Disassembly method for dissimilar-metal joint
By restraining and heating dissimilar metal joints to induce stress, the method effectively separates and recycles metals, addressing the challenge of joint separation in existing technologies.
Patent Information
- Application Number
- JP2023070291
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-04-21
AI Technical Summary
Existing methods struggle to reliably separate dissimilar metal joints, particularly those formed by friction stirring, leading to challenges in recycling and resource utilization.
A method involving restraining the dissimilar metal joint, heating it to a specific temperature below the lower melting point of the metals involved, and then cooling it to induce stress and facilitate separation, utilizing different restraining methods based on the joint's joining method and area.
Enables reliable separation of dissimilar metal joints, reducing waste generation and enabling effective recycling of metal materials.
Smart Images

Figure 2024155514000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for disassembling a dissimilar metal joint. [Background technology]
[0002] There is a constant demand for improved fuel efficiency in transportation equipment, such as automobiles, and one of the measures to improve this is to reduce the weight of the vehicle. One way to reduce weight is to replace steel, which is currently the main material, with lightweight materials such as aluminum or aluminum alloys, magnesium or magnesium alloys, etc. However, replacing all components with these lightweight materials has issues such as high costs and insufficient strength. Therefore, a design method known as multi-material, which can simultaneously achieve strength and weight reduction by joining different metals together, has been attracting attention.
[0003] Nowadays, in view of resource depletion, recycling of various things is progressing, and recycling of metals, which are consumed in large quantities, has been practiced for some time. Even in the case of joints of dissimilar metals, if the joint parts can be easily separated, the disassembled parts can be recycled as their respective metallic materials.
[0004] Therefore, for example, Patent Document 1 proposes a recyclable welded joint in which the joining surfaces of dissimilar metal welded joints are heated to a temperature below the melting points of the metals to produce a brittle intermetallic compound layer of a predetermined thickness or more, allowing the joint to be easily disassembled.
[0005] Patent Document 2 also describes a method of forming a dissimilar metal reaction phase in the vicinity of the joint interface by heating in air a dissimilar metal joint produced by friction stirring. Patent Document 2 also proposes a method of easily fracturing the dissimilar metal joint near the joint interface by preferentially destroying the dissimilar metal reaction phase, and separating the dissimilar metal joint into components each made of the dissimilar metal materials. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2005-305542 A [Patent Document 2] JP 2007-54848 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, it is difficult to reliably separate a welded joint made of dissimilar metal materials even when using the methods described in the above Patent Documents 1 and 2. In addition, the method described in Patent Document 2 is limited to a welded body produced by friction stirring.
[0008] The present invention has been made in consideration of such problems, and aims to provide a method for disassembling dissimilar metal joints that can reliably separate dissimilar metal joints in a simple manner regardless of the joining method of the joint, thereby making effective use of resources and reducing waste generation. [Means for solving the problem]
[0009] The above object of the present invention is achieved by the following configuration (1) relating to a method for disassembling a dissimilar metal joint.
[0010] (1) A method for disassembling a dissimilar metal joint having a first member made of a metal, a second member made of a metal different from the first member, and a joint between the first member and the second member, comprising: A restraining step of restraining the dissimilar metal joint; A heating step of heating the dissimilar metal joint in a restrained state; A cooling process for cooling the dissimilar metal joint after the heating process, In the restraining step, based on a joining method and a joining area of the first member and the second member, First restraining method: a method of restraining the overlapping area of the first member and the second member by clamping them at one point; A second restraining method: a method of restraining the area where the first member and the second member are overlapped at two or more separated points; and a third restraining method: a method of restraining only one of the first member and the second member at two or more separate points; In the heating step, When the melting point of the lower melting point member of the first member and the second member is Tm (°C), the heating temperature is set to be equal to or higher than (Tm-150) (°C) and lower than Tm (°C), 13. A method for disassembling a dissimilar metal joint, comprising the steps of: selecting a heating time based on a joining method for the first member and the second member.
[0011] Further, preferred embodiments of the present invention relating to a method for disassembling a dissimilar metal joint relate to the following (2) to (5).
[0012] (2) The method for disassembling a dissimilar metal joint according to (1), characterized in that the combination of the first member and the second member is any one of a first member made of iron or an iron alloy and a second member made of aluminum or an aluminum alloy, a first member made of iron or an iron alloy and a second member made of titanium or a titanium alloy, a first member made of aluminum or an aluminum alloy and a second member made of titanium or a titanium alloy, a first member made of copper or a copper alloy and a second member made of titanium or a titanium alloy, and a first member made of copper or a copper alloy and a second member made of magnesium or a magnesium alloy.
[0013] (3) The dissimilar metal joint includes the first member, the second member, and an intermediate layer disposed between the first member and the second member, The method for disassembling a dissimilar metal joint according to (1) or (2), wherein the intermediate layer is made of at least one of a pure metal, an alloy, and a compound.
[0014] (4) The method for disassembling a dissimilar metal joint according to (3), characterized in that the intermediate layer is a cold spray coating provided on a surface of either the first member or the second member.
[0015] (5) The dissimilar metal joint is formed by joining the first member and the second member by a fusion welding method, The method for disassembling a dissimilar metal joint according to (1) or (2), characterized in that in the restraint step, one of the first restraint method and the second restraint method is selected. Effect of the Invention
[0016] According to the present invention, a method for disassembling dissimilar metal joints can be provided that can reliably separate dissimilar metal joints in a simple manner regardless of the joining method of the joint, thereby making effective use of resources and reducing waste generation. [Brief description of the drawings]
[0017] [Figure 1A] FIG. 1A is a diagram showing the process steps of a disassembly method for a dissimilar metal joint according to a first embodiment of the present invention, and is a schematic cross-sectional view showing a restraint step. [Figure 1B] FIG. 1B is a diagram showing the process steps of the disassembly method for a dissimilar metal joint according to the first embodiment of the present invention, and is a schematic cross-sectional view showing a heating step. [Figure 1C] FIG. 1C is a diagram showing the process steps of the disassembly method for a dissimilar metal joint according to the first embodiment of the present invention, and is a schematic cross-sectional view showing a cooling step. [Figure 1D] FIG. 1D is a diagram showing the process steps of a disassembly method for a dissimilar metal joint according to the first embodiment of the present invention, and is a schematic cross-sectional view showing a separation step. [Diagram 2] FIG. 2 is a cross-sectional view showing a dissimilar metal joint having an intermediate layer to which the method for disassembling a dissimilar metal joint according to the embodiment of the present invention is preferably applied. [Diagram 3]FIG. 3 is a schematic cross-sectional view showing a restraining step in a disassembly method for a dissimilar metal joint according to a second embodiment of the present invention. [Figure 4] FIG. 4 is a schematic cross-sectional view showing a restraining step in a disassembly method for a dissimilar metal joint according to a third embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present inventors have conducted extensive research into a method for easily disassembling a joint in which different metal materials are joined into each of the individual metal materials. As a result, the present inventors have focused on the fact that stress occurs at the joint between the different materials due to the difference in linear expansion coefficient of the metal materials, and have found that the joint can be peeled off by heating the joint while it is restrained. The present invention is based on these findings.
[0019] The disassembly method for dissimilar metal joints according to the present invention will be described in detail below with reference to the drawings. Note that the present invention is not limited to the embodiments described below, and can be modified as desired without departing from the gist of the present invention. In addition, in this specification, iron or iron alloys may be simply referred to as iron alloys (or steel), aluminum or aluminum alloys may be simply referred to as aluminum alloys, titanium or titanium alloys may be simply referred to as titanium alloys, copper or copper alloys may be simply referred to as copper alloys, and magnesium or magnesium alloys may be simply referred to as magnesium alloys.
[0020] [How to disassemble dissimilar metal joints] First Embodiment 1A to 1D are schematic cross-sectional views showing the process steps of a disassembly method for a dissimilar metal joint according to a first embodiment of the present invention.
[0021] (Restraint process: 1st restraint method) 1A, a dissimilar metal joint 10 is formed by joining a first member 11 made of steel and a second member 12 made of an aluminum alloy at a joint 15. In the first embodiment, the dissimilar metal joint 10 is restrained by a first restraining method in which a restraining device 20 is used to clamp an area R1 where the first member 11 and the second member 12 overlap at one location.
[0022] (Heating process) Next, as shown in FIG. 1B, the dissimilar metal joint 10 is heated for a predetermined time in a restrained state. At this time, when the melting point of the member on the low melting point side of the first member 11 and the second member 12 is Tm (°C), the heating temperature is set to (Tm-150) (°C) or more and less than Tm (°C). In this embodiment, the member on the low melting point side is the second member 12 made of an aluminum alloy, and since the melting point of the second member 12 is 650°C, the dissimilar metal joint 10 is heated at a temperature of 500°C or more and less than 650°C. By this heating, a brittle intermetallic compound 16 is formed in the joint 15 between the first member 11 and the second member 12, as shown in FIG. 1C.
[0023] (cooling process) 1C, the dissimilar metal joint 10 is cooled. In this cooling process, stress is applied to the joint between the first member 11 and the second member 12, and peeling 17 occurs in the joint between the first member 11 and the second member 12. The cooling temperature is not particularly limited, but it is preferable to cool to room temperature, for example.
[0024] (separation process) 1D, the restraint by the restraining device 20 is released, and the first member 11 and the second member 12 are separated. At the time when the restraint is released, the first member 11 and the second member 12 may be joined at a part of the joint 15, but since the intermetallic compound 16 has been formed, the first member 11 and the second member 12 can be easily separated.
[0025] According to the disassembly method for dissimilar metal joints according to the present embodiment, the first member 11 and the second member 12 are heated and then cooled while the overlapping area of the first member 11 and the second member 12 is clamped at one location. At this time, since the first member 11 is made of steel and the second member 12 is made of an aluminum alloy and the linear expansion coefficients of the two members are different from each other, a strain force is applied to the joint, particularly during cooling, and peeling 17 can occur. As a result, the separated first member 11 and second member 12 can be reused as their respective metal materials, and the generation of waste can be reduced.
[0026] The method of joining the first member 11 and the second member 12 in the dissimilar metal joint 10 is not particularly limited, and the disassembly method of the dissimilar metal joint according to the present invention can be applied to the joints joined by either the fusion welding method or the solid-state welding method. Specifically, examples of the fusion welding method include laser welding, arc welding, and resistance spot welding. Examples of the solid-state welding method include joining using an intermediate layer formed by a cold spray method, and friction stir welding. However, in this embodiment, the restraining method in the restraining step and the heating time in the heating step are selected based on the joining method of the first member 11 and the second member 12 and the joining area. The method of selecting the restraining method and the heating time will be described later.
[0027] A dissimilar metal joint including an intermediate layer between a first member 11 and a second member 12 will be described below with reference to Fig. 2. Fig. 2 shows a state in which the above-mentioned heating step has been performed on a dissimilar metal joint 30 including an intermediate layer 36. However, in Fig. 2, the restraining device 20 and heat are omitted from the illustration.
[0028] 2, a steel intermediate layer 36 is formed on the surface of the aluminum alloy second member 12, and the steel first member 11 is superimposed thereon. Laser welding is then performed from the first member 11 side to form a weld metal 37 that penetrates the first member 11 and reaches the intermediate layer 36, thereby producing a dissimilar metal joint 30 in which the first member 11 and the second member 12 are joined.
[0029] In the dissimilar metal joint 30, the second member 12 and the intermediate layer 36 made of an aluminum alloy can be mechanically bonded with high strength. In addition, since the intermediate layer 36 and the first member 11 are made of the same metal, a strong bond can be obtained by laser welding. Therefore, the first member 11 and the second member are bonded with excellent strength even though they are made of different metal materials.
[0030] The intermediate layer 36 can be formed by using a method of low-temperature spraying (cold spray method) of metal powder made of steel onto the surface of the second member 12. The material of the intermediate layer 36 may be selected from at least one of pure metals, alloys, and compounds, for example, and a material that can be welded to the first member 11 may be selected.
[0031] When disassembling the dissimilar metal joint 30, the dissimilar metal joint 30 is heated in a restrained state, as in the first embodiment. This forms a brittle intermetallic compound 16 between the intermediate layer 36 and the second member 12, so that peeling can easily occur in a short time. After a predetermined heating time has elapsed, the first member 11 and the second member 12 are separated, so that the members can be disassembled into their respective metallic materials. In this way, when the disassembly method according to this embodiment is applied to a dissimilar metal joint 30 (hereinafter sometimes referred to as a cold spray joint) that has been joined using the cold spray method, disassembly can be performed even more easily in a short time.
[0032] It is not clear why applying the present invention to cold spray joints as a disassembly method for dissimilar metal joints is particularly preferable, especially for dissimilar material joints joined by fusion welding (hereinafter sometimes referred to as fusion welded joints), but the following reasons are thought to be possible.
[0033] In a cold spray joint, the second member made of an aluminum alloy and the cold spray coating (intermediate layer 36) made of steel are in close contact with each other. Therefore, a stress is applied to the interface between them, which is equal to the difference in linear expansion coefficient between the aluminum alloy and the steel. On the other hand, in a fusion welded joint, the aluminum alloy constituting the second member 12 and the weld metal are in close contact with each other, but the weld metal is a mixture of steel and aluminum, so its physical properties are closer to those of aluminum than those of steel alone. Therefore, the difference in linear expansion coefficient between the weld metal and the second member 12 is smaller than the difference in linear expansion coefficient between the aluminum alloy and the steel in a cold spray joint. As a result, it is considered that the stress generated at the interface by the cooling process after the heating process may be smaller in a fusion welded joint.
[0034] Another reason why the present invention is suitable for application to cold spray joints is the presence or absence of welding defects near the weld metal-aluminum interface. In joints made by fusion welding, the penetration depth into the aluminum is often at least 200 μm in order to ensure strength. However, melting such a large amount of aluminum is likely to induce welding defects such as cracks and blowholes at the weld metal-aluminum interface. These welding defects are thought to relieve stress at the weld metal-aluminum interface during heating and cooling. On the other hand, in cold spray joints, aluminum is not melted or only a very small amount is melted during the welding process, so there are almost no welding defects at the interface between the cold spray coating and the aluminum, and the stress generated during heating and cooling is large. Therefore, it is presumed that decomposition is possible with a short heat treatment.
[0035] In the first restraining method, the position of the region R1 restrained by the restraining device 20 is not particularly limited as long as the region R1 where the first member 11 and the second member 12 are overlapped is restrained. If the region R1 is in the vicinity of the end face of the dissimilar metal joint 10, the stress generated at the interface between the first member 11 and the second member 12 becomes large, so that the peeling 17 can be generated more easily. Therefore, the position of the region R1 is preferably in the vicinity of the end of the region where the first member 11 and the second member 12 are overlapped, or in the vicinity of the end face of the dissimilar metal joint 10.
[0036] Furthermore, in the above first embodiment, an example has been described in which only one location in the overlapping region of the first member 11 and the second member 12 is restrained. However, in the first restraining method, it is sufficient to restrain at least one location in the overlapping region, and restraint may be performed at two locations, the region R1 and, for example, the first member 11, or restraint may be performed at two locations, the region R1 and the second member 12.
[0037] The method of restraining the dissimilar metal joint is not limited to the method described in the first embodiment, and other restraining methods can be used. The other restraining methods will be described below with reference to the drawings as the second and third embodiments.
[0038] <Second embodiment> Fig. 3 is a schematic cross-sectional view showing a restraining step in a disassembly method for a dissimilar metal joint according to a second embodiment of the present invention. The second embodiment is an example in which a method of restraining a first member 11 and a second member 12 by a second restraining method is used. Note that in the second and third embodiments, the only difference from the first embodiment is the restraining method, so only the restraining step will be described using Figs. 3 and 4, respectively, and the following steps can be the same as those in the first embodiment. In Figs. 3 and 4, the same reference numerals are used to designate the same parts as those shown in Figs. 1A to 1D, and detailed description thereof will be omitted.
[0039] (Restraint process: 2nd restraint method) As shown in FIG. 3, the area where the first member 11 and the second member 12 are overlapped is restrained by two separate areas R2 and R3.
[0040] In the second restraint method, too, in the heating step, a brittle intermetallic compound is formed in the joint 15 between the first member 11 and the second member 12. Then, by performing cooling after the heating step, stress is generated in the joint 15, and peeling occurs in the region between the first member 11 and the second member 12 where the brittle intermetallic compound is formed.
[0041] Thereafter, the first member 11 and the second member 12 are separated, whereby the components suitable for recycling can be separated.
[0042] In the second restraining method, the positions of the regions R2 and R3 restrained by the restraining device 20 are not particularly limited. If the regions R2 and R3 are close to each other, stress is generated at the interface between the first member 11 and the second member 12, and the effect of peeling can be obtained, as in the case of clamping at only one point as in the first embodiment. However, if the regions R2 and R3 are separated from each other, the stress generated at the interface becomes large, and peeling can be caused more easily. Therefore, it is preferable that the regions R2 and R3 are separated from each other, and it is preferable to restrain them near both opposing end faces, for example.
[0043] In the above first embodiment, an example has been described in which only two points in the overlapping area of the first member 11 and the second member 12 are restrained. However, the second restraining method is not limited to the method of restraining only two points in the overlapping area, and the overlapping area may be restrained at two or more points.
[0044] <Third embodiment> 4 is a schematic cross-sectional view showing a restraining step in a disassembly method for a dissimilar metal joint according to a third embodiment of the present invention. The third embodiment is an example in which a first member 11 and a second member 12 are restrained by a third restraining method.
[0045] (Restraint process: 3rd restraint method) In this embodiment, regions R4 and R5 in the vicinity of both end faces of the first member 11 are restrained by the restraining device 20.
[0046] In the third restraint method, too, in the heating step, a brittle intermetallic compound is formed in the joint 15 between the first member 11 and the second member 12. Then, by performing cooling after the heating step, stress is generated in the joint 15, which causes distortion at the interface between the first member 11 and the second member 12, and causes peeling in the region between the first member 11 and the second member 12 where the brittle intermetallic compound is formed.
[0047] Thereafter, the first member 11 and the second member 12 are separated, whereby the components suitable for recycling can be separated.
[0048] In the third restraining method, the positions of the regions R4 and R5 restrained by the restraining device 20 are not particularly limited, and only one of the first member 11 and the second member 12 may be restrained in two regions. In this case, if the regions R4 and R5 are separated from each other, the stress generated at the interface increases, so that peeling can occur more easily. Therefore, it is preferable that the regions R4 and R5 are separated from each other, and it is preferable to restrain them near both opposing end faces of either the first member 11 or the second member 12, for example. It is more preferable to select the restraining position so that the joint 15 with the other member is located between the regions R4 and R5 of the member to be restrained.
[0049] In the above third embodiment, an example has been described in which either the first member 11 or the second member 12 is restrained at two locations, the region R4 and the region R5. However, as the third restraining method, either the first member 11 or the second member 12 may be restrained at two or more locations.
[0050] In the restraining steps of the above first to third embodiments, the restraining means uses a method of clamping in the plate thickness direction using the restraining device 20, but the restraining means is not particularly limited. In particular, in the second and third embodiments, the dissimilar metal joint 10 may be restrained by clamping inward from both end face sides in a direction perpendicular to the plate thickness direction. Even with such a restraining method, stress can be generated due to the difference in linear expansion coefficient between the first member 11 and the second member 12, and the first member 11 and the second member 12 can be easily separated in a short time.
[0051] As described above, in this embodiment, the following three types of restraint methods can be selected based on the joining method and joining area of the first member 11 and the second member 12. First restraint method: A method of restraining the overlapping area of the first member and the second member by clamping them at one location. Second restraint method: A method in which the area where the first member and the second member are overlapped is restrained at two or more separated points. Third restraint method: A method in which only one of the first member and the second member is restrained at two or more separated points.
[0052] For example, the disassembly method according to the present invention is more suitable as a method for disassembling a cold spray joint, and therefore disassembly is easier than that of a fusion welded joint. Therefore, using any of the first to third restraint methods described above, peeling can be caused in a short time. On the other hand, since a fusion welded joint is considered to be less susceptible to stress due to the difference in linear expansion coefficient between the first member 11 and the second member 12, it is preferable to use a restraint method that is more likely to cause stress. Therefore, using the first restraint method or the second restraint method, the first member 11 and the second member 12 can be disassembled more reliably.
[0053] In addition, a suitable heating time can also be selected based on the joining method of the first member 11 and the second member 12, etc. For example, when the disassembly method of the present invention is applied to a cold spray joint, it is possible to disassemble it into the first member 11 and the second member 12 by heating for an extremely short heating time of, for example, five minutes and then cooling. On the other hand, when the disassembly method of the present invention is applied to a fusion welded joint, the heating time can be made longer compared to that of a cold spray joint.
[0054] Furthermore, a suitable restraining location can also be selected based on the joining method and joining area of the first member 11 and the second member 12. For example, when a fusion welded joint in which weld metal is formed at only one location is restrained using the third restraining method, stress is unlikely to be applied to the joint. Therefore, it is preferable to use the first restraining method or the second restraining method. Also, when a fusion welded joint in which weld metal is formed at only one location is restrained using the first restraining method, if the position where the weld metal is formed is close to the restraining location, stress is unlikely to be applied to the joint. Therefore, it is preferable to restrain in an area away from the position where the weld metal is formed.
[0055] As described above, it is preferable to select optimal conditions for the restraint method, heating time, and restraint position depending on the joining method and joining area (joint position) of the dissimilar metal joint. As a method for selecting the conditions for the disassembly process, the restraint process, heating process, and cooling process are performed, for example, in the same manner as in the first to third embodiments, on a test material joined in the same manner and with the same size as the dissimilar metal joint that is actually required to be disassembled. Then, taking into consideration the ease of restraint, heating time, etc., the conditions that allow efficient disassembly can be selected and used as the conditions for disassembly of the actual dissimilar metal joint.
[0056] When the optimum heating time for the above test material is examined, the heating process can be divided into multiple heating steps. For example, after 30 minutes of heating, the test material is cooled, and if no peeling is found after observing the joint, a heating test can be performed for another 30 minutes. If peeling occurs due to this additional heating, the cumulative time from the initial heating time can be set as the actual heating time. In this embodiment, the heating time refers to the time during which the temperature of the dissimilar metal joint is raised to a predetermined temperature and maintained.
[0057] In the restraining device 20 that restrains the dissimilar metal joint 10, it is preferable to use a material with low thermal conductivity as the material of the restraining member that directly contacts the dissimilar metal joint 10. If a restraining member made of a material with high thermal conductivity contacts the dissimilar metal joint 10, heat is conducted during the heating process, and the temperature of the dissimilar metal joint 10 is less likely to increase in the vicinity of the restraining regions R1 to R5. As a result, peeling may be less likely to occur. Therefore, it is preferable to use, for example, a ceramic member as the restraining member that contacts the dissimilar metal joint 10 in the restraining device.
[0058] Furthermore, in the heating steps of the first to third embodiments, the heating means is not particularly limited. For example, high-frequency induction heating is preferably used because it can rapidly heat the dissimilar metal joint 10.
[0059] The combination of the first member 11 and the second member 12 is not particularly limited, and it is sufficient that one member is made of a metal and the other is made of a metal different from the one member, but a combination that forms a brittle intermetallic compound is more likely to cause peeling. Specifically, it is preferable to use any one of the following combinations: a first member made of an iron alloy such as steel and a second member made of an aluminum alloy, a first member made of an iron alloy and a second member made of a titanium alloy, a first member made of an aluminum alloy and a second member made of a titanium alloy, a first member made of a copper alloy and a second member made of a titanium alloy, and a first member made of a copper alloy and a second member made of a magnesium alloy. In the first to third embodiments, the second member is illustrated as a lower plate and the first member as an upper plate, but the first member may be illustrated as a lower plate and the second member as an upper plate. Therefore, the first member and the second member may be interchanged in the above combinations. EXAMPLES
[0060] Hereinafter, an example of the disassembly method for a dissimilar metal joint according to this embodiment will be specifically described.
[0061] <Creating dissimilar metal joints> First, a cold spray coating was formed on the surface of the second component as the lower plate by the cold spray method. Next, the first component as the upper plate was placed on top of the surface of the second component on which the cold spray coating was formed, and laser welding was performed from above the first component to create a dissimilar metal joint. In addition, a second component without a cold spray coating was prepared as the other lower plate. The first component, which will be the upper plate, was then placed on the surface of the second component, and laser welding was performed from above the first component to create a dissimilar metal joint.
[0062] <Disassembly of dissimilar metal joints> The resulting dissimilar metal joint was then heated while restrained using various restraint methods, and then cooled. The cross section of the dissimilar metal joint, divided into two equal parts in the longitudinal direction, was observed to confirm the occurrence of delamination at the joint.
[0063] The types and sizes of the first and second members, the processing conditions during cold spray coating formation, the laser welding conditions, the heat treatment conditions during disassembly, and the restraining conditions are shown below.
[0064] (Materials for dissimilar metal joints) First component (upper plate): Mild steel (width 10 mm, length 100 mm, plate thickness 1.4 mm) Second component (lower plate): Aluminum alloy material (AA7204) (width 10 mm, length 100 mm, plate thickness 3 mm) Cold spray coating (middle layer): Iron coating (thickness 1.2 mm)
[0065] (Cold spray treatment conditions) Equipment: High temperature and high pressure type Powder: Water atomized iron powder (average particle size: 43 μm) Gas type: Nitrogen Gas pressure: 5MPa Gas temperature: 1000℃
[0066] (Laser welding conditions) Welding machine: Fiber laser (IPG photonics YLS-6000) Laser power: 2100W Welding speed: 4m / min Spot diameter: 0.3mm Overlap: 100mm (full wrap) Welding length: 100mm
[0067] (Restraint method) First restraint method: A method in which the overlapping area of the first and second components is clamped at one location to restrain them (clamping one longitudinal end of the dissimilar metal joint with a clamp). Second restraint method: A method in which the area where the first and second components are overlapped is restrained at two separate locations (clamping both longitudinal ends of the dissimilar metal joint).
[0068] (Heat treatment conditions) Heating device: Processing for master test machine Heating atmosphere: Air Heat treatment temperature: Heat at 550℃~600℃ for a specified time, then cool to room temperature Heat treatment time: 5 to 60 minutes
[0069] The joining method for the first and second members, the heat treatment conditions during separation, the restraint method, and whether or not the joint separated are shown in Table 1 below.
[0070] [Table 1]
[0071] As shown in Table 1 above, regardless of the type of joint, when a dissimilar metal joint was restrained and heated using the first and second restraining methods and then cooled, peeling could be easily generated at the joint in a short time. After that, the first and second members were separated, allowing each metal material to be separated. When the type of dissimilar metal joint was a laser welded joint, the second restraining method allowed peeling to occur in a shorter heating time than the first restraining method. When the type of dissimilar metal joint was a cold spray joint, peeling could be generated even with an even shorter heating time. [Explanation of symbols]
[0072] 10,30 Dissimilar metal joints 11 First member 12 Second member 16 Intermetallic compounds 17 Peeling 20 Restraint device 36 Middle Class 37 Welding metal
Claims
1. A method for disassembling a dissimilar metal joint having a first member made of a metal, a second member made of a metal different from the first member, and a joint between the first member and the second member, comprising: A restraining step of restraining the dissimilar metal joint; A heating step of heating the dissimilar metal joint in a restrained state; A cooling process for cooling the dissimilar metal joint after the heating process, In the restraining step, based on a joining method and a joining area of the first member and the second member, First restraining method: a method of restraining the overlapping area of the first member and the second member by clamping them at one point; A second restraining method: a method of restraining the area where the first member and the second member are overlapped at two or more separated points; and a third restraining method: a method of restraining only one of the first member and the second member at two or more locations spaced apart from each other; In the heating step, When the melting point of the lower melting point member of the first member and the second member is Tm (°C), the heating temperature is set to be equal to or higher than (Tm-150) (°C) and lower than Tm (°C), A method for disassembling a dissimilar metal joint, comprising selecting a heating time based on a joining method for the first member and the second member.
2. 2. The method for disassembling a dissimilar metal joint according to claim 1, wherein the combination of the first member and the second member is any one of the following combinations: a first member made of iron or an iron alloy and a second member made of aluminum or an aluminum alloy, a first member made of iron or an iron alloy and a second member made of titanium or a titanium alloy, a first member made of aluminum or an aluminum alloy and a second member made of titanium or a titanium alloy, a first member made of copper or a copper alloy and a second member made of titanium or a titanium alloy, and a first member made of copper or a copper alloy and a second member made of magnesium or a magnesium alloy.
3. The dissimilar metal joint has the first member, the second member, and an intermediate layer disposed between the first member and the second member, 3. The method for disassembling a dissimilar metal joint according to claim 1, wherein the intermediate layer is made of at least one of a pure metal, an alloy, and a compound.
4. The method for disassembling a dissimilar metal joint according to claim 3, wherein the intermediate layer is a cold spray coating provided on a surface of either the first member or the second member.
5. The dissimilar metal joint is formed by joining the first member and the second member by a fusion welding method, 3. The method for disassembling a dissimilar metal joint according to claim 1, wherein in the restraining step, one of the first restraining method and the second restraining method is selected.
Citation Information
Patent Citations
Separating and recovering method for layered material from multilayered material
JP1982152433A
Separation of scrap of clad material
JP1993247543A
Method for recovering metallic material
JP2003170151A
Cladding material for terminal, and terminal for aluminum wire formed using cladding material
JP2005228496A
Method for separating and recovering constituent from joined constituent and easily separable joint structure
JP2005230777A