Resin composition and molded body composed of the same

The resin composition, combining fully aromatic polyamide fibers with a copolyamide resin sizing agent, addresses the issues of heat resistance and mold deposits in injection molding, enhancing performance for various mechanical parts.

JP2024155442APending Publication Date: 2024-10-31TEIJIN LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023070160
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional resin materials, particularly those containing wholly aromatic polyamide fibers, lack sufficient heat resistance and result in significant mold deposits during injection molding.

Method used

A resin composition is developed by blending fully aromatic polyamide fibers containing a specific sizing agent with a thermoplastic resin, specifically a copolyamide resin, to enhance heat resistance and reduce mold deposits.

Benefits of technology

The resin composition exhibits excellent heat resistance and minimizes mold deposits during injection molding, suitable for applications in electrical, electronic, vehicle, aircraft, industrial machinery, and housing parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155442000001
    Figure 2024155442000001
  • Figure 2024155442000002
    Figure 2024155442000002
  • Figure 2024155442000003
    Figure 2024155442000003
Patent Text Reader

Abstract

To provide a resin composition which is excellent in heat resistance and gives a small amount of mold deposits during injection molding, and a molded article composed of the same.SOLUTION: A thermoplastic resin composition contains, with respect to 100 pts.wt. of (A) a thermoplastic resin (component A) having a melting point of 270°C or higher, 5 to 80 pts.wt. of (B) a wholly aromatic polyamide fiber (component B) containing a sizing agent composed of a copolymerized polyamide resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition which has excellent heat resistance and produces little mold deposit during injection molding, and to a molded article made from the same. [Background technology]

[0002] Polyarylene sulfide resins and semi-aromatic polyamide resins are engineering plastics with excellent chemical resistance, heat resistance, and mechanical properties, and are widely used as electrical and electronic parts, vehicle-related parts, aircraft parts, industrial machinery parts, office equipment parts, and housing equipment parts. In these related applications, the use of resins instead of conventional metals has been considered in order to reduce the weight of products, and in particular, in the use of resins for these mechanical parts, resin materials that are used to replace metals, particularly for gears and bearings, are required to have impact strength, ductility, and sliding properties such as low wear and low friction coefficient. However, although resin materials containing fully aromatic polyamide fibers have excellent long-term low wear properties, they do not have sufficient heat resistance compared to those containing glass fibers or carbon fibers.

[0003] As a means for solving this problem, Patent Documents 1 and 2 disclose a resin composition consisting of a semi-aromatic polyamide resin and fully aromatic polyamide fibers, and a resin composition consisting of a polyamide resin, fully aromatic polyamide fibers, and zinc oxide whiskers, respectively, for the purpose of improving sliding properties and mechanical strength. However, although they mention sliding properties and mechanical strength, they do not consider heat resistance and mold deposits. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-105362 A [Patent Document 2] JP 2019-151802 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a resin composition which is excellent in heat resistance and produces little mold deposit during injection molding, and a molded article using the same. [Means for solving the problem]

[0006] As a result of intensive research, the present inventors have found that the above object can be achieved by blending a specific thermoplastic resin with wholly aromatic polyamide fibers containing a specific sizing agent, and have arrived at the present invention. That is, the present invention is as follows.

[0007] 1. A thermoplastic resin composition characterized by containing 100 parts by weight of (A) a thermoplastic resin (component A) having a melting point of 270°C or higher, and (B) 5 to 80 parts by weight of wholly aromatic polyamide fibers (component B) containing a bundling agent made of a copolymer polyamide resin. 2. The thermoplastic resin composition according to item 1 above, wherein the copolymer polyamide resin contains at least one repeating unit selected from the group consisting of a repeating unit represented by the following formula (B-1), a repeating unit represented by the following formula (B-2), and a repeating unit represented by the following formula (B-3), and is a copolymer polyamide resin having a melting point of 180°C or lower and a number average molecular weight of 1,000 to 50,000. -[NH(CH2)mCO]- (B-1) (In the above formula, m is an integer of 6 to 20.) -[NH(CH2)6NHCO(CH2)4CO]- (B-2) -[NH(CH2)5CO]- (B-3)

[0008] 3. A thermoplastic resin composition according to item 1 or 2 above, wherein component A is at least one thermoplastic resin selected from the group consisting of polyarylene sulfide resins and polyamide resins. 4. The thermoplastic resin composition according to item 3 above, wherein the component A is at least one thermoplastic resin selected from the group consisting of a polyarylene sulfide resin and a semi-aromatic polyamide resin. 5. A molded article comprising the thermoplastic resin composition according to any one of items 1 to 4 above.

Advantages of the Invention

[0009] According to the present invention, it is possible to provide a resin composition having excellent heat resistance and less mold deposit during injection molding, and a molded body using the same. The molded body obtained from the resin composition of the present invention can be suitably used, for example, for electric and electronic parts, vehicle-related parts, aircraft parts, industrial machine parts, OA equipment parts, and housing equipment parts.

Modes for Carrying Out the Invention

[0010] Hereinafter, the details of the present invention will be described.

[0011] <Component A: Thermoplastic Resin> The thermoplastic resin of the present invention is a matrix resin constituting a molded article. The melting point of the thermoplastic resin is 270°C or higher, preferably 272°C or higher, more preferably 275°C or higher. The upper limit of the melting point is not particularly limited, but it is preferably 280°C or lower. The melting point is the melting peak temperature when measured by the DSC method specified in JIS K7121 using a differential scanning calorimeter (DSC).

[0012] Examples of the thermoplastic resin include polyarylene sulfide resin, polyamide resin, vinyl halide resin, polyester resin, and polyaryl ether ketone resin. Two or more of these can also be used. Among these thermoplastic resins, at least one thermoplastic resin selected from the group consisting of polyarylene sulfide resin and polyamide resin, which is excellent in the balance of mechanical properties and moldability, is more preferable. Since it has excellent heat resistance, at least one thermoplastic resin selected from the group consisting of polyarylene sulfide resin and semi-aromatic polyamide resin is even more preferable.

[0013] As the polyarylene sulfide resin, any resin belonging to the category called polyarylene sulfide resin may be used. Examples of the polyarylene sulfide resin include those composed of, as its structural units, for example, p-phenylene sulfide units, m-phenylene sulfide units, o-phenylene sulfide units, phenylene sulfide sulfone units, phenylene sulfide ketone units, phenylene sulfide ether units, diphenylene sulfide units, substituent-containing phenylene sulfide units, branched structure-containing phenylene sulfide units, etc. Among them, those containing 70 mol% or more, particularly 90 mol% or more of p-phenylene sulfide units are preferred, and further, poly(p-phenylene sulfide) is more preferred.

[0014] The polyarylene sulfide resin can be produced by any method, for example, the methods described in Japanese Patent Publication No. 45-3368, Japanese Patent Publication No. 52-12240, Japanese Unexamined Patent Application Publication No. 61-7332, International Publication No. WO2013 / 176343, Japanese Unexamined Patent Application Publication No. 2012-233210, and U.S. Patent No. 5,167,276.

[0015] The semi-aromatic polyamide resin is a polyamide resin having an aromatic ring skeleton and an aliphatic skeleton, and can be synthesized, for example, using an aromatic dicarboxylic acid and an aliphatic diamine as raw materials.

[0016] Examples of the semi-aromatic polyamide resin include polyamide 4T (T: terephthalic acid), polyamide 4I (I: isophthalic acid), polyamide 6T, polyamide 6I, polyamide 7T, polyamide 8T, polyamide 9T, polyamide 10T, polyamide 11T, polyamide 12T, etc.

[0017] <Component B: wholly aromatic polyamide fiber> The wholly aromatic polyamide fiber used as the B component of the present invention may be any fiber that belongs to the category of wholly aromatic polyaramid fiber. By using the wholly aromatic polyamide fiber, it is possible to ensure both the mechanical strength and toughness required for the sliding member and to exhibit excellent low wear properties. Examples of wholly aromatic aramid fibers include meta-aramid fibers and para-aramid fibers, and among them, para-aramid fibers are preferred.

[0018] The wholly aromatic polyamide resin constituting the fiber of the present invention is substantially obtained from one or more aromatic diamines and one or more aromatic dicarboxylic acid halides. However, a condensing agent such as triphenyl phosphite and pyridine may be added to the one or more aromatic diamines and one or more aromatic dicarboxylic acids. The wholly aromatic polyamide may be para-type or meta-type, but para-type is more preferable. Preferable aromatic diamines include p-phenylenediamine, benzidine, 4,4"-diamino-p-terphenyl, 2,7-diaminofluorene, 3,4-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 1,4-bis-(4-aminophenoxy)benzene, 4,4'-bis-(4-aminophenoxy)biphenyl, and 9,10-bis-(4-aminophenyl)anthracene.

[0019] As the aromatic dicarboxylic acid halide, acid chloride is particularly preferred, and examples thereof include terephthalic acid chloride, 2,6-naphthalenedicarboxylic acid chloride, 4,4'-diphenyldicarboxylic acid chloride, and those containing one or more non-reactive functional groups on the aromatic ring, such as lower alkyl groups, lower alkoxy groups, halogeno groups, nitro groups, etc. Furthermore, when an aromatic dicarboxylic acid is used, examples thereof include terephthalic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, and those containing one or more non-reactive functional groups on the aromatic ring, such as lower alkyl groups, lower alkoxy groups, halogeno groups, nitro groups, etc. Furthermore, the structure of the wholly aromatic polyamide resin preferred in the present invention is one whose main skeleton is represented by the following formula (1). -NH-Ar1-NH-CO-Ar2-CO- (1) (Here, Ar1 and Ar2 represent at least one type of aromatic residue selected from the group consisting of the following general formulas [I] to [IV]. Note that Ar1 and Ar2 may be the same or different. In addition, in these aromatic residues, some of the hydrogen atoms may be substituted with halogen atoms or lower alkyl groups.)

[0020] [ka] [ka] [ka] [ka]

[0021] Among them, when the sum of Ar1 and Ar2 is 100 mol%, the sum of general formula [I] and general formula [II], the sum of general formula [I] and general formula [III], the sum of general formula [I] and general formula [IV], or general formula [I] is preferably 80 mol% or more. More preferably, the sum of general formula [I] and general formula [II], or the sum of general formula [I] and general formula [III] is 80 mol% or more. Even more preferably, the sum of general formula [I] and general formula [II], or the sum of general formula [I] and general formula [III] is 80 mol% or more, and general formula [II] or general formula [III] is 1 to 20 mol%.

[0022] The aromatic polyamide dope to be the spinning solution may be one obtained by solution polymerization or one obtained by dissolving a wholly aromatic polyamide obtained separately in a solvent, but it is preferable to use one obtained by solution polymerization. In addition, a small amount of inorganic salt may be added as a dissolving agent to improve solubility. Examples of such inorganic salts include lithium chloride and calcium chloride.

[0023] As the polymerization solvent or re-dissolving solvent, a generally known aprotic organic polar solvent is used, examples of which include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, N,N-dimethylpropionamide, N,N-butylamide, N,N-dimethylisobutylamide, N-methylcaprolactam, N,N-dimethylmethoxyacetamide, N-acetylpyrrolidine, N-acetylpiperidine, N-methylpiperidone-2,N,N'-dimethylethyleneurea, N,N'-dimethylpropyleneurea, N,N,N',N'-tetramethylmalonamide, N-acetylpyrrolidone, N,N,N',N'-tetramethylurea, and dimethylsulfoxide. As the re-dissolving solvent, a strong acid such as concentrated sulfuric acid or methanesulfonic acid can be used.

[0024] Although the polymerization degree of the wholly aromatic polyamide resin is not particularly limited, if it dissolves in a solvent, it is preferable that the polymerization degree is large. When the wholly aromatic polyamide resin is solution-polymerized, the acid component and the diamine component are reacted in a substantially equimolar ratio, but either component can be used in excess to control the polymerization degree. In addition, a monofunctional acid component or an amine component can be used as an end-capping agent.

[0025] When forming the wholly aromatic polyamide resin into a fiber, a method of wet forming the wholly aromatic polyamide dope is usually used, and there is a method of directly discharging the dope into a coagulation bath or a method of discharging the dope into a coagulation bath through an air gap. A poor solvent for the wholly aromatic polyamide resin is used in the coagulation bath, and a good solvent is usually added to adjust the coagulation rate so that the solvent of the wholly aromatic polyamide dope does not escape too quickly and cause defects in the wholly aromatic polyamide fiber. In general, it is preferable to use water as the poor solvent and the solvent of the wholly aromatic polyamide dope as the good solvent. The ratio of the good solvent / poor solvent is preferably 15 / 85 to 40 / 60, depending on the solubility and coagulation property of the wholly aromatic polyamide.

[0026] The fiber length of the wholly aromatic polyamide fiber is preferably 0.1 mm to 12 mm, more preferably 0.5 mm to 4 mm. If it is less than 0.1 mm, the reinforcing effect may be insufficient and the improvement in impact resistance may be insufficient, while if it exceeds 12 mm, the fluidity of the composition may be poor and moldability may be poor.

[0027] In addition, the wholly aromatic polyamide fiber must contain a sizing agent made of a copolymer polyamide resin. If the sizing agent is not made of a copolymer polyamide resin, the heat resistance is poor and mold deposits are significantly generated during injection molding.

[0028] Among them, the copolymer polyamide resin preferably contains at least one repeating unit selected from the group consisting of a repeating unit represented by the following formula (B-1), a repeating unit represented by the following formula (B-2), and a repeating unit represented by the following formula (B-3), has a melting point of 180°C or less, and has a number average molecular weight of 1000 to 50000. The melting point is more preferably 170°C or less, and more preferably 160°C or less. The lower limit of the melting point is not particularly limited, but is preferably 50°C or more. The number average molecular weight is more preferably 3000 to 40000, and even more preferably 5000 to 30000. The melting point is the melting peak temperature measured by a differential scanning calorimeter (DSC) according to the DSC method specified in JIS K7121, and the number average molecular weight is a value calculated in terms of polystyrene by gel permeation chromatography (GPC). By using a copolymerized polyamide resin having such characteristics as a sizing agent, it may be possible to obtain a resin composition which has higher heat resistance and produces less mold deposits during injection molding.

[0029] -[NH(CH2)mCO]- (B-1) (In the above formula, m is an integer of 6 to 20.) -[NH(CH2)6NHCO(CH2)4CO]- (B-2) -[NH(CH2)5CO]- (B-3)

[0030] The content of component B is 5 to 80 parts by weight, preferably 6 to 60 parts by weight, and more preferably 7 to 40 parts by weight, relative to 100 parts by weight of component A. If the content of component B is less than 5 parts by weight, heat resistance is not sufficiently improved, whereas if it exceeds 80 parts by weight, problems such as strand breakage and surging occur during kneading and extrusion, resulting in reduced productivity or processability.

[0031] <Other ingredients> <Epoxy resin> The resin composition of the present invention may contain an epoxy resin. By containing an epoxy resin, low abrasion properties, ease of feeding pellets of the resin composition to a molding machine during injection molding, and mechanical properties may be improved.

[0032] The epoxy resin may be any compound having an epoxy group in its molecular structure, and is preferably an epoxy resin having two or more epoxy groups in one molecule. When an epoxy resin having two or more epoxy groups in one molecule is used, the tensile breaking strength may be further improved by the crosslinking reaction of the epoxy resin. Specific examples include bisphenol type epoxy, novolac type epoxy, cyclic aliphatic type epoxy, glycidyl ester type epoxy, glycidyl amine type epoxy, trisphenol methane type epoxy, dicyclopentadiene type epoxy, and biphenyl type epoxy. The epoxy resin may be used alone or in combination of two or more types of compounds. Examples of such epoxy resins are jER154, jER1001, jER1010, jER1256, and YX4000 from Mitsubishi Chemical Corporation, EHPE3150 from Daicel Corporation, and NC-3000, NC-7000, XD-1000, EPPN-502H, and EOCN-104S from Nippon Kayaku Co., Ltd., and are readily available on the market.

[0033] The epoxy equivalent of the epoxy resin is preferably 100 to 10,000 g / eq, more preferably 125 to 9,500 g / eq, and even more preferably 150 to 9,000 g / eq. If the epoxy equivalent is less than 100 g / eq, thickening during kneading and extrusion tends to occur, and if it exceeds 10,000 g / eq, the feedability of the resin composition to a molding machine during injection molding of pellets may not be improved. The epoxy equivalent is measured in accordance with JIS K 7236.

[0034] The content of the epoxy resin is preferably 0.5 to 8 parts by weight, more preferably 1 to 6 parts by weight, based on 100 parts by weight of component A. When the content of the epoxy resin is within the above range, low wear properties, ease of feeding the resin composition pellets to a molding machine during injection molding, and mechanical properties may be improved.

[0035] The resin composition of the present invention may contain other thermoplastic resins, and may contain various additives, such as antioxidants, impact modifiers, plasticizers, inorganic fillers, flame retardants, colorants, light stabilizers, heat stabilizers, antistatic agents, antiblocking agents, lubricants, dispersants, flow modifiers, and crystal nucleating agents, as necessary, within the scope of the invention.

[0036] <Method of producing resin composition> Any method can be used to produce the resin composition of the present invention. For example, each component and optionally other components can be premixed, then melt-kneaded, and pelletized. Premixing means can include a Nauta mixer, a V-type blender, a Henschel mixer, a mechanochemical device, an extrusion mixer, and the like. In premixing, granulation can be performed using an extrusion granulator or a briquetting machine, etc. After premixing, the mixture is melt-kneaded using a melt kneader such as a vented twin-screw extruder, and pelletized using a pelletizer or other device. Other examples of melt kneaders include a Banbury mixer, a kneading roll, a thermostatic stirring vessel, and the like, but a vented twin-screw extruder is preferred. Alternatively, each component and optionally other components can be independently supplied to a melt kneader such as a twin-screw extruder without premixing.

[0037] <About the molded body> The molded article made of the resin composition of the present invention can be obtained by molding the pellets produced as described above. It is preferably obtained by injection molding or extrusion molding. Injection molding can be performed not only by ordinary molding methods, but also by injection compression molding, injection press molding, gas-assisted injection molding, foam molding (including a method of injecting a supercritical fluid), insert molding, in-mold coating molding, heat-insulating mold molding, rapid heating and cooling mold molding, two-color molding, multi-color molding, sandwich molding, and ultra-high speed injection molding. In addition, molding can be performed by either the cold runner method or the hot runner method. In extrusion molding, a molded article can be obtained by extruding a round bar and then cutting it into a disk shape, or by extruding a thick sheet and then punching it into a predetermined shape. EXAMPLES

[0038] The present invention will be further described below with reference to examples. In the examples, parts are by weight and % is by weight unless otherwise specified. Evaluations were performed by the following methods.

[0039] [Evaluation of resin composition] (1) Deflection temperature under load The pellets obtained by the method described below were dried at 130°C for 7 hours, and then test pieces (dimensions: length 80 mm x width 10 mm x thickness 4 mm) were made using an injection molding machine (Toshiba Machine Co., Ltd., EC130SXII-4Y) and the deflection temperature under load at a bending stress of 1.80 MPa was measured using a method in accordance with ISO 75. The higher this value, the better the heat resistance of the resin composition.

[0040] (2) Mold deposit The pellets obtained by the following method were dried at 130 °C for 7 hours, and then molded products were continuously molded using an injection molding machine (PS40E5ASE manufactured by Nissei Plastic Industrial Co., Ltd.). After 200 shots, the degree of contamination of the mold gas vent part was visually confirmed. The molding temperature was 320 °C for Example 1, Comparative Examples 1 and 2, and 330 °C for Examples 2 to 4 and Comparative Examples 3 to 5. The mold temperature was 140 °C for Example 1, Comparative Examples 1 and 2, and 130 °C for Examples 2 to 4 and Comparative Examples 3 to 5. Note that Comparative Example 6 could not be evaluated because pellets could not be produced. The visual evaluation was "〇 (contaminated area less than 25%)", "△ (contaminated area 25% or more and less than 50%)", and "× (contaminated area 50% or more)".

[0041] [Examples 1 to 4, Comparative Examples 1 to 6] According to the addition amounts shown in Table 1, Component A and Component C-1 were supplied to the twin-screw extruder from the first supply port. Here, the first supply port refers to the supply port at the root. Component B was supplied from the second supply port using a side feeder. In some cases, a part of Component A was supplied from the second supply port using a side feeder for the purpose of assisting the supply of Component B to the twin-screw extruder. Extrusion was carried out using a vented twin-screw extruder with a diameter of 30 mmΦ (manufactured by Japan Steel Works, Ltd.: TEX30α-31.5BW-2V). The pellets were obtained by melt-kneading at a screw rotation speed of 200 rpm, a discharge rate of 20 kg / h, and a vent vacuum degree of 3 kPa. The extrusion temperature was 320 °C for Example 1, Comparative Examples 1 and 2, and 330 °C for Examples 2 to 4 and Comparative Examples 3 to 6.

[0042] Each component represented by the symbol notation in Table 1 is as follows. <Component A> A-1: Polyphenylene sulfide resin obtained by the following production method [Production method] A thermocouple capable of measuring the internal temperature of the reactor, a 5L reactor with a vacuum line that can be filled with nitrogen and evacuated, was charged with 5130 g of para-diiodobenzene (p-DIB), 450 g of sulfur, and 4 g of 1,3-diiodo-4-nitrobenzene mercaptobenzothiazole as a reaction initiator. After heating to 180 °C to completely melt and mix, starting from the initial reaction conditions of 220 °C and 350 Torr, the polymerization reaction was carried out while gradually increasing the temperature and decreasing the pressure in steps until the final reaction temperature reached 300 °C and the pressure was 1 Torr or less. When the polymerization reaction had proceeded 80% (the degree of progress of the polymerization reaction was determined by measuring the relative ratio of the current viscosity to the target viscosity [(current viscosity / target viscosity)×100(%)]. The current viscosity was measured with a viscometer by taking a sample during the polymerization process.), 60 g of 2,2'-dithiobisbenzothiazole was added as a polymerization terminator, and the reaction was allowed to proceed for 10 minutes under a nitrogen atmosphere. Then, the vacuum was gradually increased to 0.5 Torr or less until the target viscosity was reached, and then the reaction was terminated to synthesize a polyarylene sulfide resin having a phenyl group at the main chain end. The resin after the reaction was produced in pellet form using a small strand cutter machine. The weight average molecular weight was 72,000 and the melting point was 280 °C. A-2: Polyamide 10T (manufactured by Unitika Ltd.: Zeconet XP500 (product name), melting point 315 °C) A-3: Polyamide 9T (manufactured by Kuraray Co., Ltd.: Genesta N1000A (product name), melting point 306 °C)

[0043] <Component B> B-1: An all-aromatic polyamide fiber containing a sizing agent obtained by the following production method (manufactured by Teijin Ltd.: Technora (product name), major axis 12 μm, cut length 3 mm) [Production method] An autoclave of 70 L was charged with 11 kg of ε-caprolactam, 8 kg of a 50% aqueous solution of hexamethyleneammonium adipate, and 10 kg of aminododecanoic acid. After purging the inside of the polymerization tank with nitrogen, it was sealed and heated to 180 °C, and then while stirring, the pressure inside the polymerization tank was increased to 17.5 kgf / cm 2The temperature in the polymerization tank was raised to 240°C while adjusting the pressure. Two hours after the polymerization temperature reached 240°C, the pressure in the polymerization tank was released to normal pressure over about two hours. After releasing the pressure, polymerization was carried out under a nitrogen stream for one hour, and then reduced pressure polymerization was carried out for two hours. After nitrogen was introduced to return the pressure to normal pressure, the agitator was stopped, and the mixture was taken out as strands and pelletized, and the unreacted monomers were extracted and removed using boiling water, and the mixture was dried to obtain ternary copolymer polyamide particles. The copolymerization ratio at this time was nylon 6 / nylon 66 / nylon 12 (weight ratio; 45 / 15 / 40wt%). In addition, the particle size D50 was 0.4μm (D10 / D50 / D90=0.12μm / 0.4μm / 0.45μm, respectively), the melting point was 140°C, and the number average molecular weight was 21000.

[0044] 120g of the nylon 6 / 66 / 12 terpolymer polyamide resin thus obtained, 179.6g of water, and 0.4g of sodium hydroxide were added to an autoclave equipped with a stirrer, and the temperature was raised to 150°C while maintaining a rotation speed of 500 rpm, and the reaction was carried out for 30 minutes at 150°C. After the reaction was completed, the mixture was cooled to 50°C as it was, and the polyamide resin aqueous dispersion was taken out. The resin concentration of the obtained polyamide resin aqueous dispersion was 40 parts by weight per 100 parts by weight of the aqueous dispersion. Finally, 75g of the obtained polyamide resin aqueous dispersion was mixed with 12.0g of an aqueous ammonium salt solution (neutralization degree by ammonia 0.75) of an ethylene-acrylic acid copolymer (manufactured by Dow Chemical Company, registered trademark PRIMACOR 5980I, acrylic acid modification amount 20% by weight) separately adjusted to 25% by weight, to obtain an aqueous dispersion of a polyamide resin composition. This aqueous dispersion contains 10 parts by weight of ethylene-acrylic acid copolymer per 100 parts by weight of polyamide resin component. This was stirred so that the copolymer polyamide resin was 100 parts by weight per 4000 parts by weight of water to prepare an emulsion solution of a sizing agent. The water content of this ternary copolymer polyamide resin was removed from the aqueous dispersion using a hot air dryer at 120°C, and the glass transition temperature was measured and found to be 32°C. A wholly aromatic polyamide fiber was continuously immersed in this emulsion solution, and then passed through a dryer at a temperature of 150°C for 1 minute to obtain a wholly aromatic polyamide long fiber multifilament having a sizing agent attachment amount of 8%. B-2 (Comparative Example): Fully aromatic polyamide fiber (Teijin Ltd.: Technora T322EH (product name) major axis 12 μm, cut length 3 mm, polyester-based sizing agent) B-3 (Comparative Example): Fully aromatic polyamide fiber (Teijin Ltd.: Technora T322UR (product name) major axis 12 μm, cut length 3 mm, polyurethane-based sizing agent)

[0045] <Epoxy resin> C-1: Trisphenolmethane type epoxy (product name: EPPN-501H, manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent: 158-178g / eq)

[0046] [Table 1]

[0047] <Examples 1 to 4> Since the resin composition is within the scope of the present claims, the heat resistance is excellent and mold deposits during injection molding are small. <Comparative Examples 1 to 4> Because the sizing agent of component B was not a copolymer polyamide resin, the heat resistance was low and a large amount of mold deposits were generated during injection molding. <Comparative Example 5> Since the content of component B was below the lower limit, the heat resistance was low. <Comparative Example 6> Since the content of component B exceeded the upper limit, strand breakage and surging occurred, making it impossible to prepare pellets.

Claims

1. A thermoplastic resin composition comprising 100 parts by weight of (A) a thermoplastic resin (component A) having a melting point of 270°C or higher and 5 to 80 parts by weight of (B) wholly aromatic polyamide fibers (component B) containing a bundling agent made of a copolymer polyamide resin.

2. The thermoplastic resin composition according to claim 1, characterized in that the copolymer polyamide resin contains at least one repeating unit selected from the group consisting of a repeating unit represented by the following formula (B-1), a repeating unit represented by the following formula (B-2), and a repeating unit represented by the following formula (B-3), and has a melting point of 180°C or lower and a number average molecular weight of 1,000 to 50,000. -[NH(CH 2 )mCO]- (B-1) (In the above formula, m is an integer from 6 to 20.) -[NH(CH 2 ) 6 I'm sorry 2 ) 4 CO]- (B-2) -[NH(CH 2 ) 5 CO]- (B-3)

3. 3. The thermoplastic resin composition according to claim 1, wherein component A is at least one thermoplastic resin selected from the group consisting of polyarylene sulfide resins and polyamide resins.

4. 4. The thermoplastic resin composition according to claim 3, wherein component A is at least one thermoplastic resin selected from the group consisting of polyarylene sulfide resins and semi-aromatic polyamide resins.

5. A molded article made of the thermoplastic resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Bundled polyparaphenylene terephthalamide fiber and staple fiber chip

    JP1988196777A

  • Resin composition

    JP2020041019A

  • Fiber-reinforced semi-aromatic polyamide resin composition and its molded product

    JP2020200431A

  • Resin composition

    JP2019151802A

  • Thermoplastic resin composition and method for producing the same, and gear

    JP2020105362A