Optical multilayer body and manufacturing method for the same, and smart window including the same
The laminate addresses uneven thickness and adhesion issues by forming a physical orientation structure on electrode layers without an alignment film, ensuring stable and flexible smart window performance.
Patent Information
- Application Number
- JP2024065362
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional variable transmittance optical laminates for vehicle windows suffer from uneven thickness and poor adhesion due to the inclusion of an alignment film, leading to product defects and reduced performance.
A variable transmittance optical laminate design that eliminates the alignment film by forming a physical orientation structure directly on the electrode layers using conductive polymers, with specific thickness and sheet resistance ranges, and optionally includes transparent conductive layers and other functional layers.
The laminate prevents defects from uneven thickness and poor adhesion, ensuring stable operation and improved bending characteristics, making it suitable for smart windows with adjustable light transmittance.
Smart Images

Figure 2024155789000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical laminate and a method for producing the same, and to a smart window including the same. [Background technology]
[0002] In general, external light blocking coating is often applied to the window glass of a vehicle or other means of transportation. However, the window glass of a conventional means of transportation has a fixed transmittance, and the external light blocking coating also has a fixed transmittance. Therefore, the windows of such conventional means of transportation have a fixed overall transmittance, which may lead to accidents. For example, if the overall transmittance is set low, there is no problem during the day when there is sufficient light in the surroundings, but there is a problem that the driver may have difficulty in properly checking the surroundings of the means of transportation at night when there is insufficient light in the surroundings. Alternatively, if the overall transmittance is set high, there is a problem that the driver may be dazzled during the day when there is sufficient light in the surroundings. Therefore, a variable transmittance optical laminate capable of changing the transmittance of light when a voltage is applied has been developed.
[0003] The variable transmittance optical laminate is driven by applying a voltage to drive the liquid crystal to change the transmittance, and the variable transmittance optical laminates developed to date generally include an alignment layer for imparting alignment to the liquid crystal compound to adjust the light transmittance.
[0004] For example, Japanese Patent Application Laid-Open No. 2018-010035 also discloses a light control film including an alignment film for imparting alignment to a liquid crystal compound provided in a liquid crystal layer.
[0005] However, when an alignment film is included to impart alignment to the liquid crystal compound, there are problems such as uneven thickness due to drying conditions of the alignment film or reduced adhesion between substrates, as well as damage to the substrate during plasma treatment of the substrate for coating the alignment film.
[0006] Therefore, there is a need to develop a variable transmittance optical laminate that can prevent uneven thickness or deterioration in appearance caused by the provision of an alignment layer. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Publication No. 2018-010035 Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to minimize product defects caused by uneven thickness or reduced adhesion due to the inclusion of an alignment film for imparting alignment to liquid crystal compounds.
[0009] However, the problems to be solved by the present invention are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]
[0010] The present invention relates to a variable transmittance optical laminate including a first polarizing plate, a first electrode layer formed on one surface of the first polarizing plate, a second polarizing plate facing the first polarizing plate, a second electrode layer formed on one surface of the second polarizing plate and facing the first electrode layer, and a liquid crystal layer provided between the first electrode layer and the second electrode layer, wherein the first electrode layer and the second electrode layer include a conductive polymer, and a physical orientation structure is formed by rubbing on at least a partial region of the first electrode layer and the second electrode layer.
[0011] In the first aspect of the present invention, the variable transmittance optical laminate may not include a separate alignment film.
[0012] In a second aspect of the present invention, the first electrode layer and the second electrode layer may have a thickness of 100 nm to 3,000 nm.
[0013] In a third aspect of the present invention, the first electrode layer and the second electrode layer may have a sheet resistance of 200 Ω / □ or less.
[0014] In a fourth aspect of the present invention, the first electrode layer and the second electrode layer may be produced from a composition for forming an electrode layer, the composition including: a conductive polymer; and one or more selected from the group consisting of an organic binder, an organic solvent, a silane coupling agent, and a surfactant.
[0015] In a fifth aspect of the present invention, the conductive polymer is selected from the group consisting of polythiophene, poly(3,4-ethylenedioxythiophene), polyaniline, polyacetylene, polydiacetylene, polyphenylene, polyphenylene vinylene, polyphenylene sulfide, polythienylene vinylene, polythiophene vinylene, polyfluorene, polypyrrole, poly(3,4-ethylenedioxythiophene):polystyrene sulfonate, poly(3,4-ethylenedioxythiophene):camphorsulfonic acid, poly(3,4-ethylenedioxythiophene):toluenesulfonic acid, poly(3 ,4-ethylenedioxythiophene):dodecylbenzenesulfonic acid, polyaniline:polystyrenesulfonate, polyaniline:camphorsulfonic acid, polypyrrole:polystyrenesulfonate, polypyrrole:camphorsulfonic acid, polypyrrole:toluenesulfonic acid, polypyrrole:dodecylbenzenesulfonic acid, polythiophene:polystyrenesulfonate, polythiophene:camphorsulfonic acid, polythiophene:toluenesulfonic acid, and polythiophene:dodecylbenzenesulfonic acid.
[0016] In a sixth aspect of the present invention, at least one of the first electrode layer and the second electrode layer may be formed in direct contact with either one of the first polarizing plate and the second polarizing plate.
[0017] In a seventh aspect, the present invention may include at least one transparent conductive layer: a first transparent conductive layer disposed between a first polarizer and a first electrode layer; and a second transparent conductive layer disposed between a second polarizer and a second electrode layer.
[0018] In an eighth aspect of the present invention, at least one of the first transparent conductive layer and the second transparent conductive layer may have a thickness of 100 nm to 1,000 nm.
[0019] In a ninth aspect of the present invention, at least one of the first transparent conductive layer and the second transparent conductive layer may contain one or more materials selected from the group consisting of transparent conductive oxides, metals, carbon-based materials, conductive inks, and nanowires.
[0020] In a tenth aspect of the present invention, at least one of the first polarizing plate and the second polarizing plate may include one or more functional layers selected from the group consisting of a protective layer, a phase difference adjusting layer, and a refractive index adjusting layer.
[0021] In an eleventh aspect of the present invention, at least one of the first polarizing plate and the second polarizing plate may have a thickness of 30 to 200 μm.
[0022] In a twelfth aspect of the present invention, the liquid crystal layer may include ball spacers.
[0023] In a thirteenth aspect of the present invention, the ball spacer may have a diameter of 1 to 10 μm.
[0024] In a fourteenth aspect of the present invention, an area of the ball spacers in the liquid crystal layer may be 0.01% to 10% of an area of the liquid crystal layer.
[0025] In a fifteenth aspect of the present invention, the variable transmittance optical laminate may further include one or more layers selected from the group consisting of an overcoat layer, an adhesive layer, an ultraviolet absorbing layer, and a hard coat layer.
[0026] The present invention also relates to a method for producing the variable transmittance optical laminate. The present invention also relates to a smart window comprising the variable transmittance optical laminate.
[0027] The present invention also relates to a means of transportation comprising said smart window. The present invention also relates to an automobile in which the smart window is applied to at least one of a front window, a rear window, a side window, a sunroof window, and an interior partition.
[0028] The present invention also relates to a wearable device or building fixture including the smart window. Effect of the Invention
[0029] The optical laminate according to the present invention does not include an alignment film, and therefore has the advantage that product defects due to uneven thickness or reduced adhesion caused by drying conditions of the alignment film do not occur. [Brief description of the drawings]
[0030] [Figure 1] FIG. 2 illustrates a stack structure of a variable transmittance optical stack according to one or more embodiments of the present invention. [Diagram 2] FIG. 2 illustrates a stack structure of a variable transmittance optical stack according to one or more embodiments of the present invention. [Diagram 3] FIG. 2 illustrates a stack structure of a variable transmittance optical stack according to one or more embodiments of the present invention. [Figure 4A]FIG. 2 is a diagram showing a stacked structure of a polarizing plate according to one or more embodiments of the present invention. [Figure 4B] FIG. 2 is a diagram showing a stacked structure of a polarizing plate according to one or more embodiments of the present invention. [Figure 4C] FIG. 2 is a diagram showing a stacked structure of a polarizing plate according to one or more embodiments of the present invention. [Figure 4D] FIG. 2 is a diagram showing a stacked structure of a polarizing plate according to one or more embodiments of the present invention. [Figure 4E] FIG. 2 is a diagram showing a stacked structure of a polarizing plate according to one or more embodiments of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] The present invention relates to a variable transmittance optical laminate that does not include an alignment film for imparting alignment to a liquid crystal compound, and therefore can prevent technical problems that may arise when an alignment film is included, such as product defects due to uneven thickness or reduced adhesion caused by drying conditions of the alignment film.
[0032] More specifically, the present invention relates to a variable transmittance optical laminate including a first polarizing plate, a first electrode layer formed on one surface of the first polarizing plate, a second polarizing plate facing the first polarizing plate, a second electrode layer formed on one surface of the second polarizing plate and facing the first electrode layer, and a liquid crystal layer provided between the first electrode layer and the second electrode layer, wherein the first electrode layer and the second electrode layer include a conductive polymer, and a physical orientation structure is formed on at least a portion of the first electrode layer and the second electrode layer by rubbing.
[0033] The variable transmittance optical laminate of the present invention is particularly suitable for technical fields in which light transmittance can be changed by applying a voltage, and can be used, for example, in smart windows.
[0034] A smart window is an optical structure that controls the amount of light or heat passing through by changing the light transmittance according to the application of an electrical signal. That is, a smart window can be changed to a transparent, opaque, or translucent state according to voltage, and is also called variable transmittance glass, light control glass, or smart glass.
[0035] A smart window can be used as a partition for dividing the interior space of a vehicle or building or for privacy, or as a light window placed in an opening of a building. It can also be used as a highway sign, bulletin board, scoreboard, clock or advertising screen, and can be used to replace glass in vehicles such as windows or sunroofs in cars, buses, airplanes, ships or trains.
[0036] The variable transmittance optical laminate of the present invention can also be used as a smart window in the various technical fields described above, but since the conductive layer is directly formed on the polarizing plate, no separate substrate is required for forming the conductive layer, and the thickness is thin and the bending characteristics are advantageous, so that the variable transmittance optical laminate of the present invention can be particularly suitably used as a smart window for vehicles or buildings. In one or more embodiments, the smart window to which the variable transmittance optical laminate of the present invention is applied can be used as a front window, rear window, side window, and sunroof window of an automobile, or a building fixture, and can be used not only for blocking external light, but also for dividing the interior space of an automobile or building, such as an interior partition, or for protecting privacy.
[0037] Hereinafter, the present invention will be described in more detail with reference to the drawings. However, the following drawings attached to this specification are for illustrating preferred embodiments of the present invention and serve to further understand the technical concept of the present invention together with the above-mentioned content of the invention, so the present invention should not be interpreted as being limited only to the matters described in the drawings.
[0038] The terms used in this specification are for the purpose of describing the embodiments and are not intended to limit the present invention. In this specification, the singular form includes the plural form unless otherwise specified in the text. For example, the term "polarizer" used in this specification means at least one polarizer of the first polarizer and the second polarizer, the term "electrode layer" means at least one electrode layer of the first electrode layer and the second electrode layer, and the term "transparent conductive layer" may mean at least one transparent conductive layer of the first transparent conductive layer and the second transparent conductive layer.
[0039] As used herein, the words "comprises" and "comprising" are used in a sense that does not exclude the presence or addition of one or more other components, steps, operations and / or elements other than the mentioned components, steps, operations and / or elements. The same reference numerals refer to the same components throughout the specification.
[0040] Spatially relative terms such as "below," "bottom," "lower," "upper," "top," "top" and the like can be used to readily describe the relationship of one element or component to another element or component as depicted in the drawings. Spatially relative terms should be understood in terms that include different orientations of elements in use or operation in addition to the orientation depicted in the drawings. For example, if an element depicted in the drawings is flipped over, an element described as "below" or "below" another element may be placed "above" the other element. Thus, the exemplary term "below" can include both an orientation of below and above. Elements can be oriented in other directions, whereby the spatially relative terms are interpreted accordingly.
[0041] As used herein, "planar direction" is interpreted as the thickness direction of the polarizer and / or electrode layer, ie, the direction viewed from the user's viewing side.
[0042] As used in this specification, "substantially" is interpreted to include not only something that is completely identical or coincident with the physical object, but also something that is within the range of error in measurement or manufacturing process, for example, an error range of 1% or less.
[0043] 1 to 3 are diagrams showing the layered structure of a variable transmittance optical laminate according to one or more embodiments of the present invention, and FIG. 4 is a diagram showing the layered structure of a polarizing plate according to one or more embodiments of the present invention.
[0044] 1 to 3, a variable transmittance optical stack according to one embodiment of the present invention may include a first polarizer 100-1, a second polarizer 100-2, a first electrode layer 200-1, a second electrode layer 200-2, and a liquid crystal layer 300, and may further include a transparent conductive layer 210 and / or an adhesive layer 400, as necessary.
[0045] 4, the polarizing plate 100 includes a polarizer 110, and may further include functional layers, such as a protective layer 120, a retardation adjustment layer 130, and a refractive index adjustment layer 140, on one or both sides of the polarizer 110. For example, the polarizing plate 100 may include a polarizer 110 and a protective layer 120 stacked on one or both sides of the polarizer 110 (see FIGS. 4A and 4B). Alternatively, the polarizing plate 100 may include a polarizer 110, a protective layer 120 stacked on one side of the polarizer 110, and a retardation adjustment layer 130 stacked on the other side of the polarizer 110 opposite to the one side (see FIG. 4C). Furthermore, it may include a polarizer 110, a protective layer 120 stacked on one side of the polarizer, and a phase difference adjusting layer 130 and a refractive index adjusting layer 140 stacked in sequence on the other side of the polarizer 110 opposite the one side (see Figure 4D), or it may include a polarizer 110, a protective layer 120 stacked on one side of the polarizer, and a protective layer 120 and a phase difference adjusting layer 130 stacked in sequence on the other side of the polarizer 110 opposite the one side (see Figure 4E).
[0046] The polarizer 110 may be any conventional or later developed polarizer, such as a stretched type polarizer or a coated type polarizer.
[0047] In one embodiment, the stretched polarizer may include a stretched polyvinyl alcohol (PVA)-based resin. The polyvinyl alcohol (PVA)-based resin may be a polyvinyl alcohol-based resin obtained by saponifying a polyvinyl acetate-based resin. Examples of the polyvinyl acetate-based resin include polyvinyl acetate, which is a homopolymer of vinyl acetate, and copolymers of vinyl acetate and other monomers copolymerizable therewith. The other monomers may be unsaturated carboxylic acid-based, unsaturated sulfonic acid-based, olefin-based, vinyl ether-based, and acrylamide-based monomers having an ammonium group. Furthermore, the polyvinyl alcohol (PVA)-based resin may be modified, for example, polyvinyl formal or polyvinyl acetal modified with aldehydes.
[0048] In one embodiment, the coating type polarizer is formed by a liquid crystal coating composition, which may include a reactive liquid crystal compound and a dichroic dye.
[0049] The reactive liquid crystal compound may refer to a compound that includes, for example, a mesogen skeleton and one or more polymerizable functional groups. Such reactive liquid crystal compounds are variously known as reactive mesogens (RMs). The reactive liquid crystal compounds can be polymerized by light or heat to form a cured film in which a polymer network is formed while maintaining the liquid crystal alignment.
[0050] The reactive liquid crystal compound may be a monofunctional or polyfunctional reactive liquid crystal compound. The monofunctional reactive liquid crystal compound is a compound having one polymerizable functional group, and the polyfunctional reactive liquid crystal compound is a compound having two or more polymerizable functional groups.
[0051] The dichroic dye is a component contained in the liquid crystal coating composition to impart polarization properties, and has a property that the absorbance in the long axis direction of the molecule is different from that in the short axis direction. The dichroic dye may be any dichroic dye that has been used or will be developed later, and may include at least one dye selected from the group consisting of azo dyes, anthraquinone dyes, perylene dyes, merocyanine dyes, azomethine dyes, phthaloperylene dyes, indigo dyes, dioxazine dyes, polythiophene dyes, and phenoxazine dyes.
[0052] The liquid crystal coating composition may further include a solvent for dissolving the reactive liquid crystal compound and the dichroic dye, and may include, for example, propylene glycol monomethyl ether acetate (PGMEA), methyl ethyl ketone (MEK), xylene, chloroform, etc. Also, the liquid crystal coating composition may further include a leveling agent, a polymerization initiator, etc., within a range that does not inhibit the polarization properties of the coating film.
[0053] The protective layer 120 serves to protect the polarization characteristics of the polarizer 110 from post-processing and external environments, and may be realized in the form of a protective film.
[0054] 4A and 4B, the protective layer 120 is formed on one or both sides of the polarizer 110 in direct contact therewith, but is not limited thereto. For example, the protective layer may be used in a multi-layer structure in which one or more protective layers are continuously stacked, or may be formed on one or both sides of another functional layer in direct contact therewith.
[0055] In one or more embodiments, the protective layer 120 may include one or more selected from the group consisting of polyethylene terephthalate (PET), polyethylene isophthalate (PEI), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), diacetyl cellulose (diacetyl cellulose), triacetyl cellulose (TAC), polycarbonate (PC), polyethylene (PE), polypropylene (PP), polymethyl acrylate (PMA), polymethyl methacrylate (PMMA), polyethyl acrylate (PEA), polyethyl methacrylate (PEMA), and cyclic olefin polymer (COP).
[0056] The retardation adjusting layer 130 is for compensating for the optical properties of the optical laminate and can be realized in the form of a retardation film, etc., and can be a conventional or later developed retardation film, etc. For example, a quarter wave plate (1 / 4 wave plate) or a half wave plate (1 / 2 wave plate) for delaying the phase of light can be used, and these can be used alone or in combination.
[0057] The retardation adjusting layer 130 is formed on one surface of the polarizer 110 in direct contact therewith as shown in Fig. 4C and Fig. 4D, but is not limited thereto. For example, as shown in Fig. 4E, the retardation adjusting layer 130 may be formed on one surface of the protective layer 120, and the polarizer 110, the protective layer 120, and the retardation adjusting layer 130 may be sequentially laminated.
[0058] The retardation adjusting layer 130 may be a polymer stretched film obtained by stretching a polymer film capable of imparting optical anisotropy by stretching in an appropriate manner, or a liquid crystal polymer film.
[0059] In one embodiment, the polymer stretched film may be a polymer layer including polyolefins such as polyethylene (PE) or polypropylene (PP), cycloolefin polymers (COP) such as polynorbornene, polyesters such as polyvinyl chloride (PVC), polyacrylonitrile (PAN), polysulfone (PSU), acrylic resins, polycarbonate (PC), and polyethylene terephthalate (PET), cellulose ester polymers such as polyacrylate, polyvinyl alcohol (PVA), and triacetyl cellulose (TAC), or copolymers of two or more monomers among the monomers forming the polymers.
[0060] The method for obtaining the polymer stretched film is not particularly limited, and for example, the polymer material can be formed into a film and then stretched. The method for forming the film is not particularly limited, and the film can be formed by known methods such as injection molding, sheet molding, blow molding, injection blow molding, inflation molding, extrusion molding, foam molding, and cast molding, and secondary processing molding methods such as compressed air molding and vacuum molding can also be used. Among them, extrusion molding and cast molding are preferably used. At this time, for example, an extruder equipped with a T-die, a circular die, or the like can be used to extrude the unstretched film. When obtaining a molded product by extrusion molding, a material in which various resin components, additives, etc. are melt-kneaded in advance may be used, or the product may be molded through melt-kneading during extrusion molding. In addition, the unstretched film may be cast molded by dissolving various resin components using a solvent common to the various resin components, such as chloroform or methylene dichloride, and then casting, drying, and solidifying the resin components.
[0061] The polymer stretched film may be produced by uniaxially stretching the formed film in the mechanical direction (MD; mechanical direction, lengthwise or longitudinal direction) or uniaxially stretching the formed film in the transverse direction (TD; transverse direction, widthwise or transverse direction) of the mechanical direction. Alternatively, a biaxially stretched film may be produced by stretching the formed film using a sequential biaxial stretching method of roll stretching and tenter stretching, a simultaneous biaxial stretching method using tenter stretching, a biaxial stretching method using tubular stretching, or the like.
[0062] The liquid crystal polymer film may include a reactive liquid crystal compound in a polymerized state. The reactive liquid crystal compound may be the same as that of the coating type polarizer.
[0063] In one or more embodiments, the thickness of the retardation adjusting layer 130 may be 10 μm to 100 μm in the case of a polymer stretched film, and 0.1 μm to 5 μm in the case of a liquid crystal polymer film.
[0064] The refractive index adjustment layer 140 is provided to compensate for the refractive index difference of the optical laminate caused by the electrode layer 200, and may play a role of improving visibility by reducing the refractive index difference. The refractive index adjustment layer 140 may also be provided to correct a hue caused by the electrode layer 200. Meanwhile, when the electrode layer has a pattern, the refractive index adjustment layer 140 can compensate for the transmittance difference between a patterned region where the pattern is formed and a non-patterned region where the pattern is not formed.
[0065] Specifically, the electrode layer 200 is stacked adjacent to another member (e.g., the polarizer 110, etc.) having a different refractive index from the electrode layer 200, and a difference in light transmittance may be induced due to the difference in refractive index with the adjacent layer, and in particular, when a pattern is formed on the electrode layer, a problem may occur in which the patterned region and the non-patterned region are visually distinguished. Therefore, by including the refractive index adjustment layer 140, the refractive index is compensated to reduce the difference in light transmittance of the optical laminate, and in particular, when a pattern is formed on the electrode layer, the patterned region and the non-patterned region are not visually distinguished.
[0066] In one embodiment, the refractive index of the refractive index adjusting layer 140 can be appropriately selected depending on the material of other adjacent members, and is preferably 1.4 to 2.6, and more preferably 1.4 to 2.4. In this case, it is possible to prevent light loss due to a sharp difference in refractive index between other members such as the polarizer 110 and the electrode layer 200.
[0067] The refractive index adjusting layer 140 is not particularly limited as long as it can prevent a sharp refractive index difference between the electrode layer 200 and other components such as the polarizer 110, and may be made of a compound used to form a conventional or later developed refractive index adjusting layer, for example, a refractive index adjusting layer-forming composition containing a polymerizable isocyanurate compound.
[0068] In one embodiment, the polarizing plate 100 may further include other functional layers to supplement or enhance the properties of the polarizer in addition to the above-mentioned functional layers, for example, may further include an overcoat layer to further improve mechanical durability.
[0069] In one or more embodiments, the polarizing plate 100 may have a thickness of 30 to 200 μm, preferably 30 to 170 μm, and more preferably 50 to 150 μm, in which case the polarizing plate 100 allows the production of a thin optical laminate while maintaining optical properties.
[0070] The electrode layer 200 is provided for driving the liquid crystal layer 300, and may be formed in direct contact with the polarizer 100. For example, as shown in Figures 1 and 2, the first electrode layer 200-1 and the second electrode layer 200-2 may be formed in direct contact with the first polarizer 100-1 and the second polarizer 100-2, respectively.
[0071] Conventional optical laminates used in the manufacture of smart windows, etc., are manufactured by forming a conductive layer for driving liquid crystal on one side of a substrate and laminating the other side of the substrate with a polarizing plate. However, the variable transmittance optical laminate according to the present invention does not include a separate substrate for forming an electrode layer, and is characterized in that the transmittance and bending characteristics in the transmission mode are improved while reducing the thickness of the laminate by directly forming an electrode layer on one side of the polarizing plate.
[0072] In one embodiment, the electrode layer 200 may be formed by direct deposition on one surface of the polarizer 100. In this case, the electrode layer 200 may be formed by directly contacting the pre-treated surface of the polarizer 100 after performing a pre-treatment such as a corona treatment or a plasma treatment on one surface of the polarizer 100 in order to improve adhesion to the polarizer 100. The pre-treatment is not limited to a corona treatment or a plasma treatment, and any conventional or later developed pre-treatment process may be used within a range that does not impede the object of the present invention.
[0073] In another embodiment, the electrode layer 200 may be formed in direct contact with the polarizer 100 via an easy-adhesion layer (not shown) provided on one side of the polarizer 100 to improve adhesion to the polarizer 100.
[0074] The electrode layer 200 may have a visible light transmittance of 50% or more, and may preferably contain a conductive polymer, or may be manufactured from a composition for forming an electrode layer, for example, containing a conductive polymer; and at least one selected from the group consisting of an organic binder, an organic solvent, a silane coupling agent, and a surfactant; or may further contain a residual amount of water according to the user's needs. In this case, even if deformation due to an external stress is applied to the electrode layer 200, it is possible to prevent cracks from occurring, and further, it is possible to prevent an excessive increase in surface resistance.
[0075] The conductive polymer (or conducting polymer) may be a conventional or later developed conductive polymer material, for example, polythiophene, poly(3,4-ethylenedioxythiophene), polyaniline, polyacetylene, polydiacetylene, polyphenylene, polyphenylenevinylene, polyphenylene sulfide, polythienylenevinylene, polythiophenevinylene, polyfluorene, polypyrrole, poly(3,4-ethylenedioxythiophene):polystyrenesulfonate, poly(3,4-ethylenedioxythiophene):camphorsulfonic acid, poly(3,4-ethylenedioxythiophene):toluenesulfonic acid, poly(3,4-ethylenedioxythiophene):dodecylsulfonate ... The polythiophene:dodecylbenzenesulfonic acid may include one or more selected from the group consisting of poly(3,4-ethylenedioxythiophene), poly(3,4-ethylenedioxythiophene):polystyrenesulfonate, poly(aniline):camphorsulfonic acid, polypyrrole:polystyrenesulfonate, polypyrrole:camphorsulfonic acid, polypyrrole:toluenesulfonic acid, polypyrrole:dodecylbenzenesulfonic acid, polythiophene:polystyrenesulfonate, polythiophene:camphorsulfonic acid, polythiophene:toluenesulfonic acid, and polythiophene:dodecylbenzenesulfonic acid, and is preferably poly(3,4-ethylenedioxythiophene) or poly(3,4-ethylenedioxythiophene):polystyrenesulfonate.
[0076] The content of the conductive polymer is not particularly limited, but may be 10% by weight to 65% by weight, preferably 10% by weight to 50% by weight, and more preferably 11% by weight to 30% by weight, based on the total weight of the composition for forming an electrode layer.
[0077] The organic binder may include at least one selected from the group consisting of a melamine resin, a polyester resin, a polyurethane resin, and a polyacrylic resin. The organic binder may be a water-dispersible resin.
[0078] In one embodiment, the weight average molecular weight of the organic binder may be 5,000 g / mol to 30,000 g / mol, preferably 10,000 g / mol to 20,000 g / mol.
[0079] The content of the organic binder is not particularly limited, but may be 1 wt % to 20 wt %, preferably 1 wt % to 10 wt %, and more preferably 1 wt % to 5 wt %, relative to the total weight of the composition for forming an electrode layer.
[0080] The organic solvent may include an alcohol-based organic solvent, an ether-based organic solvent, and / or an amide-based organic solvent.
[0081] The alcohol-based organic solvent serves to reduce the surface tension of the composition for forming an electrode layer and improve the coating property. In one embodiment, the alcohol-based organic solvent may be an alcohol having 1 to 4 carbon atoms, and examples of the alcohol-based organic solvent include methanol, ethanol, propanol, isopropanol, and n-butyl alcohol.
[0082] The ether-based organic solvent may be a conventional or later developed ether-based organic solvent, for example, propylene glycol monopropyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol-2-ethylhexyl ether, etc.
[0083] The amide-based organic solvent serves to improve the conductivity of the electrode layer. In one embodiment, the amide-based organic solvent may be acetamide, N-methylacetamide, N-dimethylacetamide, N-methylpyrrolidone, or the like.
[0084] The content of the organic solvent is not particularly limited, but may be 10% by weight to 80% by weight, preferably 40% by weight to 65% by weight, and more preferably 45% by weight to 60% by weight, based on the total weight of the composition for forming an electrode layer.
[0085] The silane coupling agent serves to improve the adhesive strength of the composition for forming an electrode layer, thereby facilitating lamination of the electrode layer 200 on the polarizing plate 100 . In one embodiment, the silane coupling agent may include one or more selected from the group consisting of trimethoxy-based silane, triethoxy-based silane, tetramethoxy-based silane, and tetraethoxy-based silane. For example, the triethoxy-based silane may be 2-(3,4-epoxycyclohexyl)ethyltriethoxy silane, (3-aminopropyl)triethoxy silane, (pentafluorophenyl)triethoxy silane, (3-glycidyloxypropyl)triethoxy silane, or (4-chlorophenyl)triethoxy silane. The trimethoxy-based silane may be (3-glycidyloxypropyl)trimethoxy silane, (3-chloropropyl)trimethoxy silane, (3-mercaptopropyl)trimethoxy silane, (3-glycidyloxypropyl)trimethoxy silane, (3-aminopropyl)trimethoxy silane, [3-(2-aminoethylamino)propyl]trimethoxy silane, (N,N-dimethylaminopropyl)trimethoxy silane,The silane may be (3-bromopropyl)trimethoxysilane, (3-iodopropyl)trimethoxysilane, or (3-iodopropyl)trimethoxysilane.
[0086] In terms of improving the adhesion between the polarizing plate 100 and the electrode layer 200, the content of the silane coupling agent may be 0.05% by weight to 0.3% by weight with respect to the total weight of the composition for forming an electrode layer.
[0087] The surfactant may be a silicone-based surfactant or an acetylene-based surfactant, and the silicone-based surfactant may be a modified silicone-based surfactant.
[0088] For example, a commercially available silicone surfactant is BYK-378 manufactured by BYK, and a commercially available acetylene surfactant is Dynol 604 manufactured by Air Products.
[0089] The content of the surfactant is not particularly limited, but may be 0.02 wt % to 0.4 wt %, and preferably 0.1 wt % to 0.4 wt %, relative to the total weight of the composition for forming an electrode layer.
[0090] The electrode layer 200 may have a physical alignment structure formed on at least a portion of the region thereof for imparting alignment to the liquid crystal compound 310 in the liquid crystal layer 300 .
[0091] Conventional optical laminates including a liquid crystal layer are produced by forming a separate alignment film in order to impart alignment to the liquid crystal compound in the liquid crystal layer. However, the optical laminate according to the present invention does not include a separate alignment film, and a physical alignment structure can be formed in the electrode layer itself including a conductive polymer. This is a technical feature that it solves problems that arise when a conventional alignment film is provided, such as uneven thickness or reduced adhesion due to drying conditions of the alignment film.
[0092] The physical orientation structure can be formed by a method commonly used in the art, for example, by rubbing with a rubbing roller wrapped with a rubbing cloth.
[0093] In one embodiment, the electrode layer 200 may have a thickness of 100 nm to 3,000 nm, preferably 150 nm to 2,000 nm, and more preferably 200 nm to 1,500 nm. The thickness of the electrode layer may refer to the thickness of the final electrode layer after a physical orientation structure is formed by rubbing. When the thickness of the electrode layer satisfies the above range, it is possible to manufacture a thin electrode film without significant change in characteristics due to external stress while ensuring a predetermined transmittance.
[0094] It is preferable that the electrode layer 200 according to an exemplary embodiment of the present invention has a sheet resistance of 200 Ω / □ or less.In this case, there is an advantage in that the product can be operated stably using only the electrode layer 200 itself having a physical orientation structure without an orientation film.
[0095] In one embodiment, the variable transmittance optical stack may further include a transparent conductive layer in addition to the electrode layer.
[0096] 2, the transparent conductive layer 210 is disposed between the polarizer 100 and the electrode layer 200, and may be realized in the form of a first transparent conductive layer 210-1 disposed between the first polarizer 100-1 and the first electrode layer 200-1, and a second transparent conductive layer 210-2 disposed between the second polarizer 100-2 and the second electrode layer 200-2, as shown in Fig. 2. However, the embodiment is not limited to that shown in Fig. 2, and the transparent conductive layer may include any one of the first transparent conductive layer and the second transparent conductive layer.
[0097] The transparent conductive layer 210 preferably has a visible light transmittance of 50% or more, and may include, for example, one or more selected from the group consisting of transparent conductive oxides, metals, carbon-based materials, conductive inks, and nanowires, but is not limited thereto, and any conventional or later developed transparent conductive layer material may be used.
[0098] In one or more embodiments, the transparent conductive oxide may include one or more selected from the group consisting of indium tin oxide (ITO), indium zinc oxide (IZO), indium zinc tin oxide (IZTO), aluminum zinc oxide (AZO), gallium zinc oxide (GZO), fluorine tin oxide (FTO), zinc oxide (ZnO), etc. The metal may include one or more selected from the group consisting of gold (Au), silver (Ag), copper (Cu), aluminum (Al), platinum (Pt), palladium (Pd), chromium (Cr), titanium (Ti), tungsten (W), niobium (Nb), tantalum (Ta), vanadium (V), iron (Fe), manganese (Mn), cobalt (Co), nickel (Ni), zinc (Zn), and alloys containing at least one of these, for example, a silver-palladium-copper (APC) alloy or a copper-calcium (CuCa) alloy. The carbon-based material may include one or more selected from the group consisting of carbon nanotubes (CNTs) and graphene, the conductive ink may be an ink containing a mixture of metal powder and a curable polymer binder, and the nanowire may be, for example, a silver nanowire (AgNW).
[0099] In addition, the transparent conductive layer 210 is formed into a two-layer structure by combining the above materials, for example, a two-layer structure including a metal layer and a transparent conductive oxide layer to reduce the reflectance and increase the transmittance of incident light.
[0100] In one embodiment, the transparent conductive layer 210 may have a thickness of 100 nm to 1,000 nm, preferably 130 nm to 800 nm, and more preferably 150 nm to 600 nm. When the thickness of the transparent conductive layer satisfies the above range, there is an advantage in terms of securing a suitable surface resistance for driving and improving the appearance quality of the product without reducing the transmittance of the product.
[0101] According to an exemplary embodiment of the present invention, when the optical stack includes the transparent conductive layer 210, the transparent conductive layer 210 is formed in direct contact with the polarizer 100, for example, the first transparent conductive layer 210-1 is formed in direct contact with the first polarizer 100-1, and / or the second transparent conductive layer 210-2 is formed in direct contact with the second polarizer 100-2. In this case, the above-mentioned contents related to the electrode layer being formed in direct contact with the polarizer are similarly applicable.
[0102] When the variable transmittance optical laminate further includes the transparent conductive layer 210 described above in addition to the electrode layer 200, this is preferable in that there is an additional advantage in terms of improving the appearance quality of the product.
[0103] The liquid crystal layer 300 can change the driving mode of the optical stack by adjusting the transmittance of light incident from one or more directions by an electric field.
[0104] The liquid crystal layer 300 may include a liquid crystal compound 310 and a spacer 320, and may be provided, for example, between the first electrode layer 200-1 and the second electrode layer 200-2 in the light control region, and may be located within a space provided by a sealant 330 formed along the outer periphery of the liquid crystal layer 300 to seal the liquid crystal layer 300.
[0105] The liquid crystal compound 310 is not particularly limited as long as it is driven by an electric field and can control the light transmittance, and any conventional or later developed liquid crystal compound can be used. For example, the contents regarding the reactive liquid crystal compound of the polarizer described above can be similarly applied.
[0106] The liquid crystal behavior mode of the liquid crystal compound is not particularly limited, and for example, TN (Twisted nematic) mode, STN (Super twisted nematic) mode, VA (Vertical alignment) mode, ECB (Electrically Controlled Birefringence) mode, etc. can be used.
[0107] The spacer 320 may include a ball spacer, and the number of the ball spacers may be one or more, and the ball spacer preferably has a diameter of 1 to 10 μm. In addition, the area of the ball spacer in the liquid crystal layer 300 as viewed in a planar direction is preferably 0.01 to 10% of the area of the liquid crystal layer 300 in terms of improving the visibility of the user and the transmittance in the light-transmitting mode.
[0108] The sealant 330 may include a curable resin as a base resin. The base resin may be a UV-curable resin or a thermosetting resin known in the art as a resin that can be used for a sealant. The UV-curable resin may be a polymer of a UV-curable monomer. The thermosetting resin may be a polymer of a thermosetting monomer.
[0109] The base resin of the sealant may be, for example, an acrylate-based resin, an epoxy-based resin, a urethane-based resin, a phenol-based resin, or a mixture of the above resins. In one embodiment, the base resin may be an acrylate-based resin, and the acrylate-based resin may be a polymer of an acrylic monomer. The acrylic monomer may be, for example, a polyfunctional acrylate. In another embodiment, the sealant may further include a monomer component in the base resin. The monomer component may be, for example, a monofunctional acrylate. In this specification, a monofunctional acrylate may mean a compound having one acrylic group, and a polyfunctional acrylate may mean a compound having two or more acrylic groups. The curable resin may be cured by irradiation with ultraviolet light and / or heating. The ultraviolet irradiation conditions or heating conditions are appropriately set within a range that does not impair the purpose of the present application. The sealant may further include an initiator, for example, a photoinitiator or a thermal initiator, if necessary.
[0110] The sealant 330 is formed by a method commonly used in the art, for example, by drawing the sealant on the outer periphery (ie, the inactive area) of the liquid crystal layer 300 using a dispenser having a nozzle.
[0111] The variable transmittance optical laminate of the present invention may further include other components within the scope of the present invention, for example, may further include an adhesive layer 400 (see FIG. 3), or may further include an adhesive layer, an ultraviolet absorbing layer, a hard coat layer, etc.
[0112] The adhesive layer 400 is formed using an adhesive, and preferably has an appropriate adhesive strength so as to prevent peeling or air bubbles from occurring during handling of the optical laminate, and at the same time, has transparency and thermal stability.
[0113] The adhesive may be a conventional or later developed adhesive, and in one or more embodiments, may be an acrylic adhesive, a rubber adhesive, a silicone adhesive, a urethane adhesive, a polyvinyl alcohol adhesive, a polyvinylpyrrolidone adhesive, a polyacrylamide adhesive, a cellulose adhesive, a vinyl alkyl ether adhesive, etc. The adhesive is not particularly limited as long as it has adhesive strength and viscoelasticity, but in terms of availability, etc., it may be preferably an acrylic adhesive, and may contain, for example, a (meth)acrylate copolymer, a crosslinking agent, and a solvent.
[0114] The crosslinking agent may be a conventional or later developed crosslinking agent, and may include, for example, a polyisocyanate compound, an epoxy resin, a melamine resin, a urea resin, a dialdehyde, a methylol polymer, or the like, and may preferably include a polyisocyanate compound.
[0115] The solvent may include ordinary solvents used in the field of resin compositions, such as alcohol-based compounds such as methanol, ethanol, isopropanol, butanol, and propylene glycol methoxy alcohol; ketone-based compounds such as methyl ethyl ketone, methyl butyl ketone, methyl isobutyl ketone, diethyl ketone, and dipropyl ketone; acetate-based compounds such as methyl acetate, ethyl acetate, butyl acetate, and propylene glycol methoxy acetate; cellosolve-based compounds such as methyl cellosolve, ethyl cellosolve, and propyl cellosolve; and hydrocarbon-based compounds such as hexane, heptane, benzene, toluene, and xylene. These may be used alone or in combination of two or more.
[0116] The adhesive layer is formed using an adhesive, and preferably has an appropriate adhesive strength so as to prevent peeling, air bubbles, etc. from occurring when the optical laminate is handled, and at the same time, has transparency and thermal stability.
[0117] The adhesive may be any conventional or later developed adhesive, for example a light curable adhesive.
[0118] The photocurable adhesive exhibits strong adhesive strength by crosslinking and curing when exposed to active energy rays such as ultraviolet (UV) and electron beam (EB), and is made of reactive oligomers, reactive monomers, photopolymerization initiators, etc.
[0119] The reactive oligomer is an important component that determines the properties of the adhesive, and forms a polymer bond by photopolymerization to form a hardened coating. Usable reactive oligomers include polyester resins, polyether resins, polyurethane resins, epoxy resins, polyacrylic resins, silicone resins, etc.
[0120] The reactive monomer acts as a crosslinking agent or diluent for the reactive oligomer and affects the adhesive properties. Usable reactive monomers include monofunctional monomers, polyfunctional monomers, epoxy monomers, vinyl ethers, cyclic ethers, etc.
[0121] The photopolymerization initiator plays a role of absorbing light energy to generate radicals or cations to initiate photopolymerization, and a suitable one can be selected and used depending on the photopolymerizable resin.
[0122] The thickness of the adhesive layer 400 or the bonding layer can be appropriately determined depending on the type of resin acting as the adhesive, the adhesive strength, the environment in which the adhesive is used, etc. In one embodiment, the adhesive layer may have a thickness of 0.01 to 50 μm, preferably 0.05 to 20 μm, and more preferably 0.1 to 10 μm, in order to ensure sufficient adhesive strength and minimize the thickness of the optical laminate.
[0123] The ultraviolet absorbing layer is not particularly limited as long as it is used to prevent deterioration of the optical laminate due to ultraviolet rays. For example, it may be a salicylic acid-based ultraviolet absorber (phenyl salicylate, p-tert-butyl salicylate, etc.), a benzophenone-based ultraviolet absorber (2,4-dihydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, etc.), a benzotriazole-based ultraviolet absorber (2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-t 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-(3”,4”,5”,6”-tetrahydrophthalimidomethyl)-5'-methylphenyl)benzotriazole, 2,2-methylenebis(4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazole- 2-yl)phenol), 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-(2-octyloxycarbonylethyl)-phenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-(1-methyl-1-phenylethyl)-5'-(1,1,3,3-tetramethylbutyl)-phenyl)benzotriazole, 2-(2H-benzotriazol-2-yl)-6-(linear and and side chain dodecyl)-4-methylphenol, a mixture of octyl-3-[3-tert-butyl-4-hydroxy-5-(chloro-2H-benzotriazol-2-yl)phenyl]propionate and 2-ethylhexyl-3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate, etc.), cyanoacrylate ultraviolet absorbers (2'-ethylhexyl-2-cyano-3,3-diphenylacrylate, ethyl-2-cyano-3-(3',4'-methylenedioxyphenyl)-acrylate, triazine-based ultraviolet absorbers, etc. can be used, and benzotriazole-based ultraviolet absorbers and triazine-based ultraviolet absorbers, which have high transparency and are excellent in preventing deterioration of the polarizing plate and the transmittance variable layer, are preferred, and benzotriazole-based ultraviolet absorbers with a more suitable spectral absorption spectrum are particularly preferred. The benzotriazole-based ultraviolet absorbers may be bis(Bis)-modified, and may be, for example, 6,6'-methylenebis(2-(2H-benzo[d][1,2,3]triazol-2-yl)-4-(2,4,4-trimethylpentan-2-yl)phenol), 6,6'-methylenebis(2-(2H-benzo[d][1,2,3]triazol-2-yl)-4-(2-hydroxyethyl)phenol), etc.,
[0124] The hard coat layer is not particularly limited as long as it is capable of protecting components such as a polarizing plate and a transmittance variable layer from external physical and chemical shocks, and any conventional or later developed hard coat layer can be used.
[0125] In one embodiment, the hard coat layer is formed by applying a composition for forming a hard coat layer onto another member and curing the composition with light or heat. The composition for forming a hard coat layer is not particularly limited and may include, for example, a photocurable compound and a photoinitiator.
[0126] The photocurable compound and photoinitiator can be any compound commonly used in the art without any restrictions. For example, the photocurable compound may be a photopolymerizable monomer, a photopolymerizable oligomer, etc., such as a monofunctional and / or polyfunctional (meth)acrylate, and the photoinitiator may be an oxime ester-based compound, etc.
[0127] In addition to the variable transmittance optical laminate, the present invention includes a smart window including the same. The present invention also includes a means of transportation including the smart window, for example, an automobile to which the smart window is applied to at least one of a front window, a rear window, a side window, a sunroof window, and an interior partition, a wearable device including the smart window, and a building fixture.
[0128] For example, an automobile including the smart window of the present invention may be manufactured by bonding a vehicle glass component onto both sides of the above-mentioned optical laminate, for example, by placing an adhesive film and a vehicle glass component on both sides of the optical laminate, and then heating the laminate at a temperature of 90°C and a vacuum of about 1 bar for 10 to 20 minutes using a press machine, and the adhesive film may include an EVA film, a PVB film, etc.
[0129] In addition, a building glass component may be bonded to one or both sides of the optical laminate. A building glass component may be bonded to one side of the optical laminate by lamination to produce a smart window product for fittings in which a building glass component is attached to one side of the optical laminate. Alternatively, a UV adhesive may be applied to both sides of the optical laminate, and then a building glass component may be bonded and UV cured to produce a smart window product for fittings in which a building glass component is attached to both sides of the optical laminate.
[0130] Hereinafter, the present invention will be described in detail with reference to the embodiments. However, the present invention is not limited to the embodiments disclosed below, and may be realized in various different forms. The embodiments are provided only to complete the disclosure of the present invention and to fully inform those skilled in the art of the scope of the invention. The present invention is defined only by the scope of the claims. EXAMPLES
[0131] Examples and Reference Examples: Preparation of Optical Laminate Example 1 A TAC protective film was laminated on both sides of a 21 μm-thick PVA stretched polarizer using a UV adhesive, and then the adhesive was cured by exposure to UV light to prepare a polarizing plate.
[0132] Thereafter, a conductive polymer solution (poly(3,4-ethylenedioxythiophene):polystyrenesulfonate (PEDOT:PSS) (Clevios TM A mixture of 0.6% by weight of ethylenediaminetetraacetate (Heraeus), 32.4% by weight of ethanol, 40% by weight of deionized water, and 27% by weight of 2-methoxyethanol was applied to the conductive polymer film and dried at 80°C for 2 minutes to form an electrode layer. Then, a rubbing roller was rotated on the conductive polymer film to provide physical alignment by rubbing alignment. The thickness of the electrode layer after the rubbing process was 100nm.
[0133] Thereafter, a ball spacer (SEKISUI SP series) was mixed on the upper surface of the electrode layer to prepare a solution, which was then placed in a spacer sprayer (SDSS-KHU02, Sindh Giken Co., Ltd.) and the mixed solution was sprayed at 110°C and dried for 20 minutes to form a ball spacer on the upper surface of the electrode layer.
[0134] Next, a sealant (UVF-006, 70,000 mPa s, Sekisui) was applied to the electrode layer of the polarizer placed at the bottom using a sealant dispenser (SHOTmini 200Ωx, Musashi) according to the product size. After that, with the polarization axes of the upper and lower polarizers aligned parallel to each other at 0° or 90°, the upper and lower polarizers were bonded by injecting liquid crystal using the ODF (One Drop Filling) process. Then, UV curing (500mJ / cm) was performed along the sealant line. 2 ) was carried out to prepare the optical laminate of Example 1.
[0135] Example 2 An optical laminate of Example 2 was produced in the same manner as in Example 1, except that the thickness of the electrode layer was set to 250 nm.
[0136] Example 3 An optical laminate of Example 3 was produced in the same manner as in Example 1, except that the thickness of the electrode layer was set to 500 nm.
[0137] Example 4 An optical laminate of Example 4 was produced in the same manner as in Example 1, except that the electrode layer was formed to a thickness of 1,000 nm.
[0138] Example 5 An optical laminate of Example 5 was produced in the same manner as in Example 1, except that the electrode layer was formed to a thickness of 2,000 nm.
[0139] Example 6 An optical laminate of Example 6 was produced in the same manner as in Example 1, except that the electrode layer was formed to a thickness of 3,000 nm.
[0140] Reference example 1 An optical laminate of Reference Example 1 was produced in the same manner as in Example 1, except that the thickness of the electrode layer was set to 90 nm.
[0141] Reference example 2 An optical laminate of Reference Example 2 was produced in the same manner as in Example 1, except that the thickness of the electrode layer was set to 3,200 nm.
[0142] Experimental example: Surface resistance and crack evaluation (1) Surface resistance evaluation For the optical laminates of the above Examples and Reference Examples, the sheet resistance of the electrode layer was measured using a sheet resistance measuring instrument (MCP-T370), and the evaluation results are shown in Table 1 below.
[0143] <Evaluation criteria> ○: The surface resistance of the electrode layer is 200Ω / □ or less ×: The surface resistance of the electrode layer exceeds 200 Ω / □ (2) Crack evaluation The optical laminates of the above Examples and Reference Examples were evaluated for cracks on the surface of the electrode layer using an optical microscope (OM), and the evaluation results are shown in Table 1 below.
[0144] <Evaluation criteria> ○: No visible cracks on the electrode layer surface ×: Cracks are visible on the surface of the electrode layer.
[0145] [Table 1]
[0146] Referring to the above table, it can be seen that the optical laminate according to the present invention does not include an alignment film, and even if physical alignment is formed in the electrode layer itself, it has excellent sheet resistance and does not cause cracks on the surface of the electrode layer.
[0147] On the other hand, the optical laminate of Reference Example 1, in which the electrode layer is less than 100 nm thick, has a surface resistance of over 200 Ω / □, which is slightly higher than that of the Examples, and the optical laminate of Reference Example 2, in which the electrode layer is more than 3,000 nm thick, is found to have cracks on the surface of the electrode layer.
[0148] Therefore, it can be seen that the optical laminate of the present invention, in which physical orientation is formed in the electrode layer itself without including an alignment film, can be operated smoothly as an optical laminate, and more preferably, the thickness of the electrode layer is 100 nm to 3,000 nm.
Claims
1. A first polarizing plate; A first electrode layer formed on one surface of the first polarizing plate; a second polarizing plate facing the first polarizing plate; a second electrode layer formed on one surface of the second polarizing plate and facing the first electrode layer; a liquid crystal layer provided between the first electrode layer and the second electrode layer; the first electrode layer and the second electrode layer contain a conductive polymer; A variable transmittance optical laminate, wherein the first electrode layer and the second electrode layer have a physical orientation structure formed on at least a partial area thereof by rubbing.
2. The variable transmittance optical stack of claim 1 , wherein the variable transmittance optical stack does not include a separate alignment film.
3. The variable transmittance optical stack of claim 1 , wherein the first and second electrode layers have a thickness of 100 nm to 3,000 nm.
4. The variable transmittance optical stack according to claim 1 , wherein the first electrode layer and the second electrode layer have a sheet resistance of 200 Ω / □ or less.
5. 2. The variable transmittance optical laminate according to claim 1, wherein the first electrode layer and the second electrode layer are manufactured from a composition for forming an electrode layer, the composition comprising: a conductive polymer; and at least one selected from the group consisting of an organic binder, an organic solvent, a silane coupling agent, and a surfactant.
6. The conductive polymer may be polythiophene, poly(3,4-ethylenedioxythiophene), polyaniline, polyacetylene, polydiacetylene, polyphenylene, polyphenylene vinylene, polyphenylene sulfide, polythienylene vinylene, polythiophene vinylene, polyfluorene, polypyrrole, poly(3,4-ethylenedioxythiophene):polystyrene sulfonate, poly(3,4-ethylenedioxythiophene):camphorsulfonic acid, poly(3,4-ethylenedioxythiophene):toluenesulfonic acid, poly(3,4-ethylenedioxythio 6. The variable transmittance optical laminate of claim 5, comprising one or more selected from the group consisting of polythiophene: dodecylbenzenesulfonic acid, polyaniline: polystyrene sulfonate, polyaniline: camphorsulfonic acid, polypyrrole: polystyrene sulfonate, polypyrrole: camphorsulfonic acid, polypyrrole: toluenesulfonic acid, polypyrrole: dodecylbenzenesulfonic acid, polythiophene: polystyrene sulfonate, polythiophene: camphorsulfonic acid, polythiophene: toluenesulfonic acid, and polythiophene: dodecylbenzenesulfonic acid.
7. The variable transmittance optical stack of claim 1 , wherein at least one of the first electrode layer and the second electrode layer is formed in direct contact with one of the first polarizer and the second polarizer.
8. 2. The variable transmittance optical stack of claim 1, comprising at least one transparent conductive layer: a first transparent conductive layer disposed between a first polarizer and a first electrode layer; and a second transparent conductive layer disposed between a second polarizer and a second electrode layer.
9. 9. The variable transmittance optical stack of claim 8, wherein at least one of the first and second transparent conductive layers has a thickness of 100 nm to 1,000 nm.
10. 9. The variable transmittance optical stack of claim 8, wherein at least one of the first transparent conductive layer and the second transparent conductive layer comprises at least one selected from the group consisting of transparent conductive oxides, metals, carbon-based materials, conductive inks, and nanowires.
11. The variable transmittance optical laminate of claim 1, wherein at least one of the first polarizing plate and the second polarizing plate includes one or more functional layers selected from the group consisting of a protective layer, a phase difference adjusting layer, and a refractive index adjusting layer.
12. 2. The variable transmittance optical laminate according to claim 1, wherein at least one of the first polarizing plate and the second polarizing plate has a thickness of 30 to 200 μm.
13. The variable transmittance optical stack of claim 1 , wherein the liquid crystal layer includes ball spacers.
14. The variable transmittance optical stack of claim 13, wherein the ball spacers have a diameter of 1 to 10 μm.
15. The variable transmittance optical laminate according to claim 13, wherein the area of the ball spacers in the liquid crystal layer is 0.01% to 10% of the area of the liquid crystal layer.
16. The variable transmittance optical laminate according to claim 1 , further comprising at least one layer selected from the group consisting of an overcoat layer, an adhesive layer, an ultraviolet absorbing layer, and a hard coat layer.
17. A method for producing the variable transmittance optical laminate according to any one of claims 1 to 16.
18. A smart window comprising the variable transmittance optical laminate according to any one of claims 1 to 16.
19. 20. A mode of transportation comprising the smart window of claim 18.
20. 20. A car comprising the smart window of claim 18 applied to at least one of a front window, a rear window, a side window, a sunroof window, and an interior partition.
21. A wearable device comprising the smart window of claim 18.
22. 19. An architectural fixture comprising the smart window of claim 18.
Citation Information