Multilayer type electronic component

A multilayer electronic component with a specific dielectric layer composition and core-shell structure enhances dielectric properties and reliability, addressing the needs of smaller, more integrated, and high-reliability capacitors for automotive applications.

JP2024155729APending Publication Date: 2024-10-31SAMSUNG ELECTRO MECHANICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024017937
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-07
Filing Date
2024-02-08
Publication Date
2024-10-31

Smart Images

  • Figure 2024155729000001_ABST
    Figure 2024155729000001_ABST
Patent Text Reader

Abstract

To improve a dielectric characteristic for a multilayer type electronic component containing CSZT as a main component and improve the reliability such as a voltage resistance characteristic or a temperature-capacity characteristic of the multilayer type electronic component containing CSZT as the main component of the dielectric layer.SOLUTION: A multilayer type electronic component in one embodiment of the present invention includes a main body including a dielectric layer and internal electrodes disposed alternately with the dielectric layer therebetween, and an external electrode disposed on the main body. The dielectric layer includes a main component containing calcium (Ca), strontium (Sr), zirconium (Zr), and titanium (Ti), and an accessory component containing manganese (Mn), yttrium (Y), and silicon (Si). The dielectric layer includes a plurality of dielectric crystal grains and a crystal grain boundary disposed between the adjacent dielectric crystal grains. At least a part of the dielectric crystal grains has a core-shell structure.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer electronic component. [Background technology]

[0002] Multilayer ceramic capacitors (MLCCs), a type of multilayer electronic component, are chip-type capacitors that are mounted on printed circuit boards of various electronic and automotive products, such as visual devices such as liquid crystal displays (LCDs) and plasma display panels (PDPs), computers, smartphones and mobile phones, infotainment systems, and automotive systems, to charge and discharge electricity.

[0003] Multilayer ceramic capacitors are made of paraelectric (CaZrO3) based ceramics according to the required characteristics. 1-x Sr x )(Zr 1-y Ti y They can be classified into Class I, which uses temperature-compensated BaTiO3 (CSZT) as the main component of the dielectric layer, and Class II, which has high dielectric constant characteristics and uses ferroelectric BaTiO3 (BT) having an (ABO3) crystal structure as the main component of the dielectric layer.

[0004] As electronic products become smaller, slimmer, and more multifunctional, chip components are also required to be smaller, and the packaging of electronic components is becoming more highly integrated. In addition, when electronic products are applied to automotive systems, they are exposed to high heat and vibration, so higher reliability is sometimes required.

[0005] As described above, there is a need for a method for improving the electrical characteristics and reliability of multilayer ceramic capacitors suitable for various purposes. Summary of the Invention [Problem to be solved by the invention]

[0006] One of the various objects of the present invention is to improve the dielectric properties of multilayer electronic components that contain CSZT as a major component of the dielectric layers.

[0007] One of the various objects of the present invention is to improve the reliability of the withstand voltage characteristics, temperature-capacity characteristics, etc. of a multilayer electronic component containing CSZT as a main component of a dielectric layer.

[0008] However, the object of the present invention is not limited to the above-mentioned contents, and can be more easily understood in the course of describing specific embodiments of the present invention. [Means for solving the problem]

[0009] A multilayer electronic component according to one embodiment of the present invention includes a main body including a dielectric layer and internal electrodes alternately arranged with the dielectric layer sandwiched therebetween, and an external electrode arranged on the main body, the dielectric layer including a main component including calcium (Ca), strontium (Sr), zirconium (Zr) and titanium (Ti) and a subcomponent including manganese (Mn), yttrium (Y) and silicon (Si), the dielectric layer including a plurality of dielectric crystal grains and crystal boundaries arranged between adjacent dielectric crystal grains, at least a portion of the plurality of dielectric crystal grains having a core-shell structure, in which, when the content of yttrium (Y) contained in the core per 100 moles of zirconium (Zr) contained in the core and shell is Yc and the content of yttrium (Y) contained in the shell per 100 moles of zirconium (Zr) contained in the core and shell is Ys, Ys / Yc>9 can be satisfied. Effect of the Invention

[0010] One of the various effects of the present invention is that in a multilayer electronic component containing CSZT as a main component of a dielectric layer, the dielectric properties of the multilayer electronic component are improved by controlling the microstructure or composition of the dielectric layer.

[0011] One of the various effects of the present invention is that, in a multilayer electronic component containing CSZT as the main component of a dielectric layer, the reliability of the multilayer electronic component, such as its withstand voltage characteristics and temperature-capacity characteristics, is improved by controlling the microstructure or composition of the dielectric layer.

[0012] However, the various yet significant advantages and effects of the present invention are not limited to the above, and can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]

[0013] [Figure 1] 1 is a perspective view of a multilayer electronic component according to an embodiment of the present invention; [Diagram 2] 2 is a cross-sectional view taken along line II' in FIG. [Diagram 3] 2 is a cross-sectional view taken along line II-II' in FIG. [Figure 4] 2 is an exploded perspective view showing a structure in which internal electrodes, dielectric layers, and a cover part are arranged according to an embodiment; FIG. [Diagram 5] FIG. 4 is an enlarged view of region P in FIG. [Figure 6a] 1 is a graph showing a change in average core-shell size depending on the content of an additive according to an embodiment. [Figure 6b] 1 is a graph showing a change in average core-shell size depending on the content of an additive according to an embodiment. [Figure 6c] 1 is a graph showing a change in average core-shell size depending on the content of an additive according to an embodiment. [Figure 7a] 1 is a graph showing changes in dielectric constant, capacitance, and quality factor depending on the content of an additive according to an embodiment. [Figure 7b] 1 is a graph showing changes in dielectric constant, capacitance, and quality factor depending on the content of an additive according to an embodiment. [Figure 7c] 1 is a graph showing changes in dielectric constant, capacitance, and quality factor depending on the content of an additive according to an embodiment. [Figure 8]1 is a graph showing changes in temperature-capacity characteristics depending on the content of an additive according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the embodiments of the present invention will be described with reference to specific embodiments and the accompanying drawings. However, the embodiments of the present invention can be modified into several other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those skilled in the art. Therefore, the shapes and sizes of elements in the drawings may be enlarged or reduced (or highlighted or simplified) for clearer explanation, and elements indicated by the same reference numerals in the drawings are the same elements.

[0015] In addition, in the drawings, parts that are not relevant to the description are omitted in order to clearly explain the present invention, and the size and thickness of each component shown in the drawings are arbitrarily shown for convenience of explanation, so the present invention is not necessarily limited by the drawings. Furthermore, components having the same function within the same concept may be described using the same reference numerals. Furthermore, throughout the specification, when a part "includes" a certain component, it does not mean that the part excludes other components, but that the part may further include other components, unless otherwise specified to the contrary.

[0016] In the drawings, the first direction may be defined as a direction in which the first and second internal electrodes are alternately arranged with a dielectric layer therebetween, or a thickness (T) direction, and among the second and third directions perpendicular to the first direction, the second direction may be defined as a length (L) direction and the third direction may be defined as a width (W) direction.

[0017] FIG. 1 is a perspective view of a multilayer electronic component according to an embodiment of the present invention, FIG. 2 is a cross-sectional view taken along line I-I' in FIG. 1, FIG. 3 is a cross-sectional view taken along line II-II' in FIG. 1, FIG. 4 is an exploded perspective view showing a structure in which internal electrodes, dielectric layers and a cover part are arranged according to an embodiment, FIG. 5 is an enlarged view of region P in FIG. 3, (a), (b) and (c) in FIG. 6 are graphs showing changes in average core-shell size depending on the content of additive according to an embodiment, (a), (b) and (c) in FIG. 7 are graphs showing changes in dielectric constant, capacitance and quality factor depending on the content of additive according to an embodiment, and FIG. 8 is a graph showing changes in temperature-capacity characteristics depending on the content of additive according to an embodiment.

[0018] Hereinafter, a multilayer electronic component according to an embodiment of the present invention and various embodiments thereof will be described in detail with reference to FIGS.

[0019] A multilayer electronic component 100 according to an embodiment of the present invention includes a body 110 including a dielectric layer 111 and internal electrodes 121, 122 arranged alternately with the dielectric layer sandwiched therebetween, and external electrodes 131, 132 arranged on the body, the dielectric layer including a main component including calcium (Ca), strontium (Sr), zirconium (Zr) and titanium (Ti) and a sub-component including manganese (Mn), yttrium (Y) and silicon (Si), the dielectric layer including a plurality of dielectric crystal grains 20 and crystal grain boundaries 30 arranged between adjacent dielectric crystal grains, at least a portion of the plurality of dielectric crystal grains having a core-shell structure, in which, when the content of yttrium (Y) contained in the core relative to 100 moles of zirconium (Zr) contained in the core and shell is Yc and the content of yttrium (Y) contained in the shell relative to 100 moles of zirconium (Zr) contained in the core and shell is Ys, Ys / Yc>9 can be satisfied.

[0020] A multilayer electronic component 100 according to one embodiment of the present invention includes a body 110 including a dielectric layer 111 and internal electrodes 121, 122 arranged alternately on either side of the dielectric layer, and external electrodes 131, 132 arranged on the body.

[0021] There is no particular limitation on the specific shape of the body 110, but the body 110 may be hexahedral or a similar shape as shown in Figures 1 to 3. Due to shrinkage of the ceramic material contained in the body 110 during the firing process, the body 110 may not be a hexahedral shape with perfectly straight edges, but may be substantially hexahedral.

[0022] The main body 110 may include first and second surfaces 1, 2 facing each other in a first direction, third and fourth surfaces 3, 4 connected to the first and second surfaces 1, 2 and facing each other in the second direction, and fifth and sixth surfaces 5, 6 connected to the first and second surfaces 1, 2, connected to the third and fourth surfaces 3, 4, and facing each other in the third direction.

[0023] The multiple dielectric layers 111 forming the body 110 are in a fired state, and the boundaries between adjacent dielectric layers 111 can be integrated to such an extent that they are difficult to see without the use of a scanning electron microscope (SEM).

[0024] The raw material for forming the dielectric layer 111 can be varied depending on the purpose. Specifically, ferroelectric BaTiO3 can be used as the material for the main purpose of achieving a high capacitance per unit volume, and paraelectric CaZrO3 can be used as the material for the main purpose of improving reliability in high temperature environments. Examples of BaTiO3-based materials include BaTiO3, BaTiO3 partially solid-dissolved with Ca (calcium), Zr (zirconium), etc. (Ba 1-x Ca x )TiO3(0 <x<1)、Ba(Ti 1-y Ca y )O3(0 <y<1)、(Ba 1-x Ca x )(Ti 1-y Zry ) O3 (0 < x < 1, 0 < y < 1) or Ba(Ti 1-y Zr y ) O3 (0 < y < 1), etc. Examples of the material of the CaZrO3 substrate include (Ca 1-x Sr x )(Zr 1-y Ti y ) O3 (0 < x < 1, 0 < y < 1).

[0025] On the other hand, in one embodiment of the present invention and these various embodiments, when forming the dielectric layer 111 using the material of the CaZrO3 substrate, various examples for ensuring the optimum quality factor (Q, Quality factor), capacitance, BDV characteristics, and capacitance-temperature characteristics will be described. That is, the dielectric layer 111 according to one embodiment of the present invention contains a main component including calcium (Ca), strontium (Sr), zirconium (Zr), and titanium (Ti).

[0026] The average thickness td of the dielectric layer 111 is not particularly limited.

[0027] For the purpose of miniaturization and high capacitance of the multilayer electronic component 100, the average thickness td of the dielectric layer 111 after firing can be 2.5 μm or less, and for improving the reliability of the multilayer electronic component 100 under high temperature and high pressure, the average thickness td of the dielectric layer 111 after firing can be 3.0 μm or more.

[0028] The average thickness td of the dielectric layer 111 can mean the average thickness of the dielectric layer 111 disposed between the first and second internal electrodes 121 and 122.

[0029] Similar to the thickness te of the internal electrode, the average thickness td of the dielectric layer 111 can also be measured by scanning an image of the cross-section (L-T cross-section) of the main body 110 in the third and first directions using a scanning electron microscope (SEM, Scanning Electron Microscope).

[0030] For example, the average thickness td of the dielectric layer 111 may be calculated by measuring the thickness of each of the dielectric layers extracted from an image obtained by scanning a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM), and measuring the average thickness of each of the dielectric layers extracted from the image obtained by scanning a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM). The average thickness td of the dielectric layer 111 may be calculated by measuring the thickness of each of the dielectric layers extracted from the image obtained by scanning a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM), and measuring the average thickness of each of the dielectric layers extracted from the image obtained by scanning a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM).

[0031] The internal electrodes 121 and 122 are arranged alternately with the dielectric layer 111 interposed therebetween.

[0032] The internal electrodes 121, 122 may include first and second internal electrodes 121, 122. The first and second internal electrodes 121, 122 are alternately arranged to face each other with the dielectric layer 111 constituting the body 110 interposed therebetween, and may be exposed at third and fourth surfaces 3, 4 of the body 110, respectively.

[0033] Referring to FIG. 2, the first internal electrode 121 may be spaced apart from the fourth surface 4 and exposed through the third surface 3, and the second internal electrode 122 may be spaced apart from the third surface 3 and exposed through the fourth surface 4.

[0034] At this time, the first and second internal electrodes 121 and 122 may be electrically isolated from each other by the dielectric layer 111 disposed therebetween.

[0035] Referring to FIG. 4, the body 110 may be formed by alternately stacking ceramic green sheets on which the first internal electrodes 121 are printed and ceramic green sheets on which the second internal electrodes 122 are printed, and then firing the stacked ceramic green sheets.

[0036] There are no particular limitations on the material forming the internal electrodes 121 and 122, and any material having excellent electrical conductivity can be used. For example, the internal electrodes 121 and 122 can be formed by printing a conductive paste for internal electrodes containing one or more of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof on a ceramic green sheet.

[0037] The method for printing the conductive paste for the internal electrodes may be a screen printing method or a gravure printing method, but the present invention is not limited thereto.

[0038] The average thickness te of the internal electrodes 121, 122 is not particularly limited and may vary depending on the purpose. In order to reduce the size of the multilayer electronic component 100, the average thickness te of the internal electrodes 121, 122 may be 0.1 μm or more and 2.5 μm or less, and in order to improve the reliability of the multilayer electronic component 100 under high temperature and high pressure, the average thickness te of the internal electrodes 121, 122 may be 0.1 μm or more and 2.5 μm or less, or 0.1 μm or more and 5.0 μm or less.

[0039] The average thickness te of the internal electrodes 121 and 122 may be calculated by measuring the thickness of each of the internal electrode layers extracted from an image obtained by scanning a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM), and then measuring the average thickness of each of the internal electrodes 121 and 122. The average thickness te of the internal electrodes 121 and 122 may be calculated by measuring the thickness of each of the internal electrode layers extracted from an image obtained by scanning a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM), and then measuring the average thickness of each of the internal electrode layers extracted from the image obtained by scanning a cross section of the body 110 in the length and thickness direction (LT) using a scanning electron microscope (SEM), and ...).

[0040] Meanwhile, referring to FIG. 2, the body 110 may include a capacitance forming portion Ac in which a capacitance is formed, the capacitance forming portion Ac including a first internal electrode 121 and a second internal electrode 122 arranged to face each other across a dielectric layer 111, and cover portions 112 and 113 formed on the upper and lower parts of the capacitance forming portion Ac.

[0041] The capacitance forming portion Ac is a portion that contributes to forming the capacitance of the capacitor, and may be formed by repeatedly laminating a plurality of first and second internal electrodes 121, 122 with the dielectric layer 111 interposed therebetween.

[0042] The upper cover part 112 and the lower cover part 113 may be formed by stacking a single dielectric layer or two or more dielectric layers on the upper and lower surfaces of the capacitance forming part Ac in the thickness direction, respectively, and may basically serve to prevent damage to the internal electrodes due to physical or chemical stress.

[0043] The upper cover part 112 and the lower cover part 113 do not include an internal electrode and may include the same material as the dielectric layer 111 .

[0044] There is no particular limitation on the average thickness tc of the covers 112, 113. In order to achieve a smaller size and higher capacity of the multilayer electronic component, the average thickness tc of the covers 112, 113 may have a value of 15 μm or less.

[0045] The average thickness tc of the cover parts 112, 113 may mean the size in the first direction, and may be the average value of the size in the first direction of the cover parts 112, 113 measured at five equally spaced points on the upper or lower part of the capacitance forming part Ac.

[0046] Moreover, margin portions 114 and 115 can be disposed on the side surfaces of the capacitance forming portion Ac.

[0047] The margin portions 114, 115 include a margin portion 114 disposed on the sixth surface 6 of the body 110 and a margin portion 115 disposed on the fifth surface 5. That is, the margin portions 114, 115 may be disposed on both side surfaces of the ceramic body 110 in the width direction.

[0048] The margin portions 114, 115 may refer to the regions between both ends of the first and second internal electrodes 121, 122 and the boundary surface of the body 110 in a cross section of the body 110 cut in the width-thickness (WT) direction, as shown in FIG. 3.

[0049] The margins 114 and 115 essentially serve to prevent damage to the internal electrodes due to physical or chemical stress.

[0050] The margin portions 114 and 115 may be formed by applying a conductive paste to the ceramic green sheet except for the areas where the margin portions are to be formed, to form internal electrodes.

[0051] In addition, in order to suppress steps caused by the internal electrodes 121, 122, after lamination, the internal electrodes can be cut so as to be exposed on the fifth and sixth faces 5, 6 of the main body, and then a single dielectric layer or two or more dielectric layers can be laminated in the width direction on both side faces of the capacitance forming portion Ac to form margin portions 114, 115.

[0052] On the other hand, there is no need to particularly limit the width of the marginal portions 114, 115. However, in order to more easily achieve a smaller size and higher capacity of the multilayer electronic component, the average width of the marginal portions 114, 115 can be 15 μm or less.

[0053] The average width of the margin portions 114, 115 may mean the average size of the margin portions 114, 115 in the third direction, and may be the average value of the sizes of the margin portions 114, 115 in the third direction measured at five equally spaced points on the side of the capacitance forming portion Ac.

[0054] External electrodes 131 and 132 are disposed on the body 110 .

[0055] The outer electrodes 131 and 132 are disposed on the body 110 and are connected to the inner electrodes 121 and 122 .

[0056] As shown in FIG. 2, the first and second external electrodes 131 and 132 may be disposed on the third and fourth surfaces 3 and 4 of the body 110, respectively, and connected to the first and second internal electrodes 121 and 122, respectively.

[0057] In this embodiment, the ceramic electronic component 100 has a structure including two external electrodes 131, 132. However, the number and shapes of the external electrodes 131, 132 may vary depending on the shape of the internal electrodes 121, 122 and other purposes.

[0058] Meanwhile, the external electrodes 131 and 132 may be formed using any material that has electrical conductivity, such as a metal, and the specific material may be determined taking into consideration electrical characteristics, structural stability, etc., and may further have a multi-layer structure.

[0059] For example, the external electrodes 131 and 132 may include an electrode layer disposed on the body 110 and a plating layer formed on the electrode layer.

[0060] More specifically, the electrode layer may be a fired electrode containing a conductive metal and glass, or a resin-based electrode containing a conductive metal and resin.

[0061] Also, the electrode layer may be in a form in which a fired electrode and a resin-based electrode are sequentially formed on the body 110. Also, the electrode layer may be formed by transferring a sheet including a conductive metal onto the body 110, or by transferring a sheet including a conductive metal onto the fired electrode.

[0062] The conductive metal contained in the electrode layer may be a material having excellent electrical conductivity, and is not particularly limited. For example, the conductive metal may be one or more of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof.

[0063] The plating layer may be a plating layer containing one or more of nickel (Ni), tin (Sn), palladium (Pd) and alloys thereof, and may be formed of a plurality of layers.

[0064] More specifically, the plating layer may be a Ni plating layer or a Sn plating layer, and may be a form in which a Ni plating layer and a Sn plating layer are sequentially formed on an electrode layer, or a form in which a Sn plating layer, a Ni plating layer and a Sn plating layer are sequentially formed. Also, the plating layer may include a plurality of Ni plating layers and / or a plurality of Sn plating layers.

[0065] In one embodiment, the dielectric layer 111 may be formed by adding additives in addition to the main component including the CaZrO3-based material. Specifically, the additives may have a composition ratio of CaZrO3 100 moles, Mn3O2: 0.98 moles (relative to CaZrO3 100 moles), Y2O3: 1.225 moles (relative to CaZrO3 100 moles), and SiO2: 1.47 moles (relative to CaZrO3 100 moles) before sintering, but are not limited thereto. The composition ratio of the additives may change after sintering the body 110 and the external electrodes 131 and 132, and the sintered dielectric layer 111 may include main components including calcium (Ca), strontium (Sr), zirconium (Zr), and titanium (Ti) and subcomponents including manganese (Mn), yttrium (Y), and silicon (Si).

[0066] Manganese (Mn) can play a role in suppressing the movement of oxygen vacancies in the dielectric layer 111, yttrium (Y) can play a role in reducing the concentration of oxygen vacancies by acting as a donor at the A-site of the ABO3 structure, and silicon (Si) can play a role in lowering the sintering temperature of the dielectric layer 111 and promoting sinterability by reacting with one or more of the other elements contained in the dielectric layer 111.

[0067] In one embodiment of the present invention, the dielectric layer 111 containing main components including calcium (Ca), strontium (Sr), zirconium (Zr), and titanium (Ti) further contains sub-components including manganese (Mn), yttrium (Y), and silicon (Si). This makes it possible to suppress the migration and concentration of oxygen vacancies in the dielectric layer 111 and improve the insulation resistance, thereby improving the reliability of the laminated electronic component 100.

[0068] In this case, in one embodiment, the content of manganese (Mn) contained in the dielectric crystal grains 20 may be 2.68 mol or more and 2.83 mol or less with respect to 100 mol of zirconium (Zr) contained in the dielectric crystal grains.

[0069] In one embodiment, the content of manganese (Mn) contained in the dielectric crystal grains 20 can be 2.68 mol or more and 2.83 mol or less with respect to 100 mol of zirconium (Zr) contained in the dielectric crystal grains.

[0070] In one embodiment, the content of yttrium (Y) contained in the dielectric crystal grains 20 can be 2.26 mol or more and 3.33 mol or less with respect to 100 mol of zirconium (Zr) contained in the dielectric crystal grains.

[0071] In this manner, by appropriately adjusting the content of the minor components contained in the dielectric crystal grains, the migration and concentration of oxygen vacancies in the dielectric layer 111 can be suppressed to improve the insulation resistance, and a high sintering density can be achieved even at a low firing temperature, minimizing the deterioration of the quality factor (Q) and temperature coefficient of capacitance (TCC) of the multilayer electronic component 100, while improving the breakdown voltage (BDV).

[0072] However, the components contained in the dielectric layer 111 are not limited to the above main and sub-components. The dielectric layer 111 may further include one or more of aluminum (Al), magnesium (Mg) and oxides thereof to improve sintering characteristics, and may further include one or more of hafnium (Hf), dysprosium (Dy), holmium (Ho), erbium (Er), terbium (Tb), vanadium (V) and oxides thereof to further improve reliability.

[0073] Meanwhile, the capacitance characteristics, reliability and temperature-capacitance characteristics may be changed depending on the microstructure of the dielectric layer 111 of the present invention, and the microstructure of the dielectric layer 111 may be changed depending on the concentration of the additive described above. However, changing the concentration of the additive may not be the only means for controlling the microstructure of the dielectric layer 111 described below, and the microstructure of the dielectric layer 111 may be controlled through various means such as the firing temperature, atmosphere, etc. Hereinafter, various microstructures of the dielectric layer 111 according to an embodiment will be described in detail.

[0074] Referring to FIG. 5 , in one embodiment of the present invention, the dielectric layer 111 includes a plurality of dielectric crystal grains 20 and grain boundaries 30 disposed between adjacent dielectric crystal grains 20, and at least a portion of the plurality of dielectric crystal grains 20 may have a core 21-shell 22 structure.

[0075] The average content of minor elements, including manganese (Mn), yttrium (Y), and silicon (Si), may be higher in the shell 22 than in the core 21 .

[0076] The criteria for distinguishing the core 21 and the shell 22 may be as follows. When a line profile is taken along a straight line passing through the center point of the dielectric crystal grain 20, the content of a specific element may suddenly change at any point inside the dielectric crystal grain 20. Based on the center of the region where the sudden change occurs, the region where the content of the specific element is low may be defined as the core 21, and the region where the content of the specific element is high may be defined as the shell 22.

[0077] In one embodiment of the present invention, the core 21 and the shell 22 can be defined based on the content of yttrium (Y). Specifically, when the content of yttrium (Y) contained in the core relative to 100 moles of zirconium (Zr) contained in the core and shell is Yc, and the content of yttrium (Y) contained in the shell relative to 100 moles of zirconium (Zr) contained in the core and shell is Ys, Ys / Yc>9 can be satisfied. Meanwhile, since yttrium (Y) can be substantially contained only in the shell, the upper limit of Ys / Yc is not particularly limited.

[0078] Meanwhile, the capacitance and quality factor (Q) of the multilayer electronic component 100 may vary depending on the specific gravity of the core 21 and the shell 22 in the dielectric crystal grains 20. As a result of an experimental example described below, the ratio of the average size of the core 21 and the shell 22 to the average size of the core 21 that can ensure appropriate dielectric constant, capacitance, and quality factor (Q) may be in the range of 2 to 2.57. That is, in one embodiment, the capacitance characteristic and quality factor (Q) of the multilayer electronic component 100 can be improved by adjusting the ratio of the average size of the core 21 and the shell 22 to the average size of the core 21 to 2 to 2.57.

[0079] Meanwhile, the average size of the core 21 may mean a value obtained by dividing the sum of the minor axis and major axis of the core 21 by 2, and the average size of the core 21 and the shell 22 may mean a value obtained by dividing the sum of the minor axis and major axis of the core 21 and the shell 22 by 2. In addition, the average size of the core 21 and the shell 22 may mean an average size of the dielectric crystal grains 20, and may mean a value obtained by dividing the sum of the minor axis and major axis of the dielectric crystal grains 20 by 2.

[0080] One example of measuring the ratio of the average size of core 21 and shell 22 to the average size of core 21 is to analyze the composition of a 2.68 μm x 2.68 μm region of dielectric layer 111 located in the center of the capacitance forming portion in a cross section in the first and third directions polished to the center in the second direction of multilayer electronic component 100 by TEM-EDS (Transmission Electron Microscope-Energy Dispersive Spectroscopy) analysis, and the point where the Y content changes abruptly is taken as the boundary between core 21 and shell 22, and the minor and major axes of core 21 and shell 22 are measured.

[0081] In one embodiment, a secondary phase 40 may be disposed in at least a portion of the grain boundaries 30. When the secondary phase 40 is disposed in at least a portion of the grain boundaries 30, the insulation resistance of the dielectric layer 111 may be improved, and thus the breakdown voltage (BDV) of the multilayer electronic component 100 may be improved.

[0082] The type of elements contained in the secondary phase 40 may vary depending on conditions such as the components of the dielectric layer 111 and the firing temperature. In one embodiment, the secondary phase 40 may include calcium (Ca), strontium (Sr), yttrium (Y), and silicon (Si), which may further improve the breakdown voltage (BDV) of the multilayer electronic component 100.

[0083] Meanwhile, silicon (Si) may be substantially only contained in the secondary phase 40, and may not be substantially contained in the grain boundaries 30 and the crystal grains 20 except for the region where the secondary phase 40 is formed. However, the content of the Si element in the grain boundaries 30 and the crystal grains 20 except for the region where the secondary phase 40 is formed may be measured at a noise level by a measurement method. For example, the content of silicon (Si) contained in the region except for the region where the secondary phase is formed may be 0.05 at% or less with respect to the total content of all elements except oxygen (O).

[0084] Meanwhile, as the specific gravity of the secondary phase 40 in the dielectric layer 111 increases, the quality factor (Q) and temperature coefficient of capacitance (TCC) may decrease. Specifically, as the area fraction of the secondary phase 40 in the dielectric layer 111 increases, the breakdown voltage (BDV) may improve, but if it exceeds 3%, the quality factor (Q) and temperature coefficient of capacitance (TCC) may decrease. Therefore, in one embodiment, the area fraction of the secondary phase 40 in the dielectric layer 111 may be 3% or less, and more preferably 2.57% or less.

[0085] Although there is no particular lower limit to the area fraction of the dielectric layer 111 occupied by the secondary phase 40, it is preferable that the area fraction of the dielectric layer 111 occupied by the secondary phase 40 be 2.27% or more in order to obtain a sufficient improvement effect in the breakdown voltage (BDV).

[0086] That is, in one embodiment, the area fraction of the secondary phase 40 in the dielectric layer 111 may be 2.27% or more and 2.57% or less, thereby minimizing the degradation of the quality factor (Q) and temperature coefficient of capacitance (TCC) of the multilayer electronic component 100 and improving the breakdown voltage (BDV).

[0087] In addition to the area fraction of the dielectric layer 111 occupied by the secondary phase 40, the average area of ​​the secondary phase 40 may also cause changes in the quality factor (Q), temperature coefficient of capacitance (TCC), and breakdown voltage (BDV) characteristics of the multilayer electronic component 100. That is, in one embodiment, the dielectric layer 111 may include a plurality of secondary phases 40, and the average area of ​​the plurality of secondary phases 40 may be 0.104 μm 2 More than 0.170μm 2 As a result, it is possible to minimize the degradation of the quality factor (Q) and the temperature coefficient of capacitance (TCC) of the multilayer electronic component 100, and at the same time, improve the breakdown voltage (BDV).

[0088] As an example of measuring the area fraction of the secondary phase 40 in the dielectric layer 111 and the average area of ​​the plurality of secondary phases 40, a method of mapping silicon (Si) elements in a 10.82 μm×10.82 μm region of the dielectric layer located at the center of a capacitance forming portion in a cross section in the first and third directions polished to the center in the second direction of the multilayer electronic component 100, using a transmission electron microscope-energy dispersive spectroscopy (TEM-EDS), and then calculating the area of ​​each region using an image analysis program (ImageJ) can be given. In this case, the area fraction of the secondary phase 40 in the dielectric layer 111 can be calculated as a ratio of the region where the secondary phase 40 is formed to the entire area of ​​the measured image, and the average area of ​​the plurality of secondary phases 40 can mean an average value of the areas of any five or more secondary phases 40.

[0089] In the case of a multilayer electronic component 100 including a dielectric layer 111 containing a main component including calcium (Ca), strontium (Sr), zirconium (Zr) and titanium (Ti) as in one embodiment of the present invention, the dielectric constant of the dielectric layer 111 is more significantly affected by the sintering density than by the average grain size of the dielectric crystal grains. That is, a high sintering density can be achieved at a low sintering temperature without excessively adjusting the average grain size of the dielectric crystal grains 20, thereby improving the dielectric constant. Specifically, in one embodiment, the average grain size of the dielectric crystal grains 20 may be 444 nm or more and 506 nm or less.

[0090] In the following, we define "100% additive" as the case where 100 moles of CaZrO3, 0.980 moles of Mn3O2, 1.225 moles of Y2O3, and 1.470 moles of SiO2 were added, and we will provide a detailed explanation of various experimental examples in which the amount of additive was varied.

[0091] In all experimental examples described below, powders for forming dielectric layers with different additive contents were mixed with a dispersant using ethanol and toluene as solvents, and then a binder was added to produce ceramic sheets. Ni electrodes were printed and stacked on the molded ceramic sheets, and the chips that were crimped and cut were pre-fired in an air atmosphere at 400°C or less, and then fired for about 1 hour at about 1,300°C or less with a hydrogen (H2) concentration of 7.0% or less. A termination process and electrode firing were then performed using copper (Cu) paste to complete the multilayer electronic component 100.

[0092] (Experimental Example 1) Table 1 shows the results of measuring the content of elements contained in dielectric layer 111 in multilayer electronic components 100 formed with different additive content.

[0093] The content of each element corresponds to a relative value based on 100 moles of zirconium (Zr) contained in the core and shell.

[0094] The element contents in Table 1 were measured by TEM-EDS (Transmission Electron Microscope-Energy Dispersive Spectroscopy) analysis of a 2.68 μm × 2.68 μm region of the dielectric layer located at the center of the capacitance forming portion in a cross section in the first and third directions polished to the center in the second direction of the multilayer electronic component 100 using a 200 kV transmission electron microscope (TEM) at a magnification of 40,000 times.

[0095] [Table 1]

[0096] Referring to Table 1, it can be seen that the secondary phase contains calcium (Ca), strontium (Sr), yttrium (Y) and silicon (Si). In particular, it can be seen that silicon (Si) is substantially only contained in the secondary phase 40.

[0097] Regarding the manganese (Mn) content, it can be confirmed that the manganese (Mn) content contained in the dielectric crystal grains with 100% additive is 2.68 mol per 100 mol of zirconium (Zr) contained in the dielectric crystal grains, and the manganese (Mn) content contained in the dielectric crystal grains with 140% additive is 2.83 mol per 100 mol of zirconium (Zr) contained in the dielectric crystal grains.

[0098] Regarding the content of yttrium (Y), it can be confirmed that the content of yttrium (Y) contained in the dielectric crystal grains when the additive is 100% is 2.26 moles per 100 moles of zirconium (Zr) contained in the dielectric crystal grains, and the content of yttrium (Y) contained in the dielectric crystal grains when the additive is 140% is 3.33 moles per 100 moles of zirconium (Zr) contained in the dielectric crystal grains.

[0099] (Experimental Example 2) Table 2 shows the results of measuring the microstructure of the dielectric layer 111 and evaluating the characteristics thereof for the multilayer electronic components 100 formed with different additive contents.

[0100] The average size of the core is represented by d1, and the average size of the core and shell (average size of the dielectric crystal grains) is represented by d2. In a cross section in the first and third directions polished to the center in the second direction of the laminated electronic component 100, a 2.68 μm × 2.68 μm region of the dielectric layer 111 located in the center of the capacitance forming portion was analyzed for composition by TEM-EDS (Transmission Electron Microscope-Energy Dispersive Spectroscopy) analysis, and the point where the Y content changes suddenly was determined to be the boundary between the core 21 and the shell 22. The sum of the short axis and long axis of the core 21 divided by 2 was determined to be d1, and the sum of the short axis and long axis of the dielectric crystal grains 20 divided by 2 was determined to be d2.

[0101] The room temperature capacitance and quality factor of the chip were calculated by averaging the capacitance values ​​measured for a total of 20 samples using an LCR meter at 1 kHz and 1.0 V. The dielectric constant was calculated from the measured capacitance and dielectric thickness. The BDV was measured for 20 samples at 25°C and 400 V / s boost, and the voltage value at the moment the current value reached 10 mA was measured as the BDV value and the average value was calculated.

[0102] [Table 2]

[0103] Referring to Table 2 and FIG. 6, it can be seen that as the additive content increases, the specific gravity of the shell in the dielectric crystal grains tends to decrease, and the specific gravity of the core in the dielectric crystal grains increases up to 'additive 140%' and then tends to decrease.

[0104] Meanwhile, referring to Table 2 and FIG. 7, it can be seen that the quality factor tends to decrease as the additive content increases. In particular, the dielectric constant and capacitance tend to decrease when the additive content exceeds 140%.

[0105] Meanwhile, referring to Table 2, it can be seen that the dielectric breakdown voltage (BDV) tends to improve as the content of the additive increases.

[0106] Taking the results of Tables 1 and 2 together, the content of the additive that can simultaneously improve the capacitance, dielectric constant, quality factor, and BDV of the multilayer electronic component 100 can be in the range of "additive 100%" or more and "additive 140%" or less.

[0107] At this time, the range of "100% additive" or more and "140% additive" or less can be expressed by the content of a specific element in the dielectric layer 111 after firing according to Table 1. For example, in one embodiment, the content of manganese (Mn) contained in the dielectric crystal grains can be 2.68 mol or more and 2.83 mol or less per 100 mol of zirconium (Zr) contained in the dielectric crystal grains, or the content of yttrium (Y) contained in the dielectric crystal grains can be 2.26 mol or more and 3.33 mol or less per 100 mol of zirconium (Zr) contained in the dielectric crystal grains.

[0108] (Experimental Example 3) Table 3 shows cross sections in the first and third directions of multilayer electronic components 100 with different additive contents, polished to the center in the second direction, in which silicon (Si) elements were mapped in a 10.82 μm×10.82 μm region of the dielectric layer located in the center of the capacitance forming portion using a Transmission Electron Microscope-Energy Dispersive Spectroscopy (TEM-EDS), and then the area fraction occupied by the secondary phase 40 and the average area of ​​a plurality of secondary phases 40 were measured using an image analysis program (ImageJ). Since silicon (Si) elements were substantially only disposed in the secondary phase 40, the region in the dielectric layer 111 where silicon (Si) elements were relatively concentrated was determined to be the region where the secondary phase 40 was formed.

[0109] In this case, the area fraction of the secondary phase 40 in the dielectric layer 111 was calculated as the ratio of the area in which the secondary phase 40 was formed to the total area of ​​the measured image, and the average area of ​​the multiple secondary phases 40 was calculated as the average value of the areas of any five or more secondary phases 40.

[0110] [Table 3]

[0111] Considering the results of Tables 2 and 3, the range of "100% additive" to "140% additive" can be expressed by a parameter related to the area of ​​the secondary phase 40. Specifically, in one embodiment, the area fraction of the dielectric layer occupied by the secondary phase is 2.27% to 2.57%, or the average area of ​​the plurality of secondary phases is 0.104 μm 2 More than 0.170μm 2 It can be the following:

[0112] (Experimental Example 4) Referring to FIG. 8, it can be seen that as the additive content increases, the temperature coefficient of capacitance (TCC) increases, but in the range of "100% additive" to "180% additive," the COG characteristic of less than 30 ppm / ℃ is met at -55 to 125℃.

[0113] However, it can be seen that the temperature coefficient of capacitance (TCC) characteristics are superior in the range of "100% additive" to "140% additive."

[0114] The size of the multilayer electronic component 100 does not need to be particularly limited.

[0115] In order to simultaneously achieve miniaturization and high capacity, the multilayer electronic component 100 may have a size of 0201 (length x width, 0.2 mm x 0.1 mm) or less, and in the case of a product in which reliability in a high temperature and high pressure environment is important, the multilayer electronic component 100 may have a size of 3225 (length x width, 3.2 mm x 2.5 mm) or more, but is not limited to this.

[0116] Here, the length of the multilayer electronic component 100 may refer to the maximum size of the multilayer electronic component 100 in the second direction, and the width of the multilayer electronic component 100 may refer to the maximum size (W) of the multilayer electronic component in the third direction.

[0117] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to the above-described embodiments and the accompanying drawings, but is limited by the scope of the accompanying claims. Therefore, various substitutions, modifications, and changes can be made by a person having ordinary knowledge in the art within the scope of the technical idea of ​​the present invention described in the claims, and these also belong to the scope of the present invention.

[0118] In addition, the expression "one embodiment" used in the present disclosure does not mean the same embodiment, but is provided to emphasize and describe each unique feature that is different from the others. However, the above-mentioned embodiment does not exclude being realized in combination with the features of another embodiment. For example, even if a matter described in a specific embodiment is not described in another embodiment, it can be understood as a description related to the other embodiment, unless there is a description that is opposite or contradictory to the matter in the other embodiment.

[0119] The terms used in the present disclosure are merely used to describe one embodiment and are not intended to limit the present disclosure. In this case, a singular expression includes a plural expression unless the context clearly indicates otherwise. [Explanation of symbols]

[0120] 100 Multilayer electronic components 110 Main unit 111 Dielectric layer 112, 113 Cover part 114, 115 Margin 121, 122 Internal electrode 131, 132 External electrode

Claims

1. a body including a dielectric layer and internal electrodes arranged alternately on either side of the dielectric layer; an external electrode disposed on the body; The dielectric layer includes a main component including calcium (Ca), strontium (Sr), zirconium (Zr), and titanium (Ti), and a subcomponent including manganese (Mn), yttrium (Y), and silicon (Si), the dielectric layer includes a plurality of dielectric grains and grain boundaries disposed between adjacent dielectric grains, at least a portion of the plurality of dielectric grains having a core-shell structure; In the core-shell structure, when the content of yttrium (Y) contained in the core relative to 100 moles of zirconium (Zr) contained in the core and shell is Yc, and the content of yttrium (Y) contained in the shell relative to 100 moles of zirconium (Zr) contained in the core and shell is Ys, A multilayer electronic component that satisfies Ys / Yc>9.

2. The multilayer electronic component according to claim 1 , wherein a secondary phase is disposed in at least a portion of the crystal grain boundaries.

3. 3. The multilayer electronic component according to claim 2, wherein an area percentage of the dielectric layer occupied by the secondary phase is 2.27% or more and 2.57% or less.

4. The dielectric layer includes a plurality of the secondary phases, and the average area of ​​the plurality of secondary phases is 0.104 μm 2 More than 0.170 μm 2 3. The multilayer electronic component according to claim 2, wherein:

5. The laminated electronic component according to claim 2 , wherein the secondary phase comprises calcium (Ca), strontium (Sr), yttrium (Y) and silicon (Si).

6. 3. The multilayer electronic component according to claim 2, wherein a content of silicon (Si) contained in the region excluding the region in which the secondary phase is formed is 0.05 at % or less with respect to a total content of all elements excluding oxygen (O).

7. 2. The multilayer electronic component according to claim 1, wherein a content of manganese (Mn) contained in said dielectric crystal grains is 2.68 mol or more and 2.83 mol or less per 100 mol of zirconium (Zr) contained in said dielectric crystal grains.

8. 2. The multilayer electronic component according to claim 1, wherein a content of yttrium (Y) contained in said dielectric crystal grains is 2.26 mol or more and 3.33 mol or less per 100 mol of zirconium (Zr) contained in said dielectric crystal grains.

9. 2. The multilayer electronic component according to claim 1, wherein a ratio of an average size of the core and the shell to the average size of the core is 2 or more and 2.57 or less.

10. 2. The multilayer electronic component according to claim 1, wherein the average grain size of the dielectric crystal grains is 444 nm or more and 506 nm or less.

11. The laminated electronic component according to claim 1 , wherein the dielectric layer further includes one or more of aluminum (Al) and magnesium (Mg).

12. 2. The laminated electronic component according to claim 1, wherein the dielectric layer further comprises one or more of hafnium (Hf), dysprosium (Dy), holmium (Ho), erbium (Er), terbium (Tb), and vanadium (V).