Adsorptive-desorptive activated carbon for per- and polyfluoroalkyl substances
The high-temperature solvent desorption method using activated carbon with specific properties effectively removes and recovers PFOS and PFOA from activated carbon, addressing inefficiencies and environmental risks of traditional disposal methods.
Patent Information
- Application Number
- JP2024068288
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
Existing methods for removing and disposing of per- and polyfluoroalkyl compounds, such as PFOS and PFOA, from activated carbon are inefficient, potentially leading to incomplete decomposition and re-release into the environment, and incur high energy costs.
A high-temperature solvent desorption method using activated carbon with specific physical properties, including a BET specific surface area of 1100 to 1800 m²/g, pore diameter of 0.50 to 0.70 nm, and acidic functional groups of 0.10 to 0.50 meq/g, allows for efficient desorption of these compounds using solvents like water or ethanol under high pressure.
The method achieves rapid and complete desorption of PFOS and PFOA from activated carbon, reducing environmental risk and energy consumption, while maintaining high adsorption efficiency.
Smart Images

Figure 2024155879000001 
Figure 2024155879000002 
Figure 2024155879000003
Abstract
Description
[Technical field]
[0001] The present invention relates to activated carbon that adsorbs per- and polyfluoroalkyl compounds in a desorbable manner, and more particularly to activated carbon that adsorbs and desorbs per- and polyfluoroalkyl compounds, and that allows the adsorbed per- and polyfluoroalkyl compounds to be desorbed and recovered using a high-temperature solvent. [Background technology]
[0002] Per- and polyfluoroalkyl compounds, which are organic fluorine compounds (PFCs), are fluorine-substituted aliphatic compounds that have high thermal stability, high chemical stability, and high surface modification activity. Taking advantage of these properties, per- and polyfluoroalkyl compounds are widely used in industrial and chemical applications, such as surface treatment agents, packaging materials, and liquid fire extinguishing agents.
[0003] Some per- and polyfluoroalkyl compounds are very stable chemical substances, and therefore are difficult to decompose under natural conditions when released into the environment. For this reason, in recent years, per- and polyfluoroalkyl compounds have been recognized as persistent organic pollutants (POPs), and the manufacture and use of perfluorooctane sulfonate (PFOS) (IUPAC name: 1,1,2,2,3,3,4,4,5,5,6,6,7,7,8,8,8-heptadecafluorooctane-1-sulfonic acid) has been restricted since 2010 under the Stockholm Convention on Persistent Organic Pollutants (POPs Convention).
[0004] In particular, perfluorooctane sulfonate (PFOS) and perfluorooctanoic acid (PFOA) (IUPAC name: 2,2,3,3,4,4,5,5,6,6,7,7,8,8,8-pentadecafluorooctanoic acid) are subject to regulation worldwide, and in Japan as well, a standard value of 50 ng / L or less for the combined value of perfluorooctane sulfonate (PFOS) and perfluorooctanoic acid (PFOA) was added to the water quality management target setting items from April 1, 2020.
[0005] Perfluoroalkyl compounds, including perfluorooctane sulfonic acid (PFOS) and perfluorooctanoic acid (PFOA), have a completely fluorinated linear alkyl group and are represented by the chemical formula (i). Polyfluoroalkyl compounds are compounds in which some of the hydrogen atoms in the alkyl group are replaced with fluorine and are represented by the chemical formula (ii). For example, there is fluorotelomer alcohol.
[0006]
number
[0007]
number
[0008] Thus, since per- and polyfluoroalkyl compounds continue to remain in the natural world (in water, soil, and air), it is required to remove them appropriately in each environment. For example, when removing harmful substances from water, etc., water purifiers using activated carbon are widely used. Since PFOS, PFOA, etc. are attracting attention as harmful substances, activated carbon for removing harmful substances such as PFOS and PFOA has been proposed (see, for example, Patent Document 1). In addition, activated carbon capable of adsorbing PFOS, PFOA, etc. can also be applied to adsorbents used in air filters, etc. that remove harmful substances from the air, etc. After using this type of activated carbon to adsorb and remove harmful substances such as PFOS and PFOA, the used activated carbon is disposed of as waste such as PFOS-containing waste or PFOA-containing waste.
[0009] The disposal of these wastes is carried out in accordance with the "Technical Considerations for the Treatment of Waste Containing PFOS and PFOA" set out by the Ministry of the Environment. In other words, it is required to carry out the disposal in a way that ensures the decomposition of PFOS, etc. and PFOA, etc., and the proposed decomposition method is incineration at approximately 850°C or higher for waste containing PFOS, and approximately 1000°C or higher (approximately 1100°C or higher is recommended) for waste containing PFOA, and the decomposition efficiency of PFOS, PFOA, etc. must be 99.999% or higher.
[0010] However, it is recognized that activated carbon may suppress the volatilization of PFOA, etc. during incineration and promote the combustion decomposition reaction. However, it cannot necessarily be said that sufficient research has been done on the changes in PFOS, PFOA, etc. in activated carbon caused by combustion, and it has been pointed out that there is a possibility that other compounds including inorganic fluorides and harmful gases may be generated by decomposition (for example, see Non-Patent Document 1).
[0011] In addition, depending on the amount of waste to be incinerated, the incineration time, the temperature rise during incineration, etc., there is a concern that incomplete combustion may occur, resulting in insufficient decomposition of PFOS, PFOA, etc. in the activated carbon, or that PFOS, PFOA, etc. may be dispersed into the air without being decomposed due to volatilization, etc. In other words, PFOS, PFOA, etc. that have been recovered as hazardous substances will be released back into the natural environment. In addition, there are problems with the energy costs required for incineration, as the incineration temperature is high at around 1000°C. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Patent Publication No. 2021-079376 [Non-patent literature]
[0013] [Non-Patent Document 1] Hidesuke Takemine, Mitsuyasu Takada, Shusaku Yamamoto, Nobuhisa Watanabe, Chisato Matsumura, Shigeo Fujii, Shuhei Tanaka, Akira Kondo, "Behavior of Perfluorooctanoic Acid Adsorbed on Granular Activated Carbon during Heating" Analytical Chemistry, Vol. 62, No. 2, pp. 107-113, 2013 Summary of the Invention [Problem to be solved by the invention]
[0014] The inventors have conducted extensive research into treating waste by desorbing and recovering harmful substances such as PFOS and PFOA adsorbed from activated carbon, without relying on incineration. As described above, when removing PFCs (desorbing and recovering adsorbed substances from activated carbon), which are harmful substances that have been attracting attention in recent years, a safe and secure treatment method that can desorb adsorbed substances with almost no residue remaining in the activated carbon and can treat waste in a short period of time is required as an alternative to incineration.
[0015] The inventors have found that contacting the activated carbon with a solvent at 130° C. or higher is an effective method for desorbing substances adsorbed on the activated carbon from the activated carbon. The present invention provides an adsorption / desorption activated carbon having physical properties that enable highly efficient desorption of adsorbed per- and polyfluoroalkyl compounds by a method using a high-temperature solvent that is effective for desorbing substances adsorbed on the activated carbon. [Means for solving the problem]
[0016] That is, the first invention is an activated carbon that adsorbs per- and polyfluoroalkyl compounds in a desorbable manner, and the adsorbed per- and polyfluoroalkyl compounds are desorbed and recovered by a solvent at a temperature of 130° C. or higher under a high pressure of 0.1 MPa or higher, and the activated carbon has a BET specific surface area of 1100 to 1800 m 2The present invention relates to a per- and polyfluoroalkyl compound adsorption / desorption activated carbon, characterized in that the adsorption capacity of the activated carbon is 0.50 to 0.70 nm, the mode diameter of the pore diameter measured by the MP method from the t-plot of the nitrogen gas adsorption isotherm is 0.50 to 0.70 nm, and the acidic functional group content determined by the Boehm method is 0.10 to 0.50 meq / g.
[0017] A second invention relates to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to the first invention, wherein the solvent is water.
[0018] A third invention relates to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to the first invention, wherein the solvent is a mixed solvent of water and an organic solvent.
[0019] A fourth invention relates to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to the third invention, wherein the organic solvent is ethanol.
[0020] A fifth invention relates to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to the first invention, wherein the solvent is an organic solvent.
[0021] A sixth invention relates to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to the fifth invention, wherein the organic solvent is ethanol.
[0022] The seventh invention is the method according to any one of the first to sixth inventions, wherein the total pore volume of the activated carbon determined by analyzing the nitrogen gas adsorption isotherm by the HK method is 0.40 to 0.75 cm 3 / g of per- and polyfluoroalkyl compound adsorption / desorption activated carbon.
[0023] The eighth invention relates to a per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to any one of the first to sixth inventions, wherein the activated carbon has an exclusion limit molecular weight of 1013 or less as measured using a polystyrene standard.
[0024] A ninth aspect of the present invention relates to a per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to the seventh aspect of the present invention, which has an exclusion limit molecular weight of 1013 or less as measured using a polystyrene standard sample of the activated carbon.
[0025] A tenth aspect of the present invention relates to a per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to the eighth aspect of the present invention, wherein the exclusion limit molecular weight is 453 or less.
[0026] An eleventh aspect of the present invention relates to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to the ninth aspect of the present invention, wherein the exclusion limit molecular weight is 453 or less.
[0027] A twelfth aspect of the present invention relates to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to any one of the first to sixth aspects of the present invention, wherein the activated carbon is a fibrous activated carbon.
[0028] A thirteenth aspect of the present invention relates to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to the seventh aspect of the present invention, wherein the activated carbon is a fibrous activated carbon.
[0029] A fourteenth aspect of the present invention relates to a per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to the eighth aspect of the present invention, wherein the activated carbon is a fibrous activated carbon.
[0030] A fifteenth aspect of the present invention relates to a per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to the ninth aspect of the present invention, wherein the activated carbon is a fibrous activated carbon.
[0031] A sixteenth aspect of the present invention relates to the per- and polyfluoroalkyl compound adsorption and desorption activated carbon according to the tenth aspect of the present invention, wherein the activated carbon is a fibrous activated carbon.
[0032] A seventeenth aspect of the present invention relates to a per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to the eleventh aspect of the present invention, wherein the activated carbon is a fibrous activated carbon. Effect of the Invention
[0033] The first aspect of the present invention provides an activated carbon for adsorbing and desorbing per- and polyfluoroalkyl compounds, which is capable of desorbing per- and polyfluoroalkyl compounds, and which is capable of desorbing and recovering the adsorbed per- and polyfluoroalkyl compounds by using a solvent at a temperature of 130° C. or higher under a high pressure of 0.1 MPa or higher. The activated carbon has a BET specific surface area of 1100 to 1800 m 2 The mode diameter of the pore diameter measured by the MP method from the t-plot of the nitrogen gas adsorption isotherm is 0.50 to 0.70 nm, and the acidic functional group determined by the Boehm method is 0.10 to 0.50 meq / g. Therefore, the adsorption and desorption performance of per- and polyfluoroalkyl compounds is excellent. In particular, by using a desorption method using a high-temperature solvent, the treatment time required for desorption is short, and yet it is possible to desorb per- and polyfluoroalkyl compounds at an extremely high rate.
[0034] According to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the second invention, since the solvent in the first invention is water, it is inexpensive, easily available, and highly convenient, and also has a small environmental impact.
[0035] According to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the third invention, since the solvent in the first invention is a mixed solvent of water and an organic solvent, the desorption efficiency can be improved.
[0036] According to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the fourth invention, since the organic solvent in the third invention is ethanol, it is inexpensive and easy to obtain, and it is possible to desorb per- and polyfluoroalkyl compounds at a higher rate.
[0037] According to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the fifth invention, since the solvent in the first invention is an organic solvent, the desorption efficiency can be improved.
[0038] According to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the sixth invention, in the fifth invention, the organic solvent is ethanol, which is inexpensive and easy to obtain, and it is possible to desorb per- and polyfluoroalkyl compounds at a higher rate.
[0039] According to the seventh aspect of the present invention, there is provided a per- and polyfluoroalkyl compound adsorption and desorption activated carbon, in any one of the first to sixth aspects, wherein the total pore volume of the activated carbon determined by analyzing the nitrogen gas adsorption isotherm by the HK method is 0.40 to 0.75 cm 3 / g, better adsorption / desorption performance can be obtained.
[0040] According to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the eighth invention, in any one of the first to sixth inventions, the exclusion limit molecular weight of the activated carbon measured using a polystyrene standard is 1013 or less, thereby achieving better desorption performance.
[0041] According to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the ninth invention, since the exclusion limit molecular weight of the activated carbon measured using a polystyrene standard in the seventh invention is 1013 or less, better desorption performance can be obtained.
[0042] According to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the tenth aspect of the present invention, since the exclusion limit molecular weight is 453 or less in the eighth aspect of the present invention, even better desorption performance can be obtained.
[0043] According to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the eleventh aspect of the present invention, since the exclusion limit molecular weight is 453 or less in the ninth aspect of the present invention, even better desorption performance can be obtained.
[0044] According to the 12th invention, the activated carbon for adsorbing and desorbing per- and polyfluoroalkyl compounds in any one of the first to sixth inventions is a fibrous activated carbon, so that the contact efficiency with per- and polyfluoroalkyl compounds is increased, and the adsorption performance can be improved.
[0045] According to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the thirteenth invention, in the seventh invention, since the activated carbon is a fibrous activated carbon, the contact efficiency with per- and polyfluoroalkyl compounds is increased, and the adsorption performance can be improved.
[0046] According to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the 14th invention, in the eighth invention, the activated carbon is a fibrous activated carbon, so that the contact efficiency with per- and polyfluoroalkyl compounds is increased, and the adsorption performance can be improved.
[0047] According to the fifteenth aspect of the present invention, the activated carbon for adsorbing and desorbing per- and polyfluoroalkyl compounds is a fibrous activated carbon in the ninth aspect of the present invention, so that the contact efficiency with per- and polyfluoroalkyl compounds is increased, and the adsorption performance can be improved.
[0048] According to the 16th invention, the activated carbon for adsorbing and desorbing per- and polyfluoroalkyl compounds is a fibrous activated carbon in the 10th invention, so that the contact efficiency with per- and polyfluoroalkyl compounds is increased, and the adsorption performance can be improved.
[0049] According to the per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the 17th invention, in the 11th invention, since the activated carbon is a fibrous activated carbon, the contact efficiency with per- and polyfluoroalkyl compounds is increased, and the adsorption performance can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0050] The present invention relates to an activated carbon that adsorbs per- and polyfluoroalkyl compounds remaining in nature, such as in water or the atmosphere, in a manner that allows them to be desorbed, and in particular, to an adsorption / desorption activated carbon that allows the adsorbed per- and polyfluoroalkyl compounds to be desorbed and recovered using a high-temperature solvent.
[0051] This activated carbon is preferably used as an adsorbent for use in household water purifiers and industrial water purification treatment devices when removing per- and polyfluoroalkyl compounds contained in water such as tap water. In addition, when removing per- and polyfluoroalkyl compounds from the atmosphere, it is preferably used as an adsorbent for use in household and industrial air purifiers and air filters. The activated carbon of the present invention can adsorb per- and polyfluoroalkyl compounds and then desorb the adsorbed per- and polyfluoroalkyl compounds at a high rate in a short time by using a desorption method using a high-temperature solvent (high-temperature solvent desorption method).
[0052] The method for desorbing per- and polyfluoroalkyl compounds from activated carbon using a high-temperature solvent is carried out by contacting the activated carbon to which the per- and polyfluoroalkyl compounds have been adsorbed with the high-temperature solvent.
[0053] The high-temperature solvent refers to a solvent heated to 130°C or higher under high pressure of 0.10 MPa (atmospheric pressure) or higher. The solvent is preferably, for example, water. Water is a common solvent, inexpensive, easily available, and highly convenient, and also has a small environmental impact. In addition, it is more preferable to use ultrapure water, which contains almost no impurities and is suitable for applications such as cleaning, as the water used as the solvent. In general, water heated to 100°C or higher under high pressure is called ultrahigh-temperature water, and the water used as the high-temperature solvent is ultrahigh-temperature water heated to 130°C or higher under high pressure.
[0054] Solvents with a temperature of 130°C or higher can be obtained by heating the solvent in a high-pressure environment corresponding to the desired temperature, since the temperature at which the solvent can exist in a liquid state changes depending on the pressure. For example, when water is heated under a pressure of 0.12 MPa, ultra-high temperature water of 105°C is obtained. Ultra-high temperature water of 130°C can be obtained by heating the water under a high-pressure environment of 0.27 MPa. The temperature of the solvent used in the present invention is set according to the type of compound to be desorbed from the activated carbon (compound adsorbed on the activated carbon), and an excellent desorption effect can be obtained by setting the temperature to 130°C or higher. If the temperature of the high-temperature solvent is too low, there is a risk that a sufficient desorption effect cannot be obtained. There is no particular limit to the upper limit of the temperature of the high-temperature solvent, but if it is too high, it is disadvantageous in terms of the energy cost required for heating and there is a risk that the improvement of the desorption effect commensurate with the temperature increase cannot be obtained, so it is preferable to set the temperature to about 200°C. Note that, in order to obtain ultra-high temperature water of 200°C, a pressure of 1.55 MPa or more is required.
[0055] The activated carbon can be contacted with a high-temperature solvent by appropriate methods such as passing a liquid through it or immersion. In particular, when the activated carbon of the present invention is used for adsorption and removal of harmful substances such as PFOS and PFOA, and then treated as "PFOS- and PFOA-containing waste," it is preferable to contact the activated carbon by passing a liquid through it in the high-temperature solvent desorption method. In the case of desorption by passing a liquid through it, the harmful substances such as PFOS and PFOA desorbed from the activated carbon are discharged together with the high-temperature solvent that has been passed through, so there is no risk of volatilization as in the case of incineration, and they can be easily recovered as they are, which is safe and efficient.
[0056] The solvent may be a mixed solvent of water and an organic solvent. The mixed solvent is an aqueous solution of an organic solvent prepared to a predetermined concentration. Examples of the organic solvent include ethanol, methanol, n-propyl alcohol, isopropyl alcohol, etc., and ethanol is particularly preferable because it is inexpensive and easy to obtain. The concentration of the organic solvent in the mixed solvent is set according to the type of organic solvent, etc., and is preferably 10% or more, more preferably 20% or more, and even more preferably 30% or more. By making the high-temperature solvent contain an organic solvent (mixed solvent), the desorption efficiency can be improved. The solvent may be only an organic solvent (100%). A solvent consisting of only an organic solvent can improve the desorption efficiency in the same way as a mixed solvent.
[0057] Activated carbon suitable for the desorption method using a high-temperature solvent is one that has excellent adsorption performance for per- and polyfluoroalkyl compounds such as PFOS and PFOA, as well as excellent desorption performance for per- and polyfluoroalkyl compounds.
[0058] Activated carbon has an appropriate form such as granular activated carbon or fibrous activated carbon, and is obtained by carbonizing and activating an activated carbon raw material. In the case of granular activated carbon, examples of the raw material for activated carbon include wood (waste wood, thinning wood, sawdust), coffee bean residue, rice husk, coconut shell, bark, and fruit. These naturally derived raw materials are easily developed into pores by carbonization and activation, and among these, coconut shell is preferable because it can be steadily procured. In addition, it can be procured at a low cost because it is a secondary use of waste. In addition, burned products derived from synthetic resins such as tires, petroleum pitch, urethane resin, and phenolic resin, and even coal can be used as raw materials. Granular activated carbon is easy to handle because the form of use can be appropriately determined.
[0059] The fibrous activated carbon is obtained by carbonizing and activating an appropriate fiber, such as a phenol resin-based, acrylic resin-based, cellulose-based, or coal pitch-based fiber. The fiber length and cross-sectional diameter of the fibrous activated carbon are appropriate. From the viewpoint of contact efficiency with the substance to be removed, the fibrous activated carbon can more efficiently adsorb per- and polyfluoroalkyl compounds.
[0060] Activated carbon is produced by heating and carbonizing an activated carbon raw material, followed by an activation treatment. The activated carbon raw material is heated and carbonized when carbonization of the raw material is required. The conditions for the heated carbonization are preferably, for example, a temperature range of 200 to 900°C. By carrying out the heated carbonization, micropores can be formed in the activated carbon raw material.
[0061] The raw material after carbonization is subjected to activation treatment to become activated carbon with various pores developed. In the activation treatment, for example, steam activation is performed in the temperature range of 600°C to 1200°C. Alternatively, carbon dioxide gas activation such as carbon dioxide and zinc chloride activation are also used. The activation time varies depending on the production scale and equipment, but is generally 0.5 to 50 hours. The activated carbon after activation is washed with dilute hydrochloric acid. The activated carbon adsorbent after washing with dilute hydrochloric acid is washed with water until the pH is 5 to 7, for example, as measured in accordance with JIS K 1474 (2014).
[0062] After washing with dilute hydrochloric acid, the activated carbon is heated in a mixed gas of oxygen and nitrogen and washed with water as necessary to remove impurities such as ash. Residual hydrochloric acid and other impurities are removed by the heat treatment. The amount of surface oxides on the activated carbon adsorbent is adjusted by each treatment. After acid washing, the amount of surface oxides on the activated carbon adsorbent is increased by heat treatment of the activated carbon.
[0063] The properties of the activated carbon thus produced determine the adsorption and desorption performance of the target adsorbate. In the present invention, we have found that the BET specific surface area, the mode diameter of the pore diameter, and the amount of acidic functional groups (amount of surface oxides) can be used as indicators of the excellent adsorption and desorption performance of activated carbon for per- and polyfluoroalkyl compounds such as PFOS and PFOA, and have derived physical properties suitable for the high-temperature solvent desorption method.
[0064] The BET specific surface area is a value calculated from a straight line in the relative pressure range of 0.05 to 0.3 of the curve obtained by measuring a nitrogen adsorption isotherm at 77K and analyzing it by a multipoint method based on the BET formula, and is used as an index showing the amount of pores formed in the activated carbon. Since the more pores in the activated carbon (the larger the BET specific surface area), the more the target adsorbate can be adsorbed, the more the adsorption performance of the activated carbon can be determined by the BET specific surface area. On the other hand, it is considered from the examples described later that, when the BET specific surface area is large, the adsorption performance is improved, but the adsorbed substance becomes difficult to desorb. Therefore, a preferable BET specific surface area for showing excellent performance in both adsorption and desorption performance is 1100 to 1800 m 2 / g, more preferably 1200 to 1400m 2 If the BET specific surface area is too small, the adsorption performance may be insufficient, whereas if the BET specific surface area is too large, the desorption performance may decrease.
[0065] The pore diameter in this specification refers to the mode diameter measured by the MP method from the t-plot of the adsorption isotherm of nitrogen gas. The mode diameter is a value indicating the mode value of the pore distribution. The pore diameter is used as one of the indicators indicating the size of a substance that can be adsorbed by activated carbon. It is considered that the adsorption and desorption of the target adsorbed substance can be smoothly performed when the pore diameter is suitable for the size of the target adsorbed substance. Therefore, the mode diameter of the pore diameter suitable for the adsorption of the target adsorbed substance such as PFOS and PFOA is 0.50 to 0.70 nm. If the pore diameter is too small, there is a risk that PFOS, PFOA, etc. with a large molecular weight cannot be properly adsorbed. If the pore diameter is too large, it becomes easy to adsorb non-target substances such as impurities, and the pores for adsorbing PFOS, PFOA, etc. may be blocked, and the adsorption performance may be reduced. In addition, it is also considered that the target adsorbed substance penetrates deep into the pores of the activated carbon due to the pore diameter being too large, making it difficult for the target adsorbed substance to be desorbed.
[0066] Acidic functional groups are present on the surface of activated carbon, and are mainly hydrophilic groups such as carboxyl groups and phenolic hydroxyl groups, and increase due to surface oxidation of activated carbon. The acidic functional groups on the surface of activated carbon affect the desorption of PFOS, PFOA, etc. The amount of these acidic functional groups is understood as the amount of surface oxide. The amount of surface oxide can be determined by applying the Boehm method. For example, it can be determined as the amount of sodium hydroxide when the activated carbon is shaken in a 0.05N aqueous solution of sodium hydroxide, filtered, and the filtrate is neutralized and titrated with 0.05N hydrochloric acid. Therefore, the preferable amount of surface oxide for properly desorbing PFOS, PFOA, etc. is 0.10 meq / g or more. If the amount of surface oxide is too small, it may lead to a decrease in desorption performance.
[0067] In addition, the amount of surface oxide of activated carbon also affects adsorption performance. For example, it is considered that a large amount of surface oxide of activated carbon increases the hydrophilicity of the surface of activated carbon, and the adsorption performance of per- and polyfluoroalkyl compounds, particularly fluorotelomer compounds having hydrophilic groups, is improved. However, when the environment in which per- and polyfluoroalkyl compounds are collected is underwater, if the amount of surface oxide of activated carbon is excessive, it is presumed that the water molecules firmly adsorbed to the surface functional groups by hydrogen bonds and the clusters of water molecules generated thereby will block the pores, thereby preventing the physical access of the target adsorbed substance to the adsorption points (micropores).
[0068] When used in water, it is believed that the pores are blocked by the water molecules adsorbed by hydrogen bonds and the clusters of water molecules generated by the acidic functional groups present on the surface of the activated carbon, so that, for example, when the amount of surface oxide is small, even an activated carbon with a small specific surface area and a small amount of pores can adsorb the compound to a certain degree. Conversely, even if the amount of surface oxide is large and the adsorption of the compound to the pores is inhibited, an activated carbon with a large specific surface area and a large amount of pores can adsorb the compound to a certain degree. Therefore, the preferred amount of surface oxide for properly adsorbing PFOS, PFOA, etc. is 0.50 meq / g or less. Therefore, it is believed that the amount of surface oxide of activated carbon with a good balance between adsorption performance and desorption performance is 0.10 to 0.50 meq / g. It is believed that this provides good desorption efficiency and adsorption performance of the target adsorbate in water.
[0069] The amount of surface oxides on activated carbon can be adjusted by the following methods. One is a method of promoting the oxidation of surface residues by passing through a heating process again, thereby increasing acidic functional groups. That is, oxidation in air or oxygen atmosphere. Alternatively, air with a temperature of 25 to 40°C and a humidity of 60 to 90% is also introduced at the same time in an air atmosphere. Then, activated carbon with an increased amount of surface oxides can be obtained by heating at 150 to 900°C for 1 to 10 hours. It is considered that the acidic functional groups increase when the activated carbon is heated with moist air, because the hydrocarbon groups such as alkyl groups present on the surface of the activated carbon are oxidized, or the hydroxyl groups of water are introduced to the surface.
[0070] Another method is to oxidize the surface of activated carbon with an oxidizing agent to increase the amount of surface oxide. Examples of oxidizing agents include hypochlorous acid and hydrogen peroxide. Activated carbon with an increased amount of surface oxide can be obtained by immersing activated carbon in a liquid containing such an oxidizing agent and then drying it. The amount of acidic functional groups on the surface of the activated carbon can be measured as the amount of surface oxide, as shown in each prototype example described below.
[0071] In addition, as a method for reducing the surface oxide of the activated carbon, a known method such as heat treatment under an inert gas atmosphere can be used, and acidic functional groups such as phenolic hydroxyl groups and carboxyl groups on the surface of the activated carbon can be reduced. In the activated carbon of the present invention, it is preferable to appropriately adjust the amount of surface oxide depending on the usage environment, such as in air or water.
[0072] In addition, in the present invention, it is preferable to specify the exclusion limit molecular weight and the total pore volume from the viewpoint of improving the performance of the activated carbon. The exclusion limit molecular weight is a value indicating the upper limit of the molecular weight of a substance that can enter the pores of the activated carbon measured using a polystyrene standard, and is used as one of the indicators indicating the size of a substance that the activated carbon can adsorb in the pores. In other words, the exclusion limit molecular weight can specify the adsorption and desorption performance of the target adsorbate from a viewpoint different from the mode diameter of the pore diameter. In the measurement of the exclusion limit molecular weight, polystyrene standards with different molecular weights are used as reagents to pass through the activated carbon and confirm the change in the retention time, and the minimum molecular weight of the reagents that did not change in retention time and did not enter the activated carbon is taken as the exclusion limit molecular weight. Therefore, the preferred exclusion limit molecular weight is 1013 or less, more preferably 589 or less, and even more preferably 453 or less. If the exclusion limit molecular weight is too large, it is considered that PFOS, PFOA, etc. will enter too deep into the pores and become difficult to desorb.
[0073] The total pore volume is a value obtained by analyzing the nitrogen gas adsorption isotherm of activated carbon by the Horvath-Kawazoe method (HK method). The total pore volume determines the adsorption and desorption performance of activated carbon from a viewpoint different from that of the BET specific surface area. Therefore, the preferred total pore volume is 0.40 to 0.75 cm 3 / g, more preferably 0.45 to 0.60 cm 3 If the total pore volume is too small, the adsorption performance may be insufficient, whereas if the total pore volume is too large, the desorption performance may be reduced.
[0074] The activated carbon of the present invention has the above-described physical properties, and therefore has excellent adsorption performance for per- and polyfluoroalkyl compounds such as PFOS and PFOA, and the adsorbed per- and polyfluoroalkyl compounds are easily desorbed, enabling efficient recovery of PFOS, PFOA, etc. The activated carbon can desorb the per- and polyfluoroalkyl compounds at a high rate in a short time by contacting with a solvent at an ultra-high temperature, particularly when the per- and polyfluoroalkyl compounds are adsorbed. The adsorption and desorption performance of the activated carbon of the present invention is preferably, for example, an adsorption performance (adsorption amount) of 50 mg / g or more, a desorption performance (desorption rate) of 50% or more, and a processing time required for desorption of 1 hour or less. In particular, it is more preferable that the desorption rate is 90% or more and the processing time is 0.5 hours or less.
[0075] Thus, the activated carbon of the present invention not only has excellent adsorption performance for per- and polyfluoroalkyl compounds, but also has excellent desorption performance for adsorbed per- and polyfluoroalkyl compounds. In particular, it has desorption performance suitable for high-temperature solvent desorption, and by using the high-temperature solvent desorption method for the activated carbon of the present invention, it is possible to desorb per- and polyfluoroalkyl compounds at an extremely high rate while shortening the processing time required for desorption. Therefore, harmful substances such as PFOS and PFOA can be appropriately removed (adsorbed) under an appropriate use (adsorption) environment, and after use (after adsorption), the adsorbed harmful substances such as PFOS and PFOA can be recovered (desorbed) with high efficiency by the high-temperature solvent desorption method. Therefore, when treating waste containing the harmful substances, efficient recovery and concentration of harmful substances is possible, and the high-temperature solvent desorption method can be selected as a treatment method other than incineration treatment. EXAMPLES
[0076] The following activated carbon and reagents were used to study methods for desorbing substances adsorbed on activated carbon from the activated carbon. The desorption methods used were high-temperature solvent desorption using ultra-high temperature water, alkaline desorption, and vacuum heating desorption. Each desorption method was performed according to the procedures described below. For each desorption method, the processing time required for desorption, the adsorption amount (mg / g), desorption amount (mg / g), and desorption rate (%) of TFA, and the adsorption amount (mg / g), desorption amount (mg / g), and desorption rate (%) of PFOA were measured. The results are shown in Table 1 below.
[0077] [Activated carbon] Phenolic resin fibers were used as the raw material and heated at 700-800°C to form a carbonized product, which was then heated to and maintained at approximately 800-950°C and activated by introducing steam to obtain a fibrous activated carbon (activated carbon 1). The activated carbon thus obtained was cut into a piece of 9 mmφ, and the materials were stacked to a thickness of 11 mm and packed into a stainless steel column (Tomoe Manufacturing Co., Ltd., "ES008050", 50 mm x 8.0 mm ID).
[0078] [reagent] As reagents to be adsorbed onto activated carbon, TFA (trifluoroacetic acid, manufactured by Kanto Chemical Co., Ltd.) and PFOA (perfluorooctanoic acid, manufactured by Tokyo Chemical Industry Co., Ltd.) were prepared and dissolved in ultrapure water to prepare sample solutions at 1000 ppm. Each sample solution was passed through a UV detector (G1314A, manufactured by Agilent Technologies, Inc.) to measure the absorbance at 1000 ppm.
[0079] [High-temperature solvent desorption method using ultra-high-temperature water] Using an HPLC system (Agilent Technologies, "G1311A"), each sample solution prepared above was passed through the activated carbon in the column at room temperature and 0.5 mL / min, and the flow was continued until the compound broke through the activated carbon and the absorbance settled to a certain value, so that the compound was adsorbed on the activated carbon in the column. Next, ultrapure water was used as a solvent, and ultrapure water was passed through at room temperature and 3.0 mL / min, and the flow was continued until the absorbance stabilized. Thereafter, ultrapure water was passed through at 3.0 mL / min, and the piping of the HPLC system was pressurized to 3 MPa to heat the ultrapure water to 150°C, and the ultrapure water was passed through at 150°C, and the compound was desorbed from the activated carbon in the column, and the change in absorbance was measured, and the flow of the ultrapure water at 150°C was continued until it stabilized.
[0080] Based on the absorbance obtained in the above test, the adsorption amount (mg / g) and desorption amount (mg / g) of TFA and PFOA per 1 g of activated carbon, as well as the desorption rate (%) were calculated. The processing time (h) required for desorption was taken as the elapsed time until the absorbance stabilized at a certain value. The desorption rate (%) of TFA can be regarded as an index of the desorption performance of organic fluorine compounds with relatively small molecular weights, and the desorption rate (%) of PFOA can be regarded as an index of the desorption performance of organic fluorine compounds with relatively large molecular weights.
[0081] In calculating the desorption rate of the high-temperature solvent desorption method using ultra-high temperature water, the absorbance at 1000 ppm was defined as C0, the absorbance during the flow was defined as C1, the point at which the flow of the sample solution started at 0.5 mL / min was defined as the starting point, and C1 / C0 at each point was defined as the breakthrough rate. An adsorption curve was then obtained by plotting the elapsed time (min) on the horizontal axis and the breakthrough rate (C1 / C0) on the vertical axis, and the adsorption amounts of TFA and PFOA were calculated from the adsorption curve, and the desorption amounts were calculated from the desorption curve obtained in the same way, and the desorption rate was calculated from the following formula. (Amount of desorption / Amount of adsorption) x 100 = Ultra-high temperature water desorption rate (%)
[0082] [Alkaline desorption method] A 0.01 mol / L NaOH aqueous solution and a 0.01 mol / L NaOH aqueous solution in which TFA or PFOA had been dissolved to a concentration of 1000 ppm were passed through a UV detector, and the absorbance of each solution was measured. Using an HPLC system, each of the sample solutions prepared above was passed through the activated carbon in a column at room temperature and at a rate of 0.5 mL / min, and the passing of the solution was continued until the compound broke through the activated carbon and the absorbance settled at a certain value, allowing the compound to be adsorbed by the activated carbon in the column.
[0083] Next, ultrapure water was passed through at room temperature at 3.0 mL / min until the absorbance stabilized. After that, 0.01 mol / L NaOH aqueous solution was passed through at 3.0 mL / min, and the column oven (Shimadzu Corporation, "GC-8A") was heated to 70°C to desorb the compounds from the activated carbon in the column, and the change in absorbance was measured. The passage of 0.01 mol / L NaOH aqueous solution was continued until the absorbance stabilized at a certain value.
[0084] Based on the absorbance obtained in the above test, the adsorption amount (mg / g) of TFA and PFOA per 1 g of activated carbon by the alkaline desorption method, the desorption amount (mg / g), and the desorption rate (%) were calculated. The treatment time (h) required for desorption was defined as the time elapsed until the absorbance stabilized at a certain value.
[0085] In calculating the desorption rate of the alkaline desorption method, the absorbance at 1000 ppm was C0, the absorbance during the solution was C2, and the time when the sample solution was started to be passed at 0.5 mL / min was set as the starting time, and C2 / C0 at each time point was set as the breakthrough rate. Next, the adsorption curve was obtained by plotting the elapsed time (min) on the horizontal axis and the breakthrough rate (C2 / C0) on the vertical axis, and the adsorption amount of TFA and PFOA was calculated from the adsorption curve. In addition, the absorbance of each 0.01 mol / L NaOH aqueous solution in which TFA or PFOA was dissolved was set as B0, and the absorbance of 0.01 mol / L NaOH aqueous solution was set as B1, and the time when the 0.01 mol / L NaOH aqueous solution was passed and heated to 70 ° C was set as the starting time, and [(C2-B1) / (B0-B1)] at each time point was set as the breakthrough rate. Then, a desorption curve was obtained by plotting the elapsed time (min) on the horizontal axis and the breakthrough rate [(C2-B1) / (B0-B1)] on the vertical axis. The desorption amounts of TFA and PFOA were calculated from the desorption curve, and the desorption rate by the alkaline desorption method was calculated using the following formula. (Amount desorbed / Amount adsorbed) x 100 = Alkali desorption rate (%)
[0086] [Vacuum thermal desorption method] Using an HPLC system, each sample solution prepared above was passed through the activated carbon in the column at room temperature and 0.5 mL / min, and the passing of the solution was continued until the compound broke through the activated carbon and the absorbance settled to a certain value, so that the compound was adsorbed on the activated carbon in the column. Next, ultrapure water was passed through the column at room temperature and 3.0 mL / min, and the passing of the solution was continued until the absorbance stabilized. After that, the column was temporarily removed from the HPLC system, and the column was connected to a vacuum heating treatment device in which a vacuum pump (manufactured by Fuji Medical Instruments Co., Ltd., OSP-90W) was connected to a nitrogen cylinder, and the vacuum pressure was set to -70 to -90 kPa, the column temperature was set to 150°C, and nitrogen was passed through the column at 10 mL / min to desorb the compound from the activated carbon in the column. The aeration was continued for 18 hours, and this was taken as the treatment time (h) required for desorption.
[0087] To confirm the amount of remaining activated carbon after the vacuum heating, the column was removed from the vacuum heat treatment device, and an HPLC system was used to pass ultrapure water through the activated carbon in the column at 3.0 mL / min, and the inside of the HPLC system piping was pressurized to 3 MPa to pass ultrapure water heated to 150°C as ultrahigh temperature water to desorb the compounds from the activated carbon in the column. The change in absorbance was measured, and the passage of ultrahigh temperature water at 150°C was continued until it stabilized.
[0088] The adsorption amount (mg / g), desorption amount (mg / g), and desorption rate (%) of TFA and PFOA by the vacuum thermal desorption method were obtained using the absorbance obtained by the above-mentioned test to confirm the remaining amount. First, the absorbance at 1000 ppm was C0, the absorbance during the flow was C3, and the time when the sample solution was started to flow at 0.5 mL / min was taken as the starting time, and C3 / C0 at each time was taken as the breakthrough rate. Then, the adsorption curve was obtained by taking the elapsed time (min) on the horizontal axis and the breakthrough rate (C3 / C0) on the vertical axis, and the adsorption amount of TFA and PFOA was calculated from the adsorption curve. Next, the time when ultrapure water was passed at 3.0 mL / min and the temperature was raised to 150 ° C. was taken as the starting time, and C3 / C0 at each time was taken as the breakthrough rate. Then, the desorption curve was obtained by taking the elapsed time (min) on the horizontal axis and the breakthrough rate (C3 / C0) on the vertical axis, and the desorption amount of TFA and PFOA was calculated from the desorption curve. The desorption rate was calculated using the following two formulas from the calculated adsorption amount and the desorption amount calculated in the remaining amount confirmation test. Adsorption amount - desorption amount in residual amount confirmation test = desorption amount by vacuum heating (Amount of desorption by vacuum heating / Amount of adsorption) x 100 = Vacuum heating desorption rate (%)
[0089] [Table 1]
[0090] [Results and Discussion (1)] For activated carbon adsorbed with TFA, which is assumed to be an organic fluorine compound with a small molecular weight, the desorption rate was relatively good for the high-temperature solvent desorption method using ultra-high temperature water, the alkaline desorption method, and the vacuum heating desorption method, and in particular the high-temperature solvent desorption method using ultra-high temperature water reached 100%. On the other hand, the processing time required for desorption was short, about 30 minutes for the high-temperature solvent desorption method using ultra-high temperature water and the alkaline desorption method, but was extremely long at 18 hours for the vacuum heating desorption method.
[0091] In addition, for activated carbon adsorbed with PFOA, a hypothetical organic fluorine compound with a large molecular weight, the desorption rate was 64% for the alkaline desorption method and 45% for the vacuum thermal desorption method, while the high-temperature solvent desorption method using ultra-high temperature water reached 100%, demonstrating significantly superior results. The processing time required for desorption was short, at around 30 minutes for the high-temperature solvent desorption method using ultra-high temperature water and the alkaline desorption method, but was extremely long at 18 hours for the vacuum thermal desorption method.
[0092] As described above, the high-temperature solvent desorption method using ultra-high temperature water produced significantly better results for both low molecular weight organic fluorine compounds (TFA) and high molecular weight organic fluorine compounds (PFOA) compared to the alkaline desorption method and vacuum heating desorption method. In particular, even though the treatment time for both TFA and PFOA was short, at around 30 minutes, per- and polyfluoroalkyl compounds were desorbed at an extremely high rate, reaching a desorption rate of 100%. Therefore, it was found that the high-temperature solvent desorption method using ultra-high temperature water is extremely effective as a method for treating waste containing PFOS and PFOA.
[0093] Next, for the high-temperature solvent desorption method using ultra-high temperature water, the solvent temperatures were set to 100°C and 130°C, and the compounds were desorbed from the activated carbon in the column using the same procedure, and the change in absorbance was measured. The measurement results at each solvent temperature are shown in Table 2, along with the measurement results at a solvent temperature of 150°C. Note that the pressure inside the pipe when the solvent temperature was 100°C was 0.1 MPa, and when the solvent temperature was 130°C, the pressure inside the pipe was 0.27 MPa.
[0094] [Table 2]
[0095] [Results and Discussion (2)] For activated carbon adsorbed with TFA, the desorption rate was extremely low when the solvent temperature was 100°C, whereas it was relatively good when the solvent temperature was 130°C and 150°C. Also, for activated carbon adsorbed with PFOA, the desorption rate was 48% when the solvent temperature was 100°C, whereas it reached 100% when the solvent temperature was 130°C and 150°C, which was a significantly better result. Therefore, it was found that the high-temperature solvent desorption method using ultra-high temperature water can effectively desorb per- and polyfluoroalkyl compounds at a solvent temperature of 130°C or higher.
[0096] Therefore, we investigated the properties of activated carbon suitable for high-temperature solvent desorption using ultra-high temperature water.
[0097] [Preparation of activated carbon] For comparative study with activated carbon 1 (trial production example 1), trial production examples 2 to 8 were prepared. In trial production examples 2 to 4, phenolic resin fiber was used as the raw material for activated carbon, and the raw material was heated at 700 to 800°C to form a carbonized product, and the carbonized product was heated to around 800 to 950°C and maintained at that temperature, and activated by introducing steam to obtain a fibrous activated carbon. In trial production example 5, activated carbon was obtained by immersing 10 g of the activated carbon of trial production example 1 in 500 ml of a 6% hydrogen peroxide solution, leaving it to stand for 70 hours, removing it, and drying it.
[0098] In addition, in prototype 6, coal was used as the raw material, the raw material was heated at 200 to 600°C to form a carbonized product, the carbonized product was heated to around 800 to 1000°C and held at that temperature, and steam was introduced to activate the activated carbon. In prototypes 7 and 8, coconut shells were used as the raw material, the raw material was heated at 200 to 600°C to form a carbonized product, the carbonized product was heated to around 800 to 1000°C and held at that temperature, and steam was introduced to activate the activated carbon.
[0099] [Measurement of activated carbon] The BET specific surface area, mode diameter of pore diameter, total pore volume, exclusion limit molecular weight, surface oxide amount, and adsorption / desorption performance were measured for the activated carbons of Prototype Examples 1 to 8. The measurement results of the exclusion limit molecular weight are shown in Table 3, which will be described later, and a summary of the results of each measurement is shown in Tables 4 and 5, which will be described later, respectively.
[0100] [BET specific surface area] For the activated carbons of Samples 1 to 8, nitrogen adsorption isotherms were measured at 77 K using a specific surface area / pore distribution measuring device (Micromeritics, "3Flex"), and the obtained nitrogen adsorption isotherms were analyzed using a multipoint method based on the BET method. The specific surface area (m 2 / g) were calculated respectively.
[0101] [Mode diameter of pore diameter] For the activated carbons of prototypes 1 to 8, a specific surface area / pore distribution measuring device (Micromeritics Corporation, "3Flex") was used to analyze the t-plot of the nitrogen gas adsorption isotherm using the MP method (Micropore method) to determine the mode diameter (nm) of the pore diameter.
[0102] [Total pore volume] For the activated carbons of Samples 1 to 8, the nitrogen gas adsorption isotherm was measured at a relative pressure of 1.0×10 -7 or 1.8 x 10 -1 The maximum amount of nitrogen adsorption (V) was measured by the HK method from the range of 0.01 to 0.11, and converted into the volume of liquid nitrogen (Vp) based on the following formula (iii) to obtain the total pore volume (cm 3 The analytical conditions for the HK method were pore geometry as slit pore geometry, and an interaction parameter of 3.49 × 10 -43 erg cm 4 It was decided.
[0103]
number
[0104] [Exclusion limit molecular weight] The exclusion limit molecular weight of the activated carbons of Prototype Examples 1 to 8 was measured using a liquid chromatograph (HPLC) (Shimadzu Corporation, "LC-20AB"). First, the activated carbons of Prototype Examples 1 to 8 were pulverized using a pulverizer (Freund Turbo Corporation, "VT-300"), and then classified using a classifier (Nippon Pneumatic Mfg. Co., Ltd., "DXF-2") to obtain a particle size of D50 = 15 to 20 μm. Each classified sample of Prototype Examples 1 to 8 was packed into a stainless steel column (Tomoe Manufacturing Co., Ltd., "ES046250", 250 mm x 4.6 mm ID), and the following polystyrene standards (reagents 1 to 5) with different molecular weights were passed through the HPLC system.
[0105] Reagent 1: Fujifilm Wako Pure Chemical Industries, Ltd., 2,4,6-triphenyl-1-hexene standard (TPH), molecular weight 312.45 Reagent 2: Tosoh Corporation, polystyrene standard (PS std.) A-300, molecular weight 453 Reagent 3: Tosoh Corporation, polystyrene standard (PS std.) A-500, molecular weight 589 Reagent 4: Tosoh Corporation, polystyrene standard (PS std.) A-1000, molecular weight 1013 Reagent 5: Tosoh Corporation, polystyrene standard (PS std.) A-2500, molecular weight 3120
[0106] The polystyrene standard sample passed through was detected by a UV detector (Shimadzu Corporation, "SPD-20A") connected downstream of the column, and the change in retention time was confirmed to evaluate whether polystyrene of each molecular weight could penetrate into each of Prototypes 1 to 8, that is, up to what molecular weight could penetrate. The conditions for the HPLC measurement were a flow rate of 0.5 mL / min, a column oven temperature of 40°C, a UV detector wavelength of 254 nm, a mobile phase of chloroform (Kanto Chemical Co., Ltd.), a sample injection amount of 40 μL, and a sample concentration of polystyrene dissolved in chloroform of 1.0 mg / mL.
[0107] In the above HPLC measurement, the retention time changed, suggesting penetration into the activated carbon, and the retention time did not change, suggesting no penetration into the activated carbon, and the smallest molecular weight among the polystyrene standards that did not penetrate the activated carbon (polystyrene standards judged as "x") in each of the prototypes 1 to 8 was determined as the exclusion limit molecular weight. The results are shown in Table 3.
[0108] [Table 3]
[0109] [Surface oxide amount] The activated carbons of Prototype Examples 1 to 8 were subjected to the Boehm method, in which each of the activated carbons of Prototype Examples 1 to 8 was shaken in a 0.05N aqueous solution of sodium hydroxide, filtered, and the amount of sodium hydroxide in the filtrate, which was then neutralized and titrated with 0.05N hydrochloric acid, was measured as the amount of surface oxide (meq / g).
[0110] [Adsorption / desorption performance] The activated carbons of prototypes 1 to 8 were treated in the same manner as the high-temperature solvent desorption method using ultra-high temperature water described above, and the adsorption amounts (mg / g), desorption amounts (mg / g), and desorption rates (%) of TFA and PFOA were determined. The results are shown in Tables 4 and 5. The treatment time required for desorption was approximately 30 minutes for all prototypes 1 to 8.
[0111] [Table 4]
[0112] [Table 5]
[0113] [Results and Discussion (3)] As can be seen from Tables 4 and 5, the amount of PFOA adsorbed (adsorption performance) was good in Prototypes 1 to 3, 5 to 8, but in Prototype 4 it was insufficient. Regarding the desorption rate (desorption performance) of Prototypes 1 to 3, 5 to 8, which had sufficient adsorption performance, in Prototypes 6 and 8, the TFA desorption rate was 40% or less and the PFOA desorption rate was 30% or less, and both desorption efficiencies were insufficient. In addition, in the activated carbon of Prototypes 2, 3, and 7, the TFA desorption rate was high (especially the activated carbon of Prototypes 2 and 3, which was around 100%) and the PFOA desorption rate was around 60%. On the other hand, the activated carbon of Prototypes 1 and 5 had high TFA desorption rates and PFOA desorption rates (especially Prototype 1, both of which were 100%). In other words, the TFA desorption rate, which is assumed to be an organic fluorine compound with a small molecular weight, was high in prototypes 1 to 3, 5, and 7, while the PFOA desorption rate, which is assumed to be an organic fluorine compound with a large molecular weight, was good in prototypes 1 to 3, 5, and 7, and prototypes 1 and 5 in particular showed a high rate and significantly excellent results.
[0114] In addition, comparing prototypes 1 to 3, prototype 1, which has a small mode diameter of the pore diameter, which is considered to be an index of the size of the target adsorbate (molecule) that can be adsorbed, had a significantly superior PFOA desorption rate. From this, it is thought that if the pore diameter is too large, the target adsorbate penetrates deep into the pores of the activated carbon, making it difficult for the target adsorbate to be desorbed. For this reason, it is thought that activated carbon with an appropriate pore diameter is more suitable for desorbing per- and polyfluoroalkyl compounds adsorbed on activated carbon in a short time and with high efficiency by the high-temperature solvent desorption method using ultra-high temperature water.
[0115] Furthermore, comparing the specific surface area of Prototype 1 with that of Prototypes 2 and 3, it was shown that the larger the specific surface area, the better the adsorption performance. On the other hand, in terms of desorption performance, while the TFA desorption rate was good in all of Prototypes 1 to 3, the PFOA desorption rate was significantly better in Prototype 1, which has a small specific surface area. From this, it is considered that when the specific surface area is below a certain level, there is a tendency for the desorption performance to improve, especially for organic fluorine compounds with large molecular weights.
[0116] Comparing prototype 1 and prototype 5 with respect to the amount of surface oxide, the desorption rate of both TFA and PFOA is 90% or more. This shows that a surface oxide amount of about 0.10 to 0.50 meq / g is sufficient for good desorption. It is said that the more the amount of surface oxide in activated carbon (for example, 0.10 meq / g or more), the more hydrophilic the surface of the activated carbon becomes, and the better the adsorption performance for hydrophilic compounds is. However, when using activated carbon in water, it is considered that the amount of surface oxide should be 0.50 meq / g or less, taking into consideration the decrease in adsorption performance due to the clusters of water molecules.
[0117] The larger the total pore volume of activated carbon (e.g., 0.40 cm 3 / g or more), but a comparison of Prototype Examples 1 to 3 suggests that when the total pore volume is below a certain level, there is a tendency for the desorption performance to improve, particularly for organic fluorine compounds with large molecular weights.
[0118] In addition, the molecular weight of PFOA is about 400. Therefore, when focusing on the exclusion limit molecular weight, which is considered to be an index indicating the size of the target adsorbed substance (molecule) that can be adsorbed as an index other than the pore diameter, for example, between prototype 2 and prototype 8, which have the same specific surface area, prototype 2, whose exclusion limit molecular weight is closer to the molecular weight of PFOA, exhibited a better desorption performance of PFOA. From this, it is considered that when per- and polyfluoroalkyl compounds are desorbed from activated carbon by the high-temperature solvent desorption method using ultra-high temperature water, it is also a preferable condition that the exclusion limit molecular weight of the activated carbon used is suitable for the molecular structure and molecular weight of the target adsorbed substance (here, PFOA). If the exclusion limit molecular weight is too large, it is considered that the target adsorbed substance will penetrate deep into the pores of the activated carbon, making it difficult for the target adsorbed substance to be desorbed. For this reason, it is preferable to have an appropriate exclusion limit molecular weight in order to desorb per- and polyfluoroalkyl compounds adsorbed on activated carbon in a short time and with high efficiency by the high-temperature solvent desorption method using ultra-high temperature water.
[0119] Considering the above, when examining the properties of activated carbon suitable for high-temperature solvent desorption using ultra-high-temperature water from Prototypes 1-3, 5, and 7, which have good adsorption and desorption performance, it is considered that the mode diameter of the pore diameter should be specified as approximately 0.50 to 0.70 nm. The BET specific surface area should be 1100 m from the viewpoint of ensuring the basic adsorption performance of activated carbon for recovering per- and polyfluoroalkyl compounds. 2 / g or more, more preferably 1200m 2 / g or more, and from the viewpoint of desorption and recovery of adsorbed per- and polyfluoroalkyl compounds, it is preferable to set the adsorption rate at 1800 m 2 / g or less, more preferably 1400m 2 The amount of surface oxide should be specified as about 0.10 to 0.50 meq / g, more preferably about 0.16 to 0.50 meq / g. The total pore volume should be specified as 0.40 to 0.75 cm, taking into consideration the adsorption performance and the adsorption / desorption performance suitable for high-temperature solvent desorption using ultra-high temperature water. 3 / g, more preferably 0.45 to 0.60 cm 3 The exclusion limit molecular weight should be specified as about 1013 or less, preferably 589 or less, and more preferably 453 or less, in consideration of suitability for the high-temperature solvent desorption method using ultra-high-temperature water and the fact that the target adsorbates range from organic fluorine compounds with small molecular weights to organic fluorine compounds with large molecular weights.
[0120] [High-temperature solvent desorption method] Next, for the high-temperature solvent desorption method, the type of solvent was examined using Solvents 1 to 4 described below. In this test, fibrous activated carbon (Prototype 1) was cut to 20.5 mmφ, stacked to a thickness of 11 mm, and packed into a stainless steel column (Tomoe Manufacturing Co., Ltd., "ES0200050", 50 mm x 20 mm ID). In addition, the following reagents were prepared as reagents to be adsorbed onto the activated carbon, and dissolved in ultrapure water to prepare a mixed sample solution at 1000 ppt. ·PFOA: Manufactured by Wellington Laboratories Inc., Perfluoro-n-octanoic acid ·L-PFOS (PFOS): Manufactured by Wellington Laboratories Inc., Sodium perfluoro-1-octanesulfonate ·FHET(6:2FTOH): Manufactured by Wellington Laboratories Inc., 2-Perfluorohexyl ehanol (6:2)
[0121] The mixed sample solution prepared above was passed through an HPLC system (Agilent Technologies, Inc., "G1311A") at 3.12 mL / min, and the compound concentration of the aqueous solution obtained from the HPLC system outlet was measured by liquid chromatography mass spectrometry (LC-MSMS) and gas chromatography mass spectrometry (GC-MSMS). After the compound concentration at the HPLC system outlet was stabilized at about 1000 ppt, a column packed with activated carbon was connected to the HPLC system. In the liquid chromatography mass spectrometry, a liquid chromatograph analyzer (Waters Corporation, Waters ACQUITY UPLC I-Class PLUS) and a mass spectrometer (Waters Corporation, Xevo TQ-S micro) were used. In the gas chromatography mass spectrometry, a gas chromatograph analyzer (Agilent Technologies, Inc., 8990 GC System) and a mass spectrometer (Waters Corporation, Xevo TQ-S micro) were used.
[0122] The mixed sample solution was passed through the activated carbon in the column at room temperature and at a rate of 3.12 mL / min for 24 hours continuously, and the compounds were adsorbed on the activated carbon in the column. After 24 hours, the aqueous solution obtained from the downstream of the column was analyzed by LC-MSMS and GC-MSMS, and it was confirmed that all the compounds were adsorbed without breakthrough, and then the column was removed. Next, the desorption solvent (solvents 1 to 4 described below) was passed through the HPLC system at 3.12 mL / min, and the HPLC system path was replaced with the desorption solvent, and the column packed with the activated carbon on which the compounds were adsorbed was connected to the HPLC system. The desorption solvent was passed through the activated carbon in the column at 3.12 mL / min, and the inside of the HPLC system was pressurized to 3 MPa, and the desorption solvent was heated to 200 ° C. to form a high-temperature solvent, which was passed through for 30 minutes, and then the passing of the solvent was stopped.
[0123] The activated carbon was removed from the column, and the compounds remaining on the activated carbon without being desorbed were extracted with an organic solvent. In the extraction of compounds from the activated carbon, the removed activated carbon was first introduced into container A (AGC Technoglass Co., Ltd., centrifuge tube 15 mL) and immersed in 10 mL of dichloromethane / ethyl acetate = 1 / 1 for 1 hour. Next, this container was shaken at room temperature (20-25 ° C) and 250 rpm for 30 minutes, and the extract in the container was transferred to container B. This operation was repeated three times in total to obtain containers B and C filled with approximately 15 mL of extract.
[0124] Nitrogen gas was sprayed onto each of the two extracts, and they were concentrated to about 7 mL at 35°C. The entire volume was then combined in container B, and container C was washed three times with a small amount (300-350 μL) of dichloromethane / ethyl acetate = 1 / 1, and transferred to container B. The extract in container B was further concentrated, and then the volume was adjusted to 10 mL with dichloromethane / ethyl acetate = 1 / 1. This extract was diluted and measured in LC-MSMS and GC-MSMS MRM mode, and the compounds extracted with dichloromethane / ethyl acetate were quantified.
[0125] Next, 1% ammonium ion (NH4 +) was added to the sample, and the sample was left to soak for 1 hour. The compound was extracted from the activated carbon in the same manner as in the above compound extraction, and the amount of the compound was quantified.
[0126] The amount of compound adsorbed on activated carbon is W A (ng), the compound concentration measured before connecting the column is C (pg / mL), the flow rate is 3.12 mL / min, and the flow time is 24 hours. A can be calculated from the following formula (iv). The amount of compound remaining in the activated carbon after desorption, W, is calculated by adding the amount of compound extracted with dichloromethane / ethyl acetate and the amount of compound extracted with ammonium ion. B The desorption rate (%) of activated carbon by the high-temperature solvent desorption method can be calculated from the following formula (v): The desorption rates (%) for each of the solvents 1 to 4 are shown in Table 6 below.
[0127]
number
[0128]
number
[0129] [solvent] Solvent 1: Ultrapure water (prepared using PURELAB flex manufactured by ELGA LabWater) Solvent 2: 10% ethanol mixed solvent (Kanto Chemical Co., Ltd., prepared by adding 100 mL of ethanol to 900 mL of ultrapure water) Solvent 3: 30% ethanol mixed solvent (Kanto Chemical Co., Ltd., prepared by adding 300 mL of ethanol to 700 mL of ultrapure water) Solvent 4: 50% ethanol mixed solvent (Kanto Chemical Co., Ltd., prepared by adding 500 mL of ethanol to 500 mL of ultrapure water)
[0130] [Table 6]
[0131] [Results and Discussion (4)] As can be seen from Table 6, extremely good results were obtained for the PFOA desorption rate for each of solvents 1 to 4. For the PFOS desorption rate, improved desorption efficiency was observed for solvents 2 to 4, which were ethanol mixed solvents, compared to solvent 1, which was ultrapure water. For the 6:2 FTOH desorption rate, improved desorption efficiency was observed for solvents 3 and 4, which were ethanol mixed solvents with higher concentrations (30%, 50%) than solvent 2, compared to solvent 1, which was ultrapure water, and solvent 2, which was a low-concentration (10%) ethanol mixed solvent.
[0132] From this, it is considered that in the desorption method using a high-temperature solvent, PFOA, which is assumed to be an organic fluorine compound with a large molecular weight, can be desorbed from activated carbon with high efficiency regardless of the type of solvent. In addition, it is considered that by using a mixed solvent containing an organic solvent, even other organic fluorine compounds with a large molecular weight (PFOS) can be effectively desorbed. Furthermore, it is considered that by using a solvent containing an organic solvent at a predetermined concentration or more, organic fluorine compounds can be desorbed with high efficiency regardless of the molecular weight. From the results of the examples, it is considered that the concentration of the organic solvent is preferably 20% or more, and more preferably 30% or more. [Industrial Applicability]
[0133] The per- and polyfluoroalkyl compound adsorption / desorption activated carbon of the present invention has excellent adsorption / desorption performance of per- and polyfluoroalkyl compounds including harmful substances such as PFOS and PFOA, and has physical properties suitable for desorption methods using high-temperature solvents. Therefore, the activated carbon of the present invention can appropriately remove (adsorb) harmful substances such as PFOS and PFOA, and can recover (desorb) them with high efficiency, so that when treating waste containing the harmful substances, it is possible to recover (desorb) and concentrate the harmful substances, making it possible to select high-temperature solvent desorption as a treatment method other than incineration. Therefore, it is possible to establish a treatment method using high-temperature solvent desorption that can eliminate concerns about re-release of harmful substances such as PFOS and PFOA into the natural world due to conventional incineration. In addition, since it shows good suitability for removal (adsorption) and recovery (desorption) of harmful substances such as PFOS and PFOA, it is promising as a replacement for activated carbon used to remove harmful substances such as conventional PFOS and PFOA.
Claims
1. Among activated carbons that adsorb per- and polyfluoroalkyl compounds in a releasable manner, The activated carbon for desorbing and recovering the adsorbed per- and polyfluoroalkyl compounds using a solvent at a temperature of 130° C. or higher under a high pressure of 0.1 MPa or higher, The activated carbon is BET specific surface area is 1100-1800m 2 / g, The mode diameter of the pore diameter measured by the MP method from the t-plot of the nitrogen gas adsorption isotherm is 0.50 to 0.70 nm, The acidic functional group content determined by the Boehm method is 0.10 to 0.50 meq / g. Activated carbon for adsorbing and desorbing per- and polyfluoroalkyl compounds.
2. The per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to claim 1, wherein the solvent is water.
3. The per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to claim 1, wherein the solvent is a mixed solvent of water and an organic solvent.
4. The per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to claim 3, wherein the organic solvent is ethanol.
5. The per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to claim 1, wherein the solvent is an organic solvent.
6. The per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to claim 5, wherein the organic solvent is ethanol.
7. The total pore volume of the activated carbon determined by analyzing the nitrogen gas adsorption isotherm by the HK method is 0.40 to 0.75 cm 3 The per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to any one of claims 1 to 6, wherein the activated carbon has a molecular weight of 1 / g.
8. 7. The per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to claim 1, wherein the activated carbon has an exclusion limit molecular weight of 1013 or less as measured using a polystyrene standard.
9. The per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to claim 7, wherein the activated carbon has an exclusion limit molecular weight of 1013 or less as measured using a polystyrene standard.
10. The per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to claim 8, wherein the exclusion limit molecular weight is 453 or less.
11. The per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to claim 9, wherein the exclusion limit molecular weight is 453 or less.
12. The per- and polyfluoroalkyl compound adsorption and desorption activated carbon according to any one of claims 1 to 6, wherein the activated carbon is a fibrous activated carbon.
13. The per- and polyfluoroalkyl compound adsorption and desorption activated carbon according to claim 7, wherein the activated carbon is a fibrous activated carbon.
14. The per- and polyfluoroalkyl compound adsorption and desorption activated carbon according to claim 8, wherein the activated carbon is a fibrous activated carbon.
15. The per- and polyfluoroalkyl compound adsorption and desorption activated carbon according to claim 9, wherein the activated carbon is a fibrous activated carbon.
16. The per- and polyfluoroalkyl compound adsorption and desorption activated carbon according to claim 10, wherein the activated carbon is a fibrous activated carbon.
17. The per- and polyfluoroalkyl compound adsorption / desorption activated carbon according to claim 11, wherein the activated carbon is a fibrous activated carbon.
Citation Information
Patent Citations
Activated carbon adsorbing per- and polyfluoroalkyl compounds in water sample
JP2021079376A