Semiconductor substrate, manufacturing method for the same, and manufacturing method for semiconductor
A wet process for manufacturing ZnS and FeS semiconductor substrates addresses the limitations of high-temperature heat treatment in Si-based methods, providing flexible, cost-effective substrates with adjustable band gaps for diverse applications.
Patent Information
- Application Number
- JP2023140361
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-01
- Filing Date
- 2023-08-30
- Publication Date
- 2024-11-01
AI Technical Summary
Conventional methods for manufacturing semiconductor substrates using Si-based materials require high-temperature heat treatment and vacuum processes, which are costly and difficult to handle, limiting their applicability and efficiency.
A wet process is used to manufacture a semiconductor substrate composed of ZnS and FeS, allowing for the formation of a semiconductor layer with adjustable band gaps, which can be applied to flexible substrates without high-temperature heat treatment, enabling attachment to curved surfaces and reducing manufacturing costs.
The process enables the production of stable, flexible semiconductor substrates with wide band gap adjustments, suitable for various applications including solar cells, and reduces manufacturing costs by utilizing general-purpose materials.
Smart Images

Figure 2024156216000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a semiconductor substrate made of an Fe2ZnS2-based semiconductor composition, a method for producing the same, and a method for producing a semiconductor. [Background technology]
[0002] Iron sulfide is composed of Fe and S, which are abundant elements on Earth, and is widely found in nature as pyrite. It is known that when the amount of S in iron sulfide is increased or decreased from the stoichiometric composition, it functions as a solid semiconductor that exhibits p-type or n-type conductivity, respectively. It is also known that the addition of impurities to iron sulfide can make it conductive.
[0003] So far, we have been studying FeS2 in which part of the Fe has been replaced with Zn. 1-x Zinc x It is known that S2 (x=0 to 1) has a band gap of about 0.5 eV when the Fe:Zn ratio is 2:1 (see, for example, the theoretical calculation in Non-Patent Document 1), and such Fe2ZnS2-based semiconductor compositions are considered to be suitable for use as light absorbers in various optical devices, including solar cells.
[0004] Meanwhile, several methods for synthesizing iron disulfide (FeS2) as a semiconductor have been proposed. For example, Patent Document 1 discloses a method for producing FeS2 by reacting ferric oxide (Fe2O3), hydrogen sulfide (H2S) and S at a temperature higher than the melting point of sulfur (S). Patent Document 2 discloses a method for producing FeS2 by mixing hydrate of iron sulfate (FeSO4), sodium thiosulfate (Na2S2O3) and S, adjusting the pH to the range of 1.0 to 7.0, and subjecting the mixture to hydrothermal treatment. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2010-540387 [Patent Document 2] JP 2011-256090 A [Non-patent literature]
[0006] [Non-Patent Document 1] Jun Hu, Yanning Zhang, Matt Law, and Ruqian Wu;"Increasing the Band Gap of Iron Pyrite by Alloying with Oxygen"; Journal of the American Chemical Society 2012, 134, 32, 13216-13219 Summary of the Invention [Problem to be solved by the invention]
[0007] In contrast to the conventional manufacturing method of semiconductor substrates made of Si-based materials using a vacuum process, the Fe2ZnS2-based semiconductor composition can be manufactured using a wet process as described above, and is superior in terms of manufacturability in terms of cost and ease of handling, but on the other hand, high-temperature heat treatment is required. Therefore, if heat treatment can be made unnecessary or at a relatively low temperature, it is expected that new semiconductor substrates can be proposed by utilizing the wet process.
[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a semiconductor substrate that can be manufactured using a wet process and is made of an Fe2ZnS2-based semiconductor composition, a manufacturing method thereof, and a manufacturing method for a semiconductor. [Means for solving the problem]
[0009] The semiconductor substrate including the semiconductor layer including ZnS and FeS2 according to the present invention can adjust the band gap by changing the composition of Zn and Fe, and has a high industrial applicability as a semiconductor substrate. In addition, it can be manufactured using a wet process, and does not require heat treatment at high temperatures, so that a substrate such as a resin can be used, which is not only excellent in terms of manufacturing cost and ease of handling, but also allows for a significant weight reduction.
[0010] That is, the semiconductor substrate according to the present invention is characterized by including a p-type semiconductor layer containing ZnS and FeS2 laminated on a flexible substrate.
[0011] This feature allows the tape to be attached to curved surfaces and is therefore highly versatile.
[0012] In the above-mentioned invention, the p-type semiconductor layer may be made of a solid solution of ZnS and FeS2. This feature provides excellent stability and wide band gap adjustment by the composition ratio of the solid solution, resulting in a wide range of applicability.
[0013] In the above-mentioned invention, it may be characterized in that an n-type semiconductor layer made of ZnO is laminated on the p-type semiconductor layer. It may also be characterized in that a transparent electrode is laminated on the n-type semiconductor layer. With such a feature, it is possible to form a pn junction from inexpensive materials, and it is possible to provide a pn element that is excellent in terms of cost.
[0014] In the above-mentioned invention, a metal electrode layer made of Al may be inserted between the substrate and the p-type semiconductor layer. The substrate may be made of PET. This feature allows the use of a general-purpose material, and allows the substrate to be attached to curved surfaces, etc., making the device highly versatile.
[0015] In addition, the method for manufacturing a semiconductor substrate according to the present invention is a method for manufacturing a semiconductor substrate in which a semiconductor layer made of ZnS and FeS2 is laminated on a flexible substrate, and is characterized by comprising a step of exposing the zinc ferrite plating layer formed on the substrate to hydrogen gas for hydrogen reduction treatment, and then exposing it to hydrogen sulfide gas to form the semiconductor layer, which is a p-type semiconductor made of a solid solution of ZnS and FeS2.
[0016] According to this feature, it is possible to efficiently manufacture a semiconductor substrate that can be attached to a curved surface or the like.
[0017] In the above-mentioned invention, the p-type semiconductor layer may be made of a solid solution of ZnS and FeS2. With this feature, it is possible to efficiently manufacture a semiconductor substrate that is excellent in stability and has a wide band gap that can be adjusted by the composition ratio of the solid solution, and is highly versatile.
[0018] In the above-mentioned invention, the belt-shaped substrate is fed in the longitudinal direction and passed through a reaction chamber to deposit Zn on the substrate. 1-x Fe 2+ x Fe 3+ The method may further include a step of forming the zinc ferrite plating layer made of 2O4 (x=0 to 1). According to this feature, the semiconductor substrate can be manufactured efficiently.
[0019] In the above-mentioned invention, the method may be characterized by comprising the steps of: moving the film-forming portion of the substrate from upstream to downstream and arranging it on the top opening of a flat plate, and arranging the film-forming portion of the substrate inside the flat plate; filling the flat plate with a reaction solution containing Fe and Zn to form a metal film; and changing the reaction solution into an oxidizing solution to oxidize the metal film and form a zinc ferrite plating layer. The method may also be characterized by repeating the steps of forming the metal film and oxidizing the metal film to form a zinc ferrite plating layer. According to such features, a semiconductor substrate with excellent smoothness can be efficiently manufactured.
[0020] In the above-mentioned invention, the reaction liquid may be a mixture of FeCl2 and ZnCl2. Furthermore, the oxidizing liquid may be NaNO2. According to this feature, a semiconductor substrate can be efficiently manufactured using general-purpose materials.
[0021] In the above-mentioned invention, in the step of forming the zinc ferrite plating layer, the back surface of the substrate may be contact-heated by a heating block to control the temperature of the film formation section at 100° C. or higher. With this feature, semiconductor substrates can be manufactured stably and efficiently.
[0022] In the above-mentioned invention, the reaction liquid and the oxidizing liquid may be caused to flow inside the flat plate along the feed direction of the substrate, respectively. With this feature, a semiconductor substrate having excellent smoothness can be efficiently manufactured.
[0023] In addition, the method for producing a semiconductor according to the present invention is a method for producing a semiconductor containing ZnS and FeS2, and is characterized by comprising a step of reducing zinc ferrite and a step of exposing the zinc ferrite that has been subjected to the reduction treatment to hydrogen sulfide gas.
[0024] According to this feature, semiconductors containing ZnS and FeS2 can be produced efficiently.
[0025] In the above-mentioned invention, the step of reducing the zinc ferrite may be a step of exposing the zinc ferrite to a gas containing hydrogen. According to this feature, the above-mentioned semiconductor can be stably and efficiently manufactured.
[0026] In the above-mentioned invention, the semiconductor containing ZnS and FeS2 may be a p-type semiconductor made of a solid solution of ZnS and FeS2. According to this feature, it is possible to obtain a semiconductor having excellent stability and a wide band gap that can be adjusted by the composition ratio of the solid solution, and thus having a wide range of applications. [Brief description of the drawings]
[0027] [Figure 1] 1A and 1B are cross-sectional views of semiconductor substrates according to the present invention, where (a) is a p-type semiconductor substrate and (b) is a pn junction semiconductor substrate. [Diagram 2] 1 is a manufacturing flow diagram of a semiconductor substrate according to the present invention. [Diagram 3] 1 is a side view of a semiconductor substrate manufacturing apparatus according to the present invention; [Figure 4] 1A is a top view of a main part of a semiconductor substrate manufacturing apparatus according to the present invention, and FIG. 1B is a side view of the main part. [Diagram 5] FIG. 11 is a block diagram of another semiconductor substrate manufacturing apparatus according to the present invention. [Figure 6] 1 is an XRD profile of a semiconductor substrate simulating a manufacturing method according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] A semiconductor substrate as one embodiment of the present invention will now be described.
[0029] As shown in FIG. 1(a), the semiconductor substrate A1 is formed by laminating a metal electrode layer 12 and a p-type semiconductor layer 14 containing ZnS and FeS2 on a substrate 10 made of, for example, resin, which has flexibility. As described later, the semiconductor substrate A1 of this embodiment is manufactured using an aqueous solution process, and can be manufactured without using a vacuum process or a high-temperature annealing process. Therefore, the substrate 10 made of a low-melting-point material such as resin can be used, and the semiconductor substrate A1 has flexibility against deformation, and can be used, for example, on a curved surface, making it highly versatile. The p-type semiconductor layer 14 may be doped with impurities as necessary.
[0030] The substrate 10 is preferably a flexible resin sheet, for example, a general-purpose resin sheet made of PET. In addition to resin, materials made of metal, wood (plywood), paper, ceramics, etc. may be used as long as they are flexible. The thickness of the substrate 10 may be determined based on the mechanical properties required for a semiconductor element. Since an aqueous solution process is used to form the semiconductor layer, the wettability of the laminated surface side of the substrate 10 is considered, but it is sufficient that at least a metal film can be provided to insert the metal electrode layer 12 between the substrate 10 and the p-type semiconductor layer 14.
[0031] From the viewpoint of the work function with the p-type semiconductor layer 14 mainly made of pyrite (FeS2), the metal electrode layer 12 is preferably made of silver, but from the viewpoint of cost, it is also preferable to use aluminum or an alloy thereof. In such a case, it is also preferable to interpose a hole transport layer (HTL) between the substrate 10 and the metal electrode layer 12.
[0032] The p-type semiconductor layer 14 is made of ZnFe2S2 containing ZnS and FeS2, and in a manufacturing method starting from zinc ferrite (ZnFe2O4) described later, it is made of a solid solution of ZnS and FeS2. That is, ZnO in the positive spinel structure of zinc ferrite is the A site (four-fold coordination), and ZnS is a four-fold coordination wurtzite type. In the hydrogen sulfide treatment step (S32, see FIG. 2), the O of Zn is 2- S 2- In this case, the crystal structure is maintained. 3+ is 6-coordinated at the B site, and has the same face-centered cubic structure as the NaCl type of pyrite (FeS2), and this is also O 2- S 2- The crystal structure is maintained even if the lattice constant of ZnS (zinc sulfide) is a = 0.542 nm, while the lattice constant of FeS2 is also a = 0.542 nm. 2+ and Fe 2+ This is because ZnS and FeS2 have a structure that allows them to form a solid solution in a crystalline solid.
[0033] Here, three types of Zn are used, with x=0.1, 0.3, and 0.5. 1-x Fe 2+ x Fe 3+ A 2O4 film (approximately 40 nm thick) was prepared and then, as described below, 2- S 2- The reaction of exchanging the ZnS with the FeS2 was promoted to convert the ZnS to pyrite, forming the p-type semiconductor layer 14. The band gaps of the films were measured by visible and far-infrared absorption, and were 0.8, 0.6, and 0.4 eV, respectively. In other words, by changing the x value in the solid solution of ZnS and FeS2, the band gap can be changed in the range from the visible to the far-infrared region. In this way, the semiconductor substrate A1 is excellent in stability, and the band gap can be adjusted widely from the composition ratio of the solid solution, making it highly applicable. For example, in a solar cell that generates electricity in the far-infrared region, it is possible to transmit light in the visible light region and combine it with another solar cell that generates electricity with light of a wavelength in that region.
[0034] 1(b), a semiconductor element A2, which is an embodiment including the semiconductor substrate A1, is formed by laminating an n-type semiconductor layer 24 constituting a pn junction and a transparent electrode layer 22 pairing with the metal electrode layer 12 on a p-type semiconductor layer 14. In addition, a transparent substrate 20 is preferably provided on the transparent electrode layer 22.
[0035] The n-type semiconductor layer 24 is typically made of ZnO, although there are no limitations on the material as long as it can form a pn junction with the p-type semiconductor layer 14. This is an inexpensive material that can be combined with the inexpensive n-type semiconductor layer 24, and is also excellent in terms of cost.
[0036] The transparent electrode layer 22 can typically be made of a known transparent conductive film such as ITO (indium tin oxide).
[0037] The transparent substrate 20 functions as a protective film for the semiconductor element A2, and may be necessary when bonding the semiconductor substrate A1 to the semiconductor substrate A1 after manufacturing the other parts of the semiconductor substrate A1. For this purpose, it is preferable to use, for example, PET.
[0038] Next, a manufacturing method as one embodiment of the above-mentioned semiconductor substrate A1 will be described with reference to Fig. 2. The manufacturing method of the semiconductor substrate A1 is roughly divided into three steps, namely, a zinc ferrite film continuous forming step (S1), a cutting step (S2), and a pyrite forming step (S3).
[0039] As shown in FIG. 3, in the zinc ferrite film continuous formation process (S1), the substrate 10 made of a strip-shaped PET film having a vapor-deposited film on its surface as the metal electrode layer 12 is fed in the longitudinal direction from the feed roll 41 through the guide roll 44a, and is passed through the reaction chamber 53 continuously after repeatedly stopping and moving within the reaction chamber 53 as described below. After passing through the reaction chamber 53, the substrate 10 is taken up by the take-up roll 43 through the guide roll 44b. In the reaction chamber 53, the substrate 10 moves and is heated on the flat plate 55 inside the reaction chamber 53, while a plating solution consisting of a reaction solution and an oxidation solution is applied in this order on the metal electrode layer 12 to cause a reaction, and a Zn ferrite film having a predetermined composition with x adjusted is formed. 1-x Fe 2+ x Fe 3+ A zinc ferrite plating layer made of 2O4 is continuously formed.
[0040] More specifically, the inside of the reaction chamber 53 is purged of inert gas such as Ar gas from the gas tank 34 by opening the valve 34a, and an inert gas atmosphere is created. Then, the delivered substrate 10 is placed on the upper opening of a flat plate 55 inside the reaction chamber 53 and stopped. Three heating blocks 51a to 51c are arranged at regular intervals in the longitudinal direction of the substrate 10 above the substrate 10 placed on the flat plate 55, and each of them can move up and down. The heating blocks 51a to 51c are preferably made to have a large thermal capacity so that the temperature is not easily changed by the flow of the plating solution, and are formed, for example, by embedding a heater in a substantially rectangular block made of marble.
[0041] Referring also to FIG. 4, the positions in the flat plate 55 below the heating blocks 51a to 51c are the film formation positions C1 to C3. Here, the substrate 10 sent onto the flat plate 55 is stopped when the film formation portion, which is a substantially rectangular area, is located on the film formation position C1. That is, the film formation portion is located at a position facing the heating block 51a. Here, the heating block 51a is moved downward so that the film formation portion of the substrate 10 is located at the film formation position C1 inside the flat plate 55, and the film formation portion is pressed with a predetermined pressure P. The heating block 51a is heated in advance to a predetermined temperature, and heats the film formation portion of the substrate 10. Here, the heating block 51a abuts against the upper surface (rear surface) of the film formation portion to perform contact heating, and since the heat capacity of the heating block 51a is large, the film formation portion can be heated stably and efficiently. The substrate 10 is sent out with the surface on which the zinc ferrite plating layer is to be formed (front surface), that is, the surface on which the metal electrode layer 12 is formed, facing downward.
[0042] The plating solution is composed of a reaction solution containing Fe and Zn, and an oxidation solution that oxidizes the precursor film formed by the reaction solution. The reaction solution is filled into the flat plate 55 by opening the first valve 31a from the first tank 31, and is sent out so as to circulate while maintaining the filled state, and contacts the metal electrode layer 12 from the bottom (see the arrow in FIG. 1B). The circulating reaction solution is discharged from the flat plate 55 to the outside by opening the drain valve 33a to the drain tank 33. The reaction solution may be further circulated and circulated into the flat plate 55. After the metal film 13 is formed in this way, the first valve 31a is closed to discharge the reaction solution.
[0043] Next, the oxidizing liquid is filled into the flat dish 55 from the second tank 32 by opening the second valve 32a, and is sent out to circulate while maintaining the filled state, contacting the formed metal film 13 and oxidizing the metal film 13. This forms a zinc ferrite plating layer on the metal electrode layer 12. Then, the heating block 51a is moved upward to discharge the oxidizing liquid and send the substrate 10 with the zinc ferrite plating layer formed downstream.
[0044] The substrate 10 sent downstream is further stopped at a position corresponding to the film formation position C2. The heating block 51b is then moved downward to press the film formation section with a predetermined pressure P while positioning it at the film formation position C2 and contact heating it. Furthermore, similar to the above, the reaction liquid and the oxidation liquid are circulated in this order and applied to form a second zinc ferrite plating layer. Similarly, the substrate 10 is further sent downstream to form a third zinc ferrite plating layer at the film formation position C3.
[0045] In this manner, a total of three zinc ferrite plating layers can be formed on the film formation portion of the substrate 10, one layer at each of the film formation positions C1 to C3.
[0046] By performing the above-mentioned operation by operating the three heating blocks 51a to 51c simultaneously, zinc ferrite plating layers can be formed simultaneously at each of the film formation positions C1 to C3. Then, the operation is repeated so that the first layer of zinc ferrite plating layer is formed simultaneously at the film formation position C1, the second layer at the film formation position C2, and the third layer at the film formation position C3. Then, from the first film formation portion of the substrate 10, film formation portions in which three zinc ferrite plating layers are formed at a position upstream (left side of the paper) can be obtained at an equal pitch. In this way, zinc ferrite plating layers can be formed continuously on the substrate 10.
[0047] Typically, a mixed solution of FeCl2 and ZnCl2 is used as the reaction solution, and a solution of NaNO2 is used as the oxidizing solution, so that semiconductor substrates can be efficiently manufactured from general-purpose materials, but other known liquid materials may also be used. Typically, the reaction temperature is controlled to 60 to 150°C, preferably 100°C or higher, and the temperature is adjusted by utilizing contact heating by heating blocks 51a to 51c with large heat capacity, so that semiconductor substrates can be manufactured stably and efficiently.
[0048] The time for which the substrate 10 is stopped in the reaction chamber 53 is determined taking into consideration the thickness of the plating layer, the reaction temperature, etc. It is also preferable that the plating solution filled in the flat dish 55 is circulated from the upstream side to the downstream side in the feed direction of the substrate 10, that is, from the film formation position C1 side to the C3 side. In this way, new plating solution can be supplied to the film formation position C1 side where the first layer is formed. In addition, although three heating blocks 51a to 51c are provided in the above, the number of heating blocks may be changed to change the number of zinc ferrite plating layers formed.
[0049] It is also possible to oxidize the precursor film obtained in the reaction liquid with air without using an oxidizing liquid. In this case, the oxidizing liquid is supplied to the substrate 10 so as to entrain air therein. For example, it is possible to consider feeding a carrier film between the flat plate 55 and the substrate 10 in the reaction chamber 53 slower or faster than the feed speed of the substrate 10, thereby entraining air between the substrate 10 and the carrier film and guiding it to the substrate 10 together with the oxidizing liquid.
[0050] The substrate 10 taken up by the take-up roll 43 in the zinc ferrite film forming step (S1) is cut in the cutting step (S2). In the cutting, the substrate 10 is cut along a plane perpendicular to the longitudinal direction so as to separate each of the film-forming portions C1 to C3.
[0051] In the subsequent pyrite formation step (S3), the zinc ferrite plating layer formed on the substrate 10 on which the metal electrode layer 12 was provided in the zinc ferrite film continuous formation step (S1) is removed. 2- S 2- The reaction proceeds by exchanging S to pyrite. 2- To convert it to hydrogen sulfide, it is treated with hydrogen sulfide (hydrogen sulfide treatment step, S32), but this treatment requires a reduction treatment (hydrogen reduction treatment step, S31) as a pretreatment.
[0052] The substrate cut in the cutting step (S2) is transferred to a separately prepared reaction chamber. In the reaction chamber, a hydrogen reduction treatment step (S31) is performed in which hydrogen gas is brought into contact with the surface of the zinc ferrite plating layer to perform hydrogen reduction treatment, and a hydrogen sulfide gas is brought into contact with the surface after the supply of hydrogen gas is stopped to reduce the surface. 2- The hydrogen sulfide treatment process (S32), in which ions are diffused inside to form FeS and FeS2, and the holding process (S22), in which the supply of hydrogen sulfide gas is stopped and the material is held to form a p-type semiconductor, are carried out in a series without exposure to the outside air. This allows semiconductor substrates to be manufactured more efficiently.
[0053] More specifically, as shown in FIG. 5, the reaction chamber 61 is provided in a reaction device 60. The reaction device 60 is provided with shelves 62-1 to 62-4 on which the cut substrate 10a cut inside the reaction chamber 61 can be placed substantially horizontally. The cut substrate 10a is placed on the shelves 62-1 to 62-4 with the zinc ferrite plating layer facing upward so as to be exposed to the circulating gas. The reaction device 60 is also provided with a gas circulation path 63 for circulating gas toward each of the shelves 62-1 to 62-4, and is connected to a hydrogen tank 65 for supplying hydrogen gas and a hydrogen sulfide tank 66 for supplying hydrogen sulfide gas via a hydrogen gas valve 65a and a hydrogen sulfide gas valve 66a, respectively. The gas circulation path 63 is further provided with a pump 67 for circulating gas, an exhaust valve 68 provided in a branch arranged downstream of the pump 67 to exhaust gas to the outside, and a stop valve 69 arranged downstream of the branch to stop the flow of gas during exhaust or the like.
[0054] That is, in the hydrogen reduction treatment step (S31), hydrogen gas can be circulated and brought into contact with the after-cut substrates 10a by opening the hydrogen gas valve 65a while operating the pump 67. After the supply of hydrogen gas is stopped, in the hydrogen sulfide treatment step (S32), hydrogen sulfide gas can be circulated and brought into contact with the after-cut substrates 10a by opening the hydrogen sulfide gas valve 66a while operating the pump 67.
[0055] Here, in the hydrogen reduction treatment step (S31) using hydrogen gas in the reaction chamber 61, Fe 3+ (δ')+O 2- (1 / 2δ')+H2(δ') =Fe 2+ (δ')+V(O 2- )(1 / 2δ')+δ'H2O (Eq. 1) The reaction proceeds as follows: where δ' is Fe 3+ The reduced component ratio of V(O 2- ) is O 2- The hydrogen gas is preferably caused to flow along the surface.
[0056] Next, in the hydrogen sulfide treatment step (S32), after stopping the supply of hydrogen gas, hydrogen sulfide gas is brought into contact with the surface of the zinc ferrite layer to form S 2- The ions are diffused inward to form FeS and FeS2 near the surface. The coating formed here is made of oxygen-deficient zinc ferrite. In other words, hydrogen sulfide is reacted with the oxygen-deficient compound formed by the reduction treatment with hydrogen gas in the above formula 1, and the reaction formula is as follows: Formula 2 and Formula 3 (the two reactions are 2e - (Proceeding through). Fe 2+ (δ) + V(O 2- )(1 / 2δ)+δH2S+2e - (δ) =δFeS+δH2 (Formula 2) Fe 2+ (2δ)=Fe 3+ (2δ)+2e - (δ) (Formula 3)
[0057] At the initial stage of the hydrogen sulfide treatment step (S32), black FeS is formed near the surface of the zinc ferrite layer (Equation 2), and at the same time, FeS is formed near the surface by reduction with hydrogen gas. 2+ Fe 3+ (Equation 3) This reaction can also be confirmed by the observation of the black coloration of FeS during the reaction.
[0058] In the holding step (S33), the supply of hydrogen sulfide gas is stopped and the state is held as it is, and FeS and FeS2 become a solid solution of ZnS and FeS2. The film exposed to hydrogen sulfide gas changes over time into a p-type semiconductor layer 14, which is a ZnFe2S2 film. In other words, a semiconductor thin film is formed in which a semiconductor layer made of a solid solution of ZnS and FeS2 is formed in a part of the zinc ferrite layer formed initially.
[0059] Here, the free energy of the reaction, ΔG, indicates the direction of change from oxide to sulfide. During the reaction, at the interface where the surface side is sulfide and the inner side is oxide, the free energy of the surface reaction, O 2- and S. 2- As shown in formula 1, when hydrogen reduction treatment is performed using hydrogen gas, the hydrogen gas converts O 2- Ions are released and a concentration gradient is created between the inside and the outside. 2- will move from the inside to the surface area. Also, at the interface (surface), O 2- / S 2- By exchange reaction, S 2- is consumed, so S 2- The O diffuses from the surface to the inside. 2- and S. 2- In the exchange reaction, the original Zn 1-x Fe 2+ x Fe 3+ The metal ions in the spinel structure of the 2O4 zinc ferrite phase do not move from their sites, but rather are transported through the S 2- The ionic crystal coordination structure is maintained as is, and ZnS and FeS2 form a single crystal structure as a mixed crystal.
[0060] Here, in the hydrogen sulfide treatment step (S32), the reactions of formulas 2 and 3 proceed in a coupled manner, and further, the following reaction proceeds in parallel with this reaction. FeS+H2S=FeS2+H2 (formula 4)
[0061] The reaction free energy of formula 4 is negative in the temperature range of 25 to 250°C (for example, -41 kJ / mol at 25°C). By setting the reaction conditions within this temperature range, it is possible to synthesize the FeS2 phase having an x value that is a thermodynamically and stoichiometrically stable phase from the FeS phase formed by the above-mentioned reaction formulas 1 to 3.
[0062] Alternatively, a semiconductor layer made of a solid solution of ZnS and FeS2 may be formed by supplying a mixed gas of hydrogen sulfide gas and hydrogen gas. In other words, the hydrogen reduction treatment step (S31) and the hydrogen sulfide treatment step (S32) are performed in a single step.
[0063] In Fig. 6, Zn with x=0.4 is 0.6 Fe 2+ 0.4 Fe 3+ The figure shows the XRD profile of the ZnFe2S2 film obtained by simulating a hydrogen reduction treatment step (S31) and a hydrogen sulfide treatment step (S32) after providing a zinc ferrite layer (65 nm thick) made of 2O4 on a PET film. In the hydrogen sulfide treatment step (S32), the reaction was carried out at a temperature in the range of 120 to 150°C. As can be seen from this XRD profile, the ZnS phase, FeS phase, and FeS2 phase formed by the reaction are mixed together with the unreacted ferrite phase. On the other hand, if the holding step (S33) is carried out sufficiently, a single-phase compound is obtained, but the Fe:Zn:S=0.4:2.6:2, which is the stoichiometric composition (Zn 0.2 Fe 2.6 S 2.0 When the hydrogen reduction treatment step (S31) was omitted, the FeS2 phase was not formed even when the hydrogen sulfide treatment step (S32) was performed at least in the temperature range of 120 to 150°C.
[0064] Furthermore, the semiconductor element A2 can be provided by preparing a multilayer structure in which a transparent electrode layer 22 made of ITO and an n-type semiconductor layer 24 made of ZnO are laminated on a transparent substrate 20 such as PET, and by combining the n-type semiconductor layer 24 with the p-type semiconductor layer 14 of the above-mentioned semiconductor substrate A1 to form a pn connection.
[0065] Semiconductors containing ZnS and FeS2 in shapes other than the above substrates can also be manufactured in the same manner. 1-x Fe 2+ x Fe 3+ A semiconductor containing ZnS and FeS2 is obtained by subjecting zinc ferrite made of 2O4 to a reduction process, such as exposing it to hydrogen gas, and then exposing it to hydrogen sulfide gas. The semiconductor obtained in the same manner as above is, for example, a p-type semiconductor made of a solid solution of ZnS and FeS2, and is formed on the surface layer of the zinc ferrite.
[0066] Although the embodiments of the present invention and modifications based thereon have been described above, the present invention is not necessarily limited to these examples. In addition, a person skilled in the art will be able to find various alternative embodiments and modifications without departing from the spirit of the present invention or the scope of the appended claims. [Explanation of symbols]
[0067] 10 Substrate 12 Metal electrode layer 14 p-type semiconductor layer 20 Transparent Substrate 22 Transparent electrode layer 24 n-type semiconductor layer 31 First Tank 32 Second Tank 41 Payout roll 43 Winding roll 44a, 44b Guide roll 53 Reaction Chamber 55 Flat Plate 51a~c Heating block 60 Reactor 61 Reaction Chamber 62-1~4 Shelves 63 Gas Circulation 65 Hydrogen Tank 66 Hydrogen Sulfide Tank 66 67 Pump A1 Semiconductor substrate A2 Semiconductor element
Claims
1. ZnS and FeS on a flexible substrate 2 A semiconductor substrate comprising a p-type semiconductor layer comprising:
2. The p-type semiconductor layer is made of ZnS and FeS 2 2. The semiconductor substrate according to claim 1, characterized in that it comprises a solid solution of
3. 2. The semiconductor substrate according to claim 1, further comprising an n-type semiconductor layer made of ZnO laminated on said p-type semiconductor layer.
4. 4. The semiconductor substrate according to claim 3, further comprising a transparent electrode laminated on the n-type semiconductor layer.
5. 5. The semiconductor substrate according to claim 4, further comprising a metal electrode layer made of Al inserted between said substrate and said p-type semiconductor layer.
6. 5. The semiconductor substrate according to claim 4, wherein the substrate is made of PET.
7. ZnS and FeS on a flexible substrate 2 A method for manufacturing a semiconductor substrate having a p-type semiconductor layer formed thereon, comprising: The zinc ferrite plating layer formed on the substrate is exposed to hydrogen gas for hydrogen reduction treatment, and then exposed to hydrogen sulfide gas to form ZnS and FeS. 2 forming a p-type semiconductor layer comprising a p-type semiconductor comprising:
8. The p-type semiconductor layer is made of ZnS and FeS 2 8. The method for manufacturing a semiconductor substrate according to claim 7, wherein the semiconductor substrate is a solid solution of
9. The belt-shaped substrate is fed in the longitudinal direction and passed through a reaction chamber, so that Zn is deposited on the substrate. 1-x Fe 2+ x Fe 3+ 2 O 4 8. The method for manufacturing a semiconductor substrate according to claim 7, further comprising the step of forming the zinc ferrite plating layer consisting of (x=0 to 1).
10. A step of moving the film formation portion of the substrate from upstream to downstream and arranging the film formation portion of the substrate on an upper surface opening of a flat plate, and arranging the film formation portion of the substrate inside the flat plate; A step of filling the dish with a reaction solution containing Fe and Zn to form a metal film; and 10. The method for manufacturing a semiconductor substrate according to claim 9, further comprising the step of changing the reaction liquid into an oxidizing liquid to oxidize the metal film and form a zinc ferrite plating layer.
11. 11. The method for manufacturing a semiconductor substrate according to claim 10, wherein the step of forming the metal film and the step of oxidizing the metal film to form a zinc ferrite plating layer are repeated.
12. The reaction solution is FeCl 2 and ZnCl 2 11. The method for manufacturing a semiconductor substrate according to claim 10, wherein the mixed solution is a mixture of the above.
13. The oxidizing solution is NaNO 2 13. The method for manufacturing a semiconductor substrate according to claim 12,
14. 11. The method for manufacturing a semiconductor substrate according to claim 10, wherein in the step of forming the zinc ferrite plating layer, the back surface of the substrate is contact-heated with a heating block to control the temperature of the film formation section to 100° C. or higher.
15. 11. The method for manufacturing a semiconductor substrate according to claim 10, wherein the reaction liquid and the oxidizing liquid are each caused to flow inside the flat plate along a feed direction of the substrate.
16. ZnS and FeS 2 A method for manufacturing a semiconductor, comprising: A step of reducing zinc ferrite; and exposing the reduced zinc ferrite to hydrogen sulfide gas; ZnS and FeS 2 A semiconductor manufacturing method comprising the steps of:
17. 17. The method for manufacturing a semiconductor according to claim 16, wherein the step of reducing the zinc ferrite is a step of exposing the zinc ferrite to a gas containing hydrogen.
18. The ZnS and FeS 2 The semiconductor containing ZnS and FeS 2 18. The method for producing a semiconductor according to claim 16, wherein the p-type semiconductor is a solid solution of
Citation Information
Patent Citations
The process of producing synthetic pyrite
JP2010540387A
Iron sulfide and method for producing the same
JP2011256090A