Production method of light-weight cellular concrete used with carbonation treated light-weight cellular concrete powder

By crushing and carbonating ALC scraps to produce calcium carbonate, the method enhances the recyclability and maintains compressive strength of lightweight cellular concrete, addressing limitations in existing recycling methods.

JP2024155544APending Publication Date: 2024-10-31CLION CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023070342
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing methods for recycling lightweight cellular concrete (ALC) are limited by the amount of recycled raw materials, require special equipment for high-temperature treatment, and result in decreased compressive strength and increased shrinkage rates when more than 20% by mass is used.

Method used

A method involving coarse crushing of ALC scraps to 1.2 mm or less and carbonating at 20°C to 80°C to produce calcium carbonate, which is then mixed with other raw materials to maintain compressive strength and reduce shrinkage, without the need for special equipment.

Benefits of technology

The method allows for the use of up to 25% by mass of recycled ALC without affecting compressive strength or increasing shrinkage, simplifying the process and reducing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155544000001_ABST
    Figure 2024155544000001_ABST
Patent Text Reader

Abstract

To realize light-weight cellular concrete that can be taken as interior wall materials even if an ALC recycling amount is large while maintaining panel strength of the light-weight cellular concrete used as a wall material, also does not require a special measuring apparatus, facilitates process control, is hardly affected by fluctuation of a recycled raw material amount to compression strength even if recycled raw materials are used with 25 mass% or more in internal percentage solids without requiring a special firing facility, has a small contraction coefficient and can be stably held.SOLUTION: A production method of light-weight cellular concrete is characterized by coarsely grinding light-weight cellular concrete wastes to a diameter of 1.2 mm or less, and adding recycled raw materials for light-weight cellular concrete containing carbonation treated calcium carbonate with 20°C to 80°C from 2 mass% to 25 mass% of the whole mass of light-weight cellular concrete materials in internal percentage solids.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing lightweight cellular concrete using a carbonated lightweight cellular concrete powder. [Background technology]

[0002] Generally, lightweight aerated concrete (hereinafter sometimes abbreviated as ALC) is made by adding water to a mixture of siliceous raw materials such as natural silica stone and silica sand, and calcareous raw materials such as quicklime made from limestone, cement, and gypsum, and then adding metallic aluminum to the mixture to foam it. The green cake obtained in the first curing step is then cut to the required size with a piano wire, and then the second curing step is steam curing at high temperature and pressure in an autoclave.

[0003] The obtained lightweight cellular concrete can be cut into various molded products of predetermined dimensions and used as building materials such as lightweight cellular concrete panels for a wide range of applications including various exterior walls, partitions, roofs, floors, etc.

[0004] In the manufacturing site, lightweight aerated concrete waste such as cutting waste or cutting waste from cutting processing is generated due to dimensional adjustment of the molded product. This is reused as recycled raw material for the production of lightweight aerated concrete. However, when the amount of recycled raw material added is increased, there is a phenomenon that the compressive strength of the lightweight aerated concrete product decreases. In Patent Document 1, even if the recycled raw material of surplus lightweight aerated concrete is used up to about 10 mass% to 20 mass% of the solid content, it is not easily affected by fluctuations in the amount of recycled raw material, and the compressive strength can be stably maintained at the same level as that of conventional products. In addition, Patent Document 2 considers burning the lightweight aerated concrete curing waste at high temperatures of 800°C to 1500°C to reuse it not only as a siliceous raw material but also as a calcareous raw material. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6644184 [Patent Document 2] Japanese Patent Application Publication No. 05-319876 Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the method of Prior Patent Document 1, the amount of ALC recycled is limited to about 25% by mass in terms of solid content, and measures must be considered when using ALC at 20% by mass or more. In addition to the effectiveness of recycling, the method of Prior Patent Document 2 has the drawback of requiring special high-temperature treatment equipment and a large amount of heat energy.

[0007] Therefore, the present invention provides a method for producing lightweight aerated concrete that can be used as a building material even if a greater amount of recycled ALC is used while maintaining the compressive strength of lightweight aerated concrete, and which does not require special measuring equipment and makes process management easy, does not require special firing equipment, and is less susceptible to fluctuations in compressive strength due to the amount of recycled raw materials used, even when 25 mass% or more of recycled raw materials is used in terms of internal solid content, and which can maintain a small and stable shrinkage rate of the ALC product. [Means for solving the problem]

[0008] As a result of extensive research, the inventors have come up with the following invention. [1] Provided is a method for producing recycled raw materials for lightweight aerated concrete containing calcium carbonate, which is obtained by coarsely crushing lightweight aerated concrete waste to a diameter of 1.2 mm or less and carbonating the coarsely crushed lightweight aerated concrete waste at 20°C to 80°C. [2] A method for producing lightweight aerated concrete is provided, which comprises coarsely crushing lightweight aerated concrete scraps to a diameter of 1.2 mm or less, and adding recycled raw material for lightweight aerated concrete containing calcium carbonate that has been carbonated at 20°C to 80°C in an amount of 2 to 25% by mass (solid content) of the total mass of the lightweight aerated concrete raw material. [3] Provided is a method for producing lightweight cellular concrete, characterized in that the lightweight cellular concrete scrap is cured scrap from the manufacturing process after autoclave curing, the coarse crusher is a hammer crusher or a pin mill, and the carbonation degree is 80% or more.

[0009] Lightweight cellular concrete waste Here, the term "lightweight aerated concrete waste" refers to cured surplus material generated during the manufacturing process of lightweight aerated concrete, including cutting scraps, cutting chips, cut chips, products that do not meet the dimensions, and their fragments, resulting from cutting processing after autoclave curing. It does not include cutting chips of semi-hardened bodies before autoclave curing, but also includes lightweight aerated concrete waste resulting from dismantling after construction of the lightweight aerated concrete.

[0010] Coarse crushing The lightweight cellular concrete waste is coarsely crushed using a coarse crushing machine with a small crushing force such as a hammer crusher or a pin mill. It is preferable to make it into powder with a diameter of 1.2 mm or less (fully passing through a 1.2 mm sieve). For example, it is preferable to use a hammer crusher with a screen opening of 1.2 mm so that coarsely crushed material with a diameter of 1.2 mm or less can be immediately collected. If the concrete is crushed too much, the subsequent carbonation will vary, making it difficult to control the specified heating temperature and heating time.

[0011] Carbonation time The lightweight aerated concrete waste with a diameter of 1.2 mm is carbonated. The carbonation method may be a method of contacting carbon dioxide after crushing, and the carbonation gas may be carbon dioxide. Carbonation may also be performed during crushing of recycled powder. Carbon dioxide gas derived from limestone in a cement factory can be used, which can greatly contribute to carbon-free, carbon recycling, and carbon fixation. The carbon dioxide gas concentration in the carbon dioxide gas atmosphere is preferably 4 to 40% by volume, more preferably 5 to 30% by volume, from the viewpoints of shortening the treatment time and easiness of forming a carbon dioxide gas atmosphere. If the concentration is less than 4% by volume, the carbonation treatment takes a long time, which is problematic. The reaction temperature during the treatment is up to 20 to 80°C, preferably about 30 to 60°C, from the viewpoint of shortening the treatment time. This is also related to the conditions for obtaining a single phase of crystal form. If the temperature is less than 20°C, it is not preferable because it takes a long time to generate calcium carbonate. If the temperature exceeds 80°C, the cost of thermal energy increases, which is not preferable. Furthermore, carbonation can be performed using solid carbon dioxide (dry ice) as a source. In this case, a carbon dioxide atmosphere close to 100% by volume can be obtained, but the temperature inside the reaction vessel is set to 20 to 80°C, preferably 30 to 60°C.

[0012] In addition, the relative humidity during the carbonation treatment is preferably 2 to 100%, more preferably 40 to 95%, and particularly preferably 50 to 80%, from the viewpoints of shortening the treatment time and facilitating the adjustment of the target relative humidity. If the humidity is less than 2%, it is not preferable because it takes a long time to generate calcium carbonate. The treatment time varies depending on the treatment conditions, but if it is extremely short, the content of calcium carbonate in the ALC may be reduced. Note that the carbonation treatment can be performed in a shorter time by increasing the treatment pressure.

[0013] In this way, the carbonation degree of the ALC recycled powder can be increased to 80% or more. The CaO mass% in the tobermorite is calculated by subtracting the CaO mass% in the gypsum from the CaO mass% in the ALC recycled powder. The carbonation degree is the ratio of the "actual CO2 mass%" calculated from the mass reduction rate due to the endothermic reaction of CO2 removal at 600°C to 800°C of the carbonated ALC recycled powder, to the "theoretical CO2 mass%" required for all of the CaO mass% in the tobermorite to become CaCO3. The carbonation degree is preferably 82% or more, and more preferably 85% or more. This is because the strength and shrinkage properties are improved by increasing the amount.

[0014] The calcium carbonate produced by carbonation of lightweight cellular concrete waste is calcite, aragonite, or vaterite. For carbonation, a normal treatment vessel such as a box-type treatment vessel can be used. The lightweight cellular concrete waste containing any type of calcium carbonate has almost the same recycling characteristics.

[0015] Recycling suitability of lightweight cellular concrete waste Carbonation and dehydration change tobermorite into calcium carbonate and silica, but there is little change in the pore shape, overall shape, and bulk density of the lightweight cellular concrete waste. Figures 1 and 2 show SEM images of coarsely crushed lightweight cellular concrete waste containing particles with a diameter of 1.2 mm or more before and after carbonation.

[0016] Figure 3 shows the X-ray diffraction chart of the lightweight cellular concrete waste before and after carbonation. Based on the quartz peak, the diffraction peak intensity of tobermorite disappears and the diffraction peak of calcite appears. In Figure 4, in addition to calcite, the diffraction peak of vaterite also appears.

[0017] In this case, the recyclability of the lightweight cellular concrete scrap cannot be immediately determined from the crystal form of calcium carbonate. In other words, both the carbonated lightweight cellular concrete scrap in Figure 3 and the carbonated cellular concrete scrap in Figure 4 can exhibit recyclability under the conditions of particle size adjustment. The form of calcium carbonate in lightweight cellular concrete may be any of calcite, vaterite, and aragonite.

[0018] Even in these scanning electron microscope images, it was confirmed that it was difficult to find any changes in appearance that would be relevant to recyclability.

[0019] As described above, the recycling suitability of lightweight cellular concrete scrap is obtained by carrying out specified coarse crushing, carbonation, and heating under specified coarse crushing conditions with specified particle size adjustment, and carbonation and heating conditions, and it is difficult to directly identify lightweight cellular concrete scrap that has this suitability based solely on its structure or characteristics.

[0020] Stable recycling suitability can be achieved by optimizing the carbonation and dehydration of tobermorite and the mixing ratio of carbonated ALC scrap.

[0021] Raw materials Mixture ratio A predetermined amount of carbonated lightweight aerated concrete scrap was used to manufacture lightweight aerated concrete. The mixing ratio of the raw materials was 5-25% by mass of carbonated lightweight aerated concrete scrap, 35-73% by mass of silica stone, 6-12% by mass of quicklime, 15-25% by mass of cement, and 1-3% by mass of gypsum, and 0.06-0.1% by mass of aluminum powder and water were added to the entire mixture to prepare a slurry. It is preferable to add water later. In particular, it is preferable to dry mix the carbonated lightweight aerated concrete scrap and silica stone.

[0022] When using carbonated ALC recycled powder, calcium dissolves from the tobermorite during the carbonation process of the main component, tobermorite, hardening the surface layer of the silica, and after carbonation, the tobermorite dissociates its crystal water, but the increase in mass due to carbonation and the shrinkage phenomenon of the recycled powder can also cause hardening. Therefore, it changes from a simple bulking agent to a type of aggregate, which is thought to suppress the decrease in strength. In addition, since tobermorite is a mineral with a stable crystal structure, dimensional change is small, but calcium carbonate and silica are minerals that are more stable than tobermorite and dimensional change is extremely small, so it can be assumed that the drying shrinkage rate will decrease if the proportion of raw materials increases. Effect of the Invention

[0023] The present invention provides a method for producing lightweight aerated concrete that can be used as a building material even if a larger amount of recycled ALC is used while maintaining the compressive strength of lightweight aerated concrete, and that does not require special measuring equipment and easy process management, does not require special firing equipment, is less susceptible to fluctuations in compressive strength due to the amount of recycled raw materials used even if 25 mass% or more of recycled raw materials are used in terms of internal solid content, and the shrinkage rate of the ALC product can be kept small and stable. [Brief description of the drawings]

[0024] [Figure 1] FIG. 2 shows an SEM image of lightweight cellular concrete waste before carbonation. [Diagram 2] FIG. 2 shows an SEM image of lightweight cellular concrete scrap after carbonation. [Diagram 3] FIG. 1 is a diagram illustrating X-ray diffraction charts of lightweight cellular concrete scrap before and after carbonation. [Figure 4] FIG. 1 is a diagram illustrating X-ray diffraction charts of lightweight cellular concrete scrap before and after carbonation. [Diagram 5] FIG. 1 is a graph illustrating the relationship between the recycled amount (mass%) of carbonated ALC powder and the compressive strength. [Figure 6] FIG. 1 is a diagram illustrating the relationship between the recycled amount (mass%) of carbonated ALC powder and the shrinkage rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Ingredients and composition Solid ingredients: Carbonated lightweight aerated concrete waste for recycling with a particle size of 1.2 mm or less, Silica powder manufactured by JFE Minerals, Yoshizawa quicklime powder, High-early-strength Portland cement manufactured by Taiheiyo Cement Corporation, Gypsum powder manufactured by Kokusai Shoji Co., Ltd. A slurry made by mixing aluminum powder with water at 70% by mass based on the solid raw material is poured into a formwork to obtain a semi-hardened body, which is then cured in an autoclave to obtain an ALC panel.

[0026] Coarse crushing of lightweight aerated concrete waste A hammer crusher was used to roughly crush the lightweight cellular concrete waste.

[0027] Carbonation and heating methods A drum was used as a heat treatment container for the coarsely crushed lightweight cellular concrete waste. The carbonation conditions were carbon dioxide concentration 40%, temperature 50℃, humidity 10%, and treatment time 24 hours.

[0028] The lightweight cellular concrete of the present invention is obtained by the following manufacturing method. The materials used are powdered siliceous raw materials such as silica stone and quartz, powdered calcareous raw materials such as quicklime and Portland cement, gypsum, and a foaming agent, in addition to carbonated lightweight cellular concrete waste that has been subjected to a fine grinding process. These are mixed with water to form a mixed slurry, which is then placed in a formwork. Next, foaming is performed by using a foaming agent made of metal powder such as aluminum, which generates gas to foam the concrete.

[0029] After that, it is cut to a specified size, and then subjected to a hydrothermal reaction in an autoclave at 180°C and 10 atm to produce tobermorite.

[0030] By appropriately combining the raw materials, conditions, ranges, and methods described above, it is possible to obtain the lightweight cellular concrete of the present invention having excellent compressive strength.

[0031] Next, experimental examples and comparative examples of the lightweight aerated concrete of the present invention are described. Among the solid raw materials, 0 to 30% by mass of lightweight aerated concrete chips with a particle size of 1.2 mm or less that had been carbonized, 38 to 68% by mass of silica powder manufactured by JFE Mineral Co., Ltd., 10% by mass of quicklime powder manufactured by Yoshizawa Co., Ltd., 20% by mass of high-early-strength Portland cement powder manufactured by Taiheiyo Cement Co., Ltd., 2% by mass of dihydrate gypsum powder manufactured by Kokusai Shoji Co., Ltd., 0.1 parts by mass of aluminum powder, and 70% by mass of water were mixed together to form a slurry, which was poured into a formwork, and after 3 hours, a semi-hardened body was obtained, and the slurry was kept in an autoclave at 180°C and 10 atm for 6 hours to obtain an ALC block of about 300 mm x about 300 mm x about 300 mm.

[0032] A 100mm x 100mm x 100mm specimen was cut from the center of this ALC block in accordance with JIS A 5416, and dried in a hot air dryer at 60℃ until the moisture content reached 10±2℃ to prepare the specimen for compressive strength measurement. After the test, the specimen was dried in a hot air dryer at 105℃, and the density was determined.

[0033] The compressive strength test was conducted in accordance with JIS A 5416-2016, with the test specimen size being 100mm x 100mm x 100mm. The bone dry density test was also conducted in accordance with JIS A 5416-2016.

[0034] In addition, in accordance with JIS A 5416, test specimens measuring 40mm x 40mm x 160mm were cut from the center of the ALC blocks and submerged in water at 20°C for three days. After that, the drying shrinkage rate from a saturated water state was determined in a constant temperature room at 20°C and a humidity of 60%.

[0035] The carbonation degree of the carbonated ALC recycled powder was determined by the following procedure. 1) From the EDX analysis results, the CaO mass% and SO3 mass% in the carbonated ALC recycled powder are determined. 2) Calculate the mass% CaO in the gypsum from the mass% SO3. 3) The CaO mass% in tobermorite is the difference between the CaO mass% in the ALC recycled powder and the CaO mass% in the gypsum. Calculate the "theoretical CO2 mass%" required to convert all of the CaO mass% in tobermorite to CaCO3. 4) Using DTA, the "actual CO2 content" is calculated from the mass loss rate due to the endothermic reaction of CO2 removal at 600°C to 800°C for the ALC recycled powder that has been carbonated in the same way as in 1). 5) "Carbonation degree = actual CO2 mass% / theoretical CO2 mass%".

[0036] [Table 1]

[0037] Table 1 shows the bone dry density, compressive strength, and drying shrinkage of ALC blocks with each recycled amount of ALC powder, carbonated ALC powder (carbonation degree 85.1%) and non-carbonated ALC powder. Figure 5 shows the relationship between the recycled amount of carbonated ALC powder (mass%) and compressive strength, and Figure 6 shows the relationship between the recycled amount of carbonated ALC powder (mass%) and shrinkage, in comparison with blocks recycled with non-carbonated ALC powder.

[0038] Here, when the ratio of carbonated ALC powder (carbonation degree 85.1%) in the solid raw material was between 5% and 25% by mass in a dry state, compressive strength was maintained. A downward trend in drying shrinkage was also confirmed, improving performance. When the ratio of carbonated ALC recycled powder reached 30%, an inconvenience occurred in the manufacturing process, in that the air bubbles were not stable.

Claims

1. A method for producing recycled raw materials for lightweight aerated concrete containing calcium carbonate, which is obtained by roughly crushing lightweight aerated concrete waste to a diameter of 1.2 mm or less and carbonating the same at 20°C to 80°C.

2. A method for producing lightweight aerated concrete, comprising coarsely crushing lightweight aerated concrete waste to a diameter of 1.2 mm or less, and adding recycled raw material for lightweight aerated concrete containing calcium carbonate that has been carbonated at 20°C to 80°C in an amount of 2% to 25% by mass (solid content) of the total mass of the lightweight aerated concrete raw material.

3. A method for producing lightweight aerated concrete, characterized in that the lightweight aerated concrete scraps are cured scraps from the manufacturing process after autoclave curing, the coarse crusher is a hammer crusher or a pin mill, and the carbonation degree is 80% or more.

Citation Information

Patent Citations

  • Method for recycling aerated lightweight concrete and material for recycle

    JP1993319876A

  • Recycled raw material for lightweight aerated concrete and method for manufacturing lightweight aerated concrete using the same

    JP6644184B1