Stickiness inhibitor for rubber for hot-air crosslinking, rubber composition for hot-air crosslinking, article, and stickiness inhibition method for rubber for hot-air crosslinking

A rubber composition using a fatty acid and fatty acid metal salt as a stickiness inhibitor enables crosslinking with organic peroxides in air, addressing stickiness and maintaining mechanical properties, thus reducing production costs and improving productivity.

JP2024155213AInactive Publication Date: 2024-10-31NOF CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023069701
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for crosslinking rubber using organic peroxides in the presence of air result in sticky surfaces, leading to lower productivity and higher equipment costs due to the need for oxygen-free environments, and existing additives like poly(alkylphenol) polysulfide and ascorbic acid derivatives have safety concerns or stability issues.

Method used

A rubber composition containing a fatty acid with 8 to 30 carbon atoms and a fatty acid metal salt with a divalent or trivalent metal is used as a stickiness inhibitor, allowing crosslinking with organic peroxides in the presence of air to suppress stickiness while maintaining mechanical properties.

Benefits of technology

The crosslinked rubber remains stable and non-sticky after wiping with alcohol, with excellent mechanical properties and reduced production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155213000001
    Figure 2024155213000001
  • Figure 2024155213000002
    Figure 2024155213000002
  • Figure 2024155213000003
    Figure 2024155213000003
Patent Text Reader

Abstract

To provide a stickiness inhibitor for rubber for hot-air crosslinking, where crosslinked rubber obtained by crosslinking using an organic peroxide in the presence of hot air has excellent mechanical properties and also can inhibit the stickiness of a surface of the crosslinked rubber.SOLUTION: The stickiness inhibitor for rubber for hot-air crosslinking is contained in a rubber composition containing rubber and an organic peroxide, and contains as an active ingredient a fatty acid metal salt of a C8-30 fatty acid and a di- or trivalent metal.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stickiness inhibitor for hot-air crosslinking rubber, a rubber composition for hot-air crosslinking, an article, and a method for suppressing stickiness of hot-air crosslinking rubber. [Background technology]

[0002] Organic peroxides are widely used as crosslinking agents for rubber, thermoplastic elastomers, and resins. Crosslinking with organic peroxides is characterized by higher mechanical properties and heat resistance of the crosslinked rubber compared to crosslinking with sulfur. This is thought to be because the carbon-carbon bond formed by organic peroxide crosslinking is more chemically stable than the carbon-sulfur bond formed by sulfur crosslinking.

[0003] The crosslinking reaction of rubber with organic peroxides occurs when oxygen radicals produced by the decomposition of the -O-O- bonds in the organic peroxides abstract hydrogen atoms from the rubber to generate polymer radicals, which then couple with each other.

[0004] When rubber is crosslinked with organic peroxides, the crosslinking reaction is inhibited on the rubber surface by oxygen molecules in the air. As a result, the crosslinking reaction does not proceed sufficiently on the rubber surface, resulting in a sticky rubber surface. For this reason, rubber is generally crosslinked with organic peroxides by heating in an oxygen-free steam tube, molten salt bath, steam autoclave, or exhaust-tight mold.

[0005] To carry out the crosslinking reaction by heating in an oxygen-free environment, the manufacturing equipment is more expensive than that required for sulfur crosslinking. In addition, preparation and maintenance are required before the crosslinking reaction can take place, which reduces productivity compared to sulfur crosslinking.

[0006] Due to these problems, there has been a demand for a method for producing crosslinked rubber using an organic peroxide that does not cause stickiness on the rubber surface even in the presence of air, as is the case with sulfur crosslinking.

[0007] As methods for solving this problem, a method using a sulfur-based compound (Patent Document 1) and a method using ascorbic acid (Patent Document 2) have been disclosed. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2020-105532 A [Patent Document 2] International Publication No. 2022 / 13114 Summary of the Invention [Problem to be solved by the invention]

[0009] Patent Document 1 discloses that the stickiness of the crosslinked rubber surface is improved by using an organic peroxide in combination with a poly(alkylphenol) polysulfide and a benzothiazyl sulfide. However, the mechanical properties of the crosslinked rubber are insufficient. In addition, poly(alkylphenol) polysulfide and benzothiazyl sulfide are highly dispersible powders, and measures to ensure work safety are required when handling them.

[0010] Patent Document 2 discloses that a crosslinked rubber having excellent mechanical properties and heat resistance can be obtained by using an organic peroxide in combination with an ascorbic acid derivative. However, ascorbic acid derivatives have a tendency to decompose over time. Therefore, there is a concern that the amount of ascorbic acid derivative in a rubber composition may vary depending on the storage temperature of the rubber composition, which may cause variations in the quality of the crosslinked rubber.

[0011] It is also known that the rubber surface can be temporarily reduced in stickiness by applying a lubricant such as silica, but in recent years, disinfection with alcohol or the like has become common, and the rubber may feel sticky after wiping. Therefore, there is a demand for rubber that has a surface that does not become sticky even after wiping with alcohol.

[0012] In view of the above circumstances, the present invention aims to provide a stickiness inhibitor for hot-air crosslinking rubber, which can suppress stickiness of the surface of the crosslinked rubber obtained by crosslinking with an organic peroxide in the presence of hot air while providing the crosslinked rubber with excellent mechanical properties. [Means for solving the problem]

[0013] That is, the present invention is as follows. (1) A stickiness inhibitor for rubber for hot air crosslinking, which is contained in a rubber composition containing rubber and an organic peroxide, and which contains as an active ingredient a fatty acid metal salt of a fatty acid having 8 to 30 carbon atoms and a divalent or trivalent metal. (2) A rubber composition for hot-air crosslinking, containing, per 100 parts by mass of rubber, 0.1 to 15 parts by mass of an organic peroxide and 0.001 to 9 parts by mass of the stickiness inhibitor for hot-air crosslinking rubber of (1) above. (3) An article formed from the hot-air crosslinking rubber composition (2) above. (4) A method for suppressing stickiness of rubber for hot-air crosslinking, comprising kneading the above-mentioned (1) stickiness suppressant for rubber for hot-air crosslinking and an organic peroxide into rubber and crosslinking the rubber at 120 to 250°C in the presence of air. Effect of the Invention

[0014] The stickiness inhibitor for hot-air crosslinking rubber of the present invention can suppress stickiness of the surface of the crosslinked rubber obtained by crosslinking with an organic peroxide in the presence of hot air while providing the crosslinked rubber with excellent mechanical properties, even after wiping with alcohol. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The stickiness inhibitor for hot-air crosslinking rubber of the present invention (hereinafter also referred to as stickiness inhibitor) is contained in a rubber composition containing rubber and an organic peroxide, and has as an active ingredient a fatty acid metal salt of a fatty acid having 8 to 30 carbon atoms and a divalent or trivalent metal.

[0016] <Rubber> Examples of the rubber include synthetic rubber, natural rubber, etc. Examples of the synthetic rubber include diene rubbers such as polybutadiene, polyisoprene, random copolymers and block copolymers of styrene-butadiene, hydrogenated block copolymers, acrylonitrile-butadiene copolymers, and butadiene-isoprene copolymers, random copolymers and block copolymers of ethylene-propylene, random copolymers and block copolymers of ethylene-butene, copolymers of ethylene and α-olefins, ethylene-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid and ethylene-methacrylic acid, and ethylene-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid esters and ethylene-methacrylic acid esters. Examples of the rubber include ester copolymers, ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid metal salt copolymers such as ethylene-acrylic acid-acrylic acid metal salt and ethylene-methacrylic acid-methacrylic acid metal salt, acrylic acid ester-butadiene copolymer, butyl acrylate-butadiene copolymer, and other acrylic elastic polymers, copolymers of ethylene and fatty acid vinyl such as ethylene-vinyl acetate, ethylene-propylene-diene copolymers, butylene-isoprene copolymers, chlorinated polyethylene, and modified products thereof, and from the viewpoint of the mechanical properties of the crosslinked rubber, ethylene-propylene-diene copolymers are preferred. The rubbers may be used alone or in combination of two or more kinds.

[0017] In the ethylene-propylene-diene copolymer, the diene monomer of the structural unit is not particularly limited, and examples thereof include cyclic dienes such as 5-ethylidene-2-norbornene, 5-propylidene-5-norbornene, dicyclopentadiene, 5-vinyl-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, and norbornadiene; and linear non-conjugated dienes such as 1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, 5-methyl-1,5-heptadiene, 6-methyl-1,5-heptadiene, and 6-methyl-1,7-octadiene. Particularly preferred is 5-ethylidene-2-norbornene.

[0018] Commercially available ethylene-propylene-diene copolymers include oil-extended grades containing plasticizers and non-oil-extended grades not containing plasticizers, and the type may be appropriately selected depending on the physical properties required for the rubber.

[0019] The ethylene content in the ethylene-propylene-diene copolymer is preferably 30% by mass to 80% by mass, more preferably 40% by mass to 70% by mass, and the diene content in the ethylene-propylene-diene copolymer is preferably 1% by mass to 15% by mass, more preferably 4% by mass to 9% by mass.

[0020] <Organic peroxide> The organic peroxide may be appropriately selected depending on the crosslinking form of the rubber. The organic peroxide may be used alone or in combination of two or more kinds.

[0021] Examples of the organic peroxides include hydroperoxides, dialkyl peroxides, peroxy esters, peroxy ketals, peroxy monocarbonates, diacyl peroxides, and peroxy dicarbonates. From the viewpoints of the thermal decomposition property of the organic peroxides, the storage stability of the rubber composition for hot air crosslinking containing the stickiness suppressant, and the mechanical properties of the crosslinked rubber, dialkyl peroxides and peroxy ketals are preferred, and dialkyl peroxides are more preferred.

[0022] Examples of the dialkyl peroxides include di(2-t-butylperoxyisopropyl)benzene, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne, t-butylcumyl peroxide, di-t-butyl peroxide, and di-t-hexyl peroxide.

[0023] Examples of the peroxyketals include 1,1-di(t-butylperoxy)cyclohexane, 1,1-di(t-hexylperoxy)cyclohexane, 2,2-di(t-butylperoxy)butane, n-butyl 4,4-di-(t-butylperoxy)valerate, and 2,2-di(4,4-di-(t-butylperoxy)cyclohexyl)propane.

[0024] Among these, di(2-t-butylperoxyisopropyl)benzene, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and 1,1-di(t-butylperoxy)cyclohexane are preferred, and di(2-t-butylperoxyisopropyl)benzene is particularly preferred, since their half-life temperatures are suitable for the crosslinking temperature of rubber.

[0025] <Fatty acid metal salts> The fatty acid metal salt is a fatty acid metal salt (metal soap) of a fatty acid having 8 to 30 carbon atoms and a divalent or trivalent metal.

[0026] From the viewpoint of water resistance, the fatty acid metal salt preferably has a carbon number of 8 to 30, more preferably a carbon number of 12 to 24, and even more preferably a carbon number of 14 to 20. In addition, the metal is not particularly limited as long as it satisfies the above valence, but is preferably divalent. Examples of the fatty acid metal salt include iron stearate, barium stearate, magnesium stearate, aluminum stearate, cobalt stearate, zinc stearate, calcium stearate, iron octylate, barium octylate, cobalt octylate, tin octylate, copper naphthenate, and manganese naphthenate. Among these, iron stearate, magnesium stearate, aluminum stearate, cobalt stearate, zinc stearate, calcium stearate, and iron octylate are preferred from the viewpoint of availability and physical properties of crosslinked rubber, magnesium stearate and cobalt stearate are more preferred, and magnesium stearate is particularly preferred. The fatty acid metal salt may be used alone or in combination of two or more kinds.

[0027] <Rubber composition for hot air crosslinking> The hot-air crosslinking rubber composition of the present invention contains 0.1 to 15 parts by mass of the organic peroxide and 0.001 to 10 parts by mass of the stickiness inhibitor for hot-air crosslinking rubber, relative to 100 parts by mass of the rubber.

[0028] The organic peroxide is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and particularly preferably 1 part by mass or more, per 100 parts by mass of the rubber, from the viewpoints of mechanical properties, heat resistance, and suppression of stickiness. Also, the organic peroxide is preferably 15 parts by mass or less, more preferably 8 parts by mass or less, and particularly preferably 5 parts by mass or less, per 100 parts by mass of the rubber, from the viewpoint of rubber elongation. When the rubber is a mixture, the total amount of the rubber components is taken as 100 parts by mass.

[0029] The amount of the anti-stickiness agent for the hot air crosslinking rubber is preferably 0.001 part by mass or more, and more preferably 0.005 part by mass or more, per 100 parts by mass of the rubber, from the viewpoint of the mechanical properties of the crosslinked rubber and anti-stickiness, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and particularly preferably 3 parts by mass or less, from the viewpoint of the mechanical properties of the crosslinked rubber.

[0030] The rubber composition for hot air crosslinking of the present invention may contain a crosslinking accelerator from the viewpoint of mechanical properties of the crosslinked rubber. The crosslinking accelerator is not particularly limited, and examples thereof include quinoid-based, resin-based, sulfur-based, triazine-based, polyol-based, polyamine-based, and maleimide-based crosslinking accelerators. The crosslinking accelerators may be used alone or in combination of two or more kinds.

[0031] Examples of the quinoid crosslinking accelerator include p-quinone dioxime, p,p'-dibenzoylquinone dioxime, tetrachloro-p-benzoquinone, poly-p-dinitrobenzene, and the like.

[0032] Examples of resin-based crosslinking accelerators include alkylphenol-formaldehyde resins, melamine-formaldehyde, dibenzothiazolyl disulfide condensates, triazine-formaldehyde condensates, octylphenol-formaldehyde resins, alkylphenol-sulfide resins, and hexamethoxymethyl-melamine resins.

[0033] Examples of sulfur-based crosslinking accelerators include 2,2'-dibenzothiazolyl disulfide, morpholine disulfide, alkylphenol disulfide, N,N'-dithio-bis(hexahydro-2H-azepinone-2), thiuram polysulfide, 2-(4'-morpholino-dithio)benzothiazole, amylphenol disulfide polymer, etc. Among these, amylphenol disulfide polymer and 2,2'-dibenzothiazolyl disulfide are preferred from the viewpoint of the physical properties of the crosslinked rubber.

[0034] Examples of polyamine crosslinking accelerators include hexamethylenediamine carbamate, hexamethylenediamine, triethylene tetramine, tetraethylene pentamine, 4,4'-methylenebis(cyclohexylamine) carbamate, N,N'-dicinnamylidene-1,6-hexanediamine, and ammonium benzoate.

[0035] Examples of the triazine-based crosslinking accelerator include 2,4,6-trimercapto-s-triazine and 2-di-n-butylamino-4,6-dimercapto-s-triazine.

[0036] Examples of the polyol crosslinking accelerator include bisphenol A, bisphenol AF, hydroquinone, and pentaerythritol.

[0037] An example of the maleimide-based crosslinking accelerator is N,N'-m-phenylenedimaleimide.

[0038] When the crosslinking accelerator is used, the amount of the crosslinking accelerator is preferably 0.01 part by mass or more, more preferably 0.05 part by mass or more, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, relative to 100 parts by mass of the rubber.

[0039] The rubber composition for hot-air crosslinking of the present invention may contain carbon black from the viewpoint of wear resistance. As the carbon black, commercially available carbon black may be used, and furnace black, which is generally used as a reinforcing agent, may be used. From the viewpoint of kneadability and moldability when highly filling bituminous fine powder, the carbon black preferably has a nitrogen adsorption specific surface area of ​​20 to 60 m. 2 / g and DBP oil absorption of 40 to 130 ml / 100 g, for example, FEF carbon black, SRF carbon black, etc., are used.

[0040] Commercially available carbon black products include trade names such as "Seest G-SO", "Seest SO", and "Seest S" (all manufactured by Tokai Carbon), "Asahi #55", "Asahi #51", and "Asahi #50" (all manufactured by Asahi Carbon).

[0041] When the carbon black is used, from the viewpoint of abrasion resistance, the amount of the carbon black is preferably 5 parts by mass or more, and more preferably 20 parts by mass or more, per 100 parts by mass of the rubber, and from the viewpoint of rubber elongation, the amount of the carbon black is preferably 150 parts by mass or less, and more preferably 120 parts by mass or less.

[0042] In addition, the rubber composition for hot air crosslinking of the present invention can be blended with other components, such as additives such as sulfur, crosslinking aids, fillers, antioxidants, anti-aging agents, ultraviolet absorbers, and flame retardants, plasticizers such as process oils, and lubricants such as stearic acid, which are generally used in processing rubbers, in any ratio. The other components may be used alone or in combination of two or more kinds.

[0043] When using the other components, they may be used within a range that does not impair the effects of the present invention. For example, the amount of the other components is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and is preferably 100 parts by mass or less, more preferably 70 parts by mass or less, per 100 parts by mass of the rubber.

[0044] <Method of manufacturing rubber composition for hot-air crosslinking> The method for producing the rubber composition for hot air crosslinking of the present invention can be obtained by mixing the above-mentioned components. The kneading method can be a known method generally used in processing rubbers, for example, a kneader such as an open roll, a Banbury mixer, a kneader, an extruder, or a transfer mixer can be used, and a kneader is preferred.

[0045] <Article and method for suppressing stickiness of hot air crosslinking rubber> The article of the present invention is a crosslinked rubber formed from the rubber composition for hot air crosslinking. Specifically, the rubber composition for hot air crosslinking is obtained by heating (crosslinking) the rubber composition for hot air crosslinking in the presence of air. The heating (crosslinking) method can be carried out by a known method, and may be appropriately determined depending on the type of organic peroxide used, the type of rubber to be crosslinked, the required physical properties, and the like. As an apparatus for performing heating (crosslinking), for example, a hot air oven or a hot air heating furnace having a preheating device such as a microwave (high frequency), far infrared, or electric heat (for example, MMV type hot air heating furnace manufactured by Micro Electronics Co., Ltd., a gear type aging tester manufactured by Toyo Seiki Co., Ltd., etc.) can be used. The heating temperature is preferably 120°C to 250°C, more preferably 130°C to 200°C. The heating time is preferably 3 minutes to 60 minutes, more preferably 5 minutes to 30 minutes. That is, in the present invention, the stickiness of the hot-air crosslinking rubber can be suppressed by kneading the stickiness inhibitor and the organic peroxide into the rubber and thermally crosslinking the rubber in the presence of air.

[0046] The articles can be used, for example, as cushioning and shock-absorbing rubber materials for outdoor use, such as window frame rubber, steam hoses, automobile parts, electric cables, rubber-coated fabrics, and vibration-proof rubber materials, but are not limited to the above uses. EXAMPLES

[0047] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples.

[0048] <Examples 1 to 30 and Comparative Examples 1 to 2> In each example and comparative example, the raw materials shown in Tables 1 to 3 were mixed (unit: parts by mass), uniformly kneaded with a kneader, and then stretched with a roller to form a plate. Then, the mixture was cooled to room temperature to produce a rubber composition (rubber sheet, 50 cm x 10 cm, thickness 2 cm). About 12 g of the composition was placed in a mold (10 cm x 5 cm), the mold was sandwiched between Teflon (registered trademark) plates, and pressure was applied with a hand press machine (30 MPa, 110 ° C) for 5 minutes to form a temporary molded shape of 10 cm x 5 cm. A hole was made in the top of this temporary molded rubber plate, which was hung by a hook in the center of an incubator and heated at 180 ° C for 15 minutes in the presence of air to obtain a crosslinked rubber.

[0049] The components shown in Tables 1 to 3 are as follows. EPDM: JSR Corporation, product name "JSREP21 (ethylene-propylene-diene copolymer) Carbon black: Tokai Carbon Co., Ltd., product name "Seat G-SO" Zinc oxide: Wako Pure Chemical Industries, Ltd. Stearic acid: Wako Pure Chemical Industries, Ltd. Process oil: Idemitsu Kosan Co., Ltd., product name "PW-90" Perbutyl P: di(2-t-butylperoxyisopropyl)benzene, manufactured by NOF Corporation Iron stearate: NOF Corporation, product name "Iron stearate" Barium stearate: NOF Corporation, product name "Barium Stearate" Magnesium stearate: manufactured by Tokyo Chemical Industry Co., Ltd. Aluminum monostearate: NOF Corporation, product name "Aluminum Stearate 300" Aluminum tristearate: NOF Corporation, product name "Aluminum Stearate 900" Cobalt stearate: manufactured by Tokyo Chemical Industry Co., Ltd. Zinc stearate: Wako Pure Chemical Industries, Ltd. Calcium stearate: manufactured by Tokyo Chemical Industry Co., Ltd. Magnesium octylate: product name "Nikka Octyx Magnesium 2%" manufactured by Nippon Chemical Industries Co., Ltd. Iron octylate: Manufactured by Nippon Chemical Industries Co., Ltd., product name "Nikka Octyx Iron 6%" Barium octylate: Manufactured by Toei Kako Co., Ltd., product name "Barium hexoate 15%" Zirconium octylate: Manufactured by Toei Kako Co., Ltd., product name "Zirconium hexoate 12%" Cobalt octylate: Kishida Chemical Co., Ltd. Stannous octoate: manufactured by Tokyo Chemical Industry Co., Ltd. Copper naphthenate: Toei Kako Co., Ltd., product name "Copper naphthenate 8%" Manganese naphthenate: manufactured by Tokyo Chemical Industry Co., Ltd. Suncellar AP: Amylphenol disulfide polymer, manufactured by Sanshin Chemical Industry Co., Ltd. MBTS: 2,2´-dibenzothiazolyl disulfide, manufactured by Tokyo Chemical Industry Co., Ltd.

[0050] The crosslinked rubber obtained above was subjected to the following evaluations, and the results are shown in Tables 1 to 3.

[0051] <Evaluation of mechanical properties> The crosslinked rubber was punched out with a No. 3 dumbbell, and a tensile test (tensile speed 500 mm / min) based on JIS K6251 was performed to measure the breaking stress and elongation. A breaking stress of less than 5 MPa was rated as ×, 5 MPa to less than 10 MPa as 〇, and 10 MPa or more as ◎. An elongation of less than 250% was rated as ×, 250% to less than 300% as 〇, and 300% or more as ◎.

[0052] <Evaluation of stickiness> The crosslinked rubber was cooled for 1 hour in a space at 23°C and 50% RH. To evaluate the durability of the stickiness suppression effect, the degree of stickiness was evaluated using a sample that had been wiped once with a Kimwipe (manufactured by Nippon Paper Crecia Co., Ltd.) moistened with ethanol. The evaluation was carried out by 10 people, who touched the entire surface with the pad of their index finger for 10 seconds and selected the stickiness according to the following 5-point scale. A total score of less than 25 points by the 10 people was evaluated as ×, 25 to 35 points as ◯, and 36 points or more as ◎. Evaluation points 5 points: No stickiness 4 points: Slightly sticky 3 points: Sticky 2 points: Sticky and slight finger marks remain on the surface 1 point: Sticky and leaves finger marks on the surface

[0053] [Table 1]

[0054] [Table 2]

[0055] [Table 3]

[0056] Comparative Example 1, which used a rubber composition for hot-air crosslinking that did not contain a stickiness inhibitor containing a fatty acid metal salt as an active ingredient, produced a crosslinked rubber with low elongation and strong stickiness. Examples 1 to 8, which used a rubber composition for hot-air crosslinking that contained a stickiness inhibitor containing a fatty acid metal salt as an active ingredient, produced crosslinked rubber with no stickiness on the surface and excellent mechanical properties (breaking stress, elongation).

[0057] In Comparative Example 2, in which a crosslinking accelerator was used in combination with a rubber composition for hot-air crosslinking that did not contain a stickiness inhibitor having a fatty acid metal salt as an active ingredient, a crosslinked rubber with low elongation and strong stickiness was obtained. In Examples 9 to 30, in which a crosslinking accelerator was used in combination with a rubber composition for hot-air crosslinking that contained a stickiness inhibitor having a fatty acid metal salt as an active ingredient, a crosslinked rubber with no stickiness on the surface and excellent mechanical properties (breaking stress, elongation) was obtained.

Claims

1. A rubber stickiness inhibitor for hot air crosslinking, which is contained in a rubber composition containing rubber and an organic peroxide, and which contains as an active ingredient a fatty acid metal salt of a fatty acid having 8 to 30 carbon atoms and a divalent or trivalent metal.

2. A rubber composition for hot-air crosslinking, comprising, per 100 parts by mass of rubber, 0.1 to 15 parts by mass of an organic peroxide, and 0.001 to 10 parts by mass of the stickiness inhibitor for hot-air crosslinking rubber according to claim 1.

3. An article formed from the hot-air crosslinkable rubber composition according to claim 2.

4. A method for suppressing stickiness of rubber for hot-air crosslinking, comprising kneading the anti-stickiness agent for rubber for hot-air crosslinking according to claim 1 and an organic peroxide into rubber and crosslinking the rubber at 120 to 250°C in the presence of air.

Citation Information

Patent Citations

  • Compositions and methods for crosslinking polymers in the presence of atmospheric oxygen

    JP2020105532A

  • Providing and displaying video data

    WO2022013114A1