Yield prediction method of sintered ore, method for controlling sintered ore production facility, method for producing sintered ore, method for generating yield prediction model and yield prediction apparatus of sintered ore
Patent Information
- Application Number
- JP2023069156
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-04-20
AI Technical Summary
【0016】 本発明に係る焼結鉱歩留り予測モデルの生成方法および焼結鉱歩留りの予測方法によれば、焼結鉱製造設備における焼結鉱の歩留りを精度よく予測できる。また、本発明に係る焼結鉱製造設備の制御方法および焼結鉱の製造方法によれば、高い歩留りで焼結鉱を製造できるようになる。
Smart Images

Figure 2024154924000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a sintered ore yield prediction method, a sintered ore manufacturing equipment control method, a sintered ore manufacturing method, a yield prediction model generation method, and a sintered ore yield prediction device. [Background technology]
[0002] A Dwight Lloyd sintering machine is used in the sintering process of iron ore. In this sintering machine, powdered iron ore is mixed with moisture, limestone, and carbonaceous material (solid fuel) such as coke powder or anthracite, and the sintering raw material is granulated in a granulator. In the Dwight Lloyd sintering machine, the sintering raw material is charged onto a pallet via a conveyor, a feed hopper, and a chute. In the Dwight Lloyd sintering machine, for example, 400 to 800 mm thick sintering raw material is charged onto the pallet, and the charged sintering raw material becomes the charging layer in the sintering machine.
[0003] The sintering machine is equipped with an ignition furnace equipped with a combustion burner (ignition furnace burner) above the pallet, and a wind box for air intake is installed below the pallet. When the carbonaceous material on the surface of the charging layer is ignited by the combustion burner of the ignition furnace, the carbonaceous material in the sintering raw material burns along the air flow from above to below generated by the air intake by the wind box. The sintering reaction caused by this combustion gradually moves from the upper layer to the lower layer of the charging layer as the pallet advances.
[0004] In the ignition furnace, multiple ignition furnace burners are arranged in the width direction of the pallet. The ignition furnace burners inject flames at approximately the same position in the width direction of the charging bed. The flames injected from the ignition furnace burners ignite (ignite) the carbonaceous material on the surface of the charging bed. Then, the limestone and some of the iron ore contained in the charging bed melt into a molten liquid, and the molten liquid bonds the raw materials together to produce a sintered cake.
[0005] In the sintering process, it is necessary to appropriately control the maximum temperature and the holding time at high temperature during the sintering reaction in the charging bed. This allows calcium ferrite, which has high strength and relatively high reducibility, to be produced in the sintered ore. For example, if the ignition temperature of the charging bed is too low, the molten liquid is not sufficiently produced in the charging bed, the bonding between the raw materials becomes weak, and the strength of the sintered ore decreases. In particular, the upper layer of the charging bed is easily cooled after ignition due to the air flow caused by the wind box. This cooling shortens the holding time at high temperature, and the yield of sintered ore decreases. On the other hand, if the ignition temperature of the charging bed is too high, the calcium ferrite in the sintered ore may decompose into amorphous silicate and secondary hematite.
[0006] Amorphous silicates reduce the strength and reducibility of sintered ore, and secondary hematite makes it easier to disintegrate during reduction. Such low-strength sintered ore is re-sintered as return ore because it is crushed into fine particles when the sintered cake is crushed, without being charged into the blast furnace. In other words, if the ignition temperature of the charging bed is too high, the strength of the sintered ore is reduced, which causes a problem in that the yield of sintered ore is reduced and the production efficiency of sintered ore is reduced.
[0007] If the yield of sintered ore can be predicted in advance, it is possible to prevent such a decrease in yield by taking measures in advance. As a technique for predicting the yield of sintered ore, Patent Document 1 discloses a method for predicting the yield of sintered ore by determining a relational expression that expresses the correlation between the calorific value of the sintering raw material fed into a sintering machine and the sintered ore yield, and applying the measured value of the calorific value to the relational expression. In Patent Document 1, the measured value of the calorific value is specified as a function of the calorific value of limestone decomposition, the sensible heat of sintering, and the sensible heat of exhaust gas, and the sensible heat of exhaust gas is calculated using the temperature of the exhaust gas.
[0008] Patent Document 2 discloses a method for predicting the return ore generation ratio, which indicates the yield of sintered ore, by accumulating data on operating conditions required for sintering, including the return ore generation ratio for each past case, and predicting the return ore generation ratio based on the data on operating conditions for each case. In Patent Document 2, the M gas flow rate, pallet speed, sintering completion point, lime ratio, coke ratio, raw material components, and average particle size are used as the operating condition data required for sintering. Here, the sintering completion point is an index indicating the position at which the charging layer on the pallet is ignited in the ignition furnace, and sintering progresses from the surface downward as the pallet advances, and sintering is completed.
[0009] Patent Document 3 discloses a technique for preventing a decrease in the cold strength of sintered ore and improving the yield of sintered ore. According to Patent Document 3, the decrease in the cold strength of sintered ore can be prevented by adjusting the fuel flow rate of the ignition furnace burner so that the surface temperature near the pallet side plate measured at the outlet of the ignition furnace is higher than the temperature at the center of the pallet. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. 8-13047 [Patent Document 2] JP 2010-7992 A [Patent Document 3] Japanese Patent Application Publication No. 2-153027 Summary of the Invention [Problem to be solved by the invention]
[0011] However, the above conventional techniques have the following problems. In Patent Document 1, the sintered ore yield is predicted using the calorific value. The calorific value is calculated using physical quantities of the sintering raw materials, such as the specific heat of limestone decomposition and the specific heat of sintering, so there is a problem that the influence of fluctuations in the operating conditions in the sintering process is not taken into consideration. In addition, although the exhaust gas temperature is used to calculate the exhaust gas sensible heat, this exhaust gas temperature is not an index that directly reflects the temperature history of the sintering bed during the process of the sintering reaction. In other words, there is a problem that it is not possible to distinguish between a case in which the temperature of the sintering bed transported by the pallet is quickly cooled from a high temperature state and a case in which a relatively low temperature state is maintained for a long time. For this reason, the technique disclosed in Patent Document 1 has a problem that the sintered ore yield cannot be predicted with high accuracy.
[0012] In Patent Document 2, the return ore generation ratio is predicted using operational condition data required for sintering. However, although the operational condition data includes information on the operational conditions of the ignition furnace, such as M gas flow rate, pallet speed, and sintering completion point, in addition to information on the composition of the sintering raw materials, these are not indicators that directly reflect the temperature history of the charging layer during the sintering reaction, so there is a problem that the prediction accuracy of the sintered ore yield is low. Therefore, the technology disclosed in Patent Document 2 has a problem that the sintered ore yield cannot be predicted with high accuracy.
[0013] In Patent Document 3, the technology improves the yield of sintered ore by adjusting the fuel flow rate of the ignition furnace burner so that the surface temperature near the pallet side plate measured at the outlet of the ignition furnace is higher than the temperature at the center of the pallet, but it is not a technology to predict the yield of sintered ore. In addition, in the ignition furnace, sintering progresses at least on the surface of the charging bed immediately after the surface of the charging bed is ignited by the ignition furnace burner. Therefore, since the temperature of the charging bed surface has already decreased at the downstream position of the ignition furnace, there is a problem that even if the temperature of the charging bed is measured using a radiation thermometer, information on the maximum temperature on the surface of the charging bed and the holding time at high temperature cannot be obtained.
[0014] The present invention has been made to solve the above problems, and its object is to provide a sintered ore yield prediction method, a sintered ore yield prediction device, and a yield prediction model generation method that can accurately predict the yield of sintered ore in a sintered ore production facility that produces sintered ore using an ignition furnace that burns carbonaceous material in a sintering bed. Another object of the present invention is to provide a sintered ore production facility control method and a sintered ore production method that can improve the yield of sintered ore. [Means for solving the problem]
[0015] The means for solving the above problems are as follows. [1] A method for predicting the yield of sintered ore in a sintered ore production facility in which sintering raw materials including carbonaceous material are charged onto an endless moving pallet to form a charging bed, and then sintered ore is produced using an ignition furnace that combusts the carbonaceous material in the charging bed, the method comprising: inputting input data including the surface temperature of the charging bed inside the ignition furnace cover, measured from the outside of the ignition furnace cover through a measurement window of the ignition furnace cover with a radiation thermometer having a measurement wavelength selected from the range of 0.5 μm or more and 4.0 μm or less, into a yield prediction model; and outputting the yield of sintered ore to predict the yield of sintered ore. [2] The method for predicting a yield of sintered ore according to [1], wherein the transmittance of the measurement window at the measurement wavelength is 50% or more. [3] A method for predicting the yield of sintered ore according to [1] or [2], wherein the pressure above the sintering bed inside the ignition furnace cover is made negative. [4] A method for predicting the yield of sintered ore according to any one of [1] to [3], wherein the surface of the charging bed that is ignited by a flame sprayed from an ignition furnace burner provided in the ignition furnace is defined as an ignition part, and the surface temperature includes the surface temperature of the ignition part. [5] A method for controlling sintered ore production equipment, comprising: identifying a surface temperature at which the sintered ore yield predicted by the sintered ore yield prediction method described in any one of [1] to [4] will be equal to or greater than a target yield value; and setting the operating conditions of the ignition furnace so that the surface temperature of the sintered ore feeding bed becomes the identified surface temperature. [6] A method for producing sintered ore, comprising the steps of: producing sintered ore using the control method for sintered ore production equipment described in [5]. [7] A method for generating a yield prediction model that predicts the yield of sintered ore in a sintering ore production facility in which sintering raw materials including carbonaceous material are charged onto an endless moving pallet to form a charging bed, and then sintered ore is produced using an ignition furnace that combusts the carbonaceous material in the charging bed, comprising: acquiring a plurality of data sets each consisting of a pair of actual values of input data including the surface temperature of the charging bed inside the ignition furnace cover measured from the outside of the ignition furnace cover through a measurement window of the ignition furnace cover with a radiation thermometer having a measurement wavelength selected from a range of 0.5 μm or more and 4.0 μm or less, and an actual value of the yield of sintered ore; and generating a yield prediction model that uses the input data as input and outputs the yield of the sintered ore through machine learning using the acquired plurality of data sets as training data. [8] A sintered ore yield prediction device that predicts the yield of sintered ore in a sintered ore production facility in which sintered raw materials including carbonaceous material are charged onto an endless movable pallet to form a charging bed, and then sintered ore is produced using an ignition furnace that combusts the carbonaceous material in the charging bed, the sintered ore yield prediction device having: a data acquisition unit that acquires input data including the surface temperature of the charging bed inside the ignition furnace cover measured from the outside of the ignition furnace cover through a measurement window of the ignition furnace cover with a radiation thermometer having a measurement wavelength selected from a range of 0.5 μm or more and 4.0 μm or less; and a sintered ore yield prediction unit that inputs the input data into a yield prediction model, outputs the sintered ore yield, and predicts the sintered ore yield. [9] The sintered ore yield prediction device according to [8], wherein the transmittance of the measurement window at the measurement wavelength is 50% or more. Effect of the Invention
[0016] According to the method for generating a sinter yield prediction model and the method for predicting the sinter yield of the present invention, the yield of sinter in a sinter production facility can be predicted with high accuracy. Also, according to the method for controlling the sinter production facility and the method for producing sinter in the present invention, sinter can be produced with a high yield. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a schematic diagram showing an example of a sintered ore production facility for producing sintered ore. [Diagram 2] FIG. 2 is a schematic side cross-sectional view of the sintering raw material charging device and the ignition furnace. [Diagram 3] FIG. 3 is a schematic cross-sectional view of the ignition furnace. [Figure 4] FIG. 4 is a schematic diagram showing one of a plurality of burner nozzles that constitute the ignition furnace burner. [Diagram 5] FIG. 5 is a schematic diagram showing an example of an ignition furnace having a measurement window provided in a side cover. [Figure 6] FIG. 6 is a graph showing the transmittance of light including the infrared wavelength band. [Figure 7] FIG. 7 is a schematic diagram showing temperature measurement positions using a radiation thermometer. [Figure 8] FIG. 8 is a graph showing the intensity distribution of infrared rays emitted from a flame. [Figure 9] FIG. 9 is a graph showing the transmittance of light passing through carbon dioxide gas. [Figure 10] FIG. 10 is a graph showing the transmittance when lead selenide (PbSe) and lead sulfide (PbS) are selected as the detection element of the radiation thermometer and quartz glass is used as the measurement window 86. [Figure 11] FIG. 11 is a graph showing the light transmittance of water vapor. [Figure 12] FIG. 12 is a diagram illustrating a schematic configuration example of a sintered ore yield prediction device 110. As shown in FIG. [Figure 13] FIG. 13 is a graph showing the relationship between the flow rate of the fuel gas supplied to the ignition furnace burner and the surface temperature of the sintering bed S. [Figure 14] FIG. 14 is a schematic diagram showing an example of a yield prediction model generated using a neural network. [Figure 15] FIG. 15 is a graph showing the change in surface temperature in the sintering bed S over time from ignition. [Figure 16]FIG. 16 is a graph showing the results of measuring the temperature distribution in the width direction of the sintering bed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. The following embodiments are preferred examples of the present invention, and the present invention is not limited to these examples.
[0019] FIG. 1 is a schematic diagram showing an example of a sintered ore production facility 140 for producing sintered ore. The sintered ore production facility 140 includes a blending tank 10, a drum mixer 16, a sintering machine 30, a crusher 50, a cooler 52, a sieving device 54, a process computer 100, and a sintered ore yield prediction device 110. The blending tank 10 is composed of a plurality of surge hoppers 12, which are storage tanks. Each of the plurality of surge hoppers 12 stores raw materials for sintered ore. In this embodiment, four surge hoppers 12 are arranged, and for example, an iron-containing raw material, a CaO-containing raw material, an MgO-containing raw material, and a carbonaceous material are stored in each of the surge hoppers 12.
[0020] The iron-containing raw material used as the raw material for sintered ore is, for example, various iron ores such as hematite and magnetite. The CaO-containing raw material is, for example, limestone and quicklime. The MgO-containing raw material is, for example, dolomite and refined nickel slag. The carbonaceous material is, for example, solid fuel such as coke powder and anthracite. The iron-containing raw material may include dust generated in a steelworks. The raw material for sintered ore may also include return ore, which is fine sintered ore that does not meet the specified size.
[0021] A predetermined amount of each raw material stored in the blending tank 10 is cut out and transported to a drum mixer 16 by a blended raw material transport conveyor 14. An appropriate amount of water is added to each raw material transported to the drum mixer 16, and the raw materials are granulated into pseudo particles having an average particle size of, for example, 3.0 to 6.0 mm.
[0022] The drum mixer 16 is an example of a granulation device that mixes each raw material and granulates it to produce a sintering raw material. A plurality of granulation devices may be used, and a pelletizer may be used instead of the drum mixer 16. A plurality of types of granulation devices may be used, for example, both a drum mixer and a pelletizer may be used. The sintering raw material 18 granulated by the drum mixer 16 is transported to the sintering machine 30 by the sintering raw material transport conveyor 20.
[0023] The sintering machine 30 is, for example, a downward suction type Dwight Lloyd type sintering machine. The sintering machine 30 has a sintering raw material charging device 32, an endless moving pallet 34, an ignition furnace 36, a gas fuel supply device 38, and a wind box 40. The sintering raw material charging device 32 charges the sintering raw material 18 transported by the sintering raw material transport conveyor 20 into the pallet 34 to form a charging bed S. The endless moving pallet 34 transports the sintering raw material in one direction (hereinafter, sometimes referred to as the traveling direction of the pallet 34). The ignition furnace 36 is provided above the pallet 34 and ignites (ignites) the surface of the charging bed S. The gas fuel supply device 38 supplies gas fuel from above the charging bed S. The wind box 40 is provided below the pallet 34 and generates an air flow from above to below by sucking in the air inside the charging bed S.
[0024] 2 is a schematic side cross-sectional view of the sintering raw material charging device 32 and the ignition furnace 36. The sintering raw material charging device 32 has a feed hopper 60, a drum feeder 62, a charging gate 64, and a chute 66. The sintering raw material 18 in the feed hopper 60 is cut out by the drum feeder 62, slides down on the chute 66, and is charged into the pallet 34. The sintering raw material 18 charged into the pallet 34 forms a charging layer S of the sintering raw material.
[0025] The charging gate 64 is a plate-like member provided along the width direction of the chute 66. Generally, a plurality of charging gates 64 are provided along the width direction of the chute 66, and the opening of the charging gate 64 is adjusted by an opening adjustment device (not shown). By adjusting the opening of the charging gate 64, the charging speed and charging state of the sintering raw material 18 charged into the pallet 34 are controlled. The thickness of the charging layer S formed by charging into the pallet 34 is adjusted by the baffle 70 when it is transported to the ignition furnace 36.
[0026] The ignition furnace 36 is a device that ignites the surface of the charging bed S, the thickness of which is adjusted by the baffle 70, to cause a sintering reaction from the upper layer to the lower layer of the charging bed S. The ignition furnace 36 has an ignition furnace burner 72 and an ignition furnace cover 74.
[0027] The ignition furnace burner 72 injects a flame toward the surface of the charging bed S charged in the ignition furnace 36. This ignites the carbonaceous material on the surface of the charging bed S. Since the wind box 40 sucks the air inside the charging bed S downward, when the carbonaceous material on the surface of the charging bed S is ignited, the carbonaceous material inside the charging bed S burns downward one by one. This combustion of the carbonaceous material forms a molten zone in the sintering raw material, and the molten zone moves downward in the charging bed S. Since the charging bed S is continuously transported by the pallet 34, the surface of the charging bed S transported to the position of the ignition furnace burner is continuously ignited by the flame of the ignition furnace burner 72. Then, as the pallet 34 advances, the sintering reaction proceeds from the upper layer to the lower layer of the charging bed S, and the sintering raw material 18 is sintered to produce a sintered cake.
[0028] Referring again to FIG. 1, a wind box 40 is provided below the pallet 34 to suck air from inside the sintered bed S downward and generate an airflow from above to below in the thickness direction of the sintered bed S. The wind box 40 is connected to a main duct 42, and the wind box 40 sucks air from inside the sintered bed S downward and generates an airflow from above to below in the thickness direction of the sintered bed S by the exhaust fan 46 sucking the gas from the main duct 42. The exhaust fan 46 is, for example, a blower or a pump. A dust collector 44 is provided between the main duct 42 and the exhaust fan 46 to remove dust and the like contained in the gas exhausted from the main duct 42. The exhaust fan 46 is connected to a chimney 48, and the gas exhausted from the main duct 42 is discharged from the chimney 48 after harmful substances are removed.
[0029] By providing a wind box 40 below the pallets 34 passing through the ignition furnace 36, the sintering reaction of the sintering raw materials progresses from the upper layer to the lower layer of the charging bed S, and a sintered cake can be efficiently produced. In addition, a gaseous fuel supplying device 38 is provided downstream of the ignition furnace 36 in the traveling direction of the pallets 34. By supplying gaseous fuel from the gaseous fuel supplying device 38 into a hood installed above the charging bed S, the upper layer of the charging bed S, which is difficult to maintain at a high temperature, can be maintained at a high temperature. However, the gaseous fuel supplying device 38 does not have to be provided in the sinter ore production facility 140.
[0030] When the sintered cake is produced downstream of the ignition furnace 36, the sintered cake is crushed by a crusher 50 to become sintered ore. The sintered ore crushed by the crusher 50 is cooled by a cooler 52. The sintered ore cooled by the cooler 52 is sieved by a sieving device 54 having a plurality of sieves into finished sintered ore 56 having a predetermined particle size or more (hereinafter, the finished sintered ore 56 may be referred to as sintered ore 56) and return ore 58 having a particle size less than the predetermined particle size. The finished sintered ore 56 obtained in this manner is called sintered ore, and the rate of sintered ore generation is the yield of sintered ore. The sintered ore 56 is charged into the blast furnace as a blast furnace raw material, while the return ore 58 is transported to the blending tank 10 and used as a raw material for the sintered ore 56.
[0031] The process computer 100 is, for example, a general-purpose computer such as a workstation or a personal computer. The process computer 100 controls the operation of each device constituting the sintered ore manufacturing equipment 140 in order to manufacture the sintered ore 56 of the desired product quality. In addition, the process computer 100 collects and stores the operation parameters of the sintered ore manufacturing equipment 140, raw material information of the sintered raw material, sensor information measured by sensors provided in each device of the sintered ore manufacturing equipment 140, and the actual value of the yield of the sintered ore. It is preferable to measure the yield of the sintered ore at intervals of 5 to 180 minutes. If the yield of the sintered ore is measured at intervals of less than 5 minutes, the change in the operating conditions is small and the actual value of the yield is unlikely to change, which is not preferable. In addition, if the yield of the sintered ore is measured at intervals longer than 180 minutes, it is difficult to obtain an actual value of the yield with high accuracy in response to changes in the operating conditions, which is not preferable. It is more preferable to measure the yield of the sintered ore at intervals of 30 to 90 minutes.
[0032] The operation parameters of the sinter ore manufacturing facility 140 include, for example, the blending ratio of coke powder, the amount of moisture added to the sintering raw materials, the conveying speed of the pallets 34, the layer thickness of the charging bed S, the fuel gas flow rate, the air flow rate, and the air-fuel ratio (air ratio) supplied to the ignition furnace 36. The sensor information includes, for example, the surface temperature of the charging bed S in the ignition furnace 36 described later, the amount of exhaust gas sucked into the wind box 40, the oxygen concentration of the atmospheric gas above the charging bed S in the ignition furnace 36, and the oxygen concentration of the exhaust gas sucked into the wind box 40. The raw material information of the sintering raw materials includes the content of quicklime and silica stone contained in the sintering raw materials, the brand of iron ore, and the average particle size of the sintering raw materials.
[0033] The sintered ore yield prediction device 110 inputs input data including the surface temperature of the charging layer S in the ignition furnace 36 into a yield prediction model, and outputs the sintered ore yield to predict the sintered ore yield. The sintered ore yield prediction device 110 also specifies a surface temperature at which the predicted sintered ore yield is equal to or greater than a target yield value, and specifies the operation parameters of the ignition furnace 36 that can achieve the specified surface temperature. The sintered ore yield prediction device 110 outputs the specified operation parameters of the ignition furnace 36 to the process computer 100, thereby setting the specified operation parameters as the operation conditions of the ignition furnace 36.
[0034] Next, the ignition furnace 36 will be described. Fig. 3 is a schematic cross-sectional view of the ignition furnace 36. Fig. 3(a) is a cross-sectional view cut along a plane perpendicular to the traveling direction of the pallet 34, and Fig. 3(b) is a cross-sectional view cut along a plane parallel to the traveling direction of the pallet 34.
[0035] The length of the ignition furnace 36 (the distance in the conveying direction of the pallet) is, for example, 2 to 4 m. The thickness of the charging bed S is, for example, 400 to 800 mm. The width of the charging bed S is, for example, 3000 to 6000 mm. Pallet side plates 88 are provided on the side portions of the charging bed S. The pallet side plates 88 are provided to support the charging bed S from the sides and maintain the layer thickness distribution of the charging bed S.
[0036] The ignition furnace cover 74 of the ignition furnace 36 has a top cover 80 covered with castable refractory and an iron shell, and a side cover 82, and is provided to cover the charging bed S. The top cover 80 covers the upper part of the charging bed S, and the side cover 82 covers the side part of the charging bed S. Although a certain gap is generated between the side cover 82 and the pallet side plate 88, the size of the gap is configured to be kept relatively small. This restricts air leakage from the side, and the airtightness inside the ignition furnace 36 is maintained to a certain degree.
[0037] A baffle 70 is provided at the entrance of the ignition furnace 36, and is configured to keep a narrow gap between the baffle 70 and the upper surface of the charging bed S. Similarly, the exit of the ignition furnace 36 is configured to keep a narrow gap between the baffle 70 and the upper surface of the charging bed S. In this way, the gaps at both the charging entrance and the discharge exit are kept narrow by the baffle 70, so that the airtightness inside the ignition furnace 36 is maintained to a certain degree.
[0038] The ignition furnace burner 72 has a plurality of burner nozzles in the width direction of the charging bed S. The ignition furnace burner 72 generates combustible gas by mixing fuel gas and combustion air, and sprays a flame from the tip of the burner nozzle. The number of burner nozzles provided in the width direction of the charging bed S may be 2 to 8.
[0039] The ignition furnace burner 72 is attached to the top cover 80, and the burner nozzle of the ignition furnace burner 72 is disposed inside the ignition furnace 36. The ignition furnace burner 72 is connected to a supply pipe for fuel gas and combustion air used for burner heating. The fuel gas and combustion air are supplied from a supply device provided outside the ignition furnace 36. The supply pipe for fuel gas to the ignition furnace burner 72 is provided with a fuel gas flow rate adjustment valve 90 for adjusting the flow rate of the fuel gas and a fuel gas flow meter 92 for measuring the flow rate of the fuel gas. This controls the flow rate of the fuel gas combusted in the ignition furnace burner 72. In addition, the supply pipe for combustion air to the ignition furnace burner 72 is provided with an air flow rate adjustment valve 94 for adjusting the flow rate of the combustion air and an air flow meter 96 for measuring the flow rate of the combustion air. This controls the air ratio during combustion of the ignition furnace burner 72.
[0040] FIG. 4 is a schematic diagram showing one of the burner nozzles 76 constituting the ignition furnace burner 72. The ignition furnace burner 72 has a plurality of burner nozzles 76 that emit flames from the upper cover 80 toward the surface of the charging layer S along the width direction of the pallet 34. In the burner nozzle 76 shown in FIG. 4, combustion air is injected toward the gas flow into which the fuel gas is injected. As a result, the fuel gas and the combustion air are mixed inside the ignition furnace 36, combustible gas is generated, and a combustion reaction occurs. For this reason, in the burner nozzle 76, the combustion air is injected at a certain angle with respect to the gas flow into which the fuel gas is injected so that the fuel gas and the combustion air are mixed.
[0041] The fuel gas for the ignition furnace burner 72 may be any of coal gas, city gas, natural gas, methane gas, ethane gas, propane gas, and shale gas. A mixed gas of two or more fuel gases selected from these may also be used as the fuel gas. The coal gas is any of coke oven gas, blast furnace gas, converter gas, and electric furnace gas. These gases are by-product gases generated in the manufacturing process at steelworks, and by using these gases, these by-product gases can be reused as fuel gas.
[0042] The combustion conditions of the ignition furnace burner 72 are, for example, a fuel gas flow rate of 1200 Nm per 1 m of the width of the sintering bed S. 3 / (m hr) and supply combustion air so that the air to fuel gas ratio is about 0.9. This makes it possible to raise the surface temperature of the sintering bed S to about 1200°C.
[0043] Referring again to Fig. 3, the ignition furnace cover 74 is provided with a measurement window 86 arranged at a position where the upper surface of the charging bed S can be directly viewed. The position where the upper surface of the charging bed S can be directly viewed is a position where the upper surface of the charging bed S inside the ignition furnace cover 74 can be visually captured from the outside of the ignition furnace cover 74 through the measurement window 86.
[0044] FIG. 5 is a schematic diagram showing an example of an ignition furnace 36 having a measurement window 86 provided in a side cover 82. FIG. 5(a) is a schematic side view of the ignition furnace 36. As shown in FIG. 5(a), the measurement window 86 is disposed at a position higher than the upper surface of the charging bed S in the ignition furnace 36. One or more measurement windows 86 may be provided in the ignition furnace cover 74. As shown in FIG. 5, by providing multiple measurement windows 86 in the ignition furnace cover 74, the surface temperature of the charging bed S can be measured at different positions in the traveling direction of the pallet 34.
[0045] Fig. 5(b) is a schematic diagram showing the field of view observed when the upper surface of the charging bed S is viewed directly through the measurement window 86. As shown in Fig. 5(b), the measurement window 86 is preferably provided at a position where the area where the flame 98 injected from the burner nozzle 76 collides with the upper surface of the charging bed S (hereinafter, this area is referred to as an ignition part 99) can be viewed directly. By measuring the temperature of the ignition part 99, the maximum temperature on the surface of the charging bed S can be grasped.
[0046] The position of the measurement window 86 is not limited to the side cover 82, as long as the upper surface of the charging bed S can be directly viewed. The measurement window 86 may be provided in the upper cover 80 of the ignition furnace 36 at a position where the upper surface of the charging bed S can be visually captured. However, if the measurement window 86 is provided in the upper cover 80, the field of view of the upper surface of the charging bed S may be limited by the supply pipes of the ignition furnace burner 72 and fuel gas, etc. In addition, if a part of the upper cover 80 is opened, the strength of the upper cover 80 decreases, making it easier for firebricks, etc. to fall off. For this reason, the measurement window 86 is preferably provided in the side cover 82.
[0047] It is preferable to use heat-resistant glass made of quartz glass or borosilicate glass for the measurement window 86. It is also preferable that the measurement window 86 is made of a material that transmits infrared rays, such as barium fluoride, calcium fluoride, zinc sulfide, zinc selenide, or germanium.
[0048] Fig. 6 is a graph showing the transmittance of light including an infrared wavelength band. The horizontal axis of Fig. 6 is wavelength (μm), and the vertical axis is transmittance (%). As shown in Fig. 6, although the transmittance of light varies depending on the material selected, it can be seen that by selecting a wavelength of light with high transmittance, light (radiated light) generated inside the ignition furnace cover 74 can be received outside the ignition furnace cover 74 through the measurement window 86.
[0049] The ignition furnace 36 has a radiation thermometer 84 that is provided outside the ignition furnace cover 74 and measures the surface temperature of the charging bed S through a measurement window 86. The radiation thermometer 84 uses a wavelength selected from the range of 0.5 μm or more and 4.0 μm or less as a measurement wavelength.
[0050] The installation position of the radiation thermometer 84 will be described with reference to FIG. 3 again. The radiation thermometer 84 is installed at a position where it can receive radiant light from the surface of the charging bed S inside the ignition furnace 36 through the measurement window 86. Since the measurement window 86 is provided at a position higher than the surface of the charging bed S, the radiation thermometer 84 is installed so that its light receiving portion faces downward. On the other hand, the direction in which the light receiving portion of the radiation thermometer 84 faces can be arbitrarily changed in the left and right directions toward the measurement window 86. Therefore, by adjusting the left and right position of the light receiving portion of the radiation thermometer 84, it is possible to measure the surface temperature of the charging bed S at any position with respect to the traveling direction of the pallet 34, such as the direction of the inlet portion or outlet portion in the ignition furnace 36, or the direction of the ignition portion 99 where the flame 98 from the ignition furnace burner 72 collides with the charging bed S.
[0051] The radiation thermometer 84 may be a spot radiation thermometer capable of measuring local temperature, a scanning radiation thermometer capable of scanning the viewing position in one axial direction by a rotating mirror or the like, or a thermograph capable of measuring the in-plane temperature distribution. When a scanning radiation thermometer is used, it may be scanned in the traveling direction of the charging bed S or in the width direction.
[0052] Fig. 7 is a schematic diagram showing the temperature measurement position by the radiation thermometer 84. Fig. 7(a) is a diagram showing an example of measuring the temperature at a specific position on the surface of the charging bed S using a spot radiation thermometer. In the example shown in Fig. 7(a), the surface temperature of the charging bed S is measured at the center in the width direction (black circle in the figure) within the range of an ignition part 99 where a flame 98 from the ignition furnace burner 72 collides with the charging bed S. This makes it possible to grasp the maximum temperature on the upper surface of the charging bed S.
[0053] Fig. 7(b) is a diagram showing an example of measuring the surface temperature by scanning the measurement points in the width direction of the charging bed S using a scanning radiation thermometer. In the example shown in Fig. 7(b), the average temperature in the width direction (black line part in the figure) within the range of the ignition part 99 where the flame 98 from the ignition furnace burner 72 collides with the charging bed S is measured. This makes it possible to grasp the surface temperature distribution in the width direction of the charging bed S.
[0054] Fig. 7(c) is a diagram showing an example in which the measurement range includes the entire width direction of the charging bed S and the surface temperature of a certain range in the longitudinal direction is measured using a thermograph. In the example shown in Fig. 7(c), the temperature is measured in a range including an ignition part 99 where a flame 98 from an ignition furnace burner 72 collides with the charging bed S (the range surrounded by a black line in the figure). This makes it possible to measure the surface temperature distribution of the charging bed S in the width direction and the longitudinal direction.
[0055] The measurement wavelength of the radiation thermometer is a wavelength selected from the range of 0.5 μm to 4.0 μm. By using this range as the measurement wavelength, the temperature measurement error is reduced, and the surface temperature of the charging bed S can be measured with high accuracy. On the other hand, if the measurement wavelength of the radiation thermometer is less than 0.5 μm, the change in radiation energy is small in the temperature range of 600 to 1400 ° C, and the temperature measurement error is large. In addition, if the measurement wavelength of the radiation thermometer is more than 4.0 μm, the temperature measurement error is increased because the temperature is affected by the flame 98 from the ignition furnace burner 72. Furthermore, if the measurement wavelength of the radiation thermometer is more than 4.0 μm, the temperature measurement error is increased because the temperature is affected by the atmospheric gas such as carbon dioxide gas generated in the ignition furnace.
[0056] Figure 8 is a graph showing the intensity distribution of infrared rays emitted from a flame. The horizontal axis of Figure 8 is wavelength (μm), and the vertical axis is relative radiation intensity (%). The relative radiation intensity is a relative value of radiation intensity normalized using the maximum value of the measured radiation intensity. The flame shown in Figure 8 is a flame produced by burning coke oven gas.
[0057] Since the hydrogen content of coke oven gas is relatively high, the flame fueled by the coke oven gas appears as a transparent flame in visible light. However, as shown in FIG. 8, the wavelength of the infrared ray emitted from the flame overlaps with the infrared ray measurement wavelength of the radiation thermometer, so that the flame becomes a disturbance in the temperature measurement. For this reason, in the ignition furnace 36 according to the present embodiment, the measurement wavelength of the radiation thermometer is set to 4.0 μm or less. As a result, even when the surface temperature of the charging layer S is measured through the flame, it is not affected by the flame, and as a result, the error in the temperature measurement by the radiation thermometer 84 can be reduced. Note that when the combustion of the ignition furnace burner 72 is in an oxygen-deficient state, the color of the flame may become yellow. To avoid this, it is preferable to perform the combustion of the ignition furnace burner 72 under oxygen-rich conditions in which the air ratio of the fuel gas to the theoretical air amount is 1 or more.
[0058] FIG. 9 is a graph showing the transmittance of light passing through carbon dioxide gas. The horizontal axis of FIG. 9 is wavelength (μm), and the vertical axis is transmittance (%). As shown in FIG. 9, it can be seen that carbon dioxide (carbon dioxide gas) generated by burning fuel gas in the ignition furnace burner also disturbs temperature measurement. For this reason, in the ignition furnace 36 according to this embodiment, the measurement wavelength of the radiation thermometer is set to 4.0 μm or less. This makes it difficult for carbon dioxide generated by the combustion of fuel gas to impede the transmission of light, thereby reducing errors in temperature measurement by the radiation thermometer 84.
[0059] Moreover, the detection element of the radiation thermometer 84 is preferably a photoelectric type. A thermoelectric type detection element such as a pyroelectric element or a thermopile has a measurement wavelength of 8 to 13 μm, and is not preferable because the measurement wavelength is affected by flames and atmospheric gases. As the photoelectric type detection element, it is preferable to use, for example, any of lead selenide (PbSe), lead sulfide (PbS), indium gallium arsenide (InGaAs), and silicon (Si). The measurement wavelength of lead selenide is 4 μm, the measurement wavelength of lead sulfide is 2 μm, the measurement wavelength of indium gallium arsenide is 1.55 μm, and the measurement wavelength of silicon is 0.9 μm. Whichever of them is used, the radiation thermometer 84 has a measurement wavelength in the range of 0.5 μm to 4.0 μm.
[0060] In addition, the transmittance of the measurement wavelength of the radiation thermometer 84 through the measurement window 86 is preferably 50% or more. FIG. 10 is a graph showing the transmittance when lead selenide (PbSe) and lead sulfide (PbS) are selected as the detection element of the radiation thermometer and quartz glass is used as the measurement window 86. Since the measurement wavelength of lead sulfide is 2.0 μm, the transmittance of quartz glass for the measurement wavelength is almost 100%. Therefore, the radiation light having a wavelength of 2.0 μm emitted from the surface of the charging bed S in the ignition furnace 36 passes through the measurement window 86 without being attenuated by the flame or atmospheric gas in the ignition furnace. This shows that the surface temperature of the charging bed S can be measured with high accuracy using the radiation thermometer 84 provided outside the measurement window 86.
[0061] On the other hand, when lead selenide is used as the detection element of the radiation thermometer 84, the measurement wavelength is 4.0 μm, and the transmittance of quartz glass for the measurement wavelength is about 70%. Therefore, although the radiation light having a wavelength of 4.0 μm emitted from the surface of the charging bed S in the ignition furnace 36 reaches the measurement window 86 without being attenuated by the flame or atmospheric gas in the ignition furnace, about 30% of the radiation light is blocked when passing through the measurement window 86. For this reason, the radiation thermometer 84 provided outside the measurement window 86 receives the radiation light with an intensity of 70% that passes through the measurement window 86 to measure the surface temperature of the charging bed S.
[0062] Therefore, in such a case, it is preferable to correct the temperature measured by the radiation thermometer 84 using the transmittance of the measurement window 86. This allows the surface temperature of the charging layer S to be measured with high accuracy even when a measurement window 86 with low transmittance at the measurement wavelength is used. On the other hand, when the transmittance is low, the amount of transmittance correction becomes large, and the measurement value varies widely. For this reason, it is preferable that the transmittance at the measurement wavelength in the measurement window 86 is 50% or more.
[0063] The correction method when the transmittance of the measurement wavelength in the measurement window 86 is less than 100% is as follows. The radiation thermometer 84 receives radiation from the measurement object and converts it into temperature. The spontaneous emission intensity E of the loading layer to be measured is expressed by the following formula (1).
[0064]
number
[0065] In addition, when the radiation light is blocked by the measurement window 86, the received light intensity Er (W / m 3 ) is expressed by the following formula (2) using the spontaneous emission intensity E and the transmittance ξ (%) in the above formula (1).
[0066] Er = ξE (2)
[0067] When the above formulas (1) and (2) are used for correction, the transmittance ξ of the window material of the measurement window is previously determined by measuring the electromagnetic waves emitted from the blackbody furnace through the window material used for measurement offline with a radiation thermometer. Then, by using the transmittance ξ and the above formulas (1) and (2), the surface temperature T of the charging bed S can be calculated with high accuracy even if the transmittance of the measurement window 86 is not 100% for the selected measurement wavelength.
[0068] In the ignition furnace 36 according to the present embodiment, it is preferable to make the pressure above the charging bed S inside the ignition furnace cover 74 negative by sucking air using the wind box 40 provided below the pallet 34. Here, negative pressure means that the pressure inside the ignition furnace 36 is lower than that outside.
[0069] Referring again to FIG. 1, the exhaust fan 46 is a device for sucking gas from the main duct 42, and is, for example, a blower or a pump. The exhaust fan 46 sucks gas from the main duct 42, thereby creating a negative pressure in the wind box 40 connected to the main duct 42. When the wind box 40 is placed under negative pressure, the wind box 40 sucks in the air inside the charging bed S, and the pressure above the charging bed S inside the ignition furnace cover 74 becomes negative. The pressure above the charging bed S may be represented by the pressure measured inside the ignition furnace cover 74. In this case, it is preferable to measure the pressure downstream of the ignition furnace 36, and it is more preferable to measure the pressure near the center of the ignition furnace 36 in the width direction.
[0070] In this way, the wind box 40 makes the pressure above the charging bed S inside the ignition furnace cover 74 negative. The pressure above the charging bed S inside the ignition furnace cover 74 is preferably a negative pressure that is 2 to 10 kPa lower than the pressure outside the ignition furnace 36. By making the pressure above the charging bed S negative, water vapor generated by the combustion of the fuel gas is sucked into the charging bed S from above the charging bed S. In addition, dust generated by the ignition of the charging bed S is prevented from floating above the charging bed S. This allows the radiation emitted from the surface of the charging bed S to pass through the measurement window 86 without being affected by water vapor and dust generated inside the ignition furnace 36. As a result, the surface temperature of the charging bed S can be measured with even higher accuracy using the radiation thermometer 84.
[0071] Specifically, when the fuel gas used in the ignition furnace burner 72 contains hydrogen (H2) or methane (CH4), water vapor is generated by the combustion of the fuel gas. Figure 11 is a graph showing the light transmittance of water vapor. The horizontal axis of Figure 11 is wavelength (μm), and the vertical axis is transmittance (%).
[0072] As shown in Fig. 11, water vapor has low transmittance of a part of the radiation light in the range of 0.5 μm to 4.0 μm, which is the measurement wavelength of the radiation thermometer 84 (range of 3 to 4 μm). Therefore, the radiation light emitted from the surface of the charging bed S is attenuated by the water vapor in the ignition furnace 36, and the light receiving intensity of the radiation thermometer 84 installed outside the measurement window 86 decreases. Therefore, it can be seen that the surface temperature of the charging bed S can be measured with high accuracy by the radiation thermometer 84 installed outside the measurement window 86, since the attenuation of the radiation light by the water vapor is suppressed by sucking the water vapor in the ignition furnace 36 into the charging bed S.
[0073] Next, the sintered ore yield prediction device 110 will be described. As described above, the sintered ore yield prediction device 110 is a device that inputs input data including the surface temperature of the charging layer S in the ignition furnace 36 into a yield prediction model, outputs the sintered ore yield, and predicts the sintered ore yield. Furthermore, the sintered ore yield prediction device 110 is also a device that specifies a surface temperature at which the predicted sintered ore yield is equal to or greater than a target yield value, and specifies the operation parameters of the ignition furnace 36 that can achieve the specified surface temperature.
[0074] FIG. 12 is a diagram showing a schematic configuration example of a sintered ore yield prediction device 110. The sintered ore yield prediction device 110 is, for example, a general-purpose computer such as a workstation or a personal computer. The sintered ore yield prediction device 110 has a control unit 112, an input unit 114, an output unit 116, and a storage unit 118. The control unit 112 is, for example, a CPU, and executes various programs stored in the storage unit 118 to cause the control unit 112 to function as a data acquisition unit 120, a yield prediction unit 122, an ignition furnace operation parameter identification unit 124, and a yield prediction model generation unit 126.
[0075] The input unit 114 is, for example, a keyboard, a touch panel integrally provided with a display, or the like. The output unit 116 is, for example, an LCD or CRT display, or the like. The storage unit 118 is, for example, an information recording medium such as an updatable flash memory, a built-in hard disk or a hard disk connected via a data communication terminal, a memory card, or the like, and a read / write device for the information recording medium. The storage unit 118 stores programs and data for realizing the production of sintered ore 56 by the sintered ore production equipment 140. The storage unit 108 also stores a database 128 and a yield prediction model 130. The database 128 stores 30 or more, preferably 100 or more, more preferably 500 or more data sets, each set being a set of a past record value of the surface temperature of the charging layer S of sintered ore produced by the sintered ore production equipment 140 and a past record value of the yield. If necessary, the database 128 may store a data set in which actual values of the operating parameters of the ignition furnace 36 described below, actual values of the operating parameters of the sintering process, and actual values of the attribute information of the sintering bed S are acquired from the process computer 100 and associated with the actual values of the surface temperature of the sintered ore sintering bed S and the actual values of the yield.
[0076] Next, the sintered ore yield prediction process by the sintered ore yield prediction device 110 will be described. The data acquisition unit 120 acquires the surface temperature of the sintered ore bed S from the process computer 100 as input data. The data acquisition unit 120 acquires the same type of surface temperature of the sintered ore bed S as the input data of the yield prediction model 130 so that the surface temperature can be input to the yield prediction model 130 generated by the yield prediction model generation unit 126 described later. Therefore, the data acquisition unit 120 may acquire the surface temperature of the sintered ore bed S at a specific position as the surface temperature of the sintered ore bed S, or may acquire the average value of the surface temperature of the sintered ore bed S. For example, the surface temperature of the sintered ore bed S at a position (ignition part) where the flame ejected from the ignition furnace burner 43 collides with the sintered ore bed S in the ignition furnace 36, or at a representative position set downstream of the ignition part, or the average temperature in the width direction of the sintered ore bed S may be used. The data acquisition unit 120 outputs the acquired input data to the yield prediction unit 122.
[0077] When the yield prediction unit 122 acquires input data from the data acquisition unit 120, it reads out the yield prediction model 130 stored in the storage unit 118. The yield prediction unit 122 inputs the input data into the yield prediction model and outputs the yield of sintered ore, thereby predicting the yield of sintered ore. The yield prediction unit 122 may display the predicted yield of sintered ore on the output unit 116. This allows the operator to check the predicted value of the yield of sintered ore by visually checking the output unit 116.
[0078] In this way, in the sintered ore yield prediction device 110 according to the present embodiment, the surface temperature of the charging layer S in the ignition furnace 36 is input to the yield prediction model 130, and the yield of the sintered ore is output to predict the yield of the sintered ore. As the surface temperature of the charging layer S, the surface temperature measured by the radiation thermometer 84, which has a measurement wavelength selected from the range of 0.5 μm to 4.0 μm, through the measurement window 86 from the outside of the ignition furnace cover 74, is used. This surface temperature is a surface temperature measured with high accuracy while suppressing the influence of the flame 98 and carbon dioxide, so that the yield of the sintered ore can be predicted with high accuracy by predicting the yield of the sintered ore using input data including the surface temperature.
[0079] Next, the operation parameter setting process of the ignition furnace 36 by the sintered ore yield prediction device 110 will be described. The yield prediction unit 122 outputs the predicted sintered ore yield to the ignition furnace operation parameter specification unit 124. The ignition furnace operation parameter specification unit 124 judges whether the predicted value of the sintered ore yield obtained from the yield prediction unit 122 is equal to or greater than the target yield value. The target yield value may be input by the operator from the input unit 114, or may be input by the operator in advance and stored in the storage unit 118.
[0080] When the acquired predicted value of the sintered ore yield is equal to or greater than the target yield, the ignition furnace operation parameter specifying unit 124 specifies that the surface temperature acquired by the data acquiring unit 120 is the surface temperature that can make the yield of the charging layer S equal to or greater than the target yield. In this case, the ignition furnace operation parameter specifying unit 124 does not change the fuel gas flow rate and the air ratio, which are the operation parameters of the ignition furnace, so that the current surface temperature is maintained.
[0081] On the other hand, if the acquired predicted value of the sintered ore yield is less than the target yield value, the ignition furnace operation parameter specification unit 124 changes the surface temperature acquired by the data acquisition unit 120 and outputs the changed surface temperature to the yield prediction unit 122. The yield prediction unit 122 inputs the changed surface temperature again to the yield prediction model 130, outputs the sintered ore yield, and predicts the sintered ore yield. The yield prediction unit 122 outputs the sintered ore yield prediction value to the ignition furnace operation parameter specification unit 124. The ignition furnace operation parameter specification unit 124 judges whether the acquired predicted value of the sintered ore yield is equal to or greater than the target yield value. The yield prediction unit 122 and the ignition furnace operation parameter specification unit 124 repeat this process until the predicted value of the sintered ore yield becomes equal to or greater than the target yield value.
[0082] If the sintered ore yield predicted at the changed surface temperature is equal to or greater than the target yield value, the ignition furnace operation parameter identification unit 124 identifies the changed surface temperature as the surface temperature that can make the sintered ore yield equal to or greater than the target yield value.
[0083] FIG. 13 is a graph showing the relationship between the flow rate of the fuel gas (C gas) supplied to the ignition furnace burner 72 and the surface temperature of the sintering bed S. In the example shown in FIG. 13, coke oven gas (C gas) was used as the fuel gas for the ignition furnace burner 72. The flow rate of the fuel gas on the horizontal axis is the flow rate of the fuel gas supplied per unit width of the sintering bed S (Nm 3 / (h m)). The radiation thermometer 84 used to measure the surface temperature of the charging bed S is a thermograph capable of measuring the surface temperature distribution of the charging bed S. The measuring element is InGaAs, the measuring wavelength is 1.55 μm, and the measuring window 86 is quartz glass. Air is sucked from the wind box 40, and the pressure inside the ignition furnace 36 is controlled to be 5 kPa lower than the outside.
[0084] 13(a) is a graph showing an example of measuring the spot temperature at the widthwise center of the charging bed S as the surface temperature of the charging bed S. The spot temperature at the widthwise center is a temperature measured using surface temperature data at a specific position 100 mm away from the ignition part 99 in the ignition furnace 36 in the conveying direction of the pallet 34.
[0085] 13(b) is a graph showing an example in which the average temperature in the width direction of the charging bed S is used as the surface temperature of the charging bed S. The average temperature in the width direction of the charging bed S was calculated as an average value from the surface temperature distribution data at a position 100 mm away from the ignition part 99 in the ignition furnace 36 in the conveying direction of the pallet 34.
[0086] As shown in Figures 13(a) and 13(b), increasing the flow rate of the fuel gas also increases the surface temperature of the charging bed S. The storage unit 118 stores the correspondence between the flow rate of the fuel gas and the surface temperature of the charging bed S as shown in Figures 13(a) and 13(b), and the operation parameter specification unit 124 of the ignition furnace reads out the correspondence from the storage unit 108 and specifies the flow rate of the fuel gas, which is an operation parameter of the ignition furnace 36, by using the correspondence and the surface temperature that can be made equal to or higher than the target yield value. The operation parameter specification unit 124 of the ignition furnace outputs the specified operation parameters of the ignition furnace 36 to the process computer 100. The process computer 100 sets the operation parameters acquired from the operation parameter specification unit 124 of the ignition furnace as the operation conditions of the ignition furnace 36, and adjusts the fuel gas flow rate control valve 90 so as to satisfy the conditions. In this way, the sintered ore yield prediction device 110 according to this embodiment can identify the operation parameters of the ignition furnace that can make the sintered ore yield equal to or higher than the target yield, and set the operation conditions of the ignition furnace 36 to the identified operation parameters. By changing the operation conditions of the ignition furnace 36 in this way, it becomes possible to produce sintered ore 56 at a yield equal to or higher than the target yield in the sintered ore production facility 140.
[0087] Next, a method for generating the yield prediction model 130 used to predict the yield of sintered ore will be described. The data acquisition unit 120 acquires the surface temperature of the sintering bed S and the actual value of the yield of sintered ore from the process computer 100, and stores a set of these data in the database 128 of the storage unit 118. The number of data sets stored in the database 128 is at least 30 or more, preferably 100 or more, and more preferably 500 or more.
[0088] The yield prediction model generating unit 126 reads out the pre-stored machine learning model from the storage unit 118, and trains the machine learning model using multiple data sets stored in the database 128 as training data to generate a trained machine learning model. This trained machine learning model becomes the yield prediction model 130. Note that, as the machine learning model used in the sintered ore yield prediction method and the sintered ore yield prediction device 110 according to the present embodiment, for example, a neural network, decision tree learning, random forest, or support vector regression may be used. In addition, as the machine learning model, an ensemble model combining multiple machine learning models may be used. Furthermore, as the machine learning model, a classification model such as a k-nearest neighbor method or logistic regression may be used.
[0089] FIG. 14 is a schematic diagram showing an example of a yield prediction model 130 generated using a neural network. The yield prediction model 130 shown in FIG. 14 is a yield prediction model 130 in which the surface temperature of the charging layer S and the operation parameters of a plurality of ignition furnaces described later are input data, and the yield of sintered ore is output data. L1, L2, and L3 respectively indicate an input layer, an intermediate layer, and an output layer. The yield prediction model 130 shown in FIG. 13 has two intermediate layers, three nodes, and uses a sigmoid function as an activation function. However, when the operation parameters of the ignition furnace are not used as input data for the yield prediction model 130, a neural network is formed in which only the surface temperature of the charging layer S is input data.
[0090] By using such a machine learning model, for example, operation parameters of an ignition furnace that are correlated with the yield of sintered ore can be freely selected as input data without considering the problem of multicollinearity. By including operation parameters of an ignition furnace that are correlated with the yield of sintered ore in the input data, the prediction accuracy of the yield of sintered ore of the yield prediction model 130 can be improved.
[0091] The yield prediction model generating unit 126 may also improve the accuracy of sinter ore yield prediction by dividing the data set stored in the database 128 into training data and test data and performing machine learning. For example, the yield prediction model generating unit 126 may perform machine learning of weight coefficients of a neural network using training data, and generate a yield prediction model 130 while appropriately changing the structure of the neural network (the number of intermediate layers and the number of nodes) so as to increase the accuracy rate of the sinter ore yield in the test data. An error propagation method may be used to update the weight coefficients.
[0092] The yield prediction model 130 may be updated to a new model by re-learning, for example, every six months or every year. This is because the more data stored in the database 128, the more accurately a yield prediction model that can predict the yield can be generated. By generating and updating the yield prediction model using the latest data, a yield prediction model that reflects the changes over time of the sinter ore manufacturing equipment 140 can be generated.
[0093] The data acquiring unit 120 may acquire the surface temperature of the sintering bed S at a specific position as the surface temperature of the sintering bed S, or may acquire multiple surface temperatures of the sintering bed S measured at multiple positions. When the data acquiring unit 120 acquires actual data measured at multiple positions as the surface temperature, the number of nodes may be adjusted so that the actual data measured at those positions are input as the surface temperature of the sintering bed S to be input to the input layer L1 of the neural network. Furthermore, when the data acquiring unit 120 acquires a temperature chart created by scanning the sintering bed S in the width direction or length direction using the radiation thermometer 84 as the surface temperature, or when acquiring two-dimensional image data of the temperature distribution on the surface of the sintering bed using a thermograph capable of measuring the in-plane temperature distribution, the sinter yield prediction model may be generated using a convolutional neural network using these as inputs.
[0094] The data acquiring unit 120 may acquire the heat retention index of the sintering bed S as the surface temperature of the sintering bed S. The heat retention index is a value obtained by integrating the temperature at or above a preset lower limit temperature by the retention time. This heat retention index is also an index representing the surface temperature of the sintering bed S.
[0095] FIG. 15 is a graph showing the time change of the surface temperature of the charging bed S from ignition. The heat retention index is the area Sk where the surface temperature of the charging bed S is maintained at 1000°C or higher in the graph showing the time change of the surface temperature from ignition shown in FIG. 15, when the lower limit temperature is 1000°C. The time change of the surface temperature of the charging bed S is obtained by extracting temperature data in the longitudinal direction at the center of the width direction of the charging bed S from surface temperature distribution data measured by thermography downstream of the ignition part 99 in the ignition furnace 36 in the conveying direction of the pallet 34. The time change of the surface temperature is obtained from this temperature data and the conveying speed of the pallet 34, and the holding time for maintaining the temperature at 1000°C or higher can be calculated from the time change of the surface temperature.
[0096] Fig. 16 is a graph showing the relationship between the flow rate of the fuel gas (C gas) supplied to the ignition furnace burner 72 and the heat retention index of the charging bed S. As shown in Fig. 16, when the flow rate of the fuel gas is increased, the heat retention index of the charging bed S also increases. Therefore, if the operation parameter specifying unit 124 of the ignition furnace specifies a heat retention index that can achieve the target yield or more in a similar manner to the above, the flow rate of the fuel gas, which is an operation parameter of the ignition furnace 36 that can achieve the target yield or more, can be specified by using the correspondence shown in Fig. 16.
[0097] In addition, the data acquiring unit 120 may acquire, as input data, operation parameters of the ignition furnace 36, operation parameters of the sintering process, and attribute information of the charging bed S, together with the surface temperature of the charging bed S. These pieces of information are collected and stored by the process computer 100.
[0098] The operation parameters of the ignition furnace 36 are at least one set value of the fuel gas flow rate, air amount, and air ratio of the ignition furnace burner 72 among the sintered ore production conditions. These affect the flame temperature and injection speed injected from the ignition furnace burner 72, and therefore affect the ignition behavior and sintering reaction of the charging layer S. Therefore, by including the operation parameters of the ignition furnace 36 in the input data, the yield prediction model 130 becomes a model that can predict the sintered ore yield with higher accuracy.
[0099] The operation parameters of the sintering process are at least one of the transport speed of the pallet 34 among the sinter ore production conditions, the amount of exhaust gas sucked into the wind box 40 among the sensor information, the oxygen concentration of the atmospheric gas above the charging layer S in the ignition furnace 36, and the oxygen concentration of the exhaust gas sucked into the wind box 40. When multiple wind boxes 40 are provided, an oxygen concentration meter may be installed in each wind box 40, and the oxygen concentration exhausted from each wind box 40 may be used.
[0100] When the conveying speed of the pallet 34 changes, the contact time between the flame and the surface of the charging bed S changes, and the surface temperature of the charging bed S changes, so the conveying speed of the pallet 34 affects the sintering reaction. In addition, the amount of exhaust gas sucked in by the wind box 40 can be said to be the amount of gas that has passed through the inside of the charging bed S. Since the temperature inside the charging bed S changes depending on the amount of gas passing through the inside of the charging bed S, the amount of exhaust gas also affects the sintering reaction. In addition, the oxygen concentration of the atmospheric gas above the charging bed S in the ignition furnace 36 affects the progress of the sintering reaction when the gas passes through the charging bed S. The oxygen concentration of the exhaust gas sucked in by the wind box 40 affects the progress of the sintering reaction in the charging bed S. Therefore, by including these operation parameters of the sintering process in the input data, the yield prediction model 130 becomes a model that can predict the yield of sintered ore with even higher accuracy.
[0101] The attribute information of the charging layer S is at least one of the following among the production conditions of sintered ore: the layer thickness of the charging layer S, the content of quicklime and silica stone contained in the sintering raw material, the blending ratio of coke powder, the brand of iron ore, the moisture content of the sintering raw material, and the average particle size of the sintering raw material. When the layer thickness of the charging layer S changes, the distance between the ignition furnace burner 72 and the surface of the charging layer S changes, and the ignition characteristics of the flame 98 change, so the layer thickness of the charging layer S affects the sintering reaction. When the content of quicklime, silica stone, and coke powder contained in the sintering raw material or the brand of iron ore changes, the speed and heat generation of the melting reaction in the charging layer S change, so these also affect the sintering reaction in the charging layer S. Furthermore, when the moisture content and average particle size of the sintering raw material change, the gas permeability passing through the charging layer S changes, which affects the amount of oxygen passing through the charging layer S, so these also affect the sintering reaction in the charging layer S. Therefore, by including the attribute information of the sintering layer S in the input data, the yield prediction model 130 becomes a model that can predict the yield of sintered ore with even higher accuracy.
[0102] Furthermore, when these are included in the input data, in the process of identifying the surface temperature that results in a sintered ore yield equal to or greater than the target yield value, instead of changing the surface temperature, it is possible to change the operation parameters of the sintering process or adjustable items among the attribute information of the sintering bed S. Then, the operation parameters and the like used when the predicted sintered ore yield is equal to or greater than the target yield value may be set as the production conditions of the sintered ore production equipment 140.
[0103] In the example shown in Fig. 1, the process computer 100 and the sintered ore yield prediction device 110 are separate devices, but this is not limited to the above. The sintered ore yield prediction device 110 may have the functions of the process computer 100, and in this case, the sintered ore production equipment 140 may not have the process computer 100.
[0104] Further, the sintered ore yield prediction device 110 has been described using an example having the ignition furnace operation parameter specification unit 124 and the yield prediction model generation unit 126, but is not limited thereto. If the yield of sintered ore is predicted, the sintered ore yield prediction device 110 does not need to have the ignition furnace operation parameter specification unit 124. Furthermore, if the yield prediction model 130 is generated externally, acquired through the data acquisition unit 120, and stored in the storage unit 118, the yield prediction model generation unit 126 may not be included. Furthermore, the yield prediction model 130 may be stored in another device capable of communicating with the sintered ore yield prediction device 110, instead of the storage unit 118 of the sintered ore yield prediction device 110. EXAMPLES
[0105] Next, an embodiment in which the yield of sintered ore was predicted using the sintered ore yield prediction device 110 of the sintered ore production facility 140 and sintered ore was produced will be described. In the embodiment, the surface temperature of the charging layer S in the ignition furnace 36 was measured from the outside of the ignition furnace cover 74 provided in the ignition furnace 36 shown in FIG. 3 through the measurement window 86 by a radiation thermometer 84 using a lead selenide (PbSe) element with a measurement wavelength of 4.0 μm. The measurement window 86 was made of calcium fluoride, quartz glass, or germanium, and the radiation light transmittances of each were 92%, 70%, and 65%. The radiation thermometer 84 was a scanning radiation thermometer thermography, and measured the in-plane temperature distribution of the charging layer S downstream of the ignition part 99 in the ignition furnace in the conveying direction of the pallet.
[0106] In the examples of the invention, the surface temperature of the charging bed S was determined by using the spot temperature at the widthwise center of the charging bed S, the average temperature of the charging bed S in the widthwise direction, and the heat retention index calculated from the surface temperature distribution of the charging bed S. The heat retention index was determined by calculating the integral value of the surface temperature during the time when the surface temperature of the charging bed S was maintained at 1000°C or higher, with the surface temperature of the charging bed S set at 1000°C as the lower limit.
[0107] In the examples of the invention, the yield of sintered ore was predicted not only using yield prediction models (Examples 1 to 5) that used the above-mentioned surface temperature as input data, but also using yield prediction models (Examples 6 to 9) that included operational parameters such as the fuel gas flow rate supplied to the ignition furnace burner 72, the conveying speed of the pallet 34, and / or the content of quicklime and powdered coke in the sintering raw materials as input data in addition to the surface temperature.
[0108] The yield prediction model 130 acquires a plurality of data sets, each of which is a pair of the actual value of the input data and the actual value of the yield of the sintered ore, from the process computer 100 and stores the data in the database 128.
[0109] When the number of data sets stored in database 128 reached 3000, 1500 pieces of learning data were extracted from database 128, and the remaining 1500 pieces of learning data were used for machine learning the machine learning model. In the machine learning, the type of input data used for the yield prediction model was changed, and a yield prediction model corresponding to each input data was generated.
[0110] The generated yield prediction model was evaluated for its prediction accuracy of sintered ore yield using 1,500 test data. The machine learning model used was a neural network with three hidden layers and five nodes in each hidden layer. The activation function used was a sigmoid function.
[0111] In Comparative Example 1, a yield prediction model was generated using 1500 pieces of learning data under the same conditions as in Example 2 of the invention, except that the measurement wavelength of the radiation temperature system was 4.5 μm, and the yield of sintered ore was evaluated using 1500 pieces of test data. In Comparative Example 2, a yield prediction model was generated using 1500 pieces of learning data under the same conditions as in Example 2 of the invention, except that the measurement window was removed and the surface temperature was measured, and the yield of sintered ore was evaluated using 1500 pieces of test data. The results of evaluating the sintered ore yield prediction error 3σ as the prediction accuracy of the sintered ore yield in the invention examples and comparative examples are shown in Table 1 below.
[0112] [Table 1]
[0113] As shown in Table 1, the prediction error 3σ of the sintered ore yield in the invention examples 1 to 9 was smaller than the prediction error 3σ of the sintered ore yield in the comparative examples 1 and 2. From this result, it was confirmed that the yield of sintered ore can be predicted with high accuracy by using the yield prediction model of the invention examples 1 to 9. By measuring the surface temperature of the sintered ore bed S with a radiation thermometer 84 having a measurement wavelength of 4.0 μm from the outside of the measurement window 86, the influence of flames and carbon dioxide is suppressed, and the surface temperature of the sintered ore bed S can be measured with high accuracy. For this reason, it is considered that the sintered ore yield could be predicted with high accuracy by using the surface temperature as input data. In addition, in the invention examples 6 to 9, the input data further included operational parameters correlated with the sintered ore yield, so that the value of the prediction error 3σ of the sintered ore yield was even smaller than that of the invention examples 1 to 5. These results confirmed that the yield of sintered ore can be predicted with even higher accuracy by using a yield prediction model that includes these operational parameters as input data.
[0114] On the other hand, in Comparative Example 1, although the conditions were similar to those of Invention Example 2, the value of the prediction error 3σ of the yield was larger than that of Invention Example 2. This result is considered to be due to the fact that the measurement wavelength of the radiation thermometer 84 was a long wavelength of 4.5 μm, and therefore carbon dioxide (carbonic acid gas) generated by the combustion of the fuel gas disturbed the temperature measurement, increasing the measurement error of the surface temperature of the charging bed obtained by the radiation thermometer 84, resulting in a lower prediction accuracy of the sintered ore yield.
[0115] In addition, although the conditions of Comparative Example 2 were similar to those of Inventive Example 2, the value of the prediction error 3σ of the yield was larger than that of Inventive Example 2. In Comparative Example 2, the measurement window 86 was opened and the surface temperature of the charging bed S was directly measured by the radiation thermometer 84, so that a local temperature drop occurred in part of the surface of the charging bed S due to the inflow of outside air when the measurement window 86 was opened. This local temperature drop increased the variation in the surface temperature measured by the radiation thermometer 84, which is thought to have reduced the accuracy of the prediction of the sintered ore yield.
[0116] Using the yield prediction model generated in Example 9, the operating parameters of the ignition furnace that can achieve a target yield or higher were specified, and sintering was carried out. Here, the target yield is, for example, 80.0%. The average temperature in the width direction that can achieve the target yield or higher was specified, and the C gas flow rate that can achieve the specified average temperature in the width direction was specified using the correspondence relationship in Figure 12(b), and the C gas flow rate was set as the operating condition of the ignition furnace 36.
[0117] The sintered ore production equipment 140 was operated for three days under the operating conditions of the ignition furnace 36 to produce sintered ore, resulting in a sintered ore yield of 81.6%. In contrast, the sintered ore production equipment 140 was operated for three days under conditions where the operating conditions of the ignition furnace 36 were not reset to produce sintered ore, resulting in a sintered ore yield of 77.3%. From these results, it was confirmed that sintered ore can be produced with a high yield by using the sintered ore production equipment control method and sintered ore production method according to this embodiment. [Explanation of symbols]
[0118] 10 Blending tank 12 Surge Hopper 14. Conveyor for mixed raw materials 16 Drum Mixer 18 Sintering materials 20 Sintering material transport conveyor 30 Sintering machine 32 Sintering raw material charging device 34 Palette 36 Ignition Furnace 38 Gaseous fuel supply device 40 Wind Box 42 Main Duct 44 Dust collector 46 Exhaust fan 48 Chimney 60 Feeding Hopper 62 Drum Feeder 64 Charging gate 66 Shots 70 Baffle 72 Ignition furnace burner 74 Ignition furnace cover 76 Burner Nozzle 80 Top cover 82 Side cover 84 Radiation thermometer 86 Measurement window 88 Pallet side panel 90 Fuel gas flow control valve 92 Fuel gas flow meter 94 Air flow control valve 96 Air flow meter 98 Flame 99 Ignition part 100 Process Computer 110 Sintered Ore Yield Prediction Device 112 Control section 114 Input section 116 Output section 118 Storage Unit 120 Data Acquisition Section 122 Yield Prediction Department 124 Ignition furnace operating parameter specification section 126 Yield prediction model generation unit 128 Databases 130 Yield Prediction Model
Claims
1. A method for predicting the yield of sintered ore in a sintered ore production facility in which sintered ore is produced using an ignition furnace that burns the carbonaceous material in a charging bed after charging sintered ore containing carbonaceous material into an endless moving pallet to form a charging bed, comprising: A method for predicting the yield of sintered ore, comprising: inputting input data including the surface temperature of the charging layer inside the ignition furnace cover, which is measured from the outside of the ignition furnace cover through a measurement window of the ignition furnace cover with a radiation thermometer having a measurement wavelength selected from a range of 0.5 μm or more and 4.0 μm or less, into a yield prediction model; and outputting the yield of sintered ore to predict the yield of sintered ore.
2. 2. The method for predicting a yield of sintered ore according to claim 1, wherein the transmittance of the measurement window at the measurement wavelength is 50% or more.
3. The method for predicting a yield of sintered ore according to claim 1, wherein a pressure above the sintering bed inside the ignition furnace cover is made negative.
4. The method for predicting a yield of sintered ore according to claim 2, wherein a pressure above the sintering bed inside the ignition furnace cover is made negative.
5. If the surface of the charging bed that is ignited by a flame sprayed from an ignition furnace burner provided in the ignition furnace is defined as an ignition part, The method for predicting a yield of sintered ore according to claim 1 , wherein the surface temperature includes a surface temperature of the ignition part.
6. If the surface of the charging bed that is ignited by a flame sprayed from an ignition furnace burner provided in the ignition furnace is defined as an ignition part, The method for predicting a yield of sintered ore according to claim 2 , wherein the surface temperature includes a surface temperature of the ignition part.
7. If the surface of the charging bed that is ignited by a flame sprayed from an ignition furnace burner provided in the ignition furnace is defined as an ignition part, The method for predicting a yield of sintered ore according to claim 3 , wherein the surface temperature includes a surface temperature of the ignition part.
8. If the surface of the charging bed that is ignited by a flame sprayed from an ignition furnace burner provided in the ignition furnace is defined as an ignition part, The method for predicting a yield of sintered ore according to claim 4 , wherein the surface temperature includes a surface temperature of the ignition part.
9. Identifying a surface temperature at which the yield of sintered ore predicted by the method for predicting the yield of sintered ore according to any one of claims 1 to 8 becomes equal to or greater than a target yield value; A method for controlling a sintered ore production facility, comprising setting operating conditions of the ignition furnace so that the surface temperature of the sintering bed becomes a specified surface temperature.
10. A method for producing sintered ore, comprising the step of producing sintered ore by using the method for controlling sintered ore production equipment according to claim 9.
11. A method for generating a yield prediction model for predicting the yield of sintered ore in a sintered ore production facility in which sintered ore is produced using an ignition furnace that burns the carbonaceous material in a charging bed after sintering raw materials including carbonaceous material are charged into an endless moving pallet to form a charging bed, the method comprising the steps of: A method for generating a yield prediction model, comprising: acquiring a plurality of data sets each consisting of a pair of actual values of input data including the surface temperature of the charging layer inside the ignition furnace cover measured from the outside of the ignition furnace cover through a measurement window of the ignition furnace cover with a radiation thermometer having a measurement wavelength selected from a range of 0.5 μm or more and 4.0 μm or less, and an actual value of the yield of sintered ore; and generating a yield prediction model using the input data as input and the yield of the sintered ore as output by machine learning using the acquired plurality of data sets as training data.
12. A sintered ore yield prediction device for predicting the yield of sintered ore in a sintered ore production facility in which sintered ore is produced by using an ignition furnace that burns the carbonaceous material in the charging bed after sintering raw materials including carbonaceous material are charged into an endless moving pallet to form a charging bed, A data acquisition unit that acquires input data including a surface temperature of the charging bed inside the ignition furnace cover measured from the outside of the ignition furnace cover of the ignition furnace through a measurement window of the ignition furnace cover by a radiation thermometer having a measurement wavelength selected from a range of 0.5 μm to 4.0 μm; a sintered ore yield prediction unit that inputs the input data into a yield prediction model and outputs the sintered ore yield to predict the sintered ore yield; The sintered ore yield prediction device has the following features.
13. The sintered ore yield prediction device according to claim 12, wherein the transmittance of the measurement window at the measurement wavelength is 50% or more.
Citation Information
Patent Citations
Sintering method by dwight-lloyd sintering machine
JP1984074243A
Method for measuring temperature and temperature distribution
JP1988183132A
Method of controlling combustion of raw material firing part on pallet of sintering machine
JP1989306528A
Production of sintered ore
JP1990153027A
Method and system for optimization of agglomeration of ores
US20220275475A1