Highly rigid polyethylene terephthalate film
By stretching polyethylene terephthalate films multiple times at high temperatures, the film's crystallinity is enhanced, addressing the low rigidity issue and achieving high elastic modulus for thin films in industrial applications.
Patent Information
- Application Number
- JP2023069555
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional biaxially stretched polyethylene terephthalate films have low elastic modulus and rigidity due to limited stretching ratios at low temperatures, which hinders the achievement of high tensile modulus and bending rigidity, especially in thin films.
The film is stretched multiple times at high temperatures below the melting point to enhance crystallinity, with controlled sequential and simultaneous biaxial stretching methods to improve rigidity and reduce breakage frequency.
The resulting film exhibits excellent bending rigidity and high elastic modulus, suitable for thin films requiring high quality in industrial applications.
Smart Images

Figure 2024155122000006 
Figure 2024155122000007 
Figure 2024155122000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyethylene terephthalate film using a resin containing polyethylene terephthalate as a main component. [Background technology]
[0002] Films made of polyesters, such as polyethylene terephthalate-based resins, are excellent in mechanical properties, heat resistance, and the like, and are used in a variety of applications. For example, they are widely used in packaging applications, electrical insulation applications, optical applications, magnetic recording applications, and the like. In recent years, polyester films used for these applications are often required to be made thinner and have higher strength in accordance with the thinner thickness.
[0003] To solve such problems, a method for increasing the strength of a polyethylene terephthalate film is known in which a film stretched in two directions, longitudinal and transverse, is stretched again in the longitudinal and transverse directions to increase the strength in the stretching directions. For example, Patent Document 1 discloses a method for improving the strength without impairing the formability by stretching in multiple stages in the longitudinal and transverse directions. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-011786 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, although the biaxially stretched polyethylene terephthalate film produced by the method of Patent Document 1 suppresses and improves elongation deformation due to tension, the stretching temperature is low, so the stretching ratio in multi-stage stretching cannot be set high, and the film has a problem of low elastic modulus.
[0006] As described above, the conventional techniques have been unable to improve the tensile modulus in the longitudinal and transverse directions and at the same time obtain the rigidity that accompanies a thinner wall.
[0007] An object of the present invention is to provide a polyethylene terephthalate film having excellent bending rigidity. [Means for solving the problem]
[0008] As a result of intensive research by the present inventors on polyethylene terephthalate-based films, the present inventors discovered a method of stretching a biaxially oriented polyester film at a high temperature below the melting point (Tm) multiple times to elongate the internal molecular chains and increase the crystallinity, thereby stretching the film near the melting point. As a result, the biaxially oriented polyethylene terephthalate-based polyester film of the present invention has been successfully improved in rigidity. To be more specific, the present invention has the following configuration in order to solve the above problems. [Item 1] A film made of a composition containing polyethylene terephthalate resin, and the sum of the bending stiffness Fa in the MD direction and the bending stiffness Fb in the TD direction converted to a thickness of 15 μm is 0.05 gf cm 2 / cm or more of polyethylene terephthalate film. [Item 2] The polyethylene terephthalate film according to Item 1, wherein the crystal size of the crystals formed by the polymer molecules constituting the film is 3.0 nm or more as measured by a small-angle X-ray scattering method. [Item 3] The polyethylene terephthalate film according to item 1 or 2, wherein the direction in which the omnidirectional bending rigidity is the maximum value is the longitudinal direction. [Item 4] A laminate film having a base layer made of the polyethylene terephthalate film according to any one of items 1 to 3, and a release layer laminated on at least one surface of the base layer. [Item 5] The laminate film according to item 4, which is a release film for producing a ceramic green sheet, and the release layer is made of a composition containing a silicone release component. [Item 6] The laminate film according to item 4, wherein the maximum protrusion height (P) of the release layer surface is 200 nm or less, and the arithmetic mean roughness (Sa) of the release layer surface is 10 nm or less. Effect of the Invention
[0009] The film of the present invention has excellent bending stiffness. Therefore, even when it is thin, it has good stiffness and a high elastic modulus, so that it is suitable for industrial applications such as optical applications that require high quality during processing. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram for explaining a method for measuring bending rigidity. [Diagram 2] FIG. 2 is a schematic diagram for explaining a method for measuring the crystal size obtained by small-angle X-ray scattering. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The film of the present invention is made from a composition containing a polyethylene terephthalate resin. Here, the polyethylene terephthalate resin is a polymer containing ethylene glycol and terephthalic acid as main components. Specifically, it means a resin in which 80 mol% or more of the repeating units are composed of ethylene terephthalate. Other dicarboxylic acid components and glycol components may be copolymerized within a range that does not impair the object of the present invention. Examples of the other dicarboxylic acid components include isophthalic acid, p-β-oxyethoxybenzoic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-dicarboxybenzophenone, bis-(4-carboxyphenylethane), adipic acid, sebacic acid, 5-sodium sulfoisophthalic acid, cyclohexane-1,4-dicarboxylic acid, etc. Examples of the other glycol components include propylene glycol, butanediol, neopentyl glycol, diethylene glycol, ethylene oxide adducts of bisphenol A, etc., polyethylene glycol, polypropylene glycol, polytetramethylene glycol, etc. In addition, oxycarboxylic acid components such as p-oxybenzoic acid can also be used.
[0012] The polymerization method of polyethylene terephthalate resin is any production method such as a direct polymerization method and an ester exchange method. The direct polymerization method is a method in which terephthalic acid and ethylene glycol, and optionally other dicarboxylic acid components and diol components, are directly reacted. The ester exchange method is a method in which a dimethyl ester of terephthalic acid (containing a methyl ester of another dicarboxylic acid as necessary) and ethylene glycol (containing another diol component as necessary) are subjected to an ester exchange reaction.
[0013] The intrinsic viscosity of the polyethylene terephthalate resin is preferably in the range of 0.57 dl / g to 0.7 dl / g, and more preferably in the range of 0.58 dl / g to 0.65 dl / g.
[0014] In addition to the polyethylene terephthalate resin, the composition containing the polyethylene terephthalate resin may contain various additives as necessary. Examples of additives include inorganic lubricants such as titanium dioxide, fine silica, kaolin, and calcium carbonate, and organic lubricants such as crosslinked polymers made of acrylic monomers such as acrylic acid, methacrylic acid, acrylic acid esters, and methacrylic acid esters as materials for fine particles made of acrylic crosslinked polymers. In addition, stabilizers, colorants, antioxidants, antifoaming agents, antistatic agents, and ultraviolet absorbing agents may be contained alone or in combination of two or more kinds as necessary.
[0015] (Method of manufacturing stretched film) The polyester film used in the present invention is preferably an oriented film, more preferably a biaxially oriented film, from the standpoints of mechanical strength, chemical resistance, heat resistance, etc.
[0016] The resin composition in the present invention is processed into an unstretched sheet by various methods, and then biaxially stretched to obtain the sheet. As a method for producing the unstretched sheet, a method using melt extrusion as well as solution casting can be used, and the melt extrusion method is preferred in the present invention.
[0017] The resin composition in the present invention is preferably melted at 280 to 300° C., more preferably at 280° C. If the temperature is less than 280° C., the molten resin may not be melted or the melt viscosity may increase, lowering productivity, which is not preferred. If the temperature exceeds 290° C., the molecular weight may be easily reduced due to thermal degradation, which is not preferred.
[0018] The die temperature for melt extrusion is the same as described above, but is preferably 280 to 300° C., and more preferably 280° C. When the die temperature during melt extrusion is 280° C. or higher, the melt viscosity falls within a suitable range, allowing stable extrusion. By keeping the temperature at 300° C. or lower, thermal decomposition of the resin can be suppressed.
[0019] Next, the unstretched film obtained by the above method is stretched biaxially successively and simultaneously, and then it is necessary to stretch again in the width direction and the longitudinal direction in multiple stages at a film temperature in the range of 100°C to 250°C.
[0020] In the conventional sequential biaxial stretching method, in order to prevent thickness unevenness in the width direction and to obtain dimensional stability, the stretching temperature in the longitudinal and transverse directions is preferably in the range of the glass transition temperature (Tg+10°C) to (Tg+50°C), and the stretching ratio in the longitudinal and transverse directions is preferably in the range of 2 to 5. Thereafter, in order to reduce the thermal shrinkage rate of the polyester film, it is recommended to carry out a heat setting treatment within 30 seconds, preferably within 10 seconds, in the heat setting step, and to carry out a longitudinal relaxation treatment and a transverse relaxation treatment of 0.5 to 10%.
[0021] However, at conventional stretching temperatures, insufficient heat induces breakage during high-ratio stretching to obtain film rigidity. Therefore, in the present invention, for example, a uniaxially stretched film stretched in the machine direction is stretched in the transverse direction at (Tg+10°C) to (Tg+50°C) to achieve a certain degree of orientation, and then the film is stretched in multiple stages at a higher temperature of (Tg+60) to (Tg+160). This makes it possible to suppress the frequency of breakage during high-ratio stretching and obtain film rigidity.
[0022] (1) Control of sequential biaxial stretching In the case of the sequential biaxial stretching method, an unstretched film is stretched in the longitudinal direction at a temperature equal to or higher than the glass transition temperature (Tg) by utilizing the speed difference between rolls to produce a uniaxially stretched film. Specifically, the sheet is heated and stretched 1.1 to 6 times between two or many rolls with different peripheral speeds. The heating means at this time may be a method using a heated roll or a method using a non-contact heating medium, or these may be used in combination. In this case, it is preferable to set the film temperature in the range of (Tg-10°C) to (Tg+50°C).
[0023] Next, the uniaxially stretched film is stretched in multiple stages in the width direction by a tenter. Specifically, for example, when stretching in two stages, it is preferable to stretch the film in the first stage by 1.1 to 4.0 times in the width direction at a film temperature of (Tg+10°C) to (Tg+50°C), and then stretch the film in the second stage by 1.1 to 3.0 times in the width direction at a film temperature of (Tg+60°C) to (Tg+160°C). In the case of two-stage stretching, it is preferable to set the total stretching ratio in the width direction to 9.0 times or less, since this reduces the frequency of breakage. When stretching in four stages, the film in the first stage is stretched by 1.1 to 3.0 times in the width direction at a film temperature of (Tg+10°C) to (Tg+40°C). Then, the film in the second stage is stretched by 1.1 to 3.0 times in the width direction at a film temperature of (Tg+50°C) to (Tg+70°C). Then, in the third stage, the film is stretched 1.1 to 3.0 times in the width direction at a film temperature of (Tg+80°C) to (Tg+110°C). Then, in the fourth stage, the film is stretched 1.1 to 3.0 times in the width direction at a film temperature of (Tg+120°C) to (Tg+160°C). In the case of four-stage stretching, it is preferable to set the total stretching ratio in the width direction of the multi-stage stretching to 9.0 times or less, since this reduces the frequency of breakage.
[0024] (2) Control of simultaneous biaxial stretching When increasing the stiffness in the longitudinal direction by the simultaneous biaxial stretching method, the following control is preferable. For example, an unstretched film is held by clips and simultaneously stretched in a heating furnace at a film temperature of (Tg+10°C) to (Tg+50°C) by 1.1 to 4.0 times in the longitudinal direction and 1.1 to 2.0 times in the transverse direction, and then again stretched in the longitudinal direction by 1.1 to 1.5 times at (Tg+160°C) to (Tg+150°C). In the case of two-stage stretching, it is preferable to set the total stretching ratio in the longitudinal direction to 8.0 times or less, since this reduces the frequency of breakage.
[0025] (Film properties) The thickness of the film of the present invention is preferably 2 μm or more and 500 μm or less, more preferably 15 μm or more and 400 μm or less, and even more preferably 20 μm or more and 250 μm or less. When the thickness of the film is 2 μm or more, the film has a minimum rigidity and is easy to handle. When the thickness of the film is 500 μm or less, the transportability of the film when transporting the film with multiple rolls and the handleability of the produced film are improved, making it easy to handle.
[0026] The breaking strength of the film is preferably 100 MPa or more in both the MD and TD directions. More preferably, it is 200 MPa or more, and even more preferably, it is 350 MPa or more. The preferable lower limit of the breaking strength is 100 MPa, more preferably, it is 150 MPa, even more preferably, it is 200 MPa, and even more preferably, it is 350 MPa. The preferable upper limit of the breaking strength is 1000 MPa or more, more preferably, it is 500 MPa or more, and even more preferably, it is 300 MPa or more. When the breaking strength of the preferable upper limit is 300 MPa or more, the mechanical strength of the polyester film becomes sufficient, and it is preferable that the occurrence of problems such as elongation and displacement during the processing step can be suppressed. Considering the manufacturing point of view, the upper limit is considered to be 1000 MPa.
[0027] The sum of the tensile modulus Ea in the MD direction and the tensile modulus Eb in the TD direction of the film is preferably 5.0 GPa or more. More preferably, it is 10.0 GPa or more, and even more preferably, it is 14 GPa or more. The preferred lower limit of the sum of the tensile modulus is 5.0 GPa, more preferably, it is 7.0 GPa, even more preferably, it is 8.0 GPa, and even more preferably, it is 10.0 GPa. The preferred upper limit of the sum of the tensile modulus is 20.0 GPa, more preferably, it is 15 GPa, and even more preferably, it is 10.0 GPa. When the preferred upper limit of the sum of the tensile modulus is 10.0 GPa or more, the rigidity of the film becomes sufficient, and it is preferable that the film is prevented from being wrinkled or warped. In consideration of the manufacturing point of view, the upper limit is considered to be 20 GPa.
[0028] The sum of the bending stiffness Fa in the MD direction and the bending stiffness Fb in the TD direction, calculated for a film thickness of 15 μm, is 0.05 gf cm 2 / cm or more, and more preferably 0.06 gf cm 2 / cm or more, and more preferably 0.07 gf cm 2 / cm or more. The preferable lower limit of the sum of the bending stiffnesses is 0.05 gf cm 2 / cm, and a more preferable lower limit is 0.06 gf cm 2 / cm, and a more preferable lower limit is 0.07 gf cm 2 / cm. The preferred upper limit of the sum of the bending stiffnesses is 0.10 gf cm 2 / cm, and a more preferable upper limit is 0.09 gf cm 2 / cm, and a more preferable upper limit is 0.08 gf cm 2 / cm. The preferred upper limit of the bending stiffness is 0.07 gf cm 2 A film with a hardness of 0.10 gf cm or more is preferable because it provides sufficient stiffness and prevents wrinkles and warping when the film is made thinner than the conventional thickness. 2 / cm.
[0029] The heat shrinkage rate when the film is heated at 150°C for 30 minutes is preferably 20% or less in both the MD and TD directions, more preferably 10% or less, and even more preferably 7% or less. If the heat shrinkage rate is large, the film may deform under high heat during post-processing, resulting in poor appearance. It is preferable that the heat shrinkage rate is low, but from the viewpoint of production, 0.01% is considered to be the lower limit.
[0030] The film's longitudinal refractive index Nx and perpendicular refractive index Ny are preferably 1.60 or more, more preferably 1.65 or more, and even more preferably 1.70 or more. The higher the refractive index, the more the molecular chains are aligned in the stretching direction, the more sufficient the mechanical strength is, and the less likely the film is to elongate or slip during processing. In consideration of manufacturing, the upper limit is thought to be 1.75.
[0031] The long period of the film analyzed by the small angle X-ray scattering method is preferably 10 nm or more, more preferably 12 nm or more, and even more preferably 15 nm or more. The longer the long period, the more the molecular chains connecting the amorphous structure and the crystalline structure of the high-order structure are extended, the more sufficient the mechanical strength is, and the more preferable it is because it is possible to suppress the occurrence of problems such as elongation and displacement during the processing step. Considering the manufacturing point of view, the upper limit is considered to be 20 nm.
[0032] Regarding the crystals formed by the polymer molecules constituting the polyethylene terephthalate film, the crystal size of the film analyzed by small angle X-ray scattering is preferably 3 nm or more, more preferably 4 nm or more, and even more preferably 5 nm or more. The larger the crystal size, the larger the crystal structure in the higher-order structure, which suppresses relaxation of the higher-order structure when the film is heated, provides sufficient thermal dimensional stability, and suppresses deformation of the film under high heat during post-processing, which is preferable. From the viewpoint of manufacturing, the upper limit is considered to be 6 nm.
[0033] (Release layer) There are no particular limitations on the resin that constitutes the release layer, and examples of resins that can be used include silicone resins, fluororesins, alkyd resins, various waxes, and aliphatic olefins. Each resin can be used alone or in combination of two or more kinds.
[0034] As the release layer of the present invention, for example, a silicone resin is a resin having a silicone structure in the molecule, and examples thereof include cured silicone, silicone graft resin, and modified silicone resin such as alkyl modified, but from the viewpoint of migration, it is preferable to use a reactive cured silicone resin. As the reactive cured silicone resin, an addition reaction type, a condensation reaction type, an ultraviolet or electron beam cured type, etc. can be used. More preferably, a low-temperature curable addition reaction type that can be processed at low temperature, and an ultraviolet or electron beam cured type are preferable. By using these, the polyester film can be processed at low temperature during coating processing. Therefore, the polyester film is less thermally damaged during processing, and a polyester film with high flatness can be obtained, and defects such as pinholes can be reduced even when manufacturing thin sheets such as ceramic green sheets.
[0035] Silicone resins of the addition reaction system are, for example, polydimethylsiloxane with vinyl groups introduced at the end or side chains and hydrogensiloxane reacted with a platinum catalyst to harden them. In this case, it is more preferable to use a resin that can be hardened within 30 seconds at 120°C, as this allows processing at low temperatures. Examples of addition reaction silicone resins include low-temperature addition curing types (LTC1006L, LTC1056L, LTC300B, LTC303E, LTC310, LTC314, LTC350G, LTC450A, LTC371G, LTC750A, LTC755, LTC760A, etc.) and thermal UV curing types (LTC851, BY24-510, BY24-561, BY24-562, etc.) manufactured by Dow-Toray, and solvent addition + UV curing types (X62-5040, X62-5065, X62-5072T, KS5508, etc.) and dual cure curing types (X62-2835, X62-2834, X62-1980, etc.) manufactured by Shin-Etsu Chemical.
[0036] Condensation reaction silicone resins, for example, are produced by condensing polydimethylsiloxane having an OH group at its terminal with polydimethylsiloxane having an H group at its terminal in the presence of an organotin catalyst to form a three-dimensional crosslinked structure.
[0037] Examples of UV-curable silicone resins include, as the most basic type, those that utilize the same radical reaction as normal silicone rubber crosslinking, those that introduce unsaturated groups to cause photocuring, those that use UV to decompose onium salts to generate strong acids that cleave epoxy groups to cause crosslinking, and those that crosslink by addition reaction of thiols to vinyl siloxanes. Electron beams can also be used instead of the UV rays. Electron beams have stronger energy than UV rays, and it is possible to carry out a radical crosslinking reaction without using an initiator as in the case of UV curing. Examples of resins that can be used include UV-curable silicones manufactured by Shin-Etsu Chemical Co., Ltd. (X62-7028A / B, X62-7052, X62-7205, X62-7622, X62-7629, X62-7660, etc.), UV-curable silicones manufactured by Momentive Performance Materials, Inc. (TPR6502, TPR6501, TPR6500, UV9300, UV9315, XS56-A2982, UV9430, etc.), and UV-curable silicones manufactured by Arakawa Chemical Co., Ltd. (Silicolise UV POLY200, POLY215, POLY201, KF-UV265AM, etc.).
[0038] The above-mentioned UV-curable silicone resin may be an acrylate-modified or glycidoxy-modified polydimethylsiloxane, etc. Good release performance can also be achieved by mixing such modified polydimethylsiloxane with a multifunctional acrylate resin or epoxy resin, etc., and using the mixture in the presence of an initiator.
[0039] Other examples of resins that can be used include alkyd resins and acrylic resins having long-chain alkyl groups, such as stearyl-modified and lauryl-modified resins, and alkyd-based resins, acrylic-based resins, and olefin-based resins obtained by reactions such as methylated melamine. When forming sheets for use in electronic parts, etc., release agents that do not contain silicone are also preferred.
[0040] Examples of the amino alkyd resins and amino acrylic resins obtained by the reaction of methylated melamine include the Tesfine series manufactured by Showa Denko Materials Co., Ltd.
[0041] When the above resin is used in the release layer of the present invention, one type may be used, or two or more types may be mixed. When two or more types are mixed, two or more types of silicone-based resins may be used, and it is also preferable to mix a plurality of different resin types, such as a binder resin and a silicone-based resin.
[0042] In particular, when forming a thin film sheet such as a ceramic green sheet, it is preferable that the release layer does not deform when peeled off, so it is preferable that the release layer is crosslinked and cured. Therefore, it is also preferable that the release layer contains a binder component, a crosslinking agent, etc. in addition to the silicone-based release agent.
[0043] The binder component contained in the release layer of the present invention is preferably, for example, a component capable of crosslinking in order to increase the crosslinking density of the release layer and improve the durability and solvent resistance of the release layer. Therefore, the binder component is preferably formed by reacting a resin having a reactive functional group with a crosslinking agent. It is also preferable that either the reactive functional group or the crosslinking agent is self-crosslinked alone. However, in the present invention, the binder component does not exclude an embodiment in which only the resin having a reactive functional group or the crosslinking agent is used as the binder component.
[0044] Suitable examples of resins having reactive functional groups include polyester resins, polyacrylic resins, polyurethane resins, polyolefin resins, etc. These resins preferably have at least one reactive functional group selected from the group consisting of carboxyl groups, hydroxyl groups, epoxy groups, amino groups, etc.
[0045] It is also preferable that the release layer of the present invention contains a crosslinking agent. Examples of crosslinking agents are melamine-based, isocyanate-based, carbodiimide-based, oxazoline-based, and epoxy-based. The crosslinking agent may be used alone or in combination of two or more. Particularly preferable is a crosslinking agent that reacts with the reactive functional group introduced into the binder component.
[0046] The release layer of the present invention may contain particles having a particle size of 1 μm or less, but from the viewpoint of preventing the occurrence of pinholes, it is preferable that the layer does not substantially contain any particles that form protrusions.
[0047] In order to adjust the release force, the release layer of the present invention may contain additives such as a light release additive or a heavy release additive, or additives such as an adhesion improver and an antistatic agent. In order to improve the adhesion to the base layer, it is also preferable to perform a pretreatment such as an anchor coat, a corona treatment, a plasma treatment, or an atmospheric pressure plasma treatment on the surface of the polylactic acid film before providing the release coating layer.
[0048] In the present invention, the thickness of the release layer may be set according to the purpose of use, and is not particularly limited, but is preferably in the range of 0.005 to 2.0 μm after curing. When the thickness of the release layer is 0.005 μm or more, the peeling performance is maintained, which is preferable. In addition, when the thickness of the release layer is 2.0 μm or less, the curing time is not too long, and there is no risk of uneven thickness of the sheet due to a decrease in the flatness of the release film, which is preferable. In addition, since the curing time is not too long, there is no risk of the resin constituting the release layer agglomerating, and there is no risk of forming protrusions, which is preferable, and pinhole defects of the sheet are unlikely to occur.
[0049] The outer surface of the film on which the release layer is formed is preferably flat so as not to cause defects in the sheet to be coated and molded thereon. The outer surface of the film is the release layer surface of the entire coated film that is not in contact with the polyester film. The arithmetic mean roughness (Sa) of the release layer surface is preferably 10 nm or less and the maximum protrusion height (P) is preferably 200 nm or less. Furthermore, the arithmetic mean roughness of the release layer surface is more preferably 10 nm or less and the maximum protrusion height is 100 nm or less, and the arithmetic mean roughness of the release layer surface is still more preferably 10 nm or less and the maximum protrusion height is 30 nm or less. If the arithmetic mean roughness of the release layer surface is 10 nm or less and the maximum protrusion height is 200 nm or less, defects such as pinholes do not occur during sheet formation, and the yield is good, which is preferable. It can be said that the smaller the arithmetic mean roughness (Sa) of the release layer surface, the more preferable it is, but it may be 0.1 nm or more, or it may be 0.3 nm or more. It can be said that the smaller the maximum projection height (P) is, the more preferable it is, but it may be 1 nm or more, or 3 nm or more.
[0050] The lower limit of the surface free energy of the release layer provided in the release film of the present invention is 8 mJ / m 2 More preferably, it is 10 mJ / m or more. 2 More than 12 mJ / m 2 More preferably, 8 mJ / m 2 If the thickness is more than this, then repelling or the like is unlikely to occur when the sheet dissolving solution is applied, which is preferable.
[0051] The upper limit of the surface free energy of the release layer provided on the release film of the present invention is 45 mJ / m 2 It is preferably less than 40 mJ / m 2 Less than or equal to 35 mJ / m 2 More preferably, it is 45 mJ / m 2 It is preferable that the thickness is not more than this because the molded sheet has good releasability.
[0052] In the present invention, the method of forming the release layer is not particularly limited, and a method is used in which a coating liquid in which a release resin is dissolved or dispersed is spread on one side of the base layer by coating or the like, and the solvent is removed by drying, and then the coating is dried by heating, heat curing, or ultraviolet curing. At this time, the drying temperature during solvent drying and heat curing is preferably 180°C or less, more preferably 150°C or less, and most preferably 120°C or less. The heating time is preferably 30 seconds or less, more preferably 20 seconds or less. When the temperature is 180°C or less, the flatness of the film is maintained and there is little risk of causing unevenness in the thickness of the sheet, which is preferable. When the temperature is 120°C or less, the film can be processed without impairing the flatness, and there is a further reduced risk of causing unevenness in the thickness of the sheet, which is particularly preferable.
[0053] In the present invention, the surface tension of the coating liquid when applying the release layer is not particularly limited, but is preferably 30 mN / m or less. By setting the surface tension as described above, the wettability after application can be improved and the unevenness of the coating film surface after drying can be reduced.
[0054] In the present invention, the coating liquid used for coating the release layer is not particularly limited, but it is preferable to add a solvent having a boiling point of 90° C. or higher. By adding a solvent having a boiling point of 90° C. or higher, bumping during drying can be prevented, the coating film can be leveled, and the smoothness of the coating film surface after drying can be improved. The amount of the solvent added is preferably about 10 to 80% by mass based on the entire coating liquid.
[0055] Examples of the method for applying the coating liquid include roll coating methods such as gravure coating and reverse coating, bar coating using a wire bar, die coating, spray coating, and air knife coating.
[0056] (Ceramic green sheets and ceramic capacitors) Generally, a multilayer ceramic capacitor has a rectangular parallelepiped ceramic body. Inside the ceramic body, first internal electrodes and second internal electrodes are alternately provided along the thickness direction. The first internal electrodes are exposed on a first end face of the ceramic body. A first external electrode is provided on the first end face. The first internal electrode is electrically connected to the first external electrode at the first end face. The second internal electrode is exposed on a second end face of the ceramic body. A second external electrode is provided on the second end face. The second internal electrode is electrically connected to the second external electrode at the second end face.
[0057] The release film for producing ceramic green sheets of the present invention is used to produce such a multilayer ceramic capacitor. For example, it is produced as follows. First, the release film of the present invention is used as a carrier film, and a ceramic slurry for forming a ceramic body is applied and dried. A conductive layer for forming a first or second internal electrode is printed on the applied and dried ceramic green sheet. A mother laminate is obtained by appropriately stacking and pressing a ceramic green sheet, a ceramic green sheet on which a conductive layer for forming a first internal electrode is printed, and a ceramic green sheet on which a conductive layer for forming a second internal electrode is printed. The mother laminate is divided into a plurality of pieces to produce a raw ceramic body. The raw ceramic body is fired to obtain a ceramic body. Then, a first and second external electrodes are formed to complete a multilayer ceramic capacitor. EXAMPLES
[0058] Next, the effects of the present invention will be described using examples and comparative examples. First, the evaluation methods of the characteristic values used in the present invention will be described below.
[0059] (Evaluation method) Breaking strength The breaking strength and breaking elongation of the film were measured in accordance with JIS-C-2318. The film was cut into strips of 120 mm in length and 10 mm in width in the MD and TD directions with a single-edged razor. The strip samples were then measured at a test speed of 5 mm / min and a chuck distance of 100 mm using an autograph AG-IS-Loadcell.1KN manufactured by Shimadzu Corporation to obtain the breaking strength (MPa) in each direction from the load-strain curve.
[0060] Elasticity The tensile modulus of the film was measured in accordance with JIS-K-7161 and ISO527-1, 527-3. The film was cut into strips of 200 mm in length and 15 mm in width in the MD and TD directions, respectively, using a single-edged razor, and two parallel marks were made at 50 mm apart in the center of the test piece. The tensile modulus of each direction was calculated from the load-strain curve obtained from the strip samples at a test speed of 0.5 mm / min, chuck distance of 100 mm, and 0.1-0.3% with a mark distance of 50 mm, using an autograph AGS-IS-Loadcell.1KN manufactured by Shimadzu Corporation.
[0061] Bending stiffness (15μm equivalent) The bending stiffness of the film was measured by automatically measuring the bending moment (rigidity) while applying a constant curvature (maximum curvature K = ±2.5 cm-1) according to the pure bending theory. The film was cut to a length of 100 mm in the stretching direction and 150 mm in the perpendicular direction. Then, automatic measurement was performed using a pure bending tester (KES-FB2A) manufactured by Kato Tech, and the bending stiffness was calculated. An outline of the pure bending tester is shown in Figure 1. The evaluation method in all directions was to determine the bending stiffness at 5° intervals according to the above measurement method, with the longitudinal direction set to 0° and the width direction set to 90°. The minimum value was Fa and the maximum value was Fb. Regarding the bending rigidity (converted to 15 μm), in the case of Example 4 having a thickness of 25 μm, for example, the bending rigidity (converted to 15 μm) is calculated by the formula 0.080×15 / 25=0.048.
[0062] 150℃ heat shrinkage rate Measurements were made in accordance with ISC-2318-1997-5.3.4 (dimensional change). In the direction to be measured (film width direction), the film was cut to a width of 10 mm and a length of 190 mm, and marks were made at 10 mm intervals, and the intervals between the marks (A) were measured. The film was then placed in an oven in an atmosphere of 150°C, and heat-treated at 150°C ± 3°C for 30 minutes under no load, after which the intervals between the marks (B) were measured. The thermal shrinkage at 150°C was calculated using the following formula. Heat shrinkage rate (%) = (AB) / A x 100
[0063] Refractive index Measurements were made in accordance with JIS-K-7142. The refractive index was measured using an Abbe refractometer with NaD line light. Methylene iodide was used as the mounting liquid, and the refractive index in the longitudinal direction (Nx), width direction (Ny), and thickness direction (Nz) were measured. Measurements were made at the center of the film width direction.
[0064] · Long period The long period was calculated from the diffraction intensity profile obtained by small-angle X-ray scattering measurement (SAXS) using an X-ray diffractometer. For X-ray evaluation, the film sample was cut to 8 mm in the width direction and 20 to 30 mm in the length direction (stretching direction), and several sheets were stacked to create a thickness of about 100 μm. Silver behenate was used as the standard calibration sample. Using the beamline (BL03XU) of the synchrotron radiation facility SPring8, X-rays were incident from the normal direction of the film surface with a wavelength of 1.2A and a camera length of 1700 mm, and measurements were made by small-angle X-ray scattering (SAXS). The long period (Lp) was calculated using the analysis software Fit2D and Fityk. The value of the profile I(q) (I: scattering intensity, q: scattering vector) was obtained from the diffraction image obtained by X-rays, and the long period (d) was calculated using the following formula.
[0065]
number
[0066] Crystal size Using the profile q2I(q) obtained by the small-angle X-ray diffraction described in (6) above, a Fourier transform is performed using the following formula to obtain the correlation function γ(r) (r = distance), and the crystal size (r c ) was calculated.
[0067]
number
[0068] Hereinafter, the crystal size (r c As shown in FIG. 2, the minimum value at r1, which is the smallest at r≧0, is calculated as γ(r1)=γ min1 (A). Next, for 0≦r≦r1, the r where the second derivative of y=γ(r) is 0 is the inflection point r2 of γ(r), and the tangent to γ(r) at r2 is y=ar+b (B). At the intersection of equations (A) and (B), r=r c is the desired crystal size, and γ min1 =ar c +b to r c =(γ min1 -b) / a, r c was calculated.
[0069] Example 1 The polyethylene terephthalate resin was dried under reduced pressure (1 Torr) at 135°C for 6 hours, and then fed to an extruder. The raw material fed to the extruder was melt-extruded from the T-die by setting the resin temperature of the melting section, kneading section, polymer tube, gear pump, polymer tube, and T-die of the extruder to 280°C, and then a sheet was produced using a cooling roll at 20°C. The sheet was stretched 3.0 times in the longitudinal direction with a heating roll at 105°C. Next, the film after the longitudinal stretching was introduced into a tenter, preheated at 90°C, and stretched 3.0 times in the width direction at 100°C to produce a film. The film was again introduced into the tenter, preheated at 120°C, and stretched 1.39 times in the width direction at 140°C to produce a film. The film was further introduced into the tenter again, preheated at 140°C, and stretched 1.39 times in the width direction at 170°C to produce a film. The film was then introduced into the tenter again, preheated at 170°C, and stretched 1.39 times in the width direction at 250°C to produce a film, which was then heat-treated at 100°C to obtain a biaxially stretched polyethylene terephthalate film with a thickness of 21 μm.
[0070] Example 2 The procedure up to the preparation of the sheet was the same as in Example 1. Then, the sheet was stretched 3.4 times in the longitudinal direction with a heated roll at 105 ° C. Then, the film after the longitudinal stretching was introduced into a tenter, preheated at 90 ° C., and stretched 1.68 times in the width direction at 100 ° C. to produce a film. The film was again introduced into the tenter, preheated at 120 ° C., and stretched 1.68 times at 140 ° C. to produce a film. The film was further introduced into the tenter again, preheated at 140 ° C., and stretched 1.68 times at 170 ° C. to produce a film. The film was further introduced into the tenter again, preheated at 170 ° C., stretched 1.58 times in the width direction at 250 ° C., and then heat-treated at 100 ° C. to obtain a biaxially stretched polyethylene terephthalate film having a thickness of 23 μm.
[0071] Example 3 The procedure up to the longitudinal direction was the same as in Example 1. Next, the film after the longitudinal stretching was introduced into a tenter, preheated at 90°C, and stretched 3.0 times in the width direction at 100°C to produce a film. The film was again introduced into the tenter, preheated at 120°C, and stretched 1.39 times at 140°C to produce a film. The film was further introduced into the tenter again, preheated at 140°C, and stretched 1.39 times at 170°C to produce a film. The film was further introduced into the tenter again, preheated at 170°C, stretched 1.47 times in the width direction at 250°C, and then heat-treated at 100°C to obtain a biaxially stretched polyethylene terephthalate film having a thickness of 21 μm.
[0072] Example 4 The process was the same as in Example 1 up to the preparation of the sheet. Next, a heating furnace capable of simultaneously stretching in the longitudinal and transverse directions was used. After stretching 4.0 times in the longitudinal direction and 2.0 times in the transverse direction at a temperature of 90°C in the first zone of the heating furnace, the film was introduced into the second zone of the heating furnace and stretched 1.5 times in the longitudinal direction at a temperature of 240°C. This resulted in a biaxially stretched polyethylene terephthalate film with a thickness of 25 μm.
[0073] Comparative Example 1 The procedure up to the longitudinal direction was the same as in Example 1. Next, the film after longitudinal stretching was introduced into a tenter, preheated at 90°C, stretched 4.0 times in the width direction at 100°C, and then heat-treated at 230°C to obtain a biaxially stretched polyethylene terephthalate film with a thickness of 25 μm.
[0074] Comparative Example 2 The procedure up to the longitudinal direction was the same as in Example 1. Next, the film after longitudinal stretching was introduced into a tenter, preheated at 90°C, stretched 6.0 times in the width direction at 100°C, and then heat-treated at 230°C to obtain a biaxially stretched polyethylene terephthalate film with a thickness of 27 μm.
[0075] [Table 1] [Table 2] [Industrial Applicability]
[0076] The polyethylene terephthalate film of the present invention has a high elastic modulus, and therefore can have a sufficient stiffness even when made thin, and can suppress scratches and deformation caused by foreign matter. The polyethylene terephthalate film of the present invention can be used in a wide range of industrial film fields, such as electronic components and panel protective films that require high quality, including those mentioned above.
Claims
1. The film is made of a composition containing polyethylene terephthalate resin, and the sum of the bending rigidity Fa in the MD direction and the bending rigidity Fb in the TD direction converted into a thickness of 15 μm is 0.05 gf cm 2 / cm or more.
2. 2. The polyethylene terephthalate film according to claim 1, wherein the crystal size of the crystals formed by the polymer molecules constituting the film is 3.0 nm or more as determined by small angle X-ray scattering.
3. 2. The polyethylene terephthalate film according to claim 1, wherein the direction in which the omnidirectional bending rigidity is maximum is the longitudinal direction.
4. A laminated film comprising the polyethylene terephthalate film according to claim 1 as a base layer, and a release layer laminated on at least one surface of the base layer.
5. 5. The laminated film according to claim 4, wherein the release layer is made of a composition containing a silicone release component and is used as a release film for producing a ceramic green sheet.
6. 5. The laminated film according to claim 4, wherein the release layer surface has a maximum protrusion height (P) of 200 nm or less and an arithmetic mean roughness (Sa) of 10 nm or less.
Citation Information
Patent Citations
Biaxially oriented polyester film
JP2002011786A
Cited By
Release film for mold molding and chip packaging method
JP2026133302A