Sheet body

The sheet body with controlled adhesive strength addresses adhesion and reusability issues, ensuring durable and weather-resistant repairs with reduced waste.

JP2024155818AInactive Publication Date: 2024-10-31KEIWA INCORPORATED
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024066940
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-04-17
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional sheet materials for repairing structures, such as roofs, face issues with adhesion durability, wrinkle formation, and difficulty in reapplication, leading to poor weather resistance and increased waste due to damage during handling.

Method used

A sheet body with controlled adhesive strength, having a 180° peel test value of 1.5N/25mm or more and less than 100% of the maximum tensile elastic region force, allowing for easy reattachment and maintaining adhesion even after weather exposure.

Benefits of technology

The sheet body ensures excellent adhesion and weather resistance while being easily handled and reused, reducing waste and improving workability at construction sites.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155818000001_ABST
    Figure 2024155818000001_ABST
Patent Text Reader

Abstract

To provide a sheet body with improved workability on construction sites, as well as excellent adhesion to structures.SOLUTION: A sheet body is attached to a structure and used for reinforcing or repairing the structure, and has an adhesive strength of 1.5 N / 25 mm or more in a 180° peel test and less than 100% of the maximum tensile elastic range test force in a state before being attached to the structure.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a sheet body that is attached to a structure to be used for reinforcing or repairing the structure. More specifically, the present disclosure relates to a sheet body that has excellent adhesiveness to the structure and can be peeled off and reattached even after being attached to the structure at a construction site. [Background technology]

[0002] Various structures such as ordinary houses and commercial buildings are known. In addition, as roofs of structures, for example, slate roofs, metal roofs, roofs made of Galvalume Steel Sheet (registered trademark), concrete roofs including flat roofs (also called "rikuyane" or "rokuyane" in Japanese), etc. are known. In these structures, deterioration due to exposure to wind and rain for a long period of time, or damage due to disasters such as typhoons, can cause leaks. For this reason, for example, when deterioration or damage occurs in the roof of a structure, emergency measures are taken.

[0003] A commonly known method of emergency roof repair is to place a tarp 31 to cover the damaged area of ​​a roof 30, and place multiple sandbags 32 as weights on top of the tarp 31 to secure the tarp 31, as shown in Fig. 23. Other examples of weights include bags filled with water, as disclosed in Patent Documents 1 and 2.

[0004] However, when repairing a roof using a conventional blue sheet 31, it is difficult to prevent wrinkles in the blue sheet 31. Also, the surface of a roof is usually not flat. This causes gaps between the blue sheet 31 and the roof, which can allow water to seep in. There is also the problem that the blue sheet 31 can be blown away by strong winds such as typhoons. Also, blue sheets 31 usually do not have a high weather resistance and deteriorate in about a year, so they need to be replaced.

[0005] In response to the above-mentioned problems, for example, as disclosed in Patent Document 3, a surface sheet material used for finishing exterior walls formed from ALC panels is known, which comprises a sheet base material that is a woven fabric formed by weaving glass fibers, waterproof paint, and an intermediate layer formed between the two and composed of a mixture of an inorganic material and a flexible resin material. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2010-144360 A [Patent Document 2] JP 2000-16886 A [Patent Document 3] Registered Utility Model No. 3009544 Summary of the Invention [Problem to be solved by the invention]

[0007] According to the facing sheet material disclosed in Patent Document 3, even if cracks occur in the joints of the ALC panel, the joints are covered with the facing sheet material. Therefore, the appearance is not affected. Also, by filling small gaps between adjacent facing sheet materials with a waterproof sealant, it is possible to prevent rainwater from entering. However, although such facing sheet materials are attached to the ALC panel with an adhesive, it is difficult to say that the facing sheet, which is exposed to various environments, can be stably attached for a long period of time.

[0008] In view of such conventional problems, the applicant of this patent application (hereinafter also referred to as the "applicant") has developed a structure protection sheet having a polymer cement layer and a resin layer and a specifically controlled thickness distribution, as previously disclosed in International Publication No. 2021 / 010456. The structure protection sheet can be applied to both preliminarily reinforcing a newly built structure and repairing a structure that has already deteriorated over time. In addition, it can be attached to the structure via an adhesive, which can significantly reduce the construction time required to install a protection sheet on the surface of the roof of the structure. In addition, since it has excellent strength, it can protect the structure for a long period of time.

[0009] Here, it has been found that although the structure protection sheet can provide excellent weather resistance to the structure, depending on the skill of the worker who applies it to the structure, it may not be applied neatly or uniformly to the structure, resulting in wrinkles and the like. When the worker does not apply it neatly or uniformly to the structure, there is a demand to peel off the applied structure protection sheet once and reapply it. However, conventional structure protection sheets have been developed with the main focus on increasing the adhesive strength when applied to the structure in order to provide adhesion to the structure. For this reason, once applied, it was not possible to peel it off and reapply it. More specifically, once peeled off, the structure protection sheet is damaged and cannot maintain its adhesiveness and weather resistance performance, so it was not possible to reapply it. As a result, the current situation was that application at the construction site was not successful in one attempt, and the peeled structure protection sheet had to be discarded. Thus, conventional structure protection sheets had problems with handling at the construction site.

[0010] Therefore, the present disclosure has been made to solve the above-mentioned problems, and its object is to provide a sheet body that has excellent adhesion to structures while improving handleability at construction sites. [Means for solving the problem]

[0011] As a result of intensive research by the present inventors, it has been found that, from the viewpoint of ensuring weather resistance, the sheet body of the present disclosure is required to have an adhesive strength of a certain value or more in a 180° peel test described later before being attached to a structure. Furthermore, from the viewpoint of improving handling such as re-attachment, it has been found that it is important to control the adhesive strength of the sheet body before being attached to a structure to a value less than 100% of the maximum test force in the tensile elastic region described later. The present disclosure has been completed based on the above findings.

[0012] A first aspect of the present disclosure is a sheet body that is attached to a structure and used to reinforce or repair the structure, and which, prior to being attached to the structure, has an adhesive strength that is a measured value of 1.5 N / 25 mm or more in a 180° peel test and is less than 100% of the maximum test force in the tensile elastic region.

[0013] According to the first aspect, the sheet body can be secured to have excellent adhesive strength to the structure while improving the ease of handling of the sheet body at the construction site. More specifically, by setting the upper limit of the adhesive strength of the sheet body to a value less than 100% of the maximum test force in the tensile elastic region, the sheet body is less likely to be plastically deformed when peeled off after being applied, and accordingly the sheet body is less likely to be damaged, making it possible to reapply the sheet body.

[0014] A second aspect of the present disclosure is based on the first aspect, and has an adhesive strength such that the measured value of the 180° peel strength after a weather load test is 1.5 N / 25 mm or more.

[0015] According to the second aspect, it is ensured that the adhesive strength after a weather resistance load test (details of the test will be described later) is the same as that before it was attached to a structure, and a sheet body with excellent weather resistance can be provided.

[0016] A third aspect of the present disclosure is based on the first aspect and further has waterproofness such that there is no water leakage in a waterproofness test after a weather load test.

[0017] According to the third aspect, a predetermined waterproof property is ensured even after the weather resistance load test, and a sheet body having excellent weather resistance can be provided.

[0018] Furthermore, a fourth aspect of the present disclosure is that, assuming the first aspect, when a deformation test is carried out by sequentially performing the operations described in the following items (1), (2), (3), and (4), the energy calculated by the calculation in (4) below is a value of 2.0 mJ or more. (1) A rectangular sheet body having short sides of 50 mm and long sides of 100 mm is prepared as a sample. (2) The sample is bent so that a pair of short sides on the same surface overlap each other, and a pair of regions of the sample from the edges of the pair of short sides to a position 15 mm away along the long side are grasped and fixed with a fixing portion, thereby forming a curved portion with a circumference of 70 mm between the pair of regions of the sample. (3) With the surfaces of the pair of regions of the sample arranged parallel to the vertical direction and the curved portion facing upward, a disk-shaped pressing tool with a pressing surface of 100 mm in diameter and 10 mm in thickness is used to contact the curved portion from above in an environment of a temperature of 23±2°C and a humidity of 50±10% RH, and the pressing tool is moved downward by 20 mm at a test speed of 30 mm / min. (4) The energy required to move the pressing jig is calculated.

[0019] According to the fourth aspect, the sheet body can be given an appropriate rigidity. Therefore, the sheet body can be easily handled when it is attached to the surface of a structure. More specifically, the sheet body can be easily laid on the surface of a structure. Note that the "deformation test" in this specification refers to the above-mentioned deformation test. Effect of the Invention

[0020] According to each of the above-mentioned aspects, the sheet body can have excellent adhesiveness to structures while improving the ease of handling at the construction site. Specifically, even if the sheet body is once attached to a structure and then peeled off, the sheet body can be reattached without being damaged (while maintaining adhesiveness and weather resistance).

[0021] That is, each of the above-mentioned aspects allows the sheet body to be applied to a structure with excellent adhesive strength, while allowing the sheet body to be re-applied as necessary, which are contradictory effects that have been difficult to obtain in the past. Therefore, according to the sheet body of each of the above-mentioned aspects, the sheet body can be reliably applied to the target area of ​​the structure, and the handling and workability during the application work at the construction site can be improved. Furthermore, since the sheet body can be reused once peeled off, waste reduction and environmental protection are also achieved. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic configuration of a sheet member according to a second embodiment having a single adhesive layer and a single weather-resistant layer. [Diagram 2] FIG. 2 is a cross-sectional view showing a schematic configuration of a sheet member according to a second embodiment having a plurality of base layers and a plurality of weather-resistant layers. [Diagram 3] FIG. 3 is a schematic diagram showing how the release sheet is peeled off from the sheet member of the present disclosure. [Figure 4] FIG. 4 is a schematic diagram showing how the sheet body of FIG. 3 is attached to a structure. [Diagram 5] 5(A), 5(B), 5(C), and 5(D) are schematic views illustrating a method for measuring the rigidity of a sheet member according to the present disclosure. [Figure 6] FIG. 6 is a schematic diagram showing an example of a reinforcing material for the sheet body of the present disclosure. [Figure 7] FIG. 7 is an enlarged partial view of the reinforcing material of FIG. [Figure 8] FIG. 8 is a schematic diagram showing the 180° peel test method. [Figure 9] FIG. 9 is a graph showing how to determine the maximum test force in the tensile elastic region based on a tensile test. [Figure 10] FIG. 10 is a graph showing how to determine the maximum test force in the tensile elastic region based on a tensile test. [Figure 11] FIG. 11 is a graph showing the relationship between the stroke (mm) of the pressing jig and the test force (N). [Figure 12] FIG. 12 is a perspective view of the roof-like platform. [Figure 13] FIG. 13 is a diagram showing a side view and dimensions of the stand of FIG. [Figure 14] FIG. 14 is a front view of the stand of FIG. [Figure 15] FIG. 15 is a schematic diagram showing a method for measuring the storage modulus. [Figure 16] FIG. 16 is a graph showing an example of measurement of storage elastic modulus. [Figure 17] FIG. 17 is a cross-sectional view illustrating a schematic configuration of a sheet member according to a third embodiment. [Figure 18] FIG. 18 is a cross-sectional view illustrating a schematic configuration of a sheet member according to a fourth embodiment. [Figure 19] FIG. 19 is a cross-sectional view illustrating a schematic configuration of a sheet member according to the fifth embodiment. [Figure 20] FIG. 20 is a schematic diagram showing the structure of a supply article containing a sheet member according to the present disclosure. [Figure 21] FIG. 21 is a schematic perspective view of a sheet member according to the sixth embodiment and a solar cell unit disposed on top of the sheet member. [Figure 22] FIG. 22 shows a schematic cross-sectional view of the sheet member and solar cell unit of FIG. [Diagram 23] FIG. 23 is an explanatory diagram of a conventional roof repair method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, the sheet body of the present disclosure will be described with reference to the drawings. Note that the present disclosure can be modified in various ways as long as it has its technical features, and is not limited to the following description and the forms in the drawings.

[0024] The sheet body of the present disclosure is a sheet body that is attached to a structure and used to reinforce or repair the structure, and has an adhesive strength that is a value of 1.5 N / 25 mm or more as measured in a 180° peel test and less than 100% of the maximum test force in the tensile elastic region before being attached to the structure. In other words, the sheet body of the present disclosure has an adhesive strength with a lower limit value of 1.5 N / 25 mm as measured in a 180° peel test and an upper limit value of approximately 100% of the maximum test force in the tensile elastic region before being attached to the structure (the method of determining the value at which the maximum test force in the tensile elastic region is 100% will be described later). For this reason, the adhesive strength of the sheet body of the present disclosure at which the maximum test force in the tensile elastic region is 100% is greater than the adhesive strength at which the measured value in the 180° peel test is 1.5 N / 25 mm. Note that the term "adhesion" used in this specification can also be replaced with the term "bonding".

[0025] [Structure] The structure to which the sheet body of the present disclosure is applied is not particularly limited. Examples of the structure include concrete, wooden, and iron structures. From the viewpoint of once applying the sheet body at the construction site and then peeling it off and reapplying it, examples of the structure include the roof, wall, eaves, fence, gatepost, gate, gate roof, etc. of a house. Such structures have a more complex shape than large structures such as bridge girders, and there is a risk of wrinkles in the sheet body, for example. For this reason, it is often the case that the sheet body cannot be applied successfully in one application operation. Therefore, the technical idea of ​​the present disclosure is easily applied to such structures. Below, the structure will be further explained by taking a roof as an example.

[0026] Further examples of the structure include ordinary houses, and large structures such as gymnasiums, hospitals, and public facilities. The sheet body of the present disclosure can be suitably attached to the roofs of such structures. The shape of the roof is not particularly limited. Examples of the roof include roofs having any shape, such as gabled, hipped, square, flat, single-sided, beckoning, and kamaboko roofs.

[0027] In addition, specific examples of roofs include slate roofs, roofs made of Galvalume Steel Sheets (registered trademark), galvanized iron roofs (roofs made of zinc-plated steel sheets), metal roofs made of iron coated with paint, and concrete roofs including flat roofs. Slate comprises a cement layer, an inorganic decorative (cement) layer disposed on the cement layer, an inorganic colored stone layer disposed on the inorganic decorative layer, and an inorganic coating film disposed on the inorganic colored stone layer. Slate has a simple appearance, a wide variety of colors, and is light and inexpensive, and is therefore widely used as a roofing material for general houses. However, slate roofs are more likely to crack than roofs made of Galvalume Steel Sheets (registered trademark), and have lower durability and waterproofness than roofs made of other materials. For this reason, problems such as breakage are more likely to occur. Therefore, slate roofs are particularly suitable as roofs to which the sheet body of the present disclosure is attached. In the following description, the roof of a structure is also referred to as a "slate roof, etc."

[0028] The surface of the roof may have steps to the same extent as a typical slate roof, etc. Here, the sheet body of the present disclosure preferably has, for example, a specific rigidity. When the sheet body is applied to the roof of a structure, even if the roof of the structure has a step-like surface such as a slate roof, the formation of gaps can be prevented.

[0029] In addition, by applying the sheet body of the present disclosure to the roof of a structure, the sheet body can follow cracks and expansions that occur in the roof of the structure. This has the special effect of preventing deterioration factors such as water and chloride ions from penetrating into the interior of the roof of the structure and discharging moisture inside the roof of the structure as water vapor. In particular, in the case of slate roofs and the above-mentioned flat roofs, which are materials that tend to accumulate rainwater, the ability to discharge water vapor is highly effective in preventing deterioration of the material.

[0030] [Characteristics of sheet body] The sheet body of the present disclosure is used to reinforce or repair the surface of a structure. Specifically, the surface of a structure is reinforced or repaired by attaching one main surface of the sheet body of the present disclosure to the surface of the structure. Note that the object to which the sheet body of the present disclosure is attached is not limited to a structure whose surface has deteriorated or been damaged. By attaching the sheet body of the present disclosure to the surface of a structure in advance, deterioration or damage can be prevented.

[0031] [1] <Adhesive strength of sheet body> The sheet body of the present disclosure has an adhesive strength (initial adhesive strength) of 1.5 N / 25 mm or more measured in a 180° peel test before being attached to a structure. This makes it difficult for the sheet body to peel off even when exposed to strong winds after being attached to the surface of the structure. This makes it easy to maintain the sheet body stably attached to the surface of the structure for a long period of time.

[0032] The measured value in the 180° peel test before application to a structure is, for example, preferably 5 N / 25 mm or more, more preferably 8 N / 25 mm or more, even more preferably 9 N / 25 mm or more, and particularly preferably 12 N / 25 mm or more, and most preferably 15 N / 25 mm or more. If the measured value is set to any of the above ranges, the effect described in [1] above is more easily achieved.

[0033] More specifically, when the measured value is set to a value of 1.5 N / 25 mm or more, a sheet body that can withstand a strong wind range of 15 m / s is easily obtained. When the measured value is set to a value of 5 N / 25 mm or more, a sheet body that can withstand a storm range of 25 m / s is easily obtained. When the measured value is set to a value of 8 N / 25 mm or more, a sheet body that can withstand a storm range of 30 m / s is easily obtained. When the measured value is set to a value of 9 N / 25 mm or more, a sheet body that can withstand a storm range of 45 m / s is easily obtained. When the measured value is set to a value of 12 N / 25 mm or more, a sheet body that can withstand a storm range of 65 m / s is easily obtained. However, the adhesive strength of the sheet body before it is attached to the structure is set to a value less than 100% of the maximum test force in the tensile elastic region, as will be described later, so that the sheet body can be peeled off and reattached after being attached at the construction site.

[0034] (180° peel test) The 180° peel test in this disclosure is performed in accordance with JIS Z0237:2022 "Test methods for adhesive tapes and adhesive sheets" as follows. Testing Equipment The "Autograph AGX-V 10kN" manufactured by Shimadzu Corporation is used. If this test device is no longer available due to discontinuation, etc., a successor model of the test device or a device capable of equivalent measurements can be used. This point is the same for other measuring devices used in this disclosure. The test specimens are prepared as follows, with reference to JIS Z0237:2022 10.1. The materials to be prepared are as follows: Materials for creating test specimens, etc. (A) A rectangular PET film cut to a size of 25 mm on the short side and 200 mm on the long side (T601E (thickness 50 μm) manufactured by Mitsubishi Chemical Corporation or an equivalent product) (B) A rectangular double-sided adhesive tape cut to a size of 25 mm on the short side and 100 mm on the long side (Nitto Denko Corporation No. 5015 (25 mm width) or an equivalent product) (C) A rectangular sheet of the present disclosure cut into a size of 25 mm on the short side and 100 mm on the long side (having a release sheet described later, but the release sheet may be omitted). (D) Adherend: SUS304 steel plate as described in JIS Z0237 10.2.2, with a BA surface finish (hereinafter also referred to as "BASUS plate"). The end side is 75 mm and the long side is 150 mm.

[0035] How to prepare 180° peel specimen (1) The surface of the BASUS plate is cleaned with a nonwoven fabric "BEMCOT M-3II" (registered trademark) manufactured by Asahi Kasei Corporation or an equivalent product to which MEK (methyl ethyl ketone) has been applied. (2) The adhesive surface of the double-sided adhesive tape of (B) is attached to the surface of the sheet body of (C) that does not have a release sheet (the surface opposite to the surface of the sheet body that is to be attached to the structure (the surface that will become the outer surface of the structure with the sheet body after the sheet body is attached to the structure) using a tape pressing roll (manual type with a load of 2 kg). (3) The release liner of the double-sided adhesive tape (B) attached to the sheet body (C) in (2) is peeled off, and then the PET film (A) is attached to the sheet body (C) and the double-sided adhesive tape (B) using a tape pressing roll (manual type with a load of 2 kg) so as to be aligned with the end of the 25 mm side. (4) The release sheet of the sheet body (C) to which the PET film prepared in (3) is attached is peeled off, and the surface of the sheet body that will be attached to the surface of the structure is attached to the BASUS plate prepared in (1) above. When attaching, the tape is attached by moving a tape pressing roll (manual type with a load of 2 kg) back and forth twice. (5) The test specimen prepared in (4) above is stored at room temperature and humidity (23±2°C, 50±10% RH) for 24 hours.

[0036] 180°Peel Test Method The test is carried out in accordance with the method described in JIS Z0237 11.5. Specifically, the test method described in 11.5.1 is "Test method in which the tape and sheet of Method 1 are peeled off at 180° from the stainless steel test plate." The load cell used is set to 1kN. The test conditions are set in an environment of temperature 23±2°C and relative humidity 50±5%RH.

[0037] FIG. 8 is a schematic diagram showing a 180° peel test method. In this test, for example, an apparatus having a configuration shown in FIG. 8 is used. In FIG. 8, the sheet body is shown as a sheet-like object. As shown in FIG. 8, while the lower end of the BASUS plate is fixed by a first chuck jig, the end of the PET film is pulled upward by a second chuck jig. At that time, the test speed is set to 300 mm / min and the peel length is set to 100 mm. After the measurement starts, the measured value of the first 30 mm length is ignored. Then, the adhesive strength of the 30 mm length peeled off from the test plate is measured multiple times. Then, the multiple measured values ​​are averaged. The average value of the obtained measured values ​​is used as the peel adhesive strength value. The adhesive strength of the 180° peel test is measured by the above procedure.

[0038] The sheet body of the present disclosure has an adhesive strength that is less than 100% of the maximum test strength in the tensile elastic region before being attached to a structure. This specifies the upper limit of the adhesive strength of the sheet body. This improves the ease of handling of the sheet body at the construction site.

[0039] Specifically, even after the sheet body has been attached to a structure, if the attachment does not go well (for example, if the sheet body becomes wrinkled), it can be peeled off and reattached. In other words, by setting the upper limit of the adhesive strength to less than 100% of the maximum test force in the tensile elastic region, the sheet body can be peeled off with the maximum tensile force that allows the sheet body to be elastically deformed. By configuring the sheet body so that it has an adhesive strength that allows it to be peeled off with a force less than 100% of the maximum test force in the tensile elastic region before it is attached to a structure, it is possible to prevent the problem of the sheet body being plastically deformed when peeling off, which reduces the adhesive strength and weather resistance, and also makes it easy to use the sheet body by reattaching it.

[0040] From the viewpoint of ease of peeling off the sheet body, the maximum test force in the tensile elastic region before being attached to a structure is preferably, for example, 90% or less of the maximum test force in the tensile elastic region, and more preferably 80% or less. More specifically, if it is 90% or less, for example, the sheet body can be easily peeled off manually without using a jig or machine. Also, if it is 80% or less, the sheet body can be easily peeled off manually.

[0041] The maximum test force in the tensile elastic region in the present disclosure is calculated as follows. (Calculation method for maximum test force in tensile elastic region) Sheet test piece size Adjust the size to 25mm wide and 100mm long. Testing Equipment The “Autograph AGX-V 10kN” manufactured by Shimadzu Corporation is used. -Device settings When using the Shimadzu Autograph AGX-V 10kN, the load cell is set to 1kN and the chuck jig is set to PFG-1kNA.

[0042] Test conditions (tensile test conditions), test method Both short sides of a sheet body (test piece) having a width of 25 mm and a length of 100 mm are fixed with chuck jigs. At this time, the portion of the sheet body (test piece) from the bottom end to 25 mm is fixed with the lower chuck jig, and the portion of the sheet body (test piece) from the top end to 25 mm is fixed with the upper chuck jig. The distance between the chucks is set to approximately 50 mm.

[0043] In this state, a preliminary load is applied to the sheet body (test piece). The preliminary load is applied by moving the upper chuck jig upward at a speed of 5 mm / min until the load applied to the test piece becomes 0.005 N. After that, the upper chuck jig is moved upward at a test speed of 200 mm / min. The point at which the maximum test force drops by 50% in one second is recognized as the breaking point. When implementing the above preliminary load method, the control program of the measuring device can also be used. Specifically, the program can be set to "stretch until a load of 0.005 N is applied as a preliminary load" and then "stretch at a test speed of 200 mm / min until the breaking point is reached." Test environment: The following procedures are performed at 23±2°C and humidity of 50±10%.

[0044] ·Definition of Tensile Elastic Region The tensile elastic region is defined as the stroke from the first maximum point to the minimum point, calculated using the following formula (1).

[0045]

number

[0046] Calculation of maximum test force in tensile elastic region Hereinafter, a specific method for calculating the maximum test force in the tensile elastic region will be described with reference to Figs. 9 and 10. The graph in Fig. 9 shows the relationship between the stroke (elongation of the test piece) and the test force when the sheet body (test piece) is stretched (the upper chuck jig is moved upward). The upper graph in Fig. 10 shows an enlarged view of the region between 0 and 2.5 mm of the stroke on the horizontal axis of the graph in Fig. 9 (the area shown in gray in the graph in Fig. 9). Furthermore, the lower graph in Fig. 10 shows a curve obtained by differentiating the upper graph (graph showing the relationship between the stroke and the test force) twice. Then, the stroke corresponding to the minimum point (the first minimum point in the graph) in the lower graph is obtained, and the test force corresponding to this stroke is calculated from the upper graph. The test force calculated corresponding to this stroke is 100% of the maximum test force in the tensile elastic region.

[0047] The upper limit of adhesive strength of the sheet member of the present disclosure before it is attached to a structure is set to a value less than the maximum test force in the tensile elastic region determined as described above, i.e., a value less than 100% of the maximum test force in the tensile elastic region.

[0048] In the present disclosure, as described above, the sheet body is configured so as to have an adhesive strength such that the measured value in the 180° peel test is 1.5 N / 25 mm or more and the measured value of the maximum test force in the tensile elastic region is less than 100% before being attached to the structure. In order to control the adhesive strength to such values, for example, it is important to control the adhesive strength of the attachment surface of the sheet body to be attached to the structure (hereinafter also simply referred to as the attachment surface). This control can be achieved, for example, by selecting an adhesive material present on or near the attachment surface of the sheet body, or by controlling the content of the adhesive material of the sheet body on or near the attachment surface.

[0049] More specifically, examples of the adhesive material include adhesives that have a low glass transition temperature, such as acrylic, silicone having a siloxane bond, rubber, and urethane, and utilize van der Waals force or electrostatic force. The surface of the sheet body to be attached to the structure may be configured to have a microstructure like a gecko's limbs (a structure that has a large surface area and can utilize intermolecular forces. For example, a structure that has a plurality of nanometer-sized fine hairs, and when these fine hairs come into contact with the target surface, van der Waals force is generated, thereby generating adhesive force to the target surface). Furthermore, a method of using the adhesive in combination with the microstructure is also conceivable. Furthermore, a method of controlling the thickness of the adhesive region (adhesive region) to an appropriate thickness that is neither too thick nor too thin is also effective for controlling the adhesive force. From the viewpoint of easy control of the adhesive force within the range, it is preferable to control the material used for the adhesive and the thickness of the adhesive region in combination.

[0050] In addition, in the sheet member of the present disclosure having a laminated structure including multiple layers, the layer having an attachment surface (for example, the adhesive layer described below) can be formed from the adhesive agent described above, or the thickness of this layer, the material constituting the layer, and the surface properties can be controlled (for example, by adopting the microstructure described above). More specific methods will be described in detail later.

[0051] [2] <Durability of the sheet body (weather resistance)> The sheet body of the present disclosure preferably has an adhesive strength of at least 1.5 N / 25 mm as measured in a 180° peel test, even after a weather load test, for example. This makes it easier to maintain the sheet body 10 attached to the surface of a structure for a long period of time after it is attached to the structure, and makes it less likely to peel off even when exposed to strong winds.

[0052] For example, the measured value in the 180° peel test after the weathering load test is preferably 5 N / 25 mm or more, more preferably 8 N / 25 mm or more. A value of 9 N / 25 mm or more is even more preferable, and a value of 12 N / 25 mm or more is particularly preferable. A value of 15 N / 25 mm or more is most preferable. If the measured value in the 180° peel test after the weathering load test is any of the values ​​in the above ranges, the effect described in [2] above is more easily achieved.

[0053] More specifically, a value of 1.5N / 25mm or more will likely result in a sheet body that can withstand a strong wind range of 15m / s. A value of 5N / 25mm or more will likely result in a sheet body that can withstand a storm range of 25m / s. A value of 8N / 25mm or more will likely result in a sheet body that can withstand a storm range of 30m / s. A value of 9N / 25mm or more will likely result in a sheet body that can withstand a storm range of 45m / s. A value of 12N / 25mm or more will likely result in a sheet body that can withstand a storm range of 65m / s.

[0054] (Weather load test) The weather resistance load test in the present disclosure is carried out by the following method. Specifically, UV irradiation, condensation, and showering are repeatedly performed on the sheet member to be tested under the following conditions. ·Equipment used The metal halide lamp weather meter, Iwasaki Electric Co., Ltd.'s iSuper UV Tester SUV-W161, is used. Test time 300 hours

[0055] Test conditions The test subject is subjected to the following UV irradiation treatment in multiple cycles until 300 hours have passed since the start of the test. One cycle of UV irradiation treatment includes 4 hours of UV irradiation, a 30-second water shower after the UV irradiation, a 4-hour condensation treatment after the shower, and a 30-second shower after the condensation treatment. UV irradiation conditions UV irradiation intensity: 120W / cm 2 Metal halide lamp used, irradiation temperature 63℃, irradiation humidity 50% Shower Conditions Shower water temperature: 25±3℃ Shower time: 30 seconds Shower water volume: 3.18L / min to 5.16L / min condensation environment After the shower, the temperature of the test environment is raised to 60°C in 30 minutes, and then lowered to 25°C over a period of 3.5 hours. The humidity during the test is controlled at 90±10% RH.

[0056] In addition, the sheet body of the present disclosure preferably does not leak water in the waterproofing test before and after the weathering load test. The term "no leaking water" used here is not limited to strictly no leaking at all, but means that no leaking water is visually confirmed from the sheet body in the waterproofing test described below. The inventors of the present application have confirmed that the weather resistance of the sheet body is sufficient if no leaking water is visually confirmed. In the present disclosure, by preventing leaking water in the waterproofing test, the effect of reinforcing and repairing the surface of the structure is easily achieved.

[0057] (Waterproof test) In the present disclosure, the waterproofing test is carried out in the following manner. Prepare two rectangular flexible boards with short sides of 50 mm, long sides of 100 mm, and a thickness of 4.0 mm. The two boards are butted together and fixed so that their long sides are in contact. This produces a square-shaped fixing adherend with a side of 100 mm and a thickness of 4.0 mm.

[0058] A test specimen is prepared by placing a sheet cut into a square shape with a side length of 100 mm on one side of the above-mentioned fixing adherend, with the adhesive surface of the sheet being attached to the surface of the fixing adherend. Then, a polyvinyl chloride pipe with an outer diameter of 42 mm, an inner diameter of 40 mm, and a length of 500 mm is placed upright on one surface of the fixing adherend (the surface that will become the outer surface of the sheet-attached structure to which the sheet has been attached) and the pipe is fixed to the fixing adherend. At this time, the pipe is securely fixed to the surface of the sheet so that when the fluorescent leakage inspection agent described below is poured into the pipe, the fluorescent leakage inspection agent does not leak visually from between the pipe and the sheet.

[0059] After that, 370±0.1g of liquid fluorescent leak detection agent is poured into the tube from the opening at one end, and the tube is left to stand in this state for 24 hours in an environment of 23±2℃ and 50±10% RH. After leaving it for 24 hours, the back surface of the fixing adherend (the surface on which the sheet body is not overlapped) is irradiated with UV light and visually checked for the presence or absence of bright spots or liquid stains. If bright spots or liquid stains are found as a result of visual inspection, the sample is judged to have leaked. If no bright spots or liquid stains are found as a result of visual inspection, it is judged to have "no leaks."

[0060] The sheet body of the present disclosure preferably has an adhesive strength of 1.5 N / 25 mm or more at 180° peel strength after a weather load test, as described above. It is also preferable that the sheet body has waterproofness with no water leakage in a waterproofing test after the weather load test. These characteristics relate to the weather resistance of the sheet body.

[0061] Furthermore, in order to control the weather resistance of the sheet body, it is important to control the weather resistance of the surface opposite to the attached surface of the sheet body (which refers to the surface corresponding to the outer surface of the sheet body-attached structure to which the sheet body is attached, and is hereinafter also referred to as the "surface of the sheet body".) This control can be achieved, for example, by selecting the material used near the surface of the sheet body and controlling the content thereof.

[0062] Furthermore, when the sheet body of the present disclosure has multiple layers, the weather resistance can be controlled by controlling the thickness and surface properties of the layer (e.g., the weather-resistant layer described below) located on the surface of the sheet body. More specifically, such weather resistance can be controlled in the case of a sheet body that contains more bond structures having a bond energy stronger than ultraviolet light (410 KJ / mol) on the surface or near the surface than in other regions. Examples of bond structures having such strong bond energy include bond structures such as siloxane bonds and carbon-fluorine bonds.

[0063] The sheet body of the present disclosure may also have a structure in which the double bonds are reduced, for example, on the surface or near the surface, compared to other regions. In this case, the chemical stability of the sheet body can be improved by reducing the reaction points on the surface or near the surface of the sheet body. An example of a structure in which double bonds are reduced is a structure in which a non-diene rubber is present in greater amounts on the surface or near the surface of the sheet body than in other regions.

[0064] The sheet body of the present disclosure may have a structure in which, for example, on the surface or near the surface, a radical trapping material that traps radicals generated by irradiation with energy rays such as ultraviolet rays (UV) is arranged in a larger amount than in other regions. Alternatively, the sheet body of the present disclosure may have a structure in which, for example, on the surface or near the surface, an additive that absorbs UV and suppresses the generation of radicals, such as a hindered amine light stabilizer (HALS), is arranged in a larger amount than in other regions. Alternatively, the sheet body of the present disclosure may have a structure in which, for example, on the surface or near the surface, an antioxidant such as a phenol or thioether is arranged in a larger amount than in other regions.

[0065] Furthermore, when the sheet member of the present disclosure has a plurality of layers, the weather resistance can also be controlled by forming a layer located on the surface of the sheet member (for example, a weather-resistant layer described later) from a predetermined material. This point will be described in detail later.

[0066] [3] <Handling of the sheet when attaching it to a structure (rigidity against bending)> The sheet body of the present disclosure preferably has, for example, an appropriate rigidity in order to facilitate improvement in handling (e.g., ease of application) when applied to a structure. This facilitates improvement in the handling (e.g., ease of installation) of the sheet body at the construction site. The rigidity of the sheet body can be confirmed by the following deformation test. Specifically, when a deformation test is carried out on the sheet body by sequentially carrying out the operations described in the following items (1), (2), (3), and (4), if the energy calculated by the calculation in the following (4) is 2.0 mJ or more, the sheet body is considered to have an appropriate rigidity. (1) A rectangular sheet body having short sides of 50 mm and long sides of 100 mm is prepared as a sample. (2) The sample is bent so that a pair of short sides on the same surface overlap each other, and a pair of regions of the sample from the edges of the pair of short sides to a position 15 mm away along the long side are grasped and fixed with a fixing portion, thereby forming a curved portion with a circumference of 70 mm between the pair of regions of the sample. (3) With the surfaces of the pair of regions of the sample arranged parallel to the vertical direction and the curved portion facing upward, a disk-shaped pressing tool with a pressing surface of 100 mm in diameter and 10 mm in thickness is used to contact the curved portion from above in an environment of a temperature of 23±2°C and a humidity of 50±10% RH, and the pressing tool is moved downward by 20 mm at a test speed of 30 mm / min. (4) Calculate the energy (movement distance x integral of force) required to move the pressing jig (20 mm).

[0067] Here, the energy in (4) is calculated based on the following formula (2).

[0068]

number

[0069] In formula (2), E is the calculated energy (mJ), F is the test force (N), and s is the displacement of the pressing jig (mm). An example of the measurement results is shown in Fig. 11. The graph in Fig. 11 shows the relationship between the displacement (stroke) (mm) of the pressing jig and the test force (N) on the vertical axis. The area of ​​the shaded part in Fig. 11 represents the energy E.

[0070] Here, Fig. 5(A), Fig. 5(B), Fig. 5(C), and Fig. 5(D) are schematic diagrams for explaining a method for measuring the rigidity of a sheet body according to the present disclosure. Fig. 5(A) is a front view of the sheet body. Fig. 5(B), Fig. 5(C), and Fig. 5(D) show views of a curved sheet body viewed from the thickness direction of the sheet body. Specifically, for example, as shown in Fig. 5(A), a rectangular sheet body with a short side of 50 mm and a long side of 100 mm is prepared as a sample 19. Thereafter, as shown in Fig. 5(B), the sample 19 is curved so that a pair of short sides on the same surface overlap each other, and a pair of regions of the sample 19 from the edge ends of the pair of short sides to a position 15 mm away along the long sides are gripped and fixed by the fixing part 18. As a result, a curved part with a perimeter of 70 mm is formed between the pair of regions of the sample 19 (viewed from the thickness direction of the sample 19).

[0071] Then, as shown in Figures 5(C) and 5(D), with the surfaces of the pair of regions of sample 19 arranged parallel to the vertical direction and with the curved portion facing upward, a disk-shaped pressing tool 17 with a pressing surface having a diameter of 100 mm and a thickness of 10 mm is used to contact the curved portion from above in an environment of a temperature of 23±2°C and a humidity of 50±10% RH, and the pressing tool 17 is moved downward by 20 mm at a test speed of 30 mm / min.

[0072] Here, it is preferable that the energy required when moving the pressing jig 17 (when moving it downward by the 20 mm) is a value of 2.0 mJ or more, which makes it easier to impart appropriate rigidity (for example, appropriate stiffness) to the sheet body.

[0073] The energy required to press and deform the curved portion of the sheet body of the present disclosure is, from the viewpoint of the handleability of the sheet body described above, preferably 2.0 mJ or more, more preferably 3.5 mJ or more, even more preferably 5 mJ or more, even more preferably 10 mJ or more, and even more preferably 20 mJ or more. On the other hand, the upper limit of the energy is, for example, 30 mJ or less from the viewpoint of ensuring the ease of handling. If the energy is any value within each of the above ranges, for example, even if the structure is a roof with steps, a sheet body that is easy to attach along the steps and has excellent handleability can be obtained.

[0074] For example, the energy can be measured using an autograph (AGX-V (10 kN) manufactured by Shimadzu Corporation) while holding a sheet body (sample 19 in FIG. 5) with a pneumatic flat gripper (PFG-1 kNA) manufactured by Shimadzu Corporation. If the test device is no longer available due to discontinuation, etc., a successor model of the test device or a device capable of equivalent measurements can be used.

[0075] In the present disclosure, as described above, in order to improve the handling of the sheet body when it is applied to a structure, the energy required for a predetermined deformation in the test is preferably, for example, 2.0 mJ or more. This can be achieved by controlling the rigidity of the sheet body. In order to control the rigidity of the sheet body, it is important to control the internal structure of the sheet body.

[0076] In order to control the internal structure of the sheet body, for example, a reinforcing material may be inserted into the sheet body to be attached to the structure. In this case, the internal structure of the sheet body can be controlled by changing the content of the reinforcing material. In addition, when the sheet body has multiple layers, the sheet body may have a reinforcing layer (for example, a reinforcing material described later) disposed therein. In this case, the reinforcing layer imparts a predetermined rigidity to the sheet body, thereby controlling the internal structure of the sheet body.

[0077] When the sheet body contains a filler for adjusting strength, specific methods for imparting rigidity to the sheet body include, for example, a method of controlling at least one of the material of the filler, the amount of the filler added to the sheet body, and the size and shape of the filler particles. In this case, the material of the filler may be either an inorganic material or an organic material, or an inorganic material and an organic material may be mixed.

[0078] In addition, nonwoven fabric can also be used as the reinforcing material. In this case, the nonwoven fabric is not particularly limited as long as it is a nonwoven fabric formed into a sheet shape without weaving fibers. In addition, at least one of natural fibers and chemical fibers can be exemplified as fibers constituting the nonwoven fabric. Examples of chemical fibers include fibers made of polyolefin resins such as polypropylene and polyethylene, polyester resins, polyacrylic resins, and polyamide resins such as nylon, as well as copolymers and modified products of these resins, and synthetic fibers made of combinations of these. Among these, polyester fibers are preferable as fibers excellent in water resistance, heat resistance, dimensional stability, weather resistance, etc.

[0079] As a specific method for imparting rigidity to the sheet body, a mesh or a film may be inserted into the sheet body. In this case, the mesh or film may contain at least one of vinylon, PET, polypropylene (polyolefin), polystyrene, and polyvinylidene fluoride. For example, the film may be a biaxially stretched film.

[0080] As a specific method for imparting rigidity to the sheet body, it is also preferable to insert a mesh or foil containing a metal material such as aluminum or steel into the inside of the sheet body. The rigidity of the sheet body can also be controlled by controlling the thickness of the sheet body. Furthermore, in the case of a sheet body having a base layer described later, the rigidity of the sheet body can also be controlled by adjusting the viscoelasticity of the base layer. In this case, the viscoelasticity of the base layer may be adjusted by adjusting the glass transition temperature (Tg, hereinafter also simply referred to as Tg) of the resin contained in the base layer or by changing the degree of crosslinking of the resin. Various methods can be used to control the rigidity of the sheet body, which will be described in detail later.

[0081] The sheet body of the present disclosure has the above-mentioned rigidity and also has a suitable flexibility. For example, the sheet body has flexibility to the extent that it can be wound into a roll. The roll-shaped winding referred to here refers to winding the sheet body on a roll core material having a diameter of, for example, several centimeters or more and several tens of centimeters or less (specifically, for example, a diameter of 10 mm or more and 300 mm or less). Even with a thinner roll core material, it is possible to wind the sheet body to about several meters by hand winding or the like. Therefore, for example, the sheet body can be managed in a roll shape. Furthermore, it is also possible to unfold the sheet body wound in a roll shape at the construction site, and quickly prepare and construct the sheet body cut into a predetermined size. Therefore, the sheet body can be easily and simply applied to a construction target having a relatively large area.

[0082] [Layer structure of sheet body, etc.] The sheet body of the present disclosure is not particularly limited in structure as long as it can be attached to the surface of a structure and has the above-described characteristics (including preferred characteristics). That is, the sheet body of the present disclosure may be composed of a single layer or may be composed of multiple layers. Hereinafter, the sheet body of the present disclosure (first embodiment) composed of a single layer and the sheet body of the present disclosure (second embodiment) composed of multiple layers will be described separately.

[0083] [1] First embodiment (sheet member of the present disclosure composed of a single layer) When the sheet body of the present disclosure is constituted by a single layer, the sheet body may have, for example, a predetermined adhesiveness on the attachment surface side. The sheet body also preferably has a predetermined weather resistance. In this case, the surface side opposite to the attachment surface side of the sheet body may have a predetermined weather resistance. Furthermore, from the viewpoint of ensuring the ease of handling when attaching to a structure, the sheet body preferably has a predetermined rigidity. In this case, for example, a reinforcing member may be disposed inside the sheet body in order to control the rigidity that can withstand bending within a predetermined range. Here, the sheet body 10 in FIG. 3 shows the configuration of the sheet body 10 of the first embodiment in a schematic manner. A specific description will be given below.

[0084] [1-1] In the present disclosure, the adhesiveness of the attachment surface of the sheet body is controlled from the viewpoint of imparting sufficient adhesiveness to structures while providing adhesive strength sufficient for re-attachment at the construction site. Specifically, this can be achieved by selecting an adhesive material present on or near the attachment surface of the sheet body, or by controlling the content of the adhesive material of the sheet body on or near the attachment surface.

[0085] More specifically, examples of the adhesive material include adhesives that have a low glass transition temperature (Tg) and can utilize van der Waals forces or electrostatic forces, such as acrylic, silicone with siloxane bonds, rubber, and urethane. The attachment surface of the sheet body may be configured to have a microstructure (a structure with a large surface area and capable of utilizing intermolecular forces) like the limbs of a gecko. Furthermore, the adhesive may be used in combination with the microstructure. Furthermore, controlling the thickness of the adhesive region of the sheet body (adhesive region) to an appropriate thickness that is neither too thick nor too thin is also effective in controlling the adhesive force. From the viewpoint of easily controlling the adhesive force within a range, it is also preferable to adjust the adhesive material and the thickness of the adhesive region in combination.

[0086] [1-2] The sheet body of the present disclosure preferably has a predetermined weather resistance. From this viewpoint, for example, it is preferable to control the weather resistance of the front surface side of the sheet body. Hereinafter, a specific description will be given.

[0087] The weather resistance of the surface side of the sheet body can be controlled, for example, by selecting a material to be placed on the surface of the sheet body or near the surface and adjusting the content of the material. More specifically, the material can be placed on the surface of the sheet body or near the surface, and the content of the material can be increased on the surface of the sheet body or near the surface, such as a siloxane bond or a carbon-fluorine bond, which can form many bond structures having a bond energy stronger than that of ultraviolet light (410 KJ / mol). Specific examples of such materials include at least one of acrylic silicone, fluororesin, and silicone resin.

[0088] In addition, from the viewpoint of reducing the number of reaction sites on the surface or in the vicinity of the surface of the sheet body and chemically stabilizing the sheet body, the sheet body may contain a material having a structure with few double bonds. When the material is present in a large amount on the surface of the sheet body or in its vicinity, the chemical stability of the surface of the sheet body and in the vicinity of the surface is increased. An example of such a material is a non-diene rubber. Specifically, the non-diene rubber may be at least one of CIIR (chlorinated butyl rubber), BIIR (brominated butyl rubber), and EPDM (ethylene propylene rubber).

[0089] Examples of methods for forming a large number of the above-mentioned bond structures on or near the surface of the sheet body include a method of unevenly distributing at least one of the following on or near the surface of the sheet body: a radical trapping material that traps radicals generated by irradiation with energy rays such as ultraviolet (UV) rays; an additive such as HALS that absorbs UV rays and suppresses the generation of radicals; and an antioxidant such as a phenol or thioether type.

[0090] [1-3] <Sheet body composed of a single layer having a predetermined rigidity> From the viewpoint of providing ease of handling when attaching the sheet body of the present disclosure to a structure, it is preferable that the sheet body has a predetermined rigidity capable of withstanding bending, etc. This will be specifically described below.

[0091] For example, a reinforcing material may be disposed inside the sheet body. For example, the rigidity of the sheet body can be controlled by adjusting the content of the reinforcing material in the sheet body. As a further specific example of a method for controlling the rigidity of the sheet body, at least one of the amount of strength-adjusting filler (which may be either an inorganic material or an organic material, or a mixture of an inorganic material and an organic material) added, the particle size of the filler, and the particle shape of the filler can be adjusted. The sheet body may also include a mesh or film (which may be a biaxially stretched film) containing any of vinylon, PET, polypropylene (polyolefin), polystyrene, polyvinylidene fluoride, etc. as a reinforcing material. Alternatively, the sheet body may preferably include a mesh or foil containing a metal material such as aluminum or steel as a reinforcing material. The rigidity of the sheet body can be controlled by adjusting the thickness of the sheet body. Furthermore, when the sheet body includes a substrate layer described later, the viscoelasticity of the substrate layer can be adjusted by adjusting the Tg of the resin of the substrate layer or changing the degree of crosslinking of the resin, thereby controlling the rigidity of the sheet body.

[0092] [1-4] <Other matters concerning the sheet body composed of a single layer> The sheet body of the present disclosure may have a configuration in which the adhesive component is unevenly distributed on the side of the surface opposite to the surface to be attached, for example. In other words, the sheet body of the present disclosure, which is composed of a single layer, may contain an adhesive component unevenly distributed on the second surface side, which is the surface to be attached to the structure, rather than on the first surface side, which is located on the opposite side to the structure. The following is a detailed description.

[0093] For example, the physical properties of the sheet body may be adjusted by the energy of the electron beam. Specifically, a method of producing a sheet body using an unvulcanized rubber sheet that can be cured by electron beam can be exemplified. In this method, when irradiating the rubber sheet with electron beams, at least one of the thickness of the rubber sheet and the amount of electron beam irradiation is adjusted to obtain a rubber sheet having a structure with different crosslinking degrees between one side and the other side, even though it is a single layer.

[0094] This structure with different crosslinking degrees includes a low crosslinking degree portion and a high crosslinking degree portion. The low crosslinking degree portion has a relatively high adhesiveness, and the high crosslinking degree portion has a relatively low adhesiveness. In the sheet body, the surface side directly irradiated with the electron beam is crosslinked by the electron beam more than the opposite surface side. Therefore, in the sheet body, the high crosslinking degree portion can be arranged on the surface side where the electron beam is irradiated in a controlled manner, and the low crosslinking degree portion can be arranged on the opposite surface side. This results in a sheet body in which the high crosslinking degree portion is arranged on one surface side and the low crosslinking degree portion is arranged on the other surface side. Therefore, in principle, the adhesiveness and water resistance (weather resistance) of the sheet body can be compatible.

[0095] Examples of rubber that can be used for the rubber sheet include isoprene rubber, SBR (styrene butadiene rubber), CR (chloroprene rubber), NBR (acrylonitrile butadiene rubber), HNBR (hydrogenated acrylonitrile butadiene rubber), CIIR (chlorinated butyl rubber), BIIR (brominated butyl rubber), EPDM (ethylene propylene rubber), and the like.

[0096] The following is an example of a method for producing rubber. First, raw rubber is masticated to obtain plasticized rubber. This plasticized rubber is kneaded to obtain a compounded rubber. This compounded rubber is crosslinked (vulcanized) to obtain a crosslinked rubber. In the vulcanization process for crosslinking (vulcanizing) this compounded rubber, one side of the compounded rubber is irradiated with an electron beam to vary the degree of crosslinking in the thickness direction of the compounded rubber, thereby producing a rubber (rubber sheet) having a structure with different degrees of crosslinking on one side and the other side. In this way, the sheet body of the present disclosure may contain rubber and have a crosslinked structure of rubber with different degrees of crosslinking on the first side and the second side.

[0097] The sheet body may have a structure in which the adhesive component is unevenly distributed on the side (first side) opposite to the side (second side) of the sheet body based on, for example, a solution diffusion method. In this case, specifically, a method of manufacturing the sheet body can be exemplified in which resin A and resin B, which have poor compatibility (in other words, solubility parameters are far from each other), are dissolved in a solvent having a solubility parameter intermediate between the solubility parameters of resin A and resin B to prepare a solution, and then the solution is applied and dried. In this case, resin A and resin B are dissolved in the solvent in the solution state, but when the solution is applied and dried, they are phase-separated from each other. This results in a gradient function that allows the sheet body to have different properties.

[0098] The combination of resin A and resin B in the sheet body can be any combination of a resin that exhibits adhesiveness and a resin that exhibits weather resistance and rigidity that can withstand bending. An example of such a combination of resin A and resin B (functionally gradient materials: FGMs) is a combination of acrylic resin and epoxy resin. In this case, the acrylic resin exhibits adhesiveness, and the epoxy resin side is responsible for weather resistance and rigidity. In order to further enhance the weather resistance function of the epoxy resin, a radical trapping material, a UV absorbing material, etc. may be added to the material of the sheet body. In addition, the rigidity of the sheet body can be improved by increasing the degree of crosslinking of the epoxy resin.

[0099] More specifically, the solution may be, for example, a solution containing an acrylic resin, an epoxy resin, and a solvent, MEK, in which the SP value (solubility parameter) of the acrylic resin is around 8, the SP value of the epoxy resin is around 10, and the SP value of the solvent, MEK, is 9.3. In the case of this solution, the acrylic resin and the epoxy resin are each dissolved in the presence of the solvent, but after the solvent volatilizes, the acrylic resin and the epoxy resin are inclined. Therefore, the sheet body can exhibit a gradient function due to the acrylic resin and the epoxy resin. In this way, the sheet body may contain an acrylic resin and an epoxy resin, and have a phase separation structure due to the acrylic resin and the epoxy resin.

[0100] [2] Second embodiment (sheet member of the present disclosure composed of multiple layers) When the sheet body of the present disclosure is composed of a plurality of layers, the sheet body may have a layer disposed on the attachment surface side and having a predetermined adhesiveness. The sheet body preferably has a predetermined weather resistance. In this case, for example, it is preferable that the sheet body has a weather-resistant layer disposed on the surface side opposite to the attachment surface side of the sheet body and having a predetermined weather resistance.

[0101] Furthermore, from the viewpoint of ensuring ease of handling when applied to a structure, the sheet body preferably has a predetermined rigidity. In this case, for example, in order to control the rigidity that can withstand bending within a predetermined range, the sheet body may be configured so that at least one of the first layer arranged on the application surface side and the second layer arranged on the opposite side to the application surface has a predetermined rigidity. Alternatively, the sheet body may be configured so that it includes the first layer arranged on the application surface side, the second layer arranged on the opposite side to the application surface, and the third layer arranged between the first layer and the second layer, and the third layer has a predetermined rigidity. The following is a specific description.

[0102] [2-1] In the present disclosure, from the viewpoint of providing sufficient adhesion to a structure to obtain weather resistance while also providing sufficient adhesive strength to allow re-application at the construction site, it is preferable that the sheet body has a layer (hereinafter this layer is also referred to as the "adhesive layer") that is arranged on the attachment surface side, has a predetermined adhesiveness, and is attached to the structure.

[0103] The adhesiveness of the adhesive layer can be controlled, for example, by adjusting the thickness and surface properties of the adhesive layer, and the material of the adhesive layer. When controlling the surface properties of the adhesive layer, for example, the above-mentioned microstructure can be adopted. Furthermore, setting the thickness of the adhesive layer to an appropriate value that is neither too thick nor too thin is also effective for controlling the adhesiveness of the adhesive layer. In addition, from the viewpoint of easily controlling the adhesive strength of the adhesive layer within a predetermined range, it is also preferable to adjust the adhesive material and the thickness of the adhesive layer in combination.

[0104] More specifically, examples of the material of the adhesive layer include adhesives having a low glass transition temperature (Tg) and capable of utilizing van der Waals force or electrostatic force, such as acrylic, silicone having a siloxane bond, rubber, and urethane. The adhesive force of the adhesive layer can be controlled by adjusting the thickness of the adhesive layer and the degree of crosslinking of the adhesive layer. The attachment surface of the adhesive layer may be configured to have a microstructure (a structure with a large surface area and capable of utilizing intermolecular forces) like the limbs of a gecko. Furthermore, the adhesive and the microstructure may be used in combination. Details of the adhesive layer will be described later.

[0105] [2-2] <Sheet body having a layer arranged on the surface side and having a predetermined weather resistance> The sheet body of the present disclosure preferably has a predetermined weather resistance. From this viewpoint, the sheet body preferably includes, for example, a layer (weather-resistant layer) disposed on the surface side and having a predetermined weather resistance. Hereinafter, the specific description will be given.

[0106] The weather resistance of the weather-resistant layer can be controlled, for example, by adjusting the material of the weather-resistant layer and the content of the material in the weather-resistant layer. More specifically, the material can be a material capable of forming a large amount of bond structures having a stronger bond energy than ultraviolet light (410 KJ / mol), such as siloxane bonds and carbon-fluorine bonds, in the weather-resistant layer, or by increasing the content of the material in the weather-resistant layer. Specific examples of the material for such a weather-resistant layer include at least one of acrylic silicone, fluororesin, and silicone resin.

[0107] In addition, from the viewpoint of reducing the number of reaction sites in the weather-resistant layer and chemically stabilizing the weather-resistant layer, the weather-resistant layer may contain a material having a structure with few double bonds. If the material is present in a large amount in the weather-resistant layer, the chemical stability of the weather-resistant layer increases. An example of such a material is a non-diene rubber. Specifically, an example of the non-diene rubber is at least one of CIIR (chlorinated butyl rubber), BIIR (brominated butyl rubber), and EPDM (ethylene propylene rubber).

[0108] Examples of a method for forming a large amount of the bond structure in the weather-resistant layer include a method of unevenly distributing at least one of a radical trapping material that traps radicals generated by irradiation with energy rays such as ultraviolet (UV) rays, an additive such as HALS that absorbs UV rays and suppresses the generation of radicals, and an antioxidant such as a phenolic or thioether type. Details of such a weather-resistant layer will be described later.

[0109] [2-3] <Sheet body having a layer with a predetermined rigidity> From the viewpoint of ensuring ease of handling when applied to a structure, the sheet body of the present disclosure is preferably controlled to have a rigidity that can withstand folding. For this reason, for example, the sheet body may be configured so that at least one of the first layer arranged on the application surface side and the second layer arranged on the opposite side to the application surface has a predetermined rigidity. Alternatively, the sheet body may be configured to include the first layer arranged on the application surface side, the second layer arranged on the opposite side to the application surface, and the third layer arranged between the first layer and the second layer, and the third layer has a predetermined rigidity. The following is a specific description.

[0110] An example of the first layer arranged on the attachment surface side of the sheet body is an adhesive layer. An example of a method for imparting rigidity to the adhesive layer is a method in which the adhesive layer is configured to include an adhesive and a filler. In this case, the adhesive layer includes an adhesive having a relatively low glass transition temperature (Tg) such as acrylic, silicone having a siloxane bond, rubber, or urethane, which can utilize van der Waals force or electrostatic force, and a filler such as silica, alumina, titanium oxide, calcium carbonate, or carbon black. For example, the rigidity of the adhesive layer can be controlled by adjusting at least one of the amount of filler added to the adhesive layer and the particle shape of the filler. Specifically, examples of the particle shape of the filler include spherical, acicular, amorphous, and tetrapod shapes. In addition, the rigidity of the sheet body can be controlled by adjusting the thickness of the weather-resistant layer. In addition, the rigidity of the sheet body can be controlled by adjusting the Tg of the adhesive in the weather-resistant layer.

[0111] The layer disposed on the surface side of the sheet body, that is, the second layer disposed on the opposite side to the attachment surface of the sheet body, can be exemplified by a weather-resistant layer. As a method for imparting rigidity to the weather-resistant layer, a method of forming the weather-resistant layer so as to include a main material and a filler can be exemplified. In this case, the weather-resistant layer includes a main material such as acrylic silicone, fluororesin, silicone resin, non-diene rubber, and a filler such as silica, alumina, titanium oxide, calcium carbonate, and carbon black. For example, the rigidity of the weather-resistant layer can be controlled by adjusting at least one of the amount of filler added to the weather-resistant layer and the particle shape of the filler. Specifically, examples of the particle shape of the filler include spherical, needle-like, amorphous, and tetrapod-like shapes. In addition, the rigidity of the sheet body can be controlled by adjusting at least one of the thickness of the weather-resistant layer and the Tg of the main material of the weather-resistant layer. In this way, at least one of the adhesive layer and the weather-resistant layer in the sheet body may include a filler.

[0112] In a sheet body having a first layer (e.g., an adhesive layer) arranged on the side to be attached, a second layer (e.g., a weather-resistant layer) arranged on the opposite side to the side to be attached, and a third layer arranged between the first and second layers, the third layer being configured to have a predetermined rigidity, a method of imparting rigidity to the third layer is, for example, to configure the third layer as a substrate layer to be described later, and impart rigidity to the substrate layer. This will be described in detail later.

[0113] [3] <Specific example of the second embodiment> Fig. 1 is a cross-sectional view showing a schematic diagram of a sheet body 10 of a second embodiment having a single adhesive layer and a single weather-resistant layer. Fig. 2 is a cross-sectional view showing a schematic diagram of a sheet body 10 of a second embodiment having multiple base layers and multiple weather-resistant layers. Both the first and second embodiments are examples of "a sheet body of the present disclosure consisting of multiple layers."

[0114] The sheet body 10 of the present disclosure may include at least one base layer 12 and at least one weather-resistant layer 13. As an example, the sheet body 10 of the second embodiment shown in FIG. 1 includes an adhesive layer 11, a single base layer 12 arranged on one side of the adhesive layer 11, a single weather-resistant layer 13 arranged on the side of the base layer 12 opposite to the adhesive layer 11 side, and a release sheet 16 arranged on the other side of the adhesive layer 11. The at least one weather-resistant layer 13 is arranged above the adhesive layer 11. The release sheet 16 is arranged on the side of the adhesive layer 11 opposite to the weather-resistant layer 13 side. The sheet body 10 shown in FIG. 1 has a laminated structure consisting of three layers when the release sheet 16 is removed.

[0115] The sheet body 10 of the second embodiment shown in Fig. 2 includes an adhesive layer 11, a plurality of (here, two) base layers 12 arranged to overlap one side of the adhesive layer 11, a plurality of (here, two) weather-resistant layers 13 arranged to overlap the outermost surface of the base layer 12 opposite to the adhesive layer 11 side, and a release sheet 16 arranged to overlap the other side of the adhesive layer 11. The base layer 12 is arranged between the adhesive layer 11 and the weather-resistant layer 13. When the release sheet 16 is removed, the sheet body 10 shown in Fig. 2 has a laminated structure consisting of five layers. Details of each layer will be described later.

[0116] 2, in the case of a sheet body 10 including a plurality of base layers 12 and a plurality of weather-resistant layers 13, a laminate structure including a plurality of base layers 12 directly laminated to each other and a laminate structure including a plurality of weather-resistant layers 13 directly laminated to each other may be laminated. By using each of such laminate structures, it is possible to easily control the overall thickness or characteristics of each of the base layers 12 or the weather-resistant layers 13 included in the sheet body 10. Therefore, for example, it is possible to easily impart the characteristics described above to the sheet body 10.

[0117] For example, the sheet body 10 may have another layer disposed between the base layer 12 and the weather-resistant layer 13. In other words, the sheet body 10 may have a third layer (another layer) disposed between the first layer (base layer 12) and the second layer (weather-resistant layer 13). This makes it easier to control, for example, the adhesiveness of the sheet body 10 and the overall rigidity of the sheet body 10. As shown in FIG. 1, the sheet body 10 may have, for example, a release sheet 16 attached to the surface of the adhesive layer 11. In this case, the adhesive layer 11 is protected by the release sheet 16, which is preferable. In addition, examples of the laminated structure of the sheet body 10 include a laminated structure including the adhesive layer 11 and the weather-resistant layer 13, as well as a laminated structure in which the base layer 12 and the adhesive layer 11, which have been given weather resistance, are laminated. In the following description, unless otherwise specified, the "sheet body 10" refers to a sheet body 10 having a three-layer laminate structure in which an adhesive layer 11, a base layer 12, and a weather-resistant layer 13 are arranged in this order, as shown in Figure 1.

[0118] (adhesive layer 11) The adhesive layer 11 is preferably composed of, for example, an acrylic adhesive. Acrylic adhesives allow easy adjustment of adhesive strength to the roof of a structure, etc., and have a high degree of freedom in material design, and are also excellent in transparency, weather resistance, and heat resistance. This allows the sheet body 10 to more suitably reinforce or repair the surface of a structure. The acrylic adhesive is not particularly limited, and commercially available products can be used. Examples include Olivine (registered trademark) BPS6574, BPS6554, BPS5565K, etc., manufactured by Toyochem Co., Ltd.

[0119] When an acrylic adhesive is used, the material of the adhesive layer 11 preferably contains an isocyanate crosslinking agent (hardening agent) at a value of, for example, 1 part by weight or more per 100 parts by weight of the acrylic adhesive. The content of the isocyanate crosslinking agent (hardening agent) of the material is more preferably, for example, 4 parts by weight or more per 100 parts by weight of the acrylic adhesive. On the other hand, the content of the isocyanate crosslinking agent (hardening agent) of the material is preferably, for example, 10 parts by weight or less per 100 parts by weight of the acrylic adhesive. The content of the isocyanate crosslinking agent (hardening agent) of the material is more preferably, for example, 6 parts by weight or less per 100 parts by weight of the acrylic adhesive. This makes it easier to control the adhesion of the adhesive layer to the range specified in the present disclosure.

[0120] In addition, when an acrylic adhesive is used, the material of the adhesive layer 11 preferably contains a tackifier (e.g., a rosin-based, terpene-based, petroleum resin-based, phenolic resin-based, or other tackifier) ​​at a value of, for example, 1 part by weight or more per 100 parts by weight of the acrylic adhesive. On the other hand, the content of the tackifier in the material is more preferably, for example, 20 parts by weight or less, and even more preferably 10 parts by weight or less per 100 parts by weight of the acrylic adhesive. This makes it easier to control the adhesiveness of the adhesive layer within the range specified in the present disclosure. In addition, by configuring the sheet body to have multiple (e.g., two) adhesive layers and changing the ratio of the crosslinking agent (curing agent) in each adhesive layer, the adhesive layer 11 is more likely to exhibit stable adhesive force even if the temperature changes to a certain extent.

[0121] The thickness of the adhesive layer 11 is generally 15 μm or more from the viewpoint of exerting sufficient adhesive strength to the surface of the structure. The thickness of the adhesive layer 11 is, for example, preferably 30 μm or more, more preferably 40 μm or more. Furthermore, a value of 50 μm or more is even more preferable, and a value of 70 μm or more is particularly preferable. On the other hand, taking into consideration productivity and the like, the thickness is generally 180 μm or less. The thickness of the adhesive layer 11 is, for example, preferably 170 μm or less, more preferably 160 μm or less. Furthermore, a value of 140 μm or less is even more preferable, and a value of 125 μm or less is most preferable.

[0122] In this way, for example, by appropriately adjusting the thickness of the adhesive layer 11, the initial adhesive strength of the sheet body 10 when the sheet body 10 is attached to the surface of a structure via the adhesive layer 11 and the adhesive strength after a weather resistance load test can be adjusted to be within the above-mentioned range. The optimal range of the thickness of the adhesive layer 11 may vary depending on the type of adhesive used. For example, in the examples described below, an acrylic adhesive, Olivine (registered trademark) BPS5565K manufactured by Toyochem Co., Ltd., is used as the adhesive. When this adhesive is used, the thickness of the adhesive layer 11 is preferably, for example, 20 μm or more and 180 μm or less.

[0123] The storage modulus G' of the adhesive layer 11 at 23±2° C. is, for example, 1×10 3 A value of 1×10 Pa or more is preferable. 4 A value of 1×10 Pa or more is more preferable. 6 A value of 1×10 Pa or less is preferable. 5 A value of 0.1 Pa or less is more preferable. By setting the storage modulus G' of the adhesive layer 11 at 23±2° C. to any value within these ranges, for example, it becomes easy to control the adhesive layer 11 to an appropriate softness. Thus, in the sheet member 10, the adhesive strength can be ensured while the handleability (for example, the sheet member 10 is less likely to slip when attached to a structure) can be easily improved.

[0124] The method for measuring the storage modulus G' will be described. FIG. 15 is a schematic diagram of the method for measuring the storage modulus G'. A DMAQ850 Rheometer DHR-2 (manufactured by TA Instruments Japan, Inc.) is used as a viscoelasticity measuring device. If the test device is no longer manufactured and is difficult to obtain, a successor model of the test device or a device capable of performing equivalent measurements can be used.

[0125] Sample preparation and measurement methods: First, an adhesive layer 11 having a thickness of about 2 mm is prepared. A sample is prepared by punching the adhesive layer 11 into a disk shape of 5 mm. Next, as shown in FIG. 15, the punched sample is sandwiched and fixed between a parallel plate and a lower plate. Then, a vibration having a frequency of 1.0 Hz is applied to the punched sample, and the temperature of the punched sample is changed at 5°C / min in a temperature range of -80°C to 80°C. The storage modulus G' of the punched sample at this time is measured in a shear mode. Here, FIG. 16 is a graph showing an example of measuring the storage modulus G'. For convenience, FIG. 16 shows an example in which the upper limit of the temperature range of the sample is set to 120°C.

[0126] Specific examples of the material of the adhesive layer 11 include Olivine (registered trademark) BPS5565K manufactured by Toyochem Co., Ltd., which is an acrylic adhesive, and BHS8515 manufactured by Toyochem Co., Ltd., which is an isocyanate crosslinking agent (curing agent).

[0127] (Base material layer 12) The base material layer 12 is, for example, a layer that defines the shape of the sheet body 10 of the present disclosure. The base material layer 12 is, for example, preferably a layer that has a function of maintaining the overall shape of the sheet body 10 and imparts a predetermined rigidity to the sheet body 10. The sheet body 10 may have a single base material layer 12 as shown in FIG. 1, or may have a plurality of base material layers 12 as shown in FIG. 2. The number of base material layers 12 included in the sheet body 10 is set in consideration of, for example, the overall thickness of the sheet body 10, the function imparted to the base material layer 12, the length of the factory production line, or the production cost of the sheet body 10. For example, when a single base material layer 12 having a predetermined thickness cannot be obtained because the factory production line is short, a laminated structure of a plurality of base material layers 12 having a predetermined overall thickness may be formed by applying the material of the base material layer 12 in layers.

[0128] The configuration of the base layer 12 is not particularly limited. For example, the base layer 12 preferably contains a composite material of a resin material and a material that imparts rigidity to the sheet body 10. This makes it easier to impart a predetermined rigidity to the sheet body 10. Examples of the resin material contained in the base layer 12 include acrylic resin, acrylic silicone resin, fluororesin, and silicone resin.

[0129] Furthermore, the material that imparts rigidity to the sheet body 10 contained in the base layer 12 can be exemplified by a filler. In this case, examples of fillers include cement, mortar, silica, alumina, titanium oxide, calcium carbonate, and carbon black. In addition, for example, the rigidity of the sheet body 10 can be controlled by adjusting the particle shape of the filler. Specific examples of the particle shape of the filler include spherical, acicular, amorphous, and tetrapod shapes.

[0130] Furthermore, the rigidity of the sheet body 10 can be controlled by adjusting the thickness of the base layer 12. The base layer 12 is preferably composed of, for example, a resin component containing acrylic and mortar. The base layer 12 more preferably contains polymer cement. By controlling the ratio of the resin component and mortar, which are the materials of the base layer 12, the rigidity of the sheet body 10 can be easily controlled and the degree of freedom in material design can be improved. In addition, since the thickness of the base layer 12 that is easy to handle can be obtained, the sheet body 10 can be used more suitably to reinforce or repair the surface of a structure.

[0131] More specifically, as the composition for forming the base layer containing an acrylic resin, Spring Coat (Brush) Mixture manufactured by Kikusui Chemical Industry Co., Ltd., Aronble Coat A450 Base manufactured by Toagosei Co., Ltd., etc. can be used. In addition, as the mortar used in the base layer 12, Spring Coat (Brush) Powder manufactured by Kikusui Chemical Industry Co., Ltd., Aronble Coat A450 Setter manufactured by Toagosei Co., Ltd., etc. can be used. Each of the materials for the composition for forming the base layer and the mortar exemplified above may be used alone or in combination.

[0132] When a resin component and a mortar component are used as the material of the base layer 12, the amount of the resin component relative to the total amount of the mixture of the mortar component and the resin component is preferably, for example, 10 parts by weight or more. The amount of the resin component relative to the total amount of the mixture is more preferably, for example, 20 parts by weight or more, more preferably, 30 parts by weight or more, and most preferably, 40 parts by weight or more. On the other hand, the amount of the resin component relative to the total amount of the mixture is preferably 90 parts by weight or less, more preferably, 80 parts by weight or less, more preferably, 70 parts by weight or less, and most preferably, 60 parts by weight or less. This makes it easier to ensure the adhesion of the base layer 12 to the weather-resistant layer 13 described later, and to impart appropriate rigidity to the sheet body 10.

[0133] A film- or mesh-shaped reinforcing material may be used as a material for imparting rigidity. This reinforcing material is disposed, for example, inside the base layer 12. Examples of the reinforcing material contained in the base layer 12 include meshes and films (which may be biaxially stretched films) made of vinylon, PET, polypropylene (polyolefin), polystyrene, polyvinylidene fluoride, and the like. Also, meshes and foils made of metal materials such as aluminum and steel are preferable as the reinforcing material contained in the base layer 12. In this way, the base layer 12 may include a reinforcing material in the form of a mesh, film, or foil.

[0134] FIG. 6 is a schematic diagram showing an example of the reinforcing material 15 of the sheet body 10 of the present disclosure. FIG. 7 is a partially enlarged view of the reinforcing material 15 of FIG. 6. The reinforcing material 15 shown in FIGS. 6 and 7 is a material used in the base layer 12, and has, as an example, a biaxially woven structure in which warp and weft fibers are arranged in a lattice pattern. The shape of the reinforcing material 15 is not particularly limited. In addition to the biaxially woven structure shown in FIGS. 6 and 7, any shape such as a triaxially woven structure can be exemplified as the shape of the reinforcing material 15. As the reinforcing material 15, for example, a mesh material such as a high-strength vinylon mesh (for example, for civil engineering applications) or a cheesecloth formed of vinylon (for example, for agricultural applications), polyester, polyvinyl alcohol, or the like is preferable. These reinforcing materials 15 can easily widen the elastic range of the sheet body 10. In addition, it can easily impart appropriate rigidity to the sheet body 10. Furthermore, the handling of the sheet body 10 can be improved.

[0135] For example, the line pitch of the reinforcing material 15 is preferably 50 mm or more and 1.2 mm or less. In other words, the line density of the reinforcing material 15 is preferably 0.2 lines / cm or more and 8.0 lines / cm or less. Such a reinforcing material 15 can easily impart rigidity to the sheet body 10 while ensuring the tensile strength of the sheet body 10.

[0136] For example, when the base material layer 12 is viewed in a plane, the reinforcing material 15 may have a size sufficient to cover the entire surface of the base material layer 12, or may have a size smaller than the base material layer 12. That is, the area of ​​the reinforcing material 15 when viewed in a plane may be equal to or smaller than the area of ​​the base material layer 12 when viewed in a plane.

[0137] The area of ​​the reinforcing material 15 in plan view (area in plan view) is preferably, for example, 60% or more and 95% or less of the area in plan view of the base layer 12. If the area in plan view of the reinforcing material 15 is 60% or more, for example, it is easy to ensure the rigidity of the sheet body 10 and easy to control the elongation rate of the sheet body 10. In addition, it is easy to suppress the variation in rigidity in different regions of the sheet body 10. In addition, if the area in plan view of the reinforcing material 15 is 95% or less, for example, when the base layer 12 is formed so as to sandwich the reinforcing material 15 in the thickness direction of the sheet body 10, it is easy to ensure the adhesive strength of the reinforcing material 15 to the base layer 12 in the entire base layer 12. The area in plan view of the reinforcing material 15 can be measured by a known method.

[0138] The thickness of the reinforcing material 15 is, for example, 10% or more of the thickness of the base layer 12. The thickness of the reinforcing material 15 is, for example, preferably 20% or more of the thickness of the base layer 12, more preferably 30% or more, particularly preferably 40% or more, and most preferably 50% or more. On the other hand, the thickness of the reinforcing material 15 is, for example, 80% or less of the thickness of the base layer 12. The thickness of the reinforcing material 15 is, for example, preferably 70% or less of the thickness of the base layer 12, more preferably 60% or less, and particularly preferably 55% or less. By setting the thickness of the base layer 12 in this way, it is possible to easily impart appropriate rigidity to the sheet body 10.

[0139] Furthermore, by setting the thickness of the reinforcing material 15 and the thickness of the base layer 12 to have the above-mentioned relationship, the sheet body 10 of the present disclosure can be configured to have excellent adhesion between the adhesive layer 11 and the base layer 12 and appropriate rigidity. Therefore, excellent handleability can be obtained when the sheet body 10 is attached to the roof of a structure, and the structure can be protected by the sheet body 10 for a long period of time without causing wrinkles or gaps with the roof of the structure. For example, the lower limit of the thickness of the reinforcing material 15 relative to the thickness of the base layer 12 is preferably 45%, and the upper limit of the thickness is preferably 55%.

[0140] Furthermore, the rigidity of the sheet body 10 can be controlled by adjusting the Tg of the resin component contained in the base layer 12. The rigidity of the sheet body 10 can also be controlled by adjusting the amount and diameter of voids in the base layer 12. When the sheet body 10 includes a plurality of base layers 12, the sheet body 10 may include, for example, a first base layer 12 including a resin component having a Tg of a predetermined value, and a second base layer 12 including a resin component having a Tg lower than that of the resin component included in the first base layer 12.

[0141] From the viewpoint of ensuring the rigidity of the sheet body 10, the thickness of the base layer 12 is, for example, 100 μm or more. The thickness of the base layer 12 is, for example, preferably 200 μm or more, more preferably 300 μm or more, and most preferably 350 μm or more. On the other hand, taking into consideration the productivity and the like, the thickness of the base layer 12 is, for example, 1500 μm or less. The thickness of the base layer 12 is preferably 1200 μm or less, more preferably 1000 μm or less, and most preferably 750 μm or less. In this way, by appropriately adjusting the thickness of the base layer 12, the appropriate rigidity of the sheet body 10 can be obtained.

[0142] When a resin component, a mortar component, and a reinforcing material 15 are used as materials for the base layer 12, as a specific example, a Spring Coat (Brush) admixture liquid manufactured by Kikusui Chemical Industry Co., Ltd. can be used as the resin component. Also, a Spring Coat (Brush) powder manufactured by Kikusui Chemical Industry Co., Ltd. can be used as the mortar component. Also, a vinylon-based mesh material (cheesecloth (BINEO (registered trademark) "V520") manufactured by Unitika Co., Ltd. can be used as the reinforcing material 15 (mesh component).

[0143] (Weatherproof layer 13) The weather-resistant layer 13 is a layer disposed on the opposite side of the surface of the structure and exposed to the outside. The sheet body 10 may have a single weather-resistant layer 13 as shown in FIG. 1, or may have multiple weather-resistant layers 13 as shown in FIG. 2. The number of weather-resistant layers provided in the sheet body 10 is set in consideration of the overall thickness of the sheet body 10, the functions to be provided (weather resistance, waterproofness, salt barrier properties, neutralization prevention properties, water vapor permeability, etc.), the length of the factory production line, production costs, etc. For example, if a single weather-resistant layer 13 having a predetermined thickness cannot be obtained due to a short production line, a layered structure of multiple weather-resistant layers 13 having a predetermined overall thickness may be formed by applying the material of the weather-resistant layer 13 in layers.

[0144] The weather-resistant layer 13 is preferably, for example, a layer that ensures the weather resistance of the sheet body 10. For example, the weather-resistant layer 13 is preferably formed by applying a paint that is flexible and can conform to cracks and fissures that occur on the roof of the structure, and that can form a weather-resistant layer 13 that is excellent in waterproofing, salt insulation, neutralization prevention, and water vapor permeability.

[0145] When the weather-resistant layer 13 contains a resin, the resin is preferably a resin having a bond structure with a bond energy stronger than that of ultraviolet light (410 KJ / mol). Examples of such resins include acrylic resins exhibiting rubber properties (e.g., synthetic rubbers mainly composed of acrylic esters), acrylic urethane resins, acrylic silicone resins, fluororesins, soft epoxy resins, polybutadiene rubbers, and the like. Among these, acrylic silicone resins are preferred from the viewpoint of making it easier to ensure weather resistance. The resin contained in the weather-resistant layer 13 may be the same as the resin component contained in the base layer 12. The resin contained in the weather-resistant layer 13 is preferably a resin containing an elastic film-forming component such as rubber. Among these resins, acrylic silicone resins are preferred because they are excellent in safety and coatability and are non-hazardous materials under the Fire Service Act.

[0146] An example of a method for forming the weather-resistant layer 13 is to prepare a coating liquid by mixing a resin and a solvent, apply the coating liquid onto a release sheet, and then dry and remove the solvent from the coating film. The solvent may be water or an aqueous solvent, or may be an organic solvent such as xylene or mineral spirits.

[0147] The weather-resistant layer 13 may contain a pigment from the viewpoint of providing a wide variety of colors for the sheet member 10. The weather-resistant layer 13 may contain an inorganic substance. When the weather-resistant layer 13 contains an inorganic substance, the weather-resistant layer 13 can be provided with scratch resistance. The inorganic substance contained in the weather-resistant layer 13 is not particularly limited, and examples thereof include conventionally known materials such as metal oxide particles such as silica, alumina, and titania.

[0148] The weather-resistant layer 13 may also contain a known antifouling agent. The sheet body 10 is usually used to reinforce or repair a structure installed outdoors. For this reason, the weather-resistant layer 13 is often stained, but by having the weather-resistant layer 13 contain an antifouling agent, the sheet body 10 can be suitably prevented from being stained. The antifouling agent contained in the weather-resistant layer 13 is not particularly limited, and for example, a known material can be used. The weather-resistant layer 13 may also contain an additive that can impart various functions to the sheet body 10. Examples of such additives include cellulose nanofibers.

[0149] The weather-resistant layer 13 preferably contains, for example, an acrylic silicone resin. The acrylic silicone resin allows easy control of weather resistance, color, and the degree of resin deterioration by adjusting the ratio of siloxane bonds, and has a high degree of freedom in material design. In addition, since it has excellent heat resistance and cold resistance, the sheet body 10 can more suitably reinforce or repair the surface of a structure. Examples of the acrylic silicone resin contained in the weather-resistant layer 13 include a weather-resistant layer forming composition containing an acrylic resin (Cool Life SP Black (CB1) P5-0 manufactured by Dainichi Seikagaku Kogyo Co., Ltd., Bell Earth Elastic Black manufactured by Fujikura Kasei Co., Ltd., Aronble Coat T-1000 manufactured by Toagosei Co., Ltd., Acryset EMN325E manufactured by Nippon Shokubai Co., Ltd., and U-Double EF008 manufactured by Nippon Shokubai Co., Ltd.). Each of these materials may be used alone or in combination.

[0150] When using an acrylic silicone resin, an acrylic silicone resin having a Tg of 0° C. or less and an acrylic silicone resin having a Tg of more than 0° C. may be used. In this case, for example, the acrylic silicone resin having a Tg of more than 0° C. may be added in an amount of 0 parts by weight or more to 100 parts by weight of the acrylic silicone resin having a Tg of 0° C. or less.

[0151] The amount of the acrylic silicone resin having a Tg greater than 0°C added is, for example, more preferably 20 parts by weight or more, even more preferably 50 parts by weight or more, and most preferably 80 parts by weight or more, per 100 parts by weight of the acrylic silicone resin having a Tg of 0°C or less.

[0152] On the other hand, the amount of the acrylic silicone resin having a Tg greater than 0 ° C. added is preferably 200 parts by weight or less, more preferably 180 parts by weight or less, even more preferably 150 parts by weight or less, and most preferably 120 parts by weight or less, relative to 100 parts by weight of the acrylic silicone resin having a Tg of 0 ° C. or less. By using an acrylic silicone resin having a Tg of 0 ° C. or less and an acrylic silicone resin having a Tg of greater than 0 ° C. at any value within each of the above ranges, the heat resistance of the weather-resistant layer 13 that can prevent blocking from occurring in summer and the cold resistance of the weather-resistant layer 13 that can prevent problems such as cracking in winter can be maintained. Therefore, it is easy to control the sheet body 10 to the desired performance.

[0153] The thickness of the weather-resistant layer 13 is set arbitrarily depending on, for example, the use form, age, or shape of the roof of the structure. The thickness of the weather-resistant layer 13 is, for example, 10 μm or more from the viewpoint of ensuring weather resistance. The thickness of the weather-resistant layer 13 is, for example, preferably 30 μm or more, more preferably 50 μm or more, even more preferably 70 μm or more, and particularly preferably 90 μm or more. In another example, a value of 100 μm or more is even more preferable. On the other hand, the thickness of the weather-resistant layer 13 is, for example, 500 μm or less, taking into consideration productivity and the like. The thickness of the weather-resistant layer 13 is, for example, preferably 400 μm or less, more preferably 300 μm or less, even more preferably 200 μm or less, and most preferably 150 μm or less. If the thickness of the weather-resistant layer 13 is any value within each of the above ranges, the weather resistance of the sheet body 10 required in the present disclosure can be easily ensured. Moreover, from the viewpoint of ensuring weather resistance, it is preferable, for example, that there is little variation in the thickness of the weather-resistant layer 13. Specifically, it is preferable that the variation in the thickness of the weather-resistant layer 13 is within ±30% of the thickness of the weather-resistant layer 13. Such precision in the thickness of the weather-resistant layer 13 can be easily achieved by manufacturing the sheet body 10 on a production line in a factory.

[0154] In this way, by appropriately adjusting the thickness of the weather-resistant layer 13 to any value within the above ranges, the sheet body 10 can be easily adjusted so that the sheet body 10 has an adhesive strength of 1.5 N / 25 mm or more measured in a 180° peel test and less than 100% of the maximum test force in the tensile elastic region before being attached to a structure. In this case, it is preferable that the weather-resistant layer 13 contains an acrylic silicone resin as a specific example of the material. As the acrylic silicone resin contained in the weather-resistant layer 13, for example, a weather-resistant layer forming composition containing an acrylic resin (Cool Life SP Black (CB1) P5-0 manufactured by Dainichi Seikagaku Kogyo Co., Ltd., Bell Earth Elastic Black manufactured by Fujikura Kasei Co., Ltd., etc.) can be used.

[0155] (Sheet body 10) The thickness of the sheet body 10 in the present disclosure is, for example, 10 μm or more from the viewpoint of imparting a predetermined characteristic to the sheet body 10. The thickness of the sheet body 10 is, for example, preferably 100 μm or more, more preferably 300 μm or more. Furthermore, a value of 500 μm or more is even more preferable, and a value of 600 μm or more is most preferable. Furthermore, for example, the thickness of the sheet body 10 is a value of 10 cm or less. The thickness of the sheet body 10 is, for example, preferably 5 cm or less, more preferably 1 cm or less, and even more preferably 5 mm or less. Furthermore, a value of 1 mm or less is particularly preferable, and a value of 800 μm or less is most preferable.

[0156] From the viewpoint of stably imparting predetermined properties to the sheet body 10, the thickness distribution of the sheet body 10 is preferably, for example, a value of ±10% or less of the total thickness of the sheet body 10. By having the thickness distribution of the sheet body 10 within the above range, for example, even an unskilled worker can easily and stably provide a layer with small thickness variation on the surface of a structure. Furthermore, by controlling the thickness distribution within the above range, it becomes easier to uniformly reinforce the structure.

[0157] The method for producing the sheet body 10 is not particularly limited, but will be exemplified below. First, a coating liquid, which is a material for the weather-resistant layer 13, is applied onto a predetermined shape-imparting sheet 14 (see FIG. 19) which is a substrate. Thereafter, the solvent in the coating film formed by the above application is removed by heating, or the resin in the coating film is cured, or the like. In this way, the weather-resistant layer 13 is formed. Next, a coating liquid, which is a material for the substrate layer 12, is applied onto the weather-resistant layer 13. Thereafter, the solvent in the coating film formed by the above application is removed by heating, or the resin in the coating film is cured, or the like. In this way, the substrate layer 12 is formed.

[0158] On the other hand, a coating liquid, which is a material for the adhesive layer 11, is applied onto the release sheet 16. Thereafter, the solvent in the coating film formed by the above application is removed by heating, or the resin in the coating film is cured, etc., thereby forming the adhesive layer 11. Thereafter, the weather-resistant layer 13 and the base layer 12 are joined to form a bonded body. The shape-imparting sheet 14 is peeled off from this bonded body, and the adhesive layer 11 is attached to the base layer 12 side. In this manner, the sheet body 10 is manufactured.

[0159] A more specific method for producing the sheet body 10 will be described below. First, a coating liquid, which is the material of the weather-resistant layer 13, is applied onto a previously prepared shape-imparting sheet 14. Thereafter, the solvent in the coating film formed by the above application is dried and removed, thereby forming the weather-resistant layer 13.

[0160] Next, a coating liquid, which is the material of the base layer 12, is applied to the upper surface of the weather-resistant layer 13. At this time, a reinforcing material 15 such as a mesh, film, or foil is inserted into the applied coating liquid as necessary. Thereafter, the solvent in the coating film formed by the above application is dried and removed, thereby forming the coating film of the base layer 12.

[0161] On the other hand, a coating liquid, which is a material for the adhesive layer 11, is applied onto the release sheet 16. The solvent in the coating film formed by the above application is then dried and removed to form the adhesive layer 11. The adhesive layer 11 is then superimposed on and adhered to the base layer 12. The shape-imparting sheet 14 is then peeled off from the weather-resistant layer 13. In this manner, the sheet body 10 is manufactured.

[0162] When the sheet body 10 of the present disclosure is applied to a structure, a protective structure for the structure is obtained that includes the sheet body 10 and the structure on which the sheet body 10 is disposed. In this case, the sheet body 10 according to any one of the aspects of the present disclosure described herein is applied to the protective structure.

[0163] The sheet body 10 of the present disclosure may be used in a state where two or more layers are stacked. In this case, a protective structure for a structure is obtained that includes a laminate including a plurality of sheet bodies 10 arranged in the thickness direction and a structure on which the laminate is arranged. In this case, a plurality of sheet bodies 10 according to any of the aspects of the present disclosure described herein are applied to the laminate.

[0164] In this case, by placing another sheet body 10 on the surface of the structure protected by one sheet body 10, the surface of the structure can be further protected by the sheet body 10. In this laminate, for example, at least a part of one sheet body 10 may be placed on top of a part of the other sheet body 10. In other words, for example, an end of one sheet body 10 may be placed on top of an end of the other sheet body 10. Alternatively, for example, the entirety of the other sheet body 10 may be placed on top of the entirety of one sheet body 10. In the laminate, the multiple sheet bodies 10 may be attached to each other.

[0165] (Release sheet 16) The release sheet 16 is attached to the surface of the adhesive layer 11 opposite to the base layer 12 side. It is preferable that the release sheet 16 is attached to the sheet body 10 for the purpose of surface protection of the adhesive layer 11 before use. Here, FIG. 3 is a schematic diagram showing how the release sheet 16 is peeled off from the sheet body 10 of the present disclosure. FIG. 4 is a schematic diagram showing how the sheet body 10 of FIG. 3 is attached to a structure. As shown in FIG. 3, the release sheet 16 is peeled off when the sheet body 10 is attached to the roof of the structure 21. As shown in FIG. 4, the sheet body 10 in which the adhesive layer 11 is exposed by peeling off the release sheet 16 is attached to the roof of the structure 21 by bringing the adhesive layer 11 into contact with the roof of the structure 21.

[0166] The structure of the release sheet 16 is not particularly limited, and may be, for example, a sheet having a support layer and a release layer. Examples of materials constituting the support layer include polyesters such as polyethylene terephthalate and polyethylene naphthalate, polyolefins such as polyethylene, polypropylene, and polymethylpentene, polyamides such as nylon 6, vinyl resins such as polyvinyl chloride, acrylic resins such as polymethyl methacrylate, cellulose resins such as cellulose acetate, and synthetic resins such as polycarbonate. The support layer may be formed mainly from paper. Furthermore, the support layer may be a laminate having two or more constituent layers.

[0167] Examples of materials constituting the release layer include silicone resins, melamine resins, fluorinated polymers, etc. The release layer can be formed, for example, by applying a coating liquid containing the material constituting the release layer and an organic solvent onto the support layer by a known coating method such as gravure coating, roll coating, comma coating, or lip coating, and drying and curing the coating film formed by the application. In addition, when forming the release layer, the surface of the support layer on which the release layer is to be formed may be previously subjected to corona treatment or easy-adhesion treatment.

[0168] (Shape-imparting sheet 14) The shape-imparting sheet 14 is used as a base material when the sheet body 10 is manufactured. The shape-imparting sheet 14 may include a resin laminated paper or a resin film, which is a process paper used in the manufacturing process of the sheet body 10. The resin laminated paper referred to here may have an olefin resin layer such as polypropylene or polyethylene. Specifically, the shape-imparting sheet 14 may be, for example, a PP laminated sheet (manufactured by, for example, Lintec Corporation). The thickness of this PP laminated sheet is, for example, 50 μm or more and 200 μm or less.

[0169] As described above, the sheet body 10 has a degree of flexibility that allows it to be wound into a roll. Therefore, by rolling up the sheet body 10, a roll body 26 can be formed, for example, as shown in Fig. 20 described later.

[0170] Further configurations of the sheet body 10 are illustrated below. Fig. 17 is a cross-sectional view showing a schematic configuration of the sheet body 10 according to the third embodiment. When the above-mentioned release sheet 16 is the first release sheet 16, the sheet body 10 of this embodiment includes a second release sheet 25 arranged on the opposite side of the weather-resistant layer 13 from the adhesive layer 11 side. As an example, the sheet body 10 has the first release sheet 16, the adhesive layer 11, the base layer 12, the weather-resistant layer 13, and the second release sheet 25 arranged in this order in the thickness direction.

[0171] The second release sheet 25 is configured such that when the surface 25a exposed to the outside comes into contact with the surface 16a exposed to the outside of the first release sheet 16, the surfaces 25a, 16a are unlikely to adhere to each other. Therefore, when the sheet body 10 is unwound from the roll body 26, the first release sheet 16 can be easily separated from the second release sheet 25, and the sheet body 10 can be easily unwound.

[0172] In addition, the second release sheet 25 has a predetermined rigidity. Therefore, the rigidity of the remaining sheet body 10 after the first release sheet 16 is peeled off can be improved. Therefore, even if the rigidity of the remaining sheet body 10 after the first release sheet 16 and the second release sheet 25 are peeled off is low, the handling when attaching the sheet 10 can be improved, and the sheet body 10 can be easily attached to the surface of the structure. In addition, the remaining sheet body 10 after the first release sheet 16 and the second release sheet 25 are peeled off can be designed to have a relatively small rigidity. Therefore, for example, even if the shape of the surface of the structure to which the sheet body 10 is attached is not flat due to height differences caused by unevenness or defects, the sheet body 10 can be attached by being well conformed to the surface. In addition, for example, the anchor effect on the surface can be improved, so that the adhesive force of the sheet body 10 can be sufficiently improved within an allowable range.

[0173] The structure of the second release sheet 25 can be appropriately set. For example, as shown in Fig. 17, the second release sheet 25 has a contact layer 23 that contacts the first release sheet 16 when the sheet body 10 is wound into a roll, and a weak adhesive layer 24 that is disposed on the first release sheet 16 side of the contact layer 23 when the sheet body 10 is disposed flat.

[0174] The contact layer 23 may be composed of a single layer or multiple layers. The contact layer 23 may contain a resin. In other words, the contact layer 23 may be a resin layer. Examples of the resin contained in the contact layer 23 include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefins such as polyethylene, polypropylene, and polymethylpentene, polyamides such as nylon 6 and aramid, vinyl resins such as polyvinyl chloride, acrylic resins such as polymethyl methacrylate, cellulose resins such as cellulose acetate, synthetic resins such as polycarbonate, and urethane.

[0175] Alternatively, the contact layer 23 may be a fiber layer containing a fiber component and a binder component that binds the fiber component. Alternatively, the contact layer 23 may contain paper. In this case, the contact layer 23 may contain paper as a main component, or may contain paper together with a predetermined main component. When the contact layer 23 contains paper, the contact layer 23 preferably contains paper having a strength such that the contact layer 23 is not accidentally torn when the sheet body 10 is attached to the application target. When the contact layer 23 contains paper, the contact layer 23 preferably contains silicone having a siloxane bond together with paper. The contact layer 23 has a higher rigidity than, for example, the remaining portion of the sheet body 10 from which the release sheet 16 and the second release sheet 25 are omitted and the contact layer 23 and the weak adhesive layer 24 are omitted.

[0176] The thickness of the contact layer 23 can be appropriately set, for example, to a value of 20 μm or more and 500 μm or less. When the contact layer 23 contains polyethylene terephthalate (PET), the thickness of the contact layer 23 is preferably, for example, a value of 20 μm or more and 50 μm or less.

[0177] The weakly adhesive layer 24 has a relatively low adhesive strength. For example, the adhesive strength of the weakly adhesive layer 24 to the weather-resistant layer 13 is lower than the adhesive strength of the adhesive layer 11 to the base material layer 12. Also, for example, the adhesive strength of the weakly adhesive layer 24 to the contact layer 23 is higher than the adhesive strength of the weakly adhesive layer 24 to the weather-resistant layer 13. The weakly adhesive layer 24 may be attached to the weather-resistant layer 13 by, for example, static electricity. The weakly adhesive layer 24 may contain a main component whose Tg is substantially 0. The weakly adhesive layer 24 may contain, for example, ethylene vinyl acetate (EVA), urethane, silicone having a siloxane bond, acrylic, or the like. The second release sheet 25 is not limited to the above-mentioned configuration, and may be, for example, the shape-imparting sheet 14.

[0178] 18 is a cross-sectional view showing a schematic configuration of a sheet body 10 according to a fourth embodiment. The sheet body 10 of this embodiment includes a release sheet 29 arranged on the opposite side of the weather-resistant layer 13 from the adhesive layer 11. As an example, the sheet body 10 has the adhesive layer 11, the base layer 12, the weather-resistant layer 13, and the release sheet 29 arranged in this order in the thickness direction. In the sheet body 10 of this embodiment, the release sheet 16 is omitted.

[0179] The release sheet 29 contains a surface 29a exposed to the outside and a release agent disposed in the vicinity thereof. An example of the release agent is silicone having a siloxane bond. This makes it difficult for the surface 29a and the attachment surface 11a of the adhesive layer 11 to adhere to each other when the surface 29a exposed to the outside of the release sheet 29 comes into contact with the attachment surface 11a of the adhesive layer 11 in the roll body 26. Therefore, when the sheet body 10 is unwound from the roll body 26, the adhesive layer 11 can be easily peeled off from the release sheet 29, and the sheet body 10 can be easily unwound.

[0180] In this manner, in the present disclosure, when the sheet body 10 is unwound from the roll body 26, for example, the sheet body 10 may be made easy to unwound from the roll body 26 in advance so that the portion of the sheet body 10 provided with the adhesive component does not adhere to other portions of the sheet body 10 and become difficult to remove. The release sheet 29 has a predetermined rigidity. Therefore, in this embodiment, even if the release sheet 16 is omitted, the rigidity of the sheet body 10 can be improved. Therefore, the handleability of the sheet body 10 is improved, and the sheet body 10 can be easily attached to the attachment target of the structure. In this case, the release sheet 29 has a higher rigidity than the remaining sheet body 10 from which the release sheet 29 has been peeled off.

[0181] The structure of the release sheet 29 can be set appropriately. For example, as shown in Fig. 18, the release sheet 29 has a release base layer 28 having a surface 29a that contacts the attachment surface 11a of the adhesive layer 11 when the sheet body 10 is wound into a roll, and a weak adhesive layer 24 arranged on the adhesive layer 11 side of the release base layer 28 when the sheet body 10 is arranged flat. The release base layer 28 may have the same structure as the contact layer 23, except that it contains a release agent. The release sheet 29 may also have a release agent layer arranged on the surface 29a.

[0182] 19 is a cross-sectional view showing a schematic configuration of a sheet body 10 according to a fifth embodiment. The sheet body 10 of this embodiment includes a shape-imparting sheet 14 arranged on the opposite side of the weather-resistant layer 13 from the adhesive layer 11 side when arranged flat. The shape-imparting sheet 14 is a sheet used when forming the weather-resistant layer 13 described above. The sheet body 10 of this embodiment includes the shape-imparting sheet 14, which is not peeled off even after the weather-resistant layer 13 is formed.

[0183] As an example, the sheet body 10 has a release sheet 16, an adhesive layer 11, a base layer 12, a weather-resistant layer 13, and a shape-imparting sheet 14 arranged in this order in the thickness direction. The surface 14a exposed to the outside of the shape-imparting sheet 14 and the surface 16a exposed to the outside of the release sheet 16 are configured so as not to adhere to each other when they come into contact with each other. Therefore, when the sheet body 10 is unwound from the roll body 26, it can be easily unwound. The shape-imparting sheet 14 has a predetermined rigidity. In this case, the shape-imparting sheet 14 has a higher rigidity than the remaining sheet body 10 from which the release sheet 16 and the shape-imparting sheet 14 have been peeled off. Therefore, in the remaining sheet body 10 from which the release sheet 16 has been peeled off, the rigidity of the sheet body 10 can be improved by the shape-imparting sheet 14. Therefore, even if the rigidity of the remaining sheet body 10 after the first release sheet 16 and the shape-imparting sheet 14 are peeled off and removed is low, the handleability of the sheet body 10 can be improved and the sheet body 10 can be easily attached to the target object of the structure.

[0184] The shape-imparting sheet 14 may contain a resin-laminated paper having pseudo-adhesion, which is a property in which two components attached to each other cannot be adhered again once they are peeled off. In this case, for example, the shape-imparting sheet 14 may contain a resin-laminated paper in which a resin layer and paper are laminated, and the resin layer and the paper are adhered to each other by pseudo-adhesion in the resin-laminated paper. According to this configuration, when the paper in the resin-laminated paper is peeled off from the resin layer while the resin layer is attached to the weather-resistant layer 13, only the paper is peeled off and removed, and the resin layer remains attached to the weather-resistant layer 13 of the sheet body 10.

[0185] Next, in the third to fifth embodiments, a construction method for reinforcing or repairing a structure by attaching a sheet body 10 to the structure will be illustrated. In this construction method, a worker unrolls a required length of the sheet body 10 from a roll body 26. Next, in the third and fifth embodiments, the worker peels off the release sheet 16 of the sheet body 10 and attaches the exposed attachment surface 11a of the adhesive layer 11 to the surface of the structure to which the sheet body is to be attached. At this time, the worker may peel off the release sheet 16 little by little from the sheet body 10 and attach the exposed attachment surface 11a of the adhesive layer 11 to the surface of the structure to which the sheet body is to be attached. On the other hand, in the fourth embodiment, the worker attaches the attachment surface 11a of the adhesive layer 11 of the sheet body 10 to the surface of the structure to which the sheet body is to be attached.

[0186] Then, in the cases of the third to fifth embodiments, after the worker has attached the sheet body 10 to the attachment target, the worker peels and removes the corresponding second peel-off sheet 25, release sheet 29, or shape-imparting sheet 14 from the sheet body 10.

[0187] That is, the present application methods according to the third to fifth embodiments include a preparation step of preparing a roll body 26 in which the sheet body 10 is wound in a roll shape, a payout step of paying out the sheet body 10 from the roll body 26, and an attachment step of peeling the first release sheet 16 from the paid-out sheet body 10 and attaching the attachment surface exposed to the outside to the surface of a structure. Here, in the preparation step of the third and fifth embodiments, the roll body 26 is prepared using the sheet body 10 in which the attachment surface 11a is covered with the first release sheet 16.

[0188] In this application method, the sheet body 10 of the roll body 26 prepared in the preparation step has a laminated structure including a weather-resistant layer 13 and an adhesive layer 11, a cover sheet is disposed on the side of the weather-resistant layer 13 opposite to the adhesive layer 11, and the sheet body 10 including this cover sheet is wound in a roll shape in the roll body 26, and the cover sheet may be peeled off and removed during or after the attachment step. This cover sheet may be any one of the second peel sheet 25, the release sheet 29, and the shape-imparting sheet 14.

[0189] Furthermore, in the construction method of the fourth embodiment, the sheet body 10 of the roll body 26 prepared in the preparation step has a laminated structure including a weather-resistant layer 13 and an adhesive layer 11, and has a release sheet 29 that is arranged on the opposite side of the weather-resistant layer 13 to the adhesive layer 11 and is separate from the peel-off sheet 16, and in the preparation step, a roll body 26 in which the sheet body 10 is wound into a roll shape so that the release sheet 29 is in contact with the adhesive layer 11 may be prepared.

[0190] When using the sheet body 10 of the present disclosure, for example, a supply item 38 shown below can be used. FIG. 20 is a schematic diagram showing the structure of a supply item 38 containing the sheet body 10 of the present disclosure. FIG. 17 shows a sheet body 10 with a release sheet 16 as an example. The supply item 38 shown in FIG. 20 includes a roll body 26 around which a strip-shaped sheet body 10 is wound, and a container 27 having a storage space 27a for storing the roll body 26. The container 27 has a supply port 27b that can unwind and supply the sheet body 10 from the roll body 26 stored in the storage space 27a to the outside. The supply port 27b has a width dimension equal to or greater than the width dimension of the sheet body 10 in the axial direction of the roll body 26.

[0191] For example, a worker can carry the supply item 38 to a construction site, unwind the required length of the sheet body 10 from the supply item 38, and use the sheet body 10 for construction. Therefore, the supply item 38 allows the sheet body 10 to be stored in the form of a roll body 26 suitable for storage. Furthermore, when using the sheet body 10, only the required amount can be unwound from the supply item 38. This improves work efficiency.

[0192] In addition, when the sheet body 10 is unwound from the supply port 27b, the worker can unwound the sheet body 10 while applying uniform tension to the entire widthwise area of ​​the sheet body 10 by, for example, pressing the entire widthwise area of ​​the sheet body 10 against the opening periphery of the supply port 27b. This allows the sheet body 10 to be attached to the surface of the structure 21 with uniform tension. Therefore, it is possible to prevent the sheet body 10 from unexpectedly shrinking or expanding after application due to uneven tension acting on the sheet body 10 after application. Note that, in order to apply uniform tension to the entire widthwise area of ​​the sheet body 10, a separate member such as a long member that extends in the widthwise direction of the sheet body 10 and comes into contact with the sheet body 10 may be disposed, for example, on the opening periphery of the supply port 27b.

[0193] Furthermore, the sheet body provided in the supply article 38 may be any sheet body of the present disclosure, and may be, for example, the sheet body 10 of any of the third to fifth embodiments, or the sheet body 10 of the other embodiments.

[0194] [4] Sixth embodiment (a sheet body according to the present disclosure in which a separate body is placed on the side opposite to the structure side) An object separate from the sheet body 10 may be placed (attached) on the upper surface of the sheet body 10 attached to the structure 21. An example of such an object is a solar cell unit 33. FIG. 21 shows a schematic perspective view of the sheet body 10 and the solar cell unit 33 placed on top of it. FIG. 22 shows a schematic cross-sectional view of the sheet body 10 and the solar cell unit 33 of FIG. 21. FIG. 22 is a cross-sectional view taken along line XXI-XXI of FIG. 21. In FIGS. 21 and 22, the solar cell unit 33 is shown as an example of an object 33 separate from the sheet body 10.

[0195] In this embodiment, as shown in Figs. 21 and 22, the solar cell unit has a plurality of power generating units 33a-33c arranged side by side and connected by electrical wiring. As an example, the solar cell unit 33 is fixed to the surface of the sheet body 10 opposite to the structure 21 side by adhesion or the like. The roof 30, which is the structure 21, has a plurality of plate members 35-37 arranged to overlap each other. As a result, in the roof 30, steps 30a are formed between the adjacent plate members 35-37 in a plan view. The sheet body 10 is attached to the roof 30 so as to follow the plate surfaces of the plate members 35-37 and the surfaces of the steps 30a. The plurality of power generating units 33a-33c are arranged corresponding to the plate surfaces of the plate members 35-37. This prevents the power generating units 33a-33c from being influenced by the steps 30a and restricting the angle of the outer surface with respect to the horizontal direction.

[0196] The structure of the solar cell unit 33 is not limited, and may be a known one. For example, a thin or lightweight one is preferable. The type of solar cell is also not limited. Examples of the types of solar cells include amorphous silicon solar cells, crystalline silicon solar cells, cadmium telluride solar cells, copper indium gallium selenium solar cells, organic thin-film solar cells, perovskite solar cells, and gallium arsenide solar cells. For example, amorphous silicon solar cells, cadmium telluride solar cells, copper indium gallium selenium solar cells, organic thin-film solar cells, and perovskite solar cells that are flexible are suitable for combination with the sheet body 10 of the present disclosure.

[0197] 21 and 22 show a sheet body-attached solar cell unit 40 including a sheet body 10 that is attached to a structure 21 and used to reinforce or repair the structure 21, and a solar cell unit 33 directly or indirectly attached to the sheet body 10. The sheet body 10 included in the sheet body-attached solar cell unit 40 has an adhesive strength such that the measured value in a 180° peel test is 1.5 N / 25 mm or more and the maximum test force in the tensile elastic region is 100% or less before being attached to the structure 21. In this embodiment as well, the various effects of the sheet body 10 of the present disclosure are achieved.

[0198] Furthermore, the solar cell unit is usually fixed to a structure such as a roof or a frame by various methods, such as adhesion using an adhesive or fastening using a fastening member, with the solar cell unit adjusted to a position and angle suitable for power generation. In order to ensure this fixing, the solar cell unit is fixed to the structure by various methods. Depending on the fixing method of the solar cell unit and the conditions of the construction site, the solar cell unit may not be easy to handle, which increases the workload of workers. In addition, when it becomes necessary to remove the solar cell unit, the solar cell unit cannot be easily removed from the structure, which increases the workload of removal. Furthermore, deterioration of the structure also easily invites deterioration of the solar cell unit.

[0199] In contrast, in this embodiment, for example, if the solar cell unit 33 is attached to the sheet body 10 in advance, the solar cell unit 33 can be appropriately fixed to the structure 21 together with the sheet body 10 when the sheet body 10 is attached to the structure. In addition, since the sheet body 10 can be reattached, the solar cell unit 33 can be removed from the structure 21 together with the sheet body 10 without undue burden. As a result, the solar cell unit 33 can be reliably attached to the structure 21 while reducing the workload of the worker through simple construction, and when the solar cell unit 33 is to be removed from the structure 21, the solar cell unit 33 can be easily removed together with the sheet body 10.

[0200] For example, perovskite solar cells and copper indium gallium selenide solar cells are required to have higher durability than other solar cells. If the sheet body 10 of the present disclosure is applied to a solar cell unit 33 including a solar cell that is required to have high durability, the sheet body 10 can reliably fix the solar cell unit 33 to the structure 21. In addition, deterioration of the solar cell unit 33 due to deterioration of the structure 21 is less likely to occur, making it easier to achieve high durability for the solar cell unit 33. In addition, the solar cell unit 33 can generate stable power with high conversion efficiency.

[0201] 21 and 22, even if the surface shape of the structure 21 to which the sheet body 10 is to be attached is not flat due to height differences caused by irregularities or defects, the sheet body 10 can be attached by smoothly conforming to the surface. Therefore, the sheet body 10 can be suitably applied. However, the present invention is not limited to this, and even if the surface shape of the structure 21 to which the sheet body 10 is to be attached is flat, the use of the sheet body 10 is preferable because it makes it easier to obtain high durability of the solar cell unit 33 and enables the solar cell unit 33 to generate stable power with high conversion efficiency.

[0202] Furthermore, the sheet member 10 of this embodiment has an adhesive strength of 1.5 N / 25 mm or more as measured in a 180° peel test and less than 100% of the maximum test force in the tensile elastic region before being attached to the structure 21, and exhibits excellent weather resistance. Therefore, the solar cell unit 33 can be fixed to the structure 21 while protecting the structure 21 with the sheet member 10 for a long period of time. Therefore, the solar cell unit 33 can be used stably while deterioration of the solar cell unit 33 associated with deterioration of the structure 21 is suppressed.

[0203] Furthermore, the sheet member 10 of the present embodiment has waterproofness that does not cause water leakage in a waterproofing test after a weather load test before being attached to the structure 21, so that the solar cell unit 33 can be fixed to the structure 21 while protecting the structure 21 from deterioration due to water leakage over a long period of time. Therefore, the solar cell unit 33 can be used stably while suppressing deterioration of the solar cell unit 33 associated with deterioration of the structure 21.

[0204] Furthermore, when a deformation test is carried out in which the operations described in (1), (2), (3), and (4) above are carried out in sequence, the energy calculated in the calculation in (4) above is 2.0 mJ or more. Therefore, the sheet body 10 has an appropriate rigidity. This can easily improve the ease of handling when an operator installs the solar cell unit 33 on the structure 21.

[0205] Furthermore, when a plurality of sheet bodies 10 to which solar cell units 33 are attached are attached to the surface of a structure 21, even if gaps occur between the sheet bodies 10 and the surface of the structure 21 is exposed to the outside, the surface of the structure 21 can be easily covered by separately attaching a sheet body 10 of the present disclosure to the surface of the structure 21 corresponding to the gap. In this case, for example, a sheet body 10 having a long shape (for example, a rectangular shape) can be used to match the shape of the gap.

[0206] Furthermore, since the sheet body 10 has flexibility to the extent that it can be wound up in a roll, when a solar cell unit 33 having a predetermined flexibility is attached to the sheet body 10, flexibility is ensured in the entire sheet-attached solar cell unit 40. Therefore, the sheet-attached solar cell unit 40 can be easily installed and arranged on various structures 21. It is also possible to manage the sheet-attached solar cell unit 40 in a rolled-up state. For example, the sheet-attached solar cell unit 40 can be brought to the installation site in a rolled-up state and installed easily on a relatively wide installation surface.

[0207] In this way, the sheet body 10 provided with the solar cell unit 33 of the present disclosure can be suitably attached to various structures 21, such as an outdoor building structure 21, a mounting that is a structure 21 provided on land, or a window that is a structure 21 provided integrally with a building material.

[0208] (Installation of sheet body on structure) The application of the sheet body of the present disclosure to the structure 21 will be described below. The sheet body 10 of the present disclosure has excellent adhesive strength. Therefore, when the sheet body 10 is applied to the surface of the structure 21, such as the roof, the sheet body 10 can be applied without gaps even to the surface of the structure 21 having steps. By applying the sheet body 10, it is possible to prevent water from entering the structure 21 from the outside and to prevent the intrusion of deterioration factors such as salt water and oxygen that cause rust for several decades. Therefore, it is possible to appropriately suppress the deterioration of the structure 21. In addition, the sheet body 10 can be applied by simply applying it to the surface of the structure 21. Therefore, the sheet body 10 can be applied without relying on the skill of the worker, and it is possible to shorten the construction period and reduce labor costs.

[0209] When applying the sheet body of the present disclosure, a primer layer containing a curable resin material may be formed in advance on the surface of the structure 21. Examples of properties required for the primer layer include excellent initial adhesion to the structure protection sheet to which it is applied, long-term adhesion enabling long-term storage, sealing properties that can firmly fix the coating film on the deteriorated structure surface and prevent harmful substances from scattering from the deteriorated structure when it is reapplied, curability that hardens in a short time, pot life that can ensure fluidity for a certain period of time, and paint workability that does not require strict mixing work at the work site.

[0210] The material of the primer layer is not particularly limited as long as it can provide the properties required for the primer layer. For example, there is no particular limitation as long as the material has the property of being cured by moisture curing, heat curing, photocuring or other methods to form a resin. Examples of such materials include resins such as acrylic, polyester, urethane, epoxy and silicone. For example, a material containing a reaction product of a polymer containing a (meth)acrylic acid alkyl ester monomer unit in the main chain and a raw material compound containing an epoxy compound and an aminosilane compound is preferable.

[0211] The primer layer is generally used as an undercoat material for the structure 21. In the present disclosure, the primer may be applied to the surface of the structure 21. The undercoat material may be applied by a conventional method. For example, a paint is applied to the surface of the structure 21 by a conventional method such as application with a brush or roller, or spraying with a spray gun, to form a coating film, thereby obtaining a primer layer as an undercoat material.

[0212] The thickness of the primer layer is not particularly limited. For example, the thickness of the primer layer is 20 g / m 2 The thickness of the primer layer is, for example, 30 g / m2 in a wet state. 2 Values ​​of 50 g / m or more are preferred. 2 Values ​​of 100 g / m or more are more preferable. 2 More preferably, the value is 200 g / m 2 The above values ​​are particularly preferred.

[0213] On the other hand, the thickness of the primer layer is, for example, 800 g / m2 in a wet state. 2 The thickness of the primer layer is, for example, 700 g / m2 in a wet state. 2 The following values ​​are preferred: 600 g / m 2 Values ​​below 500 g / m are more preferable. 2 The following values ​​are more preferable. In particular, the thickness of the primer layer is, for example, 400 g / m2 in a wet state. 2 The following values ​​are preferable because they can stabilize the adhesive strength of the sheet body 10 to the surface of a structure under various conditions. The "wet state" referred to here refers to the state before the coating liquid dries, and the above values ​​indicating the wet state refer to the coating weight. EXAMPLES

[0214] A number of examples according to the present disclosure and a number of comparative examples were produced. The examples and the comparative examples according to the present disclosure will be specifically described. Example 1 A 130 μm-thick shape-imparting sheet 14, which was a PP laminate sheet manufactured by Lintec Corporation, was prepared. A weather-resistant layer-forming composition containing an acrylic resin (a mixture of Cool Life SP Black (CB1) P5-0 manufactured by Dainichi Seika Chemicals Mfg. Co., Ltd. and FC Coat Water-Based Silicone Elastic Black manufactured by Fujikura Kasei Co., Ltd. in a weight ratio of 50:50) was applied onto this shape-imparting sheet 14. The formed coating was dried to form a single-layer weather-resistant layer having a thickness of 110 μm.

[0215] Next, a mixture was prepared by mixing the cement and admixture of a composition for forming a base layer (Kikusui Chemical, Spring Coat (trowel)) in a ratio of 60:40. This mixture was applied to the weather-resistant layer. A vinylon-based mesh material (Kuraray Co., Ltd., cheesecloth "Cremona", #600 (600 grit, thickness 230 μm) was pressed against the surface of the coating of this mixture. This caused the coating to harden, and a base layer with a hardened thickness of 450 μm was formed on the weather-resistant layer.

[0216] On the other hand, 100 parts by weight of an acrylic adhesive (Olivine (registered trademark) BPS5565K) manufactured by Toyochem Co., Ltd. was mixed with 5 parts by weight of an isocyanate-based crosslinking agent (curing agent) (BHS8515) manufactured by Toyochem Co., Ltd. to prepare an adhesive mixture. This adhesive mixture was applied to the surface of a release sheet and dried to form an adhesive layer with a thickness of 100 μm. The adhesive layer was then superimposed on and adhered to the base layer to form the sheet body 10 according to Example 1. The adhesive (main adhesive) contained in the adhesive layer of Example 1 was "BPS5565K".

[0217] Example 2 A sheet member 10 according to Example 2 was constructed in the same manner as in Example 1, except that the thickness of the adhesive layer in Example 1 was changed to 30 μm.

[0218] Example 3 In the configuration of the adhesive layer of Example 1, the adhesive (main adhesive) was changed to an acrylic adhesive (Olivine (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., the curing agent ratio (crosslinking agent ratio) was set to 20 parts by weight, and the thickness of the adhesive layer was set to 100 μm. The reinforcing material 15 was made of a vinylon-based mesh material (cheesecloth (BINEO (registered trademark) "V520")) manufactured by Unitika Co., Ltd. The rest was set in the same way as in Example 1, and a sheet body 10 according to Example 3 was constructed.

[0219] Example 4 In the configuration of the adhesive layer of Example 1, the adhesive (main adhesive) was changed to an acrylic adhesive (Olivine (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., the curing agent ratio (crosslinking agent ratio) was set to 50 parts by weight, and the thickness of the adhesive layer was set to 50 μm. In addition, the reinforcing material 15 was omitted. The rest was set in the same manner as in Example 1, and a sheet body 10 according to Example 4 was constructed.

[0220] Example 5 In the configuration of the adhesive layer of Example 1, the adhesive (main adhesive) was changed to an acrylic adhesive (Olivine (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., the curing agent ratio (crosslinking agent ratio) was set to 50 parts by weight, and the thickness of the adhesive layer was set to 50 μm. In addition, the reinforcing material 15 was composed of a polyester nonwoven fabric (ELTAS (registered trademark) "E01012") manufactured by Asahi Kasei Co., Ltd. The rest was set in the same manner as in Example 1, and a sheet body 10 according to Example 4 was constructed.

[0221] Example 6 In the configuration of the adhesive layer of Example 1, the adhesive (main adhesive) was changed to an acrylic adhesive (Olivine (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., the curing agent ratio (crosslinking agent ratio) was set to 12 parts by weight, and the thickness of the adhesive layer was set to 100 μm. The reinforcing material 15 was made of a vinylon-based mesh material (cheesecloth (BINEO (registered trademark) "V520")) manufactured by Unitika Co., Ltd. The rest was set in the same manner as in Example 1, and a sheet body 10 according to Example 6 was constructed.

[0222] Example 7 In the configuration of the adhesive layer of Example 1, the adhesive (main adhesive) was changed to an acrylic adhesive (Olivine (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., the curing agent ratio (crosslinking agent ratio) was set to 6 parts by weight, and the thickness of the adhesive layer was set to 100 μm. In addition, the reinforcing material 15 was composed of a vinylon-based mesh material (cheesecloth (BINEO (registered trademark) "V520")) manufactured by Unitika Co., Ltd. The rest was set in the same manner as in Example 1, and a sheet body 10 according to Example 7 was constructed.

[0223] Comparative Example 1 A sheet member according to Comparative Example 1 was fabricated in the same manner as in Example 1, except that the thickness of the adhesive layer in Example 1 was changed to 10 μm.

[0224] Comparative Example 2 A sheet member according to Comparative Example 2 was constructed in the same manner as in Comparative Example 1, except that the thickness of the adhesive layer in Comparative Example 1 was changed to 200 μm.

[0225] Comparative Example 3 A sheet body for Comparative Example 3 was constructed in the same manner as Comparative Example 1, except that the thickness of the adhesive layer in Comparative Example 1 was changed to 100 μm and the adhesive (main adhesive) of the adhesive layer in Comparative Example 1 was changed to a two-component curing acrylic adhesive (Olivine (registered trademark) BPS6617) manufactured by Toyochem Co., Ltd.

[0226] Comparative Example 4 The thickness of the adhesive layer of Comparative Example 1 was changed to 50 μm, the adhesive (main adhesive) of the adhesive layer of Comparative Example 1 was changed to an acrylic adhesive (Oribain (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., and the curing agent ratio (crosslinking agent ratio) was set to 50 parts by weight. In addition, the material of the reinforcing fiber, which is the reinforcing material, was set to a vinylon-based mesh material (cheesecloth (BINEO (registered trademark) "V520")) manufactured by Unitika Co., Ltd. The rest was set in the same way as in Comparative Example 1, and a sheet body according to Comparative Example 4 was constructed.

[0227] Comparative Example 5 In the adhesive layer of Comparative Example 1, the adhesive (main adhesive) was changed to an acrylic adhesive (Olivine (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., the thickness of the adhesive layer was changed to 100 μm, and the curing agent ratio (crosslinking agent ratio) of the adhesive layer of Comparative Example 1 was changed to 11 parts by weight. The reinforcing material was made of polyester nonwoven fabric (ELTAS (registered trademark) "E01012") manufactured by Asahi Kasei Corporation. The rest was set in the same manner as in Comparative Example 1, and a sheet body according to Comparative Example 5 was constructed.

[0228] Comparative Example 6 The thickness of the adhesive layer was changed to 100 μm, the adhesive (main adhesive) of the adhesive layer of Comparative Example 1 was changed to an acrylic adhesive (Olivine (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., and the curing agent ratio (crosslinking agent ratio) of the adhesive layer was set to 6 parts by weight. In addition, the reinforcing material was omitted. The rest was set in the same manner as in Comparative Example 1, and a sheet body according to Comparative Example 6 was constructed.

[0229] Comparative Example 7 The thickness of the adhesive layer of Comparative Example 1 was changed to 100 μm, the adhesive (main adhesive) of the adhesive layer of Comparative Example 1 was changed to an acrylic adhesive (Olivine (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., and the curing agent ratio (crosslinking agent ratio) of the adhesive layer was changed to 6 parts by weight. The reinforcing material was made of polyester nonwoven fabric (ELTAS (registered trademark) "E01012") manufactured by Asahi Kasei Co., Ltd. The rest was set in the same manner as in Comparative Example 1, and a sheet body according to Comparative Example 7 was constructed.

[0230] Comparative Example 8 The thickness of the adhesive layer of Comparative Example 1 was changed to 50 μm, the adhesive (main adhesive) of the adhesive layer of Comparative Example 1 was changed to an acrylic adhesive (Olivine (registered trademark) "BPS6574") manufactured by Toyochem Co., Ltd., and the curing agent ratio (crosslinking agent ratio) of the adhesive layer was changed to 50 parts by weight. In addition, the base material layer and reinforcing material were omitted. The rest were set in the same manner as in Comparative Example 1, and a sheet body according to Comparative Example 8 was constructed.

[0231] For the sheet bodies 10 according to Examples 1 to 7 and the sheet bodies according to Comparative Examples 1 to 8, a 180° peel test (adhesive strength (N / 25 mm)), measurement of tensile elasticity (maximum test force in tensile elasticity region (N / 25 mm)) before and after the weather load test, calculation of adhesive strength / tensile elasticity (%) before the weather load test, evaluation of rework (re-pasting) before the weather load test, overlapping waterproof test (waterproofness test), and deformation test were performed. In addition, the following air blowing and water sprinkling test was performed for the sheet bodies 10 according to Examples 1 to 7 and the sheet bodies according to Comparative Examples 1 to 8 before and after the weather load test.

[0232] (Air and water spray test) The air-blow and water-spray test (strong wind resistance test) was conducted in accordance with the JSTM J6403:2020 [Method for testing water leakage from metal roofs], a group standard of the Construction Materials Testing Center. Specifically, the large-scale water-spray test equipment owned by the Construction Materials Testing Center was used. As test specimens, a plurality of belt-shaped sheet bodies 10 of the present disclosure were prepared. Here, FIG. 12 is a perspective view of a stand imitating a roof. FIG. 13 is a diagram showing the side and dimensions of the stand in FIG. 12. FIG. 14 is a front view of the stand in FIG. 12. In this test, the stands shown in FIGS. 12 to 14 were further prepared.

[0233] The above-prepared sheet bodies 10 of the embodiment were lined up in the width direction, and each sheet body 10 was attached to a stand simulating a roof previously coated with a primer, with a part of the sheet body 10 in the width direction overlapping the adjacent sheet body 10. Then, an air and water spray test was performed under the following test conditions, and it was visually confirmed whether the sheet body 10 was peeled off from the stand. Note that the same procedure was followed for the comparative example as well, and the operation and visual confirmation were performed.

[0234] The test conditions were as follows: roof slope of the rack: 4 sun; wind speed level: 9 (lower limit wind speed: 38±2 m / min; upper limit wind speed: 62±2 m / min); water spray rate: 4 L / min m 2 The air and water spray retention time was set to 15 minutes.

[0235] The method of attaching the test specimens was to first apply a primer to the surface of the stand. Then, multiple sheets were placed on top of each other on the top surface of the primer so as to form an overlapping section of 15 mm width in the width direction, and the multiple sheets were attached to the top surface of the primer so as to cover the entire surface of the stand. The wind direction relative to the stand was set to blow from the eaves toward the ridge.

[0236] The specifications of each Example and Comparative Example are shown in Table 1. Tables 2 and 3 show the test results of the 180° peel test (adhesive strength (N / 25 mm)), tensile elasticity (maximum test force in the tensile elastic region (N / 25 mm)), adhesive strength / tensile elasticity (%) before the weather resistance load test, whether or not the product could be reworked (reapplied) before the weather resistance load test, the overlapping waterproof test (waterproofness test), and the deformation test before and after the weather resistance load test.

[0237] [Table 1]

[0238] [Table 2]

[0239] [Table 3]

[0240] First, we will describe representative Examples 1 and 2, and representative Comparative Examples 1 to 3. The measured values ​​of the 180° peel test and the maximum test force in the tensile elastic region before the weather load test are values ​​measured immediately after the sheet body is attached to the structure and before a substantial load is applied to the sheet body, and therefore are considered to be values ​​close to the measured values ​​of the 180° peel test and the maximum test force in the tensile elastic region before the sheet body is attached to the structure.

[0241] As shown in Tables 2 and 3, the sheet body 10 according to Example 1 had a measured value of 17.6 N / 25 mm in a 180° peel test and a maximum test force in the tensile elastic region of 20 N / 25 mm before the weather load test. Furthermore, when the sheet body 10 of Example 1 was applied to a structure (a folded roof) at a construction site and then peeled off, no plastic deformation was observed in the sheet body 10 and it could be reapplied.

[0242] Furthermore, the measured value of the 180° peel test after the weather load test for the sheet member 10 according to Example 1 was 41.4 N / 25 mm. The reason why the adhesive strength in the 180° peel test was higher than that before the weather load test is presumed to be that the adhesive layer softened under high heat of 70° C. to 80° C., increasing the contact area and improving the adhesive strength due to the anchor effect.

[0243] Furthermore, in the results of the waterproofing test after the weather load test, the sheet body 10 of Example 1 was judged to have "no water leakage" since no bright spots or water stains were found on the back surface of the fixing adherend (the surface on which the sheet body was not overlapped) when visually inspected.

[0244] In addition, in the deformation test, the energy required for moving the pressing jig downward by 20 mm at a test speed of 30 mm / min for the sheet body 10 according to Example 1 was 23.0 mJ. The sheet body 10 according to Example 1 having such rigidity was easy to lay at the construction site and had excellent handleability. In addition, the sheet body 10 according to Example 1 did not peel off even after the air blowing and water sprinkling test.

[0245] The sheet body 10 according to Example 2 had a measured value of 3 N / 25 mm in a 180° peel test and a maximum test force in the tensile elastic region of 20 N / 25 mm. When the sheet body 10 according to Example 2 was attached to a structure (steel roof) at a construction site and then peeled off, no plastic deformation was observed in the sheet body 10 and it could be reattached.

[0246] Furthermore, the measured value of the 180° peel test after the weather load test for the sheet body 10 according to Example 2 was 5 N / 25 mm. Furthermore, in the results of the waterproofing test after the weather load test for the sheet body 10 according to Example 2, no bright spots or water stains were found by visual inspection on the back surface of the fixing adherend (the surface on which the sheet body is not overlapped), and it was determined that there was "no water leakage."

[0247] In addition, in the deformation test, the energy required for moving the pressing jig 20 mm at a test speed of 30 mm / min for the sheet body 10 according to Example 2 was 18.7 mJ. The sheet body 10 according to Example 2 having such rigidity was easy to lay at the construction site and had excellent handleability. In addition, the sheet body 10 according to Example 2 did not peel off even after the air blowing and water sprinkling test.

[0248] As shown in Tables 1 and 3, the sheet body according to Comparative Example 1 had a measured value of 0.25 N / 25 mm in the 180° peel test, and peeling occurred after the air-blowing and water-spraying test. On the other hand, the sheet body according to Comparative Example 1 had a maximum test force in the tensile elastic region of 20 N / 25 mm. When the sheet body according to Comparative Example 1 was applied to a structure (a folded-half roof) at the construction site and then peeled off, no plastic deformation was observed in the sheet body, and it was possible to reapply it.

[0249] Furthermore, the sheet body according to Comparative Example 1 had a measured value of 1.0N / 25mm in a 180° peel test after the weather load test. In addition, peeling occurred in an air-spraying test after the weather load test. In addition, in the waterproofing test results after the weather load test, the back surface of the fixing adherend (the surface on which the sheet body is not overlapped) of the sheet body according to Comparative Example 1 was visually inspected to find no bright spots or water stains, and was judged to be "water-free." In addition, in the deformation test, the energy required to move the pressing jig 20 mm at a test speed of 30 mm / min for the sheet body according to Comparative Example 1 was 16 mJ. The sheet body according to Comparative Example 1, which has such rigidity, was easy to lay even at the construction site and had excellent handleability.

[0250] The measured value of the sheet body according to Comparative Example 2 in the 180° peel test was 25N / 25mm. Furthermore, no peeling occurred after the air-blowing and water-spraying test. Meanwhile, the maximum test force in the tensile elastic region of the sheet body according to Comparative Example 2 was 20N / 25mm. When the sheet body according to Comparative Example 2 was applied to a structure (a folded-half roof) at the construction site and then peeled off, plastic deformation was observed in the peeled-off sheet body, and it could not be reapplied, so it had to be discarded.

[0251] Furthermore, the sheet body according to Comparative Example 2 had a measured value of 60N / 25mm in a 180° peel test after the weather load test. In addition, no peeling occurred in the air-spraying test after the weather load test. Furthermore, in the results of the waterproofing test after the weather load test for the sheet body according to Comparative Example 2, the back surface of the fixing adherend (the surface on which the sheet body is not overlapped) was visually inspected to find no bright spots or water stains, and it was judged to be "water-free." In addition, in the deformation test for the sheet body according to Comparative Example 2, the energy required to move the pressing jig 20 mm at a test speed of 30 mm / min was 25 mJ. The sheet body according to Comparative Example 2, which has such rigidity, was easy to lay even at the construction site and had excellent handleability.

[0252] The measured value of the 180° peel test for the sheet body according to Comparative Example 3 was 0.2 N / 25 mm. In addition, peeling occurred after the air-blowing and water-spraying test. On the other hand, the maximum test force in the tensile elastic region for the sheet body according to Comparative Example 3 was 20 N / 25 mm. When the sheet body according to Comparative Example 3 was applied to a structure (a folded-half roof) at the construction site and then peeled off, no plastic deformation was observed in the sheet body, and it was possible to reapply it.

[0253] Furthermore, the sheet according to Comparative Example 3 had a measured value of 1.3 N / 25 mm in a 180° peel test after the weather load test, and peeling occurred in an air / water spray test after the weather load test.

[0254] Furthermore, in the waterproofing test results after the weathering load test, the back surface of the fixing adherend (the surface on which the sheet body is not overlapped) of the sheet body of Comparative Example 3 was visually inspected to find no bright spots or water stains, and was judged to be "water-free." In addition, in the deformation test of the sheet body of Comparative Example 3, the energy required to move the pressing jig 20 mm at a test speed of 30 mm / min was 22 mJ. The sheet body of Comparative Example 3, which has such rigidity, was easy to install even at the construction site and had excellent handleability.

[0255] Additionally, as shown in Tables 2 and 3, it was confirmed that all of the sheet bodies 10 according to Examples 3 to 7 had performance equivalent to or better than that of Examples 1 and 2. In contrast, it was confirmed that in Comparative Examples 4 to 8, the measured value of the 180° peel test before the weathering load test was less than 1.5 N / 25 mm (Comparative Example 4), or the adhesive strength before the weathering load test was 100% or more of the maximum test strength in the tensile elastic region (Comparative Examples 5 to 7). As a result, it is considered difficult for any of Comparative Examples 3 to 8 to obtain, compared to Examples 1 to 7, the effect of ensuring excellent adhesiveness to structures and the effect of improving handleability so as to enable reapplication of the sheet body at the construction site.

[0256] As shown in Table 3, the deformation test results were good for all of Examples 1 to 7 (the energy required to move the pressing jig 17 was at least 2.0 mJ), confirming that they had excellent durability. For this reason, it is believed that Examples 1 to 7 can be fully used to reinforce or repair structures even when re-pasted. Comparative Example 8 had low rigidity, and it was not possible to measure the deformation test. In addition, in the air and water spray tests conducted on the sheet bodies 10 according to Examples 1 to 7 and the sheet bodies according to Comparative Examples 1 to 8 before and after the weather load test, no significant differences were confirmed between Examples 1 to 7 and Comparative Examples 1 to 8.

[0257] (Disclosure items) The following items disclose preferred embodiments of the sheet body of the present disclosure.

[0258] [Item 1] A sheet body to be attached to a structure for reinforcing or repairing the structure, A sheet body having an adhesive strength, before being attached to the structure, of 1.5 N / 25 mm or more as measured in a 180° peel test and less than 100% of the maximum test force in the tensile elastic region.

[0259] According to the above-mentioned configuration, the sheet body has an adhesive strength of 1.5N / 25mm or more as measured by a 180° peel test before being attached to a structure, so that excellent adhesive strength of the sheet body to the structure can be ensured. This allows the structure to be appropriately repaired or restored. In addition, the sheet body has an adhesive strength of 100% or less as measured by a tensile elastic region maximum test force before being attached to a structure, so that the handling of the sheet body at the construction site can be improved. That is, when the sheet body is peeled off after being attached once, the sheet body is less likely to be plastically deformed, so that the sheet body is less likely to be damaged, and the sheet body can be reattached. This allows the sheet body to have excellent adhesive strength to the structure while improving the handling of the sheet body at the construction site.

[0260] [Item 2] Item 2. The sheet according to item 1, further having an adhesive strength such that the measured 180° peel strength is 1.5 N / 25 mm or more after a weather load test.

[0261] According to the above-mentioned configuration, it is ensured that the adhesive strength after the weather resistance load test is the same as that before the sheet is attached to the structure, and therefore a sheet body with excellent weather resistance can be provided.

[0262] [Item 3] 3. The sheet body according to item 1 or 2, further having waterproofness such that there is no water leakage in a waterproofness test after a weather load test.

[0263] According to the above-mentioned configuration, the predetermined waterproof property of the sheet body is ensured even after the weather resistance load test, and therefore, a sheet body with excellent weather resistance can be provided.

[0264] [Item 4] The sheet body according to any one of items 1 to 3, in which, when a deformation test is carried out by sequentially carrying out the operations described in the following items (1), (2), (3), and (4), the energy calculated by the calculation in the following item (4) is 2.0 mJ or more. (1) A rectangular sheet body having short sides of 50 mm and long sides of 100 mm is prepared as a sample. (2) The sample is bent so that a pair of short sides on the same surface overlap each other, and a pair of regions of the sample from the edges of the pair of short sides to a position 15 mm away along the long side are grasped and fixed with a fixing portion, thereby forming a curved portion with a circumference of 70 mm between the pair of regions of the sample. (3) With the surfaces of the pair of regions of the sample arranged parallel to the vertical direction and the curved portion facing upward, a disk-shaped pressing tool with a pressing surface of 100 mm in diameter and 10 mm in thickness is used to contact the curved portion from above in an environment of a temperature of 23±2°C and a humidity of 50±10% RH, and the pressing tool is moved downward by 20 mm at a test speed of 30 mm / min. (4) The energy required to move the pressing jig is calculated.

[0265] According to the above-mentioned configuration, it is possible to impart an appropriate rigidity to the sheet body, which makes it easy to handle the sheet body when it is applied to the surface of a structure. More specifically, it becomes easy to lay the sheet body on the surface of a structure.

[0266] [Item 5] An adhesive layer attached to the structure; 5. The sheet member according to any one of items 1 to 4, further comprising at least one weather-resistant layer disposed above the adhesive layer.

[0267] [Item 6] Item 6. The sheet body according to item 5, further comprising a substrate layer disposed between the adhesive layer and the weather-resistant layer.

[0268] [Item 7] 7. The sheet body according to claim 6, wherein the base layer includes a reinforcing material.

[0269] [Item 8] Item 8. The sheet body according to item 6 or 7, wherein at least one of the adhesive layer and the weather-resistant layer contains a filler.

[0270] [Item 9] 8. The sheet member according to any one of items 5 to 7, further comprising: a release sheet disposed on a surface of the pressure-sensitive adhesive layer opposite to the weather-resistant layer.

[0271] [Item 10] 5. The sheet member according to any one of items 1 to 4, which is constituted by a single layer and contains an adhesive component that is unevenly distributed on a second surface side, which is an attachment surface to be attached to the structure, rather than on a first surface side, which is an attachment surface to be attached to the structure.

[0272] [Item 11] Item 11. The sheet member according to item 10, comprising rubber and having a crosslinked structure of the rubber having a different degree of crosslinking on the first surface side and the second surface side.

[0273] [Item 12] The resin composition includes an acrylic resin and an epoxy resin, Item 12. The sheet body according to item 10 or 11, having a phase-separated structure of the acrylic resin and the epoxy resin.

[0274] The configuration of the present disclosure is not limited to the above-described embodiment and example, and the configuration and method can be changed, added, or deleted without departing from the spirit of the present disclosure. Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. [Explanation of symbols]

[0275] 10 Sheet body 11 Adhesive layer 12 Base material layer 13 Weatherproof layer 15 Reinforcement materials 16 Release sheet 17 Pressing jig 18 Fixed part 19 Samples 21 Structures 30 Roof 31 Blue Sheet 32 Sandbags

Claims

1. A sheet body to be attached to a structure for reinforcing or repairing the structure, A sheet body having an adhesive strength, before being attached to the structure, of 1.5 N / 25 mm or more as measured in a 180° peel test and less than 100% of the maximum test force in the tensile elastic region.

2. 2. The sheet member according to claim 1, further having an adhesive strength such that a measured 180° peel strength is 1.5 N / 25 mm or more after a weather load test.

3. The sheet member according to claim 1 , further having waterproofness such that there is no water leakage in a waterproofness test after a weather load test.

4. The sheet body according to claim 1, wherein when a deformation test is carried out by sequentially performing the operations described in the following items (1), (2), (3), and (4), the energy calculated by the calculation in (4) below is 2.0 mJ or more. (1) A rectangular sheet having short sides of 50 mm and long sides of 100 mm is prepared as a sample. (2) The sample is bent so that a pair of short sides on the same surface overlap each other, and a pair of regions of the sample from the edges of the pair of short sides to a position 15 mm away along the long side are grasped and fixed with a fixing portion, thereby forming a curved portion with a circumference of 70 mm between the pair of regions of the sample. (3) With the surfaces of the pair of regions of the sample arranged parallel to the vertical direction and the curved portion facing upward, a disk-shaped pressing tool with a pressing surface having a diameter of 100 mm and a thickness of 10 mm is used to contact the curved portion from above in an environment of a temperature of 23±2°C and a humidity of 50±10% RH, and the pressing tool is moved downward by 20 mm at a test speed of 30 mm / min. (4) The energy required to move the pressing jig is calculated.

5. An adhesive layer attached to the structure; The sheet member according to any one of claims 1 to 4, further comprising at least one weather-resistant layer disposed above the adhesive layer.

6. The sheet member according to claim 5 , further comprising a base layer disposed between the adhesive layer and the weather-resistant layer.

7. The sheet member according to claim 6 , wherein the base layer includes a reinforcing material.

8. The sheet member according to claim 6 , wherein at least one of the adhesive layer and the weather-resistant layer contains a filler.

9. The sheet body according to claim 5 , further comprising a release sheet disposed on a surface of the adhesive layer opposite to the weather-resistant layer.

10. The sheet body according to any one of claims 1 to 4, which is constituted by a single layer and contains an adhesive component that is unevenly distributed on a second surface side, which is an attachment surface to be attached to the structure, rather than on a first surface side, which is located opposite to the structure.

11. The sheet member according to claim 10 , comprising a rubber and having a cross-linked structure of the rubber having a different degree of cross-linking between the first surface side and the second surface side.

12. The resin composition includes an acrylic resin and an epoxy resin, The sheet member according to claim 10 , having a phase-separated structure between the acrylic resin and the epoxy resin.

Citation Information

Patent Citations

  • Sheet and method for repairing and reinforcing concrete structure

    JP2002256707A

  • Coating film protective sheet

    JP2011084655A

  • Tacky adhesive layer and tacky adhesive sheet

    JP2014065889A

  • Method of repairing or reinforcing target structure and tacky adhesive sheet used for the same

    JP2015209633A

  • Method of repairing or reinforcing target structure and tacky adhesive sheet used for the same

    JP2016169576A