excellent electrical properties and flexibility, and therefore applications to transparent conductive films and flexible devices have been attempted. Graphene has a strong interaction with light, and in recent years, it is expected to be applied to optical sensors using photoconductors containing graphene. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-005655 A [Patent Document 2] JP 2011-216714 A [Patent Document 3] JP 2019-029365 A Summary of the Invention [Problem to be solved by the invention]
[0004] Conventional optical sensors using photoconductors containing graphene have a large dark current, making it difficult to improve sensitivity.
[0005] An object of the present disclosure is to provide an optical sensor capable of improving sensitivity and a method for manufacturing the optical sensor. [Means for solving the problem]
[0006] According to one embodiment of the present disclosure, there is provided an optical sensor having a nano-carbon material layer having a first region and a second region, a first electrode connected to the first region, a second electrode connected to the second region, a first film that imparts a first conductivity type to the first region, a second film that imparts a second conductivity type different from the first conductivity type to the second region, a first control electrode that applies an electric field to the first region, and a second control electrode that applies an electric field to the second region. Effect of the Invention
[0007] According to the present disclosure, sensitivity can be improved. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a plan view showing the optical sensor according to the first embodiment. [Diagram 2] 1 is a cross-sectional view showing an optical sensor according to a first embodiment. [Diagram 3] FIG. 2 is a schematic diagram showing a first monomolecular film. [Figure 4] FIG. 2 is a schematic diagram showing a second monolayer. [Diagram 5] 1A to 1C are cross-sectional views (part 1) illustrating a first example of a method for manufacturing the optical sensor according to the first embodiment. [Figure 6] 5A to 5C are cross-sectional views (part 2) illustrating the first example of the method for manufacturing the optical sensor according to the first embodiment. [Figure 7] 5A to 5C are cross-sectional views (part 3) illustrating the first example of the method for manufacturing the optical sensor according to the first embodiment. [Figure 8] 4 is a cross-sectional view (part 4) illustrating the first example of the method for manufacturing the optical sensor according to the first embodiment. FIG. [Figure 9] 5 is a cross-sectional view (part 5) illustrating the first example of the method for manufacturing the optical sensor according to the first embodiment. FIG. [Figure 10] 6 is a cross-sectional view (part 6) illustrating the first example of the method for manufacturing the optical sensor according to the first embodiment. FIG. [Figure 11] 7 is a cross-sectional view (part 7) illustrating the first example of the method for manufacturing the optical sensor according to the first embodiment. FIG. [Figure 12]8 is a cross-sectional view (part 8) illustrating the first example of the method for manufacturing the optical sensor according to the first embodiment. FIG. [Figure 13] 6A to 6C are cross-sectional views (part 1) illustrating a second example of the method for manufacturing the optical sensor according to the first embodiment. [Figure 14] 6 is a cross-sectional view (part 2) showing a second example of the method for manufacturing the optical sensor according to the first embodiment. FIG. [Figure 15] FIG. 11 is a cross-sectional view showing an optical sensor according to a second embodiment. [Figure 16] 10A to 10C are cross-sectional views (part 1) illustrating a method for manufacturing an optical sensor according to a second embodiment. [Figure 17] 11A to 11C are cross-sectional views (part 2) illustrating the method for manufacturing the optical sensor according to the second embodiment. [Figure 18] 11A to 11C are cross-sectional views (part 3) illustrating the method for manufacturing the optical sensor according to the second embodiment. [Figure 19] 11A to 11C are cross-sectional views (part 4) illustrating the method for manufacturing the optical sensor according to the second embodiment. [Figure 20] 13A to 13C are cross-sectional views (part 5) illustrating the method for manufacturing the optical sensor according to the second embodiment. [Figure 21] 13A to 13C are cross-sectional views (part 6) illustrating the method for manufacturing the optical sensor according to the second embodiment. [Figure 22] 7 is a cross-sectional view (part 7) illustrating the method for manufacturing the optical sensor according to the second embodiment. [Diagram 23] 8 is a cross-sectional view (part 8) illustrating the method for manufacturing the optical sensor according to the second embodiment. FIG. [Figure 24] 9A to 9C are cross-sectional views illustrating the method for manufacturing the optical sensor according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configurations are denoted by the same reference numerals, and redundant description may be omitted.
[0010] (First embodiment) First, a first embodiment will be described. The first embodiment relates to an optical sensor. Fig. 1 is a plan view showing an optical sensor according to the first embodiment. Fig. 2 is a cross-sectional view showing an optical sensor according to the first embodiment. Fig. 2 corresponds to a cross-sectional view taken along line II-II in Fig. 1.
[0011] 1 and 2, the optical sensor 100 according to the first embodiment has a substrate 101 and a base material 103 including a silicon oxide (SiO2) film 102. For example, the substrate 101 is a silicon (Si) substrate, and the silicon oxide film 102 is formed on the surface of the substrate 101. The base material 103 is, for example, a Si substrate with a thermal oxide film.
[0012] A first control electrode 151 is provided on the silicon oxide film 102. The first control electrode 151 applies an electric field to a first region 131 of the graphene layer 130 described below, and injects charges into the first region 131. The first control electrode 151 modulates the carrier concentration of the first region 131. The material of the first control electrode 151 is not particularly limited, and may be, for example, Au or Pd.
[0013] A first insulating film 111 is provided on the silicon oxide film 102 to cover the first control electrode 151. The material of the first insulating film 111 is not particularly limited, and may be, for example, silicon oxide (SiO2), aluminum oxide (Al2O3), hafnium oxide (HfO2), titanium oxide (TiO2), zirconium oxide (ZrO2), tantalum oxide (Ta2O5), silicon nitride (Si3N4), or aluminum nitride (AlN). The thickness of the first insulating film 111 is, for example, about 1 nm to 1 μm.
[0014] The second control electrode 152 is provided on the first insulating film 111. The second control electrode 152 is provided at a position away from the first control electrode 151 in a plan view. Specifically, the first control electrode 151 and the second control electrode 152 are aligned with each other in a first direction parallel to the surface of the substrate 101, and the second control electrode 152 is provided on the negative side of the first control electrode 151 in the first direction. The second control electrode 152 applies an electric field to a second region 132 of the graphene layer 130 described later, and injects charges into the second region 132. The second control electrode 152 modulates the carrier concentration of the second region 132. The material of the second control electrode 152 is not particularly limited, and for example, Au or Pd may be used.
[0015] The second insulating film 112 is provided on the first insulating film 111 to cover the second control electrode 152. The second insulating film 112 is provided at a position away from the first control electrode 151 in a plan view. Specifically, the second insulating film 112 is provided on the negative side of the first control electrode 151 in the first direction. That is, the second insulating film 112 does not exist above the first control electrode 151. The material of the second insulating film 112 is different from the material of the first insulating film 111. The material of the second insulating film 112 is not particularly limited as long as it is different from the material of the first insulating film 111, and may be, for example, SiO2, Al2O3, HfO2, TiO2, ZrO2, Ta2O5, Si3N4, or AlN. The thickness of the second insulating film 112 is, for example, about 1 nm to 1 μm.
[0016] The first film 121 is provided on a portion of the upper surface of the first insulating film 111 where the second insulating film 112 is not provided, i.e., on a portion of the upper surface of the first insulating film 111 exposed from the second insulating film 112. The first film 121 imparts a first conductivity type, here a p-type conductivity type, to a nanocarbon material such as graphene by chemical doping. The first film 121 has, for example, a first monomolecular film.
[0017] Here, a first monolayer, which is an example of the first film 121, will be described. FIG. 3 is a schematic diagram showing the first monolayer. The first monolayer 21, which is an example of the first film 121, has a structure in which a plurality of molecules 160 are arranged on the upper surface of the first insulating film 111. The first monolayer 21 is, for example, a self-assembled monolayer (SAM) film. The molecule 160 has an alkyl group 161, a binding functional group 162, and an electron-withdrawing functional group 163. The binding functional group 162 is connected to one end of the alkyl group 161, and the functional group 163 is connected to the other end of the alkyl group 161.
[0018] The bonding functional group 162 has a property of easily bonding to the first insulating film 111. If the first insulating film 111 is a SiO2 film, the bonding functional group 162 is, for example, -Si(CH3)2H or -OH. If the first insulating film 111 is an Al2O3 film, the bonding functional group 162 is, for example, -COOH or -PO3H2. If the first insulating film 111 is a HfO2 film, the bonding functional group 162 is, for example, -PO3H2, -COOH, or C6H6O2 (catechol group). If the first insulating film 111 is a ZrO2 film, TiO2 film, or Ta2O5 film, the bonding functional group 162 is, for example, -PO3H2. If the first insulating film 111 is a Si3N4 film, the bonding functional group 162 is, for example, -Br or -CH=CH2. If the first insulating film 111 is an AlN film, the bonding functional group 162 is, for example, —SiOCH 3 or —SiOC 2 H 5. Due to the function of the bonding functional group 162, the molecule 160 is adsorbed to the first insulating film 111.
[0019] The electron-withdrawing functional group 163 is, for example, -CHO, -COOR, -COOH, -COR, -SO3H, -CN, -NO2, -NR3 or halogen, and draws electrons from the nanocarbon material to impart p-type conductivity to the nanocarbon material. R is a hydrocarbon group such as a methyl group or an ethyl group.
[0020] A second film 122 is provided on the upper surface of the second insulating film 112. The second film 122 imparts a second conductivity type, here an n-type conductivity type, to a nanocarbon material such as graphene by chemical doping. The second film 122 has, for example, a second monolayer.
[0021] Here, the second monomolecular film, which is an example of the second film 122, will be described. FIG. 4 is a schematic diagram showing the second monomolecular film. The second monomolecular film 22, which is an example of the second film 122, has a structure in which a plurality of molecules 170 are arranged on the upper surface of the second insulating film 112. The second monomolecular film 22 is, for example, a SAM film. The molecule 170 has an alkyl group 171, a binding functional group 172, and an electron-donating functional group 173. The binding functional group 172 is connected to one end of the alkyl group 171, and the functional functional group 173 is connected to the other end of the alkyl group 171.
[0022] The bonding functional group 172 has a property of easily bonding to the second insulating film 112. If the second insulating film 112 is a SiO2 film, the bonding functional group 172 is, for example, -Si(CH3)2H or -OH. If the second insulating film 112 is an Al2O3 film, the bonding functional group 172 is, for example, -COOH or -PO3H2. If the second insulating film 112 is a ZrO2 film, a TiO2 film, or a Ta2O5 film, the bonding functional group 172 is, for example, -PO3H2. If the second insulating film 112 is a Si3N4 film, the bonding functional group 172 is, for example, -Br or -CH=CH2. If the second insulating film 112 is an AlN film, the bonding functional group 172 is, for example, -SiOCH3 or -SiOC2H5. Due to the function of the bonding functional group 172, the molecule 170 is adsorbed to the second insulating film 112.
[0023] The electron-donating functional group 173 is, for example, -NH2, -NR2, -OH, -OR, -NHCOR, -OCOR, -R, or an aryl group, and donates electrons to the nanocarbon material to impart n-type conductivity to the nanocarbon material. The aryl group is a functional group such as a phenyl group, a tolyl group, or a xylyl group derived from an aromatic hydrocarbon.
[0024] A graphene layer 130 is provided on the first film 121 and the second film 122. The graphene layer 130 includes one or more graphenes stacked on each other. The graphene layer 130 has a first region 131 on the first film 121 and a second region 132 on the second film 122.
[0025] The first electrode 141 is provided on the first region 131, and the second electrode 142 is provided on the second region 132. The first electrode 141 is provided on the positive side of the first control electrode 151 in the first direction, and the second electrode 142 is provided on the negative side of the second control electrode 152 in the first direction. Therefore, the first control electrode 151 and the second control electrode 152 are located between the first electrode 141 and the second electrode 142 in the first direction. The material of the first electrode 141 and the second electrode 142 is not particularly limited, and for example, Au, Pd, Ni, Cr, or Ti may be used. The first electrode 141 and the second electrode 142 may include a laminate of these metals. For example, the first electrode 141 and the second electrode 142 may include a laminate of a Ti film and an Au film formed on the Ti film, or may include a laminate of a Cr film and an Au film formed on the Cr film. The first electrode 141 and the second electrode 142 may be made of the same material or different materials.
[0026] In the optical sensor 100 according to the first embodiment configured as described above, when a negative voltage is applied to the first control electrode 151, holes are injected into the first region 131 of the graphene layer 130 by the electric field generated by the first control electrode 151. When a positive voltage is applied to the second control electrode 152, electrons are injected into the second region 132 of the graphene layer 130 by the electric field generated by the second control electrode 152. Therefore, the graphene layer 130 functions as a pn junction photodiode. Therefore, according to the first embodiment, it is possible to reduce the dark current compared to a photoconductor including graphene.
[0027] Moreover, the first region 131 is given a p-type conductivity by the first film 121, and the second region 132 is given an n-type conductivity by the second film 122. Therefore, the conductivity type of the first region 131 is more inclined toward p-type than in the case where only the electric field generated by the first control electrode 151 is applied, and the conductivity type of the second region 132 is more inclined toward n-type than in the case where only the electric field generated by the second control electrode 152 is applied. Therefore, the conductivity type of the first region 131 can be sufficiently greatly inclined toward p-type without applying a high voltage from the first control electrode 151 to the first insulating film 111 that would cause dielectric breakdown. Moreover, the conductivity type of the second region 132 can be sufficiently greatly inclined toward n-type without applying a high voltage from the second control electrode 152 to the second insulating film 112 that would cause dielectric breakdown.
[0028] Therefore, according to the first embodiment, it is possible to suppress the dark current and improve the sensitivity.
[0029] Next, a first example of a method for manufacturing the optical sensor 200 according to the first embodiment will be described. Figures 5 to 12 are cross-sectional views showing the first example of a method for manufacturing the optical sensor 100 according to the first embodiment.
[0030] In the first example, first, as shown in FIG. 5, a base material 103 is prepared. The base material 103 is, for example, a Si substrate with a thermal oxide film. Next, a first control electrode 151 is formed on the silicon oxide film 102. In forming the first control electrode 151, for example, a resist mask having an opening by lithography where the first control electrode 151 is to be formed is formed, then the material of the first control electrode 151 is deposited by a vapor deposition method or a sputtering method, and then the resist mask is removed. That is, for example, a lift-off process is adopted.
[0031] 6, a first insulating film 111 covering the first control electrode 151 is formed on the silicon oxide film 102. The first insulating film 111 can be formed by, for example, an atomic layer deposition (ALD) method, a chemical vapor deposition (CVD) method, an evaporation method, or a sputtering method.
[0032] 7, the second control electrode 152 is formed on the first insulating film 111. In forming the second control electrode 152, for example, a resist mask having an opening at a portion where the second control electrode 152 is to be formed is formed by lithography, then the material of the second control electrode 152 is deposited by a vapor deposition method or a sputtering method, and then the resist mask is removed. That is, for example, a lift-off process is adopted.
[0033] Subsequently, as shown in FIG. 8, a resist mask 191 having an opening formed by lithography in a portion where the second insulating film 112 is to be formed is formed on the first insulating film 111.
[0034] 9, an insulating film 112A made of the material of the second insulating film 112 is deposited on the first insulating film 111, the second control electrode 152, and the resist mask 191. The insulating film 112A is formed so as to cover the second control electrode 152. The insulating film 112A can be formed by, for example, the ALD method, the CVD method, the vapor deposition method, or the sputtering method. Note that the insulating film 112A is formed under conditions in which the resist mask 191 is not cured.
[0035] 10, the resist mask 191 is removed together with the insulating film 112A thereon, thereby obtaining the second insulating film 112.
[0036] 11, the first film 121 is formed on the first insulating film 111, and the second film 122 is formed on the second insulating film 112. The method of forming the first film 121 and the second film 122 is not limited, but the first film 121 and the second film 122 can be formed by, for example, a dip coating method. Here, the method of forming the first film 121 and the second film 122 by the dip coating method will be described. First, a solution in which the raw material of the first film 121 and the raw material of the second film 122 are dissolved in an organic solvent is prepared in a tank. The raw material of the first film 121 includes the molecule 160 (see FIG. 3), and the raw material of the second film 122 includes the molecule 170 (see FIG. 4). The organic solvent is, for example, ethanol, anisole, toluene, or hexane. It is preferable to use an organic solvent in which the molecule 160 and the molecule 170 are uniformly dissolved. The concentration of the molecule 160 and the concentration of the molecule 170 in the solution are, for example, 1 μmol to 100 mmol. After the solution is prepared, the structure shown in FIG. 10 is immersed in the solution in the tank. The immersion time is about several minutes to several tens of hours. The lower the concentration of the solution, the longer the immersion time is preferable. After immersion, the structure shown in FIG. 10 is taken out of the tank together with the attached solution. Then, the excess attached solution is washed away using an organic solvent, and the structure is dried. The organic solvent used for washing may be the same type as the organic solvent contained in the solution. As a result, a first monomolecular film 21 is formed as the first film 121, and a second monomolecular film 22 is formed as the second film 122.
[0037] For example, when the first insulating film 111 is a SiO2 film and the second insulating film 112 is an Al2O3 film, the bonding functional group 162 of the molecule 160 is -Si(CH3)2H or -OH, and the bonding functional group 172 of the molecule 170 is -COOH or -PO3H2.
[0038] In addition, a solution in which the raw materials of the first film 121 are dissolved in an organic solvent and a solution in which the raw materials of the second film 122 are dissolved in an organic solvent may be prepared separately, and the first film 121 and the second film 122 may be formed separately rather than simultaneously.
[0039] After the first film 121 and the second film 122 are formed, as shown in FIG. 12, a graphene layer 130 is provided on the first film 121 and the second film 122. The graphene layer 130 may be directly synthesized on the first film 121 and the second film 122, or a graphene layer 130 synthesized separately may be transferred onto the first film 121 and the second film 122. The graphene layer 130 may be synthesized by, for example, a CVD method. When the graphene layer 130 is directly synthesized on the first film 121 and the second film 122, the graphene layer is synthesized on the entire first film 121 and the second film 122, and then a resist mask is formed to cover the portion where the graphene layer 130 is to be formed, and then the portion exposed from the resist mask is removed by irradiation with oxygen plasma, and then the resist mask is removed.
[0040] Next, a first electrode 141 is formed on the first region 131 of the graphene layer 130, and a second electrode 142 is formed on the second region 132 (see FIGS. 1 and 2). In forming the first electrode 141 and the second electrode 142, for example, a resist mask is formed by lithography in which the portions where the first electrode 141 and the second electrode 142 are to be formed are opened, and then materials for the first electrode 141 and the second electrode 142 are deposited by a vapor deposition method or a sputtering method, and then the resist mask is removed. That is, for example, a lift-off process is adopted.
[0041] In this manner, the optical sensor 100 according to the first embodiment can be manufactured.
[0042] Next, a second example of the method for manufacturing the optical sensor 100 according to the first embodiment will be described. Figures 13 and 14 are cross-sectional views showing the second example of the method for manufacturing the optical sensor 100 according to the first embodiment.
[0043] In the second example, first, similarly to the first example, processing up to the formation of the second control electrode 152 is performed (see FIG. 7). Next, as shown in FIG. 13, an insulating film 112B made of the material of the second insulating film 112 is deposited on the first insulating film 111 by a deposition method or a sputtering method. The insulating film 112B is formed so as to cover the second control electrode 152. The insulating film 112B can be formed by, for example, an ALD method, a CVD method, a deposition method, or a sputtering method, similarly to the insulating film 112A.
[0044] 14, a resist mask 192 is formed on the insulating film 112B to cover a portion of the insulating film 112B that will become the second insulating film 112 and to expose the other portions. Next, the portion of the insulating film 112B that is exposed from the resist mask 192 is removed by etching. For example, wet etching using a solvent such as hydrofluoric acid is performed as the etching. It is preferable to control the time so as not to remove too much of the first insulating film 111. Next, the resist mask 192 is removed.
[0045] Thereafter, similarly to the first example, the processes subsequent to the formation of the first film 121 and the second film 122 are carried out.
[0046] In this manner, the optical sensor 100 according to the first embodiment can be manufactured.
[0047] Second embodiment Next, a second embodiment will be described. The second embodiment differs from the first embodiment mainly in the base of the second film. Fig. 15 is a cross-sectional view showing the photosensor according to the second embodiment.
[0048] 15, in the optical sensor 200 according to the second embodiment, the second control electrode 152 is provided on the silicon oxide film 102, and the second control electrode 152 is covered with the first insulating film 111. Moreover, the second insulating film 112 is not provided, and the second film 122 is provided on the first insulating film 111.
[0049] Other configurations of the second embodiment are similar to those of the first embodiment.
[0050] In the optical sensor 200 according to the second embodiment configured in this manner, the graphene layer 130 also functions as a pn junction photodiode, and the second embodiment also allows for a reduction in dark current compared to a photoconductor including graphene.
[0051] Furthermore, the conductivity type of the first region 131 can be sufficiently largely tilted toward p-type without applying a high voltage from the first control electrode 151 to the first insulating film 111 that would cause dielectric breakdown. Also, the conductivity type of the second region 132 can be sufficiently largely tilted toward n-type without applying a high voltage from the second control electrode 152 to the first insulating film 111 that would cause dielectric breakdown.
[0052] Therefore, the second embodiment also makes it possible to suppress dark current and improve sensitivity.
[0053] Next, a method for manufacturing the optical sensor 200 according to the second embodiment will be described. Figures 16 to 24 are cross-sectional views showing the method for manufacturing the optical sensor 200 according to the second embodiment.
[0054] First, similarly to the first embodiment, a base material 103 is prepared. Next, a first control electrode 151 and a second control electrode 152 are formed on a silicon oxide film 102, as shown in FIG.
[0055] Thereafter, as shown in FIG. 17, a first insulating film 111 that covers the first control electrode 151 and the second control electrode 152 is formed on the silicon oxide film .
[0056] 18, a resist mask 291 is formed on the first insulating film 111, the resist mask 291 having an opening formed by lithography where the first film 121 is to be formed.
[0057] Next, as shown in FIG. 19, a film 121A made of the material of the first film 121 is deposited on the first insulating film 111 and the resist mask 291 by a vapor deposition method.
[0058] 20, the resist mask 291 is removed together with the film 121A thereon, thereby obtaining the first film 121.
[0059] Subsequently, as shown in FIG. 21, a resist mask 292 having an opening formed by lithography in a portion where the second film 122 is to be formed is formed on the first film 121.
[0060] Next, as shown in FIG. 22, a film 122A made of the material of the second film 122 is deposited on the first insulating film 111 and the resist mask 292 by evaporation.
[0061] 23, the resist mask 292 is removed together with the film 122A thereon, thereby obtaining the second film 122.
[0062] Next, as shown in FIG. 24, a graphene layer 130 is provided on the first film 121 and the second film 122.
[0063] Next, a first electrode 141 is formed on the first region 131 of the graphene layer 130, and a second electrode 142 is formed on the second region 132 (see FIG. 15).
[0064] In this manner, the optical sensor 200 according to the second embodiment can be manufactured.
[0065] The nanocarbon material is not limited to graphene, and carbon nanotubes, fullerenes, etc. may also be used.
[0066] Optical sensors can be used, for example, in space satellites, and in distance measuring devices in automobiles.
[0067] Although the preferred embodiments have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications and substitutions can be made to the above-described embodiments without departing from the scope of the claims.
[0068] Various aspects of the present disclosure are summarized below as appendices.
[0069] (Appendix 1) a nanocarbon material layer having a first region and a second region; A first electrode connected to the first region; A second electrode connected to the second region; a first film that imparts a first conductivity type to the first region; a second film that imparts a second conductivity type different from the first conductivity type to the second region; a first control electrode that applies an electric field to the first region; a second control electrode that applies an electric field to the second region; An optical sensor having (Appendix 2) 2. The optical sensor of claim 1, wherein the nanocarbon material layer is a graphene layer. (Appendix 3) The first film has a first monolayer having an electron-withdrawing functional group, 3. The optical sensor according to claim 1, wherein the second film has a second monolayer having an electron-donating functional group. (Appendix 4) The optical sensor of claim 3, wherein the electron-withdrawing functional group comprises -CHO, -COOR, -COOH, -COR, -SO3H, -CN, -NO2, -NR3 or a halogen (wherein R is a hydrocarbon group). (Appendix 5) The optical sensor according to claim 3 or 4, wherein the electron donating functional group comprises -NH2, -NR2, -OH, -OR, -NHCOR, -OCOR, -R, or an aryl group (wherein R is a hydrocarbon group). (Appendix 6) a first insulating film in contact with the first monomolecular film; a second insulating film in contact with the second monomolecular film; having the first monomolecular film is between the first insulating film and the first region, 6. The optical sensor according to claim 3, wherein the second monolayer is between the second insulating film and the second region. (Appendix 7) the first insulating film is a silicon oxide film, 7. The optical sensor according to claim 6, wherein the second insulating film is an aluminum oxide film. (Appendix 8) providing a nanocarbon material layer having a first region and a second region; providing a first electrode connected to the first region; providing a second electrode connected to the second region; providing a first film that imparts a first conductivity type to the first region; providing a second film that imparts a second conductivity type different from the first conductivity type to the second region; providing a first control electrode for applying an electric field to the first region; providing a second control electrode for applying an electric field to the second region; A method for manufacturing an optical sensor having the above structure. (Appendix 9) providing a first insulating film covering the first control electrode after the step of providing the first control electrode; providing a second insulating film covering the second control electrode after the step of providing the second control electrode; the first film is provided so as to be in contact with the first insulating film, the second film is provided so as to be in contact with the second insulating film, The method for manufacturing an optical sensor according to claim 8, wherein the nano-carbon material layer is provided so that the first region is in contact with the first film and the second region is in contact with the second film. (Appendix 10) The method for producing an optical sensor according to claim 8 or 9, wherein the nanocarbon material layer is a graphene layer. [Explanation of symbols]
[0070] 100, 200: Optical sensor 21: First monolayer 22: Second monolayer 111: First insulating film 112: second insulating film 121:First membrane 122:Second membrane 130: Graphene layer 131:First area 132:Second area 141: 1st electrode 142:Second electrode 151: First control electrode 152: second control electrode 160, 170: Molecule 161, 171: Alkyl group 162, 172: Binding functional group 163, 173: Functional functional group
Claims
1. A nanocarbon material layer having a first region and a second region; A first electrode connected to the first region; A second electrode connected to the second region; a first film that imparts a first conductivity type to the first region; a second film that imparts a second conductivity type different from the first conductivity type to the second region; a first control electrode for applying an electric field to the first region; a second control electrode for applying an electric field to the second region; An optical sensor having
2. The optical sensor of claim 1 , wherein the nano-carbon material layer is a graphene layer.
3. The first film has a first monolayer having an electron-withdrawing functional group, 3. The optical sensor according to claim 1, wherein the second film comprises a second monolayer having an electron-donating functional group.
4. a first insulating film in contact with the first film; a second insulating film in contact with the second film; having the first film is between the first insulating film and the first region, The optical sensor according to claim 1 , wherein the second film is located between the second insulating film and the second region.
5. providing a nano-carbon material layer having a first region and a second region; providing a first electrode connected to the first region; providing a second electrode connected to the second region; providing a first film that imparts a first conductivity type to the first region; providing a second film that imparts a second conductivity type different from the first conductivity type to the second region; providing a first control electrode for applying an electric field to the first region; providing a second control electrode for applying an electric field to the second region; A method for manufacturing an optical sensor having the above structure.
6. providing a first insulating film covering the first control electrode after the step of providing the first control electrode; providing a second insulating film covering the second control electrode after the step of providing the second control electrode; the first film is provided so as to be in contact with the first insulating film, the second film is provided so as to be in contact with the second insulating film, The method for manufacturing an optical sensor according to claim 5 , wherein the nano-carbon material layer is provided such that the first region is in contact with the first film and the second region is in contact with the second film.
7. The method for manufacturing an optical sensor according to claim 5 or 6, wherein the nano-carbon material layer is a graphene layer.
Citation Information
Patent Citations
Electronic device and method for manufacturing the same
JP2015005655A
Graphene light receiving element and graphene light modulator
JP2017011209A
Photodetector
JP2022054180A
Semiconductor device partially doped single graphene by using palladium-hydrogen system and method of manufacturing the same
KR1020130134539A
Apparatus and method for detecting radiation
US20120001761A1