Method for producing conductive polymer dispersion, and method for producing conductive laminate
By controlling the polymerization of thiophene-based conductive polymers through a catalyst addition method, the viscosity increase issue is addressed, resulting in stable and conductive polymer dispersions suitable for capacitors and laminates.
Patent Information
- Application Number
- JP2023070035
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-04-21
AI Technical Summary
Conductive polymer dispersions used in manufacturing capacitors and conductive laminates face issues with viscosity increase during storage, affecting their conductivity and production efficiency.
A method involving gradual addition of an iron compound catalyst to a mixed solution of thiophene compound, polyanion, and oxidizing agent to control the polymerization of thiophene-based conductive polymers, maintaining low viscosity and high conductivity.
The method produces a conductive polymer dispersion with suppressed viscosity increase during storage, enabling stable production of capacitors and conductive laminates with improved conductivity.
Smart Images

Figure 2024155372000003 
Figure 2024155372000001 
Figure 2024155372000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a conductive polymer dispersion containing a π-conjugated conductive polymer, and a method for producing a conductive laminate. [Background technology]
[0002] A π-conjugated conductive polymer, the main chain of which is composed of a π-conjugated system, forms a conductive complex by being doped with a polyanion having an anionic group, and becomes dispersible in water. A method for manufacturing a capacitor has been disclosed in which a paint made of a conductive polymer dispersion liquid containing a conductive complex is applied to a dielectric layer provided on the surface of an anode made of a valve metal, the paint is dried to form a solid electrolyte layer, and a cathode is placed opposite the solid electrolyte layer (for example, Patent Document 1). According to this disclosure, the performance of the capacitor is improved by adding a specific unsaturated aliphatic alcohol compound to the paint. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2022-071400 Summary of the Invention [Problem to be solved by the invention]
[0004] The conductive polymer dispersion liquid used in the manufacture of the capacitor is required to have low viscosity so that it can permeate the porous structure of the dielectric layer, and the solid electrolyte layer formed by drying the permeated conductive polymer dispersion is also required to have high conductivity. However, there is a problem in that the viscosity of conventional conductive polymer dispersions increases during storage. The increase in viscosity can be a problem not only in the production of capacitors, but also in the production of conductive laminates in which a conductive polymer dispersion is applied to a substrate to form a conductive layer.
[0005] The present invention provides a method for producing a conductive polymer dispersion in which the increase in viscosity during storage is reduced and which has good conductivity after drying and curing, and a method for producing a conductive laminate. [Means for solving the problem]
[0006] [1] A method for producing a conductive polymer dispersion, comprising: gradually dropping an aqueous catalyst solution containing an iron compound that catalyzes decomposition of the oxidant and generation of radicals into a mixed solution containing water, a thiophene-based compound, a polyanion, and an oxidant to obtain a reaction solution; and polymerizing the thiophene-based compound, to obtain a conductive polymer dispersion containing a polythiophene-based conductive polymer formed by polymerization of the thiophene-based compound and a conductive complex containing the polyanion, and water. [2] The method for producing a conductive polymer dispersion liquid according to [1], wherein a total concentration of the thiophene compound and the polyanion incorporated in the reaction liquid is 2.5 to 10.0 mass % based on the total mass of the reaction liquid. [3] The method for producing a conductive polymer dispersion liquid according to [1] or [2], wherein the concentration of the oxidizing agent mixed in the mixed liquid is 0.5 to 10.0 mass % based on the total mass of the mixed liquid. [4] The method for producing a conductive polymer dispersion according to any one of [1] to [3], wherein a concentration of the iron compound blended in the aqueous catalyst solution is 0.1 to 5.0 mass % based on a total mass of the aqueous catalyst solution. [5] The method for producing a conductive polymer dispersion according to any one of [1] to [4], wherein the oxidizing agent is peroxodisulfuric acid or a salt thereof. [6] The method for producing a conductive polymer dispersion according to any one of [1] to [5], wherein the iron compound is a ferric compound. [7] The method for producing a conductive polymer dispersion according to any one of [1] to [6], wherein the polythiophene-based conductive polymer is poly(3,4-ethylenedioxythiophene), or the polyanion is polystyrenesulfonic acid. [8] The method for producing a conductive polymer dispersion according to any one of [1] to [7], further comprising an ion exchange step of contacting the conductive polymer dispersion obtained in the polymerization step with at least one of a cation exchange resin and an anion exchange resin. [9] The method for producing a conductive polymer dispersion according to [8], further comprising adding a water-soluble organic solvent to the conductive polymer dispersion obtained in the ion exchange step.
[10] A method for producing a conductive laminate, comprising: obtaining the conductive polymer dispersion by the production method according to any one of [1] to [9]; and applying the conductive polymer dispersion to at least a partial surface of a substrate to form a conductive layer. Effect of the Invention
[0007] According to the method for producing a conductive polymer dispersion of the present invention, it is possible to obtain a conductive polymer dispersion in which an increase in viscosity during storage is suppressed. In addition, the conductive polymer dispersion has good electrical conductivity in a cured product thereof. According to the method for producing a conductive laminate of the present invention, a conductive polymer dispersion in which an increase in viscosity during storage is suppressed is used, so that a conductive laminate with stable quality can be easily produced.
[0008] This invention is believed to contribute to SDGs Goal 12, "Responsible Consumption and Production."
[0009] In this specification and claims, the lower limit and upper limit of a numerical range indicated with "to" are included in the numerical range. [Brief description of the drawings]
[0010] [Figure 1] 1 is a cross-sectional view showing an embodiment of a capacitor of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <Method for producing conductive polymer dispersion> A first aspect of the present invention is a method for producing a conductive polymer dispersion, comprising a polymerization step of gradually dropping an aqueous catalyst solution containing an iron compound that catalyzes the decomposition of the oxidant and the generation of radicals into a mixed solution containing water, a thiophene-based compound, a polyanion, and an oxidant to obtain a reaction solution, and polymerizing the thiophene-based compound. The production method of this aspect provides a conductive polymer dispersion containing a polythiophene-based conductive polymer formed by polymerization of the thiophene-based compound, a conductive complex containing the polyanion, and water.
[0012] A mixed solution (monomer aqueous solution) containing a thiophene-based compound as a monomer and a polyanion at an arbitrary content ratio is prepared, and an aqueous catalyst solution is gradually dropped therein. The catalyst concentration in the reaction solution gradually increases with the dropping. Since the catalyst concentration is low at the initial stage of the reaction, the thiophene-based compound is gently chemically polymerized to form a polythiophene-based conductive polymer. In the reaction solution, the polythiophene-based conductive polymer is naturally doped with a polyanion, and a conductive complex consisting of a polythiophene-based conductive polymer and a polyanion is formed. The water dispersibility and storage stability of the conductive complex formed by the manufacturing method of this embodiment are improved compared to the conventional method of dropping an oxidizing agent. Although the details of this mechanism are not yet clear, it is believed that the reason is that the polymerization reaction proceeds gently at the initial stage of the reaction.
[0013] The content ratio (by mass) of polythiophene-based conductive polymer:polyanion contained in the conductive complex formed in the reaction solution is approximately the same as the content ratio of the thiophene-based compound and the polyanion contained in the reaction solution immediately before the start of polymerization. In other words, the content ratio of the monomer and the polyanion blended in the reaction solution is reflected in the content ratio of the polythiophene-based conductive polymer and the polyanion in the conductive complex formed.
[0014] The content ratio of the thiophene compound to the polyanion in the reaction solution is preferably from (1.0:2.0) to (1.0:5.0) by mass, more preferably from (1.0:2.0) to (1.0:4.0), and even more preferably from (1.0:2.5) to (1.0:3.5). When in the above range, a conductive polymer dispersion having excellent water dispersibility can be formed.
[0015] The total concentration of the thiophene compound and the polyanion blended in the reaction solution is preferably 2.5 to 10.0% by mass, more preferably 2.5 to 8.0% by mass, and even more preferably 2.5 to 6.0% by mass, based on the total mass of the reaction solution. When the concentration is equal to or higher than the lower limit, the production efficiency of the conductive composite (the amount produced in one reaction) is increased. When the concentration is equal to or lower than the upper limit, a conductive polymer dispersion having better storage stability is obtained.
[0016] The concentration of the oxidizing agent preliminarily mixed in the mixed liquid before the aqueous catalyst solution is dropped into the mixed liquid is preferably 0.5 to 10.0 mass %, more preferably 1.0 to 6.0 mass %, and even more preferably 1.5 to 4.0 mass %, based on the total mass of the mixed liquid. If it is equal to or more than the lower limit, the polymerization reaction can be completed in a relatively short time. If it is equal to or less than the upper limit, a conductive polymer dispersion having better storage stability can be obtained. It is preferable that the mixed solution does not already contain an iron compound as a catalyst before the aqueous catalyst solution is dropped, so that the catalyst concentration in the reaction solution can be gradually increased by dropping the aqueous catalyst solution, and the polymerization reaction can proceed gently.
[0017] The concentration of the iron compound contained in the aqueous catalyst solution to be dropped into the mixed solution is preferably 0.1 to 5.0 mass %, more preferably 0.2 to 2.5 mass %, and even more preferably 0.3 to 1.5 mass %, based on the total mass of the aqueous catalyst solution. When the concentration is equal to or higher than the lower limit, the polymerization reaction can be completed in a relatively short time. When the concentration is equal to or lower than the upper limit, a conductive polymer dispersion having better storage stability can be obtained.
[0018] The type of the oxidizing agent is not particularly limited as long as it can chemically polymerize the thiophene compound and can generate radicals by decomposing it under the catalytic action of the iron compound. The oxidizing agent preferably has a peracid structure represented by "-SO2-OO-" in the molecule. Specifically, peroxodisulfuric acid or a salt thereof, or peroxomonosulfuric acid or a salt thereof is preferable. Here, the salt has a counter cation such as sodium or potassium. The type of the oxidizing agent blended in the mixed liquid may be one type, or two or more types.
[0019] The type of the iron compound is not particularly limited as long as it catalyzes the generation of radicals by decomposing the oxidizing agent. From the viewpoint of enhancing this catalytic action, the iron compound is preferably a ferric compound. Generally, iron in a ferric compound is trivalent (Fe 3+ Specifically, preferred iron compounds include iron(III) sulfate, iron(III) nitrate, iron(III) citrate, and ammonium iron citrate. The type of the oxidizing agent blended in the aqueous catalyst solution may be one type, or two or more types. The aqueous catalyst solution may contain an oxidizing agent. However, from the viewpoint of improving storage stability and reducing the initial viscosity (viscosity before storage), it is preferable that the aqueous catalyst solution does not contain an oxidizing agent.
[0020] The method of gradually dropping the aqueous catalyst solution into the mixed solution is not particularly limited, and may be, for example, a method using a metering pump. The time for dropping the aqueous catalyst solution into the mixed solution from the start of dropping to the end of dropping is, for example, preferably about 0.1 to 10 hours, more preferably 0.5 to 7.5 hours, and even more preferably 1.0 to 5.0 hours. If the time is equal to or more than the lower limit, the polymerization reaction in the reaction solution can proceed gently, and the storage stability of the obtained conductive polymer dispersion can be further improved. If the time is equal to or less than the upper limit, the production efficiency is improved.
[0021] The volume ratio V1 / V2 of the volume of the mixed solution V1 to the volume V2 of the aqueous catalyst solution (total volume to be dropped) is preferably 2.0 to 30.0, more preferably 2.5 to 20.0, even more preferably 3.0 to 15.0, and most preferably 4.0 to 10.0. Within the above range, a conductive polymer dispersion having a low initial viscosity and suppressing an increase in viscosity after storage, and having good conductivity for the conductive layer to be formed, is easily obtained. The volume of the reaction solution is the sum of V1 and V2.
[0022] After completion of the dropwise addition of the aqueous catalyst solution, it is preferable to complete the polymerization reaction while stirring the reaction solution. The temperature during stirring of the reaction solution is preferably 10 to 40°C, more preferably 10 to 30°C, and even more preferably 10 to 20°C. The stirring time of the reaction solution is preferably 1 to 20 hours, and more preferably 3 to 12 hours. When within the above range, the polymerization reaction continues gently, the initial viscosity is low, and an increase in viscosity after storage is suppressed, and a conductive polymer dispersion having good conductivity for the conductive layer to be formed is easily obtained.
[0023] (Thiophene compounds) The thiophene compound added to the mixture is a monomer that polymerizes to form a polythiophene conductive polymer, the main chain of which constitutes a π-conjugated system. Polythiophene-based conductive polymers include polythiophene, poly(3-methylthiophene), poly(3-ethylthiophene), poly(3-propylthiophene), poly(3-butylthiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3-bromothiophene), poly(3-chlorothiophene), and poly(3-iodothiophene). thiophene), poly(3-cyanothiophene), poly(3-phenylthiophene), poly(3,4-dimethylthiophene), poly(3,4-dibutylthiophene), poly(3-hydroxythiophene), poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), oxythiophene), poly(3-octadecyloxythiophene), poly(3,4-dihydroxythiophene), poly(3,4-dimethoxythiophene), poly(3,4-diethoxythiophene), poly(3,4-dipropoxythiophene), poly(3,4-dibutoxythiophene), poly(3,4-dihexyloxythiophene), poly(3,4-diheptyloxythiophene), poly(3,4-dioctyloxythiophene), poly(3,4-didecyloxythiophene), poly(3,4-di dodecyloxythiophene), poly(3,4-ethylenedioxythiophene), poly(3,4-propylenedioxythiophene), poly(3,4-butylenedioxythiophene), poly(3-methyl-4-methoxythiophene), poly(3-methyl-4-ethoxythiophene), poly(3-carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4-carboxyethylthiophene), and poly(3-methyl-4-carboxybutylthiophene). Among these polythiophene-based conductive polymers, poly(3,4-ethylenedioxythiophene) is particularly preferred because of its excellent conductivity, transparency, and heat resistance. The thiophene-based compound to be mixed in the mixed liquid may be one type or two or more types.
[0024] (Polyanion) The polyanion to be added to the mixed solution is a polymer having two or more monomer units each having an anionic group in the molecule. The anionic group of the polyanion functions as a dopant for the polythiophene-based conductive polymer, improving the conductivity of the polythiophene-based conductive polymer. The anion group of the polyanion is preferably a sulfo group or a carboxy group. Specific examples of such polyanions include polymers having a sulfo group, such as polystyrene sulfonic acid, polyvinyl sulfonic acid, polyallyl sulfonic acid, polyacrylic acid esters having a sulfo group, polymethacrylic acid esters having a sulfo group (for example, poly(4-sulfobutyl methacrylate, polysulfoethyl methacrylate, polymethacryloyloxybenzenesulfonic acid), poly(2-acrylamido-2-methylpropanesulfonic acid), and polyisoprene sulfonic acid; and polymers having a carboxy group, such as polyvinyl carboxylic acid, polystyrene carboxylic acid, polyallyl carboxylic acid, polyacrylic acid, polymethacrylic acid, poly(2-acrylamido-2-methylpropanecarboxylic acid), and polyisoprene carboxylic acid. The polyanion may be a homopolymer in which a single monomer is polymerized, or a copolymer in which two or more monomers are polymerized. Among these polyanions, polymers having a sulfo group are preferred, and polystyrene sulfonic acid is more preferred, since they can provide higher electrical conductivity. The polyanion to be blended in the mixed liquid may be one type or two or more types.
[0025] The weight average molecular weight Mw of the polyanion is preferably 20,000 or more and 1,000,000 or less, and more preferably 50,000 or more and 800,000 or less. When the weight average molecular weight Mw is within the above preferred range, the storage stability of the conductive polymer dispersion of this embodiment is further improved. The weight average molecular weight Mw is an average molecular weight based on mass measured by gel filtration chromatography and calculated as pullulan.
[0026] In the polyanion doped into the polythiophene conductive polymer, some of the anion groups are not doped into the polythiophene conductive polymer, and there are excess anion groups that are not involved in the doping. Since these excess anion groups are hydrophilic groups, the conductive complex has high water dispersibility and low organic solvent dispersibility. When the number of all anionic groups in the polyanion is taken as 100 mol %, the excess anionic groups are preferably from 30 mol % to 90 mol %, more preferably from 45 mol % to 75 mol %.
[0027] [Conductive composite] Since the polyanion is preliminarily mixed in the mixed solution, the polyanion naturally dopes the polythiophene-based conductive polymer formed by the polymerization reaction, forming a conductive complex having electrical conductivity.
[0028] The content of the polyanion in the conductive complex is preferably in the range of 1 part by mass to 1000 parts by mass, more preferably 10 parts by mass to 700 parts by mass, and even more preferably 100 parts by mass to 500 parts by mass, per 100 parts by mass of the polythiophene-based conductive polymer. If the content of the polyanion is equal to or greater than the lower limit, the doping effect on the polythiophene-based conductive polymer tends to be stronger, and the conductivity becomes higher. On the other hand, if the content of the polyanion is equal to or less than the upper limit, the relative proportion of the polythiophene-based conductive polymer can be increased, so that the conductivity can be ensured.
[0029] When the polymerization reaction in the reaction solution is completed by the above method, the reaction solution becomes the target conductive polymer dispersion solution. The content of the monomer in the reaction solution is measured by gas chromatography or the like, and it is preferable that the presence of the monomer is not substantially confirmed as a criterion for the completion of the polymerization reaction.
[0030] Since the conductive polymer dispersion (reaction liquid) after the polymerization reaction contains residual decomposition products of the added catalyst and oxidizing agent, it may be preferable to remove these before using the conductive polymer dispersion. Examples of the removal method include a method of contacting the conductive polymer dispersion with an ion exchange resin to adsorb the catalyst and oxidizing agent to the ion exchange resin, and a method of ultrafiltrating the conductive polymer dispersion to remove them together with replacement of the dispersion medium. Among these, the method of using an ion exchange resin is preferable because it is simple. It is preferable to use a cation exchange resin and an anion exchange resin in combination as the ion exchange resin.
[0031] The conductive polymer dispersion may be subjected to a dispersion treatment by a conventional method such as using a high-pressure homogenizer.
[0032] The content of the conductive complex relative to the total mass of the conductive polymer dispersion is preferably from 0.01 to 5.0 mass%, more preferably from 1.0 to 4.0 mass%, and even more preferably from 1.5 to 3.0 mass%. When the content is at least as large as the lower limit of the above range, the conductivity of the conductive layer formed by curing the conductive polymer dispersion can be further improved. When the content is equal to or less than the upper limit of the above range, the dispersibility of the conductive composite in the conductive polymer dispersion can be improved, and the storage stability can be further improved.
[0033] The viscosity of the conductive polymer dispersion at 23°C is preferably 90 mPa·s or less, more preferably 70 mPa·s or less, and even more preferably 50 mPa·s or less, when the concentration of the conductive complex relative to the total mass of the conductive polymer dispersion is adjusted to 1.8 mass%. The lower limit of the viscosity is not particularly limited, and a guideline is 1 mPa·s or more. When a viscosity in such a suitable range is used in the production of a capacitor, the production of a solid electrolyte becomes easy and the capacitor performance can be improved. In measuring the viscosity, the conductive polymer dispersion preferably contains only ion-exchanged water as a dispersion medium, and preferably does not contain any additives other than the conductive complex. The viscosity was measured at 23° C. using a tuning fork vibration viscometer in accordance with JIS Z8803:2011 (viscosity measurement method using a vibration viscometer).
[0034] In order to improve the wettability of the conductive polymer dispersion to the substrate, a water-soluble organic solvent may be added to the conductive polymer dispersion. The conductive polymer dispersion to which the water-soluble organic solvent has been added is sometimes called a coating composition (paint).
[0035] <Coating composition (paint)> The coating composition contains water, the conductive composite obtained by the production method of the first embodiment, and a water-soluble organic solvent. A mixture of water and a water-soluble organic solvent is sometimes called an aqueous dispersion medium.
[0036] A water-soluble organic solvent is an organic solvent that dissolves in an amount of 1 g or more in 100 g of water at 20°C. Examples of the water-soluble organic solvent include alcohol-based solvents, ether-based solvents, ketone-based solvents, nitrogen atom-containing solvents, and ester-based solvents. Examples of alcohol-based solvents include methanol, ethanol, 1-propanol, 2-propanol (isopropanol), 2-methyl-2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, allyl alcohol, ethylene glycol, propylene glycol, propylene glycol monomethyl ether, and ethylene glycol monomethyl ether. Examples of the ether solvent include diethyl ether, dimethyl ether, propylene glycol dialkyl ether, and diethylene glycol diethyl ether. Examples of the ketone solvent include diethyl ketone, methyl propyl ketone, methyl butyl ketone, methyl isopropyl ketone, methyl isobutyl ketone, methyl amyl ketone, diisopropyl ketone, methyl ethyl ketone, acetone, and diacetone alcohol. Examples of the nitrogen atom-containing solvent include N-methylpyrrolidone, dimethylacetamide, and dimethylformamide. The water-soluble organic solvent may be contained alone or in combination of two or more kinds. As the water-soluble organic solvent, an alcohol-based solvent or a ketone-based solvent is preferred, and an alcohol-based solvent is more preferred, since this improves the applicability of the coating composition to the substrate.
[0037] The content of the water-soluble organic solvent relative to the total mass of the aqueous dispersion medium is preferably 30 to 70 mass %, more preferably 40 to 60 mass % or more, and the content of water relative to the total mass of the aqueous dispersion medium is preferably 70 to 30 mass %, more preferably 60 to 40 mass % or less. When the content is within the above suitable range, it is possible to improve the wettability of the conductive composite to the substrate while suppressing deterioration over time of the dispersion stability of the conductive composite in the coating composition.
[0038] The content of the conductive complex relative to the total mass of the coating composition is, for example, preferably 0.1 to 2.5 mass%, more preferably 0.3 to 2.0 mass%, and even more preferably 0.5 to 1.5 mass%. Within the above range, it is possible to suppress the deterioration of the dispersion stability of the conductive complex in the coating composition over time, and it is possible to form a conductive layer or the like with good conductivity.
[0039] (Polyol Compound) The coating composition may further contain one or more polyol compounds. Here, the polyol compound refers to a compound having two or more hydroxyl groups. By containing the polyol compound, the conductivity of the conductive layer formed by curing the conductive polymer dispersion can be increased, and the equivalent series resistance in the solid electrolyte layer of the capacitor can be reduced.
[0040] Examples of the polyol compound include one or more selected from ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, glycerin, pentaerythritol, trimethylolpropane, and trimethylolethane.
[0041] The content of the polyol compound in the coating composition is, for example, preferably 100 parts by mass or more and 10,000 parts by mass or less, more preferably 200 parts by mass or more and 2,000 parts by mass or less, and even more preferably 300 parts by mass or more and 1,000 parts by mass or less, relative to 100 parts by mass of the conductive composite. When the content is within the above range, the above-mentioned effects can be more effectively obtained.
[0042] The content of the polyol compound relative to the total mass of the coating composition is, for example, preferably from 1 to 20 mass%, more preferably from 2 to 10 mass%, and further preferably from 3 to 8 mass%. When the content is within the above range, the coatability of the coating composition is improved, and the above-mentioned effects are more effectively obtained.
[0043] (Other additives) The coating composition and the conductive polymer dispersion may contain other known additives. Examples of the additives that can be used include surfactants, inorganic conductive agents, antifoaming agents, coupling agents, antioxidants, and ultraviolet absorbing agents. The surfactant may be a nonionic, anionic or cationic surfactant, with the nonionic surfactant being preferred from the standpoint of storage stability. A polymer surfactant such as polyvinylpyrrolidone may also be added. Examples of the inorganic conductive agent include metal ions, conductive carbon, etc. Metal ions can be generated by dissolving a metal salt in water. The antifoaming agent includes silicone resin, polydimethylsiloxane, silicone oil, and the like. The coupling agent may be a silane coupling agent having a vinyl group or an amino group. Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, cyanoacrylate-based ultraviolet absorbers, oxanilide-based ultraviolet absorbers, hindered amine-based ultraviolet absorbers, and benzoate-based ultraviolet absorbers. When the above-mentioned additives are contained, the content ratio is appropriately determined depending on the type of additive, but can be, for example, in the range of 0.001 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the conductive composite.
[0044] <Method for manufacturing conductive laminate> A second aspect of the present invention is a method for producing a conductive laminate, the method comprising the steps of obtaining a conductive polymer dispersion by the production method of the first aspect, and applying the conductive polymer dispersion to at least a partial surface of a substrate to form a conductive layer.
[0045] Examples of a method for applying (coating) the conductive polymer dispersion on an arbitrary surface of a substrate include a method using a coater such as a gravure coater, a roll coater, a curtain flow coater, a spin coater, a bar coater, a reverse coater, a kiss coater, a fountain coater, a rod coater, an air doctor coater, a knife coater, a blade coater, a cast coater, or a screen coater; a method using a sprayer such as an air spray, an airless spray, or a rotor dampening; and an immersion method such as dipping.
[0046] The amount of the conductive polymer dispersion applied to the substrate is not particularly limited, but may be, for example, 0.01 to 10.0 g / m as a non-volatile component. 2 The range is preferably:
[0047] The conductive layer can be formed by drying the coating film made of the conductive polymer dispersion applied onto the substrate to remove at least a portion of the dispersion medium and curing the coating film. Methods for drying the coating film include heat drying, vacuum drying, etc. Examples of heat drying that can be used include hot air heating and infrared heating. When applying heat drying, the heating temperature is appropriately set depending on the dispersion medium used, but is usually within the range of 50° C. to 200° C. Here, the heating temperature is the set temperature of the drying device. A suitable drying time within the above heating temperature range is preferably 0.5 minutes to 30 minutes, more preferably 1 minute to 15 minutes.
[0048] <Conductive laminate> The conductive laminate obtained by the production method of the second aspect comprises a substrate and a conductive layer made of a cured product of the conductive polymer dispersion of the first aspect, formed on at least a partial surface of the substrate.
[0049] [Conductive layer] The conductive layer may be formed over the entire surface of any surface of the substrate, or over a portion of the entire surface. In the conductive film, it is preferable that a conductive layer of substantially uniform thickness is formed over substantially the entire surface of one surface or the other surface of the film substrate. When a conductive layer is formed only over a portion of the surface of the substrate, the conductive layer may be, for example, a fine conductive pattern such as a circuit or an electrode, or the conductive layer may be provided on the same surface and the conductive layer may be not provided on the same surface and may be roughly divided.
[0050] The average thickness of the conductive layer is, for example, preferably 10 nm or more and 100 μm or less, more preferably 20 nm or more and 50 μm or less, and even more preferably 30 nm or more and 30 μm or less. When the average thickness of the conductive layer is equal to or greater than the lower limit, high conductivity can be exhibited, and when the average thickness is equal to or less than the upper limit, the adhesion of the conductive layer to the substrate is further improved.
[0051] [Base material] The substrate may be a substrate made of an insulating material or a substrate made of a conductive material. The shape of the substrate is not particularly limited, and examples thereof include a shape mainly having a flat surface, such as a film or a substrate. Examples of insulating materials include glass, synthetic resin, and ceramics. The conductive material may be a metal, a conductive metal oxide, carbon, or the like.
[0052] (Film substrate) When a film substrate is used as the substrate, the conductive laminate becomes a conductive film. The film substrate may be, for example, a plastic film made of a synthetic resin, such as ethylene-methyl methacrylate copolymer resin, ethylene-vinyl acetate copolymer resin, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinyl alcohol, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyacrylate, polycarbonate, polyvinylidene fluoride, polyarylate, styrene-based elastomer, polyester-based elastomer, polyethersulfone, polyetherimide, polyetheretherketone, polyphenylene sulfide, polyimide, cellulose triacetate, cellulose acetate propionate, etc. From the viewpoint of improving the adhesion between the film substrate and the conductive layer, the synthetic resin for the film substrate is preferably a polyester resin, and among these, polyethylene terephthalate is preferable.
[0053] The synthetic resin for the film substrate may be either amorphous or crystalline. The film substrate may be either unstretched or stretched. The film substrate may be subjected to a surface treatment such as a corona discharge treatment, a plasma treatment, or a flame treatment in order to further improve the adhesion of the conductive layer.
[0054] The average thickness of the film substrate is preferably 5 μm to 500 μm, more preferably 20 μm to 200 μm. If the average thickness of the film substrate is equal to or more than the lower limit, the film is less likely to break, and if the average thickness is equal to or less than the upper limit, the film can have sufficient flexibility. The average thickness of the film substrate is calculated by measuring the thickness at 10 randomly selected points and averaging the measured values.
[0055] (Glass substrate) Examples of the glass substrate include an alkali-free glass substrate, a soda-lime glass substrate, a borosilicate glass substrate, and a quartz glass substrate. If the substrate contains an alkali component, the conductivity of the conductive layer tends to decrease, so among the above glass substrates, an alkali-free glass is preferred. Here, the alkali-free glass refers to a glass composition in which the content of the alkali component is 0.1 mass% or less with respect to the total mass of the glass composition.
[0056] The average thickness of the glass substrate is preferably from 100 μm to 3000 μm, more preferably from 100 μm to 1000 μm. If the average thickness of the glass substrate is equal to or more than the lower limit, the substrate is less likely to break, and if the average thickness is equal to or less than the upper limit, the substrate can contribute to a thinner conductive laminate. The average thickness of the glass substrate is calculated by measuring the thickness at 10 randomly selected points and averaging the measured values.
[0057] <Capacitor manufacturing method> A third aspect of the present invention is a method for producing a capacitor, comprising the steps of obtaining a conductive polymer dispersion by the production method of the first aspect, and applying the conductive polymer dispersion to a surface of a dielectric layer formed on the surface of an anode made of a porous valve metal, and drying the applied conductive polymer dispersion to form a solid electrolyte layer.
[0058] The method for manufacturing a capacitor of this embodiment preferably includes a step of oxidizing the surface of an anode made of a porous valve metal to form a dielectric layer (dielectric forming step), a step of arranging a cathode in a position facing the dielectric layer (cathode forming step), and a step of forming a solid electrolyte layer on at least a part of the surface of the dielectric layer (film forming step). Each step will be described below with reference to FIG.
[0059] [Dielectric formation process] In this step, the surface of anode 11 made of a porous valve metal is oxidized to form dielectric layer 12. The method for forming dielectric layer 12 is not particularly limited, and examples thereof include a method in which the surface of anode 11 is anodized in an electrolyte for chemical conversion treatment, such as an aqueous solution of ammonium adipate, an aqueous solution of ammonium borate, or an aqueous solution of ammonium phosphate.
[0060] [Cathode formation process] In this step, the cathode 13 is disposed at a position facing the dielectric layer 12. The method for disposing the cathode 13 is not particularly limited, and examples thereof include a method of forming the cathode 13 using a conductive paste such as a carbon paste or a silver paste, and a method of disposing a metal foil such as an aluminum foil facing the dielectric layer 12.
[0061] [Film forming process] In this step, the conductive polymer dispersion liquid described above is applied to at least a portion of the surface of the dielectric layer 12, and then dried to form the solid electrolyte layer 14.
[0062] Examples of the conductive polymer dispersion coating method include immersion (dip coating), comma coating, reverse coating, lip coating, and microgravure coating. Of these, a method of immersing the anode 11 in the conductive polymer dispersion under reduced pressure is preferred. The immersion method allows the conductive polymer dispersion to be sufficiently applied even to the inside of the porous structure on the surface of the dielectric layer 12. After immersion, the anode is removed and subjected to the next drying process.
[0063] Examples of the drying method include room temperature drying, hot air drying, far infrared drying, etc. Among these, hot air drying is preferred. The drying temperature is, for example, preferably 100 to 180° C., and more preferably 120 to 150° C. The drying time is, for example, preferably 0.2 to 1 hour. After drying, the capacitor can be assembled in the usual manner.
[0064] <Capacitor> A fourth aspect of the present invention comprises an anode made of a porous body of a valve metal, a dielectric layer made of an oxide of the valve metal, a cathode made of a conductive material provided on the side of the dielectric layer opposite the anode, and a solid electrolyte layer formed between the dielectric layer and the cathode, wherein the solid electrolyte layer contains a cured product of the conductive polymer dispersion obtained by the manufacturing method of the first aspect. The capacitor of the fourth embodiment can be manufactured by the manufacturing method of the third embodiment.
[0065] An example of an embodiment of the fourth aspect will be described with reference to Fig. 1. A capacitor 10 shown in Fig. 1 includes an anode 11 made of a porous body of a valve metal, a dielectric layer 12 made of an oxide of the valve metal, a solid electrolyte layer 14 formed on the surface of the dielectric layer 12, and a cathode 13 provided on the outermost side. The cathode 13 is provided on the opposite side to the anode 11, with the dielectric layer 12 and the solid electrolyte layer 14 sandwiched therebetween.
[0066] Examples of valve metals constituting the anode 11 include aluminum, tantalum, niobium, titanium, hafnium, zirconium, zinc, tungsten, bismuth, and antimony. Among these, aluminum, tantalum, and niobium are preferable. Specific examples of the anode 11 include an aluminum foil that has been etched to increase its surface area and then oxidized, and a tantalum or niobium particle sintered body that has been oxidized and pelletized. Such a processed body is a porous body with irregularities on the surface.
[0067] The dielectric layer 12 in this embodiment is a layer formed by oxidizing the surface of the anode 11, for example, by anodizing the surface of the metallic anode 11 in an electrolyte such as an aqueous solution of ammonium adipate. Similar to the anode 11, the dielectric layer 12 also has projections and recesses.
[0068] The cathode 13 in this embodiment may be a conductive layer formed from a conductive paste or a metal layer made of a conductive material such as aluminum foil.
[0069] The solid electrolyte layer 14 in this embodiment is formed on the surface of the dielectric layer 12. The solid electrolyte layer 14 covers at least a portion of the surface of the dielectric layer 12, and may cover the entire surface of the dielectric layer 12. The thickness of the solid electrolyte layer 14 may be constant or may not be constant, and may be, for example, between 1 μm and 100 μm.
[0070] [Electrolyte] The capacitor of this embodiment may have an electrolyte that impregnates the solid electrolyte layer. Examples of the solvent constituting the electrolytic solution include alcohol-based solvents such as ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, and glycerin; lactone-based solvents such as γ-butyrolactone, γ-valerolactone, and δ-valerolactone; sulfur-based solvents such as sulfolane, dimethyl sulfoxide, and dimethyl sulfone; amide-based solvents such as N-methylformamide, N,N-dimethylformamide, N-methylacetamide, and N-methylpyrrolidinone; nitrile-based solvents such as acetonitrile and 3-methoxypropionitrile; and water. Examples of the electrolyte constituting the electrolytic solution include organic acids such as adipic acid, glutaric acid, succinic acid, benzoic acid, isophthalic acid, phthalic acid, terephthalic acid, maleic acid, toluic acid, enanthic acid, malonic acid, formic acid, decanedicarboxylic acids such as 1,6-decanedicarboxylic acid and 5,6-decanedicarboxylic acid, octanedicarboxylic acids such as 1,7-octanedicarboxylic acid, azelaic acid, and sebacic acid; or boric acid, a polyhydric alcohol complex compound of boric acid obtained from boric acid and a polyhydric alcohol; inorganic acids such as phosphoric acid, carbonic acid, and silicic acid as anion components, and primary amines (methylamine, ethylamine, propylamine, butylamine, ethylenediamine, etc.), secondary amines (dimethylamine, diethylamine, dipropylamine, methylethylamine, diphenylamine, etc.), tertiary amines (trimethylamine, triethylamine, tripropylamine, triphenylamine, 1,8-diazabicyclo(5,4,0)-undecene-7, etc.), tetraalkylammonium (tetramethylammonium, tetraethylammonium, tetrapropylammonium, tetrabutylammonium, methyltriethylammonium, dimethyldiethylammonium, etc.), etc., as a cationic component.
[0071] The capacitor of this embodiment is not limited to the above configuration, and a separator may be provided between the dielectric layer and the cathode. An example of a capacitor having a separator provided between the dielectric layer and the cathode is a wound capacitor. Examples of the separator include sheets (including nonwoven fabrics) made of cellulose, polyvinyl alcohol, polyester, polyethylene, polystyrene, polypropylene, polyimide, polyamide, polyvinylidene fluoride, etc., and nonwoven fabrics of glass fibers. The density of the separator is, for example, 0.1 g / cm 3 More than 1.0g / cm 3 The following are included: When a separator is provided, a method of forming a cathode by impregnating the separator with carbon paste or silver paste can also be applied. EXAMPLES
[0072] [Preparation of polyanions] As a raw material, an aqueous solution (concentration 30%) of poly(sodium 4-styrenesulfonate) having a weight average molecular weight of 200,000 manufactured by Sigma-Aldrich was used. First, ion-exchanged water was added to an aqueous solution of poly(sodium 4-styrenesulfonate) to adjust it to a uniform aqueous solution with a solid concentration of 15 wt%, and cation-exchange resin was added until the pH became less than 1. After that, the cation-exchange resin was filtered off using a stainless steel mesh filter, and the solid concentration was adjusted to 10 wt% with ion-exchanged water to obtain an aqueous solution of polystyrenesulfonic acid (PSS aqueous solution).
[0073] [Preparation of thiophene compounds] Commercially available 3,4-ethylenedioxythiophene (Tokyo Chemical Industry Co., Ltd.) was purchased and purified by vacuum distillation before use in the reaction.
[0074] [Example 1] 91g of PSS aqueous solution, 100g of ion-exchanged water, and 7.09g of sodium peroxodisulfate (manufactured by Junsei Chemical Co., Ltd.) were added to a 1000ml three-neck flask, and the mixture was bubbled with nitrogen at a flow rate of 1L / min for 10 minutes, stirred under a nitrogen atmosphere, and maintained at 25°C. 3.5g of 3,4-ethylenedioxythiophene purified by distillation was added to this solution, and the mixture was stirred for another hour. 49.6g of a 1wt% aqueous solution of iron (III) sulfate heptahydrate (ferric sulfate, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to this solution using a metering pump over a period of 2 hours. The mixture was then stirred for 3 hours at 25°C to cause a reaction, synthesizing PEDOT-PSS, a conductive polymer. In this reaction, the sum of the solid concentration of the thiophene compound and the polyanion was 5.0wt%. The ratio (V1 / V2) of the volume V1 of the mixed solution to the volume V2 of the aqueous catalyst solution was about 4. 100g of ion-exchanged water, 100g of cation-exchange resin (Duolite C255LFH, exchange capacity 2.0eq / L, manufactured by Sumika Chemtex Co., Ltd.), and 100g of anion-exchange resin (Duolite A368MS, exchange capacity 1.7eq / L, manufactured by Sumika Chemtex Co., Ltd.) were added to this reaction solution, and the mixture was stirred for 30 minutes. The ion-exchange resin was filtered out using a stainless steel mesh filter, and a dispersion treatment was carried out using a high-pressure wet-type atomizer to obtain a conductive polymer dispersion liquid with a solid concentration of 3.2wt%. Ion-exchanged water was added to this conductive polymer dispersion liquid to adjust the solid concentration to 1.8wt%.
[0075] [Example 2] 91g of PSS aqueous solution, 200g of ion-exchanged water, and 7.09g of sodium peroxodisulfate were added to a 1000ml three-neck flask, and the mixture was bubbled with nitrogen at a flow rate of 1L / min for 10 minutes, stirred under a nitrogen atmosphere, and maintained at 25°C. 3.5g of 3,4-ethylenedioxythiophene purified by distillation was added to this solution, and the mixture was stirred for another hour. 29.9g of a 1wt% aqueous solution of iron (III) nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to this solution using a metering pump over 15 minutes. The mixture was then stirred at 25°C for 3 hours to react, synthesizing PEDOT-PSS, a conductive polymer. In this reaction, the sum of the solid concentration of the thiophene compound and the polyanion was 3.8wt%. The ratio (V1 / V2) of the volume V1 of the mixed solution to the volume V2 of the aqueous catalyst solution was about 10. 100g of ion-exchanged water, 100g of cation-exchanged resin, and 100g of anion-exchanged resin were added to this reaction solution and stirred for 30 minutes. The ion-exchanged resin was filtered out using a stainless steel mesh filter, and a dispersion process was carried out using a high-pressure wet-type atomizer to obtain a conductive polymer dispersion with a solid concentration of 2.5wt%. Ion-exchanged water was added to this conductive polymer dispersion to adjust the solid concentration to 1.8wt%.
[0076] [Example 3] 91g of PSS aqueous solution, 300g of ion-exchanged water, and 7.09g of sodium peroxodisulfate were added to a 1000ml three-neck flask, and the mixture was stirred under an air atmosphere and kept at 15°C. 3.5g of 3,4-ethylenedioxythiophene purified by distillation was added to this solution, and the mixture was stirred for another hour. 60.8g of 0.5wt% aqueous solution of iron(III) citrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to this solution using a metering pump over 4 hours. The mixture was then stirred for 10 hours at 15°C to react, synthesizing PEDOT-PSS, a conductive polymer. In this reaction, the sum of the solid concentration of the thiophene compound and the polyanion was 2.7wt%. The ratio (V1 / V2) of the volume V1 of the mixture to the volume V2 of the aqueous catalyst solution was about 7. 100g of ion-exchanged water, 100g of cation-exchanged resin, and 100g of anion-exchanged resin were added to this reaction solution and stirred for 30 minutes. The ion-exchanged resin was filtered out using a stainless steel mesh filter, and a dispersion treatment was carried out using a high-pressure wet-type atomizer to obtain a conductive polymer dispersion with a solid concentration of 1.9wt%. Ion-exchanged water was added to this conductive polymer dispersion to adjust the solid concentration to 1.8wt%.
[0077] [Example 4] 91g of PSS aqueous solution, 45g of ion-exchanged water, and 7.09g of sodium peroxodisulfate were added to a 1000ml three-neck flask, and the mixture was bubbled with nitrogen at a flow rate of 1L / min for 10 minutes, stirred under a nitrogen atmosphere, and maintained at 25°C. 3.5g of 3,4-ethylenedioxythiophene purified by distillation was added to this solution, and the mixture was stirred for another hour. 32.9g of 1wt% aqueous solution of ammonium iron citrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to this solution using a metering pump over a period of 2 hours. The mixture was then stirred at 25°C for 3 hours to react, synthesizing PEDOT-PSS, a conductive polymer. In this reaction, the sum of the solid concentration of the thiophene compound and the polyanion was 7.0wt%. The ratio (V1 / V2) of the volume V1 of the mixed solution to the volume V2 of the aqueous catalyst solution was about 5. 200g of ion-exchanged water, 100g of cation-exchanged resin, and 100g of anion-exchanged resin were added to this reaction solution and stirred for 30 minutes. The ion-exchanged resin was filtered out using a stainless steel mesh filter, and a dispersion treatment was carried out using a high-pressure wet-type atomizer to obtain a conductive polymer dispersion with a solid concentration of 2.9wt%. Ion-exchanged water was added to this conductive polymer dispersion to adjust the solid concentration to 1.8wt%.
[0078] [Example 5] 91g of PSS aqueous solution, 550g of ion-exchanged water, and 3.55g of sodium peroxodisulfate were added to a 1000ml three-neck flask, and the mixture was bubbled with nitrogen at a flow rate of 1L / min for 10 minutes, stirred under a nitrogen atmosphere, and maintained at 25°C. 3.5g of 3,4-ethylenedioxythiophene purified by distillation was added to this solution, and the mixture was stirred for another hour. 29.9g of a 1wt% aqueous solution of iron (III) nitrate nonahydrate was added to this solution using a metering pump over a period of 2 hours. The mixture was then stirred at 25°C for 6 hours to react, synthesizing PEDOT-PSS, a conductive polymer. In this reaction, the sum of the solid concentration of the thiophene compound and the polyanion was 1.9wt%. The ratio (V1 / V2) of the volume V1 of the mixture to the volume V2 of the aqueous catalyst solution was about 22. 100g of cation exchange resin and 100g of anion exchange resin were added to this reaction solution and stirred for 30 minutes. The ion exchange resin was filtered off using a stainless steel mesh filter and dispersed using a high-pressure wet-type atomizer to obtain a conductive polymer dispersion with a solid concentration of 1.6wt%. This conductive polymer dispersion was concentrated under reduced pressure to adjust the solid concentration to 1.8wt%.
[0079] [Example 6] A 1000ml three-neck flask was charged with 91g of PSS aqueous solution, 100g of ion-exchanged water, and 3.55g of sodium peroxodisulfate, and the mixture was bubbled with nitrogen at a flow rate of 1L / min for 10 minutes, stirred under a nitrogen atmosphere, and maintained at 25°C. 3.5g of 3,4-ethylenedioxythiophene purified by distillation was added to this solution, and the mixture was stirred for another hour. Separately from this solution, an aqueous solution was prepared by stirring and dissolving 0.50g of ferric sulfate, iron(III) sulfate heptahydrate, and 3.55g of sodium peroxodisulfate in 85g of ion-exchanged water, and added to the above solution over a period of 2 hours using a metering pump. The mixture was then stirred at 25°C for 3 hours to react, synthesizing the conductive polymer PEDOT-PSS. In this reaction, the sum of the solid concentrations of the thiophene compound and polyanion was 4.5wt%. The ratio (V1 / V2) of the volume V1 of the mixed liquid to the volume V2 of the aqueous catalyst solution was about 2. 100g of cation exchange resin and 100g of anion exchange resin were added to this reaction solution and stirred for 30 minutes. The ion exchange resin was filtered off using a stainless steel mesh filter and dispersed using a high-pressure wet-type atomizer to obtain a conductive polymer dispersion with a solid concentration of 3.1wt%. This conductive polymer dispersion was concentrated under reduced pressure to adjust the solid concentration to 1.8wt%.
[0080] [Comparative Example 1] 91g of PSS aqueous solution, 100g of ion-exchanged water, and 0.5g of iron (III) sulfate heptahydrate were added to a 1000ml three-neck flask, and nitrogen was bubbled at a flow rate of 1L / min for 10 minutes, and the mixture was stirred under a nitrogen atmosphere and maintained at 25°C. 3.5g of 3,4-ethylenedioxythiophene that had been distilled and purified was added to this solution, and the mixture was stirred for another hour. 35.5g of a 20wt% aqueous solution of sodium peroxodisulfate was added to this solution using a metering pump over a period of 2 hours. After that, the mixture was stirred and reacted at 25°C, but the reaction solution gelled within 2 hours, and the conductive polymer PEDOT-PSS could not be obtained.
[0081] [Comparative Example 2] 91g of PSS aqueous solution, 450g of ion-exchanged water, and 0.30g of iron(III) nitrate nonahydrate were added to a 1000ml three-neck flask, and the mixture was bubbled with nitrogen at a flow rate of 1L / min for 10 minutes, stirred under a nitrogen atmosphere, and maintained at 25°C. 3.5g of 3,4-ethylenedioxythiophene purified by distillation was added to this solution and stirred for another hour. 70.9g of a 10wt% aqueous solution of sodium peroxodisulfate was added to this solution using a metering pump over a period of 2 hours. The mixture was then stirred at 25°C for 3 hours to react, synthesizing the conductive polymer PEDOT-PSS. In this reaction, the sum of the solid concentrations of the thiophene compound and polyanion was 2.0wt%. 100g of cation exchange resin and 100g of anion exchange resin were added to this reaction solution and stirred for 30 minutes. The ion exchange resin was filtered off using a stainless steel mesh filter and dispersed using a high-pressure wet-type atomizer to obtain a conductive polymer dispersion with a solid concentration of 1.7wt%. This conductive polymer dispersion was concentrated under reduced pressure to adjust the solid concentration to 1.8wt%.
[0082] [Comparative Example 3] 91g of PSS aqueous solution, 1000g of ion-exchanged water, and 0.5g of iron(III) sulfate heptahydrate were added to a 2000ml three-neck flask, and nitrogen was bubbled at a flow rate of 1L / min for 20 minutes, and the mixture was stirred under a nitrogen atmosphere and kept at 25°C. 3.5g of 3,4-ethylenedioxythiophene purified by distillation was added to this solution and stirred for another hour. 70.9g of a 10wt% aqueous solution of sodium peroxodisulfate was added to this solution using a metering pump over a period of 2 hours. The mixture was then stirred at 25°C for 3 hours to react, synthesizing the conductive polymer PEDOT-PSS. In this reaction, the sum of the solid concentrations of the thiophene compound and polyanion was 1.1wt%. 100g of cation exchange resin and 100g of anion exchange resin were added to this reaction solution and stirred for 30 minutes. The ion exchange resin was filtered off using a stainless steel mesh filter and dispersed using a high-pressure wet-type atomizer to obtain a conductive polymer dispersion with a solid concentration of 0.9wt%. This conductive polymer dispersion was concentrated under reduced pressure to adjust the solid concentration to 1.8wt%.
[0083] [Table 1]
[0084] The conductive polymer dispersions obtained in Examples 1 to 6 and Comparative Examples 2 and 3 were evaluated by the following method.
[0085] <Evaluation of Viscosity> The viscosity of the conductive polymer dispersion having a solid content concentration of 1.8 wt % obtained in each example was measured at 23° C. using a vibration viscometer. The measurement results of the initial viscosity are shown in Table 2. The above viscosity is a value measured at 23° C. using a tuning fork vibration viscometer in accordance with JIS Z8803:2011 (viscosity measurement method using a vibration viscometer).
[0086] <Evaluation of storage stability> The conductive polymer dispersion obtained in each example was stored at 40°C for 10 days, after which the viscosity was measured. The measurement results of the viscosity after storage and the calculated increase rate (%) based on the ratio to the initial viscosity are shown in Table 2. Note that a lower increase rate indicates less viscosity change and better storage stability.
[0087] <Evaluation of electrical conductivity> To 50 g of the conductive polymer dispersion obtained in each example, 0.01 g of an acetylene-based surfactant (Dinol 604, manufactured by Nissin Chemical Industry Co., Ltd.), 45 g of methanol, and 5 g of ethylene glycol were added and thoroughly mixed to prepare a coating composition. This coating material was applied to a polyethylene terephthalate film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater with a wet film thickness of 8 μm, and a conductive film was obtained by heating and drying at a drying temperature of 100° C. for 1 minute. The surface resistance value of the obtained conductive film was measured using a resistivity meter (Loresta, manufactured by Nitto Seiko Analytech Co., Ltd.) under the condition of an applied voltage of 10 V. The results are shown in Table 2.
[0088] [Table 2]
[0089] From the above, it is clear that the production methods of Examples 1 to 6 according to the present invention can provide conductive polymer dispersions with high storage stability. [Explanation of symbols]
[0090] 10 Capacitor 11 Anode 12 Dielectric layer 13 Cathode 14 Solid electrolyte layer
Claims
1. A mixed solution containing water, a thiophene-based compound, a polyanion, and an oxidizing agent is added. a polymerization step of slowly dropping an aqueous catalyst solution containing an iron compound that catalyzes the decomposition of the oxidizing agent and the generation of radicals to obtain a reaction solution, and polymerizing the thiophene compound; obtaining a conductive polymer dispersion liquid containing a conductive complex including a polythiophene-based conductive polymer obtained by polymerization of the thiophene-based compound and the polyanion, and water; A method for producing a conductive polymer dispersion.
2. 2. The method for producing a conductive polymer dispersion according to claim 1, wherein a total concentration of the thiophene compound and the polyanion blended in the reaction solution is 2.5 to 10.0% by mass with respect to a total mass of the reaction solution.
3. 3. The method for producing a conductive polymer dispersion according to claim 2, wherein a concentration of the oxidizing agent mixed in the mixed liquid is 0.5 to 10.0 mass % with respect to a total mass of the mixed liquid.
4. 4. The method for producing a conductive polymer dispersion according to claim 3, wherein a concentration of the iron compound blended in the aqueous catalyst solution is 0.1 to 5.0 mass % with respect to a total mass of the aqueous catalyst solution.
5. The method for producing a conductive polymer dispersion according to claim 3 , wherein the oxidizing agent is peroxodisulfuric acid or a salt thereof.
6. The method for producing a conductive polymer dispersion according to claim 4 , wherein the iron compound is a ferric compound.
7. 3. The method for producing a conductive polymer dispersion according to claim 2, wherein the polythiophene-based conductive polymer is poly(3,4-ethylenedioxythiophene), or the polyanion is polystyrenesulfonic acid.
8. The method for producing a conductive polymer dispersion according to claim 7 , further comprising an ion exchange step of contacting the conductive polymer dispersion obtained in the polymerization step with at least one of a cation exchange resin and an anion exchange resin.
9. The method for producing a conductive polymer dispersion according to claim 8 , further comprising the step of adding a water-soluble organic solvent to the conductive polymer dispersion obtained in the ion exchange step.
10. 10. A method for producing a conductive laminate, comprising: obtaining the conductive polymer dispersion by the production method according to any one of claims 1 to 9; and applying the conductive polymer dispersion to at least a partial surface of a substrate to form a conductive layer.
Citation Information
Patent Citations
Compositions of conductive polymers and non-polymeric fluorinated organic acids
JP2007532758A
Method for producing conductive polymer solution
JP2008115215A
Method for producing polymer of aromatic compound and heterocyclic aromatic compound by using hypervalent iodine reagent
JP2009046653A
photodiode
JP2022090832A
Method for producing conductive polymer-containing solution and method for producing conductive laminate
JP2023023955A