Method for analyzing crosslinking degree of peroxide crosslinked rubber

The method uses thermogravimetric measurement to quantify peroxide consumption in crosslinked rubber, addressing the inadequacies of existing methods and enhancing process control and product quality by accurately determining the degree of crosslinking.

JP2024156267AActive Publication Date: 2024-11-06MITSUBISHI CABLE INDUSTRIES LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023070589
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-06
Estimated Expiration
2043-04-24

AI Technical Summary

Technical Problem

Existing methods for analyzing the degree of crosslinking in peroxide crosslinked rubber are inadequate, particularly in identifying the consumption of peroxide as a crosslinking agent, which affects the quality and appearance of molded products.

Method used

A method involving thermogravimetric measurement of uncrosslinked and completely crosslinked rubber compositions, determining the weight loss rates to calculate the consumption of peroxide, thereby assessing the degree of crosslinking through the difference in weight loss rates between these states.

Benefits of technology

Accurately determines the degree of crosslinking in peroxide crosslinked rubber, enabling better process control and product quality assurance by quantifying peroxide consumption, thus improving the analysis of crosslinking in rubber compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156267000003
    Figure 2024156267000003
  • Figure 2024156267000004
    Figure 2024156267000004
  • Figure 2024156267000005
    Figure 2024156267000005
Patent Text Reader

Abstract

To provide a method for analyzing a crosslinking degree of peroxide crosslinked rubber.SOLUTION: There is provided a method for analyzing a crosslinking degree of peroxide crosslinked rubber obtained from an uncrosslinked rubber composition containing a rubber component and a peroxide of a crosslinking agent. Thermogravimetry in a predetermined peroxide decomposition temperature range is performed for each of the uncrosslinked rubber composition, a complete crosslinked product thereof, and peroxide crosslinked rubber to be analyzed. On the basis of a result of thermogravimetry, a difference between a weight reduction ratio of the uncrosslinked rubber composition and the complete crosslinked product is used as a consumption amount of peroxide of the crosslinking agent which is consumed in obtaining a complete crosslinked product from the uncrosslinked rubber composition, and a difference between a weight reduction ratio of the uncrosslinked rubber composition and the peroxide crosslinked rubber is used as a consumption amount of the peroxide of the crosslinking agent which is consumed in obtaining the peroxide crosslinked rubber from the uncrosslinked rubber composition, and a crosslinking degree of the peroxide crosslinked rubber is calculated.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for analyzing the degree of crosslinking of a peroxide-crosslinked rubber. [Background technology]

[0002] It is known to use thermogravimetry to analyze crosslinked rubber. Patent Document 1 describes that in multilayered polymer particles having an inner layer of crosslinked rubber and an outer layer of thermoplastic resin, if the weight loss rate in thermogravimetry is 5% or less, it is possible to suppress poor appearance and mold staining that occurs during molding processing. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-130745 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a method for analyzing the degree of crosslinking of a peroxide-crosslinked rubber. [Means for solving the problem]

[0005] The present invention is a method for analyzing the degree of crosslinking of a peroxide-crosslinked rubber obtained from an uncrosslinked rubber composition containing a rubber component and a peroxide crosslinking agent, and comprises carrying out thermogravimetry on each of the uncrosslinked rubber composition, the completely crosslinked product of the uncrosslinked rubber composition, and the peroxide-crosslinked rubber to be analyzed, and from the results of the thermogravimetry, regarding the difference in weight reduction rate between the uncrosslinked rubber composition and the completely crosslinked product as the consumption of the peroxide crosslinking agent consumed when obtaining the completely crosslinked product from the uncrosslinked rubber composition, and regarding the difference in weight reduction rate between the uncrosslinked rubber composition and the peroxide-crosslinked rubber as the consumption of the peroxide crosslinking agent consumed when obtaining the peroxide-crosslinked rubber from the uncrosslinked rubber composition, thereby calculating the degree of crosslinking of the peroxide-crosslinked rubber. Effect of the Invention

[0006] According to the present invention, the degree of crosslinking of the peroxide-crosslinked rubber can be analyzed by using the results of thermogravimetry of the uncrosslinked rubber composition, the completely crosslinked product thereof, and the peroxide-crosslinked rubber to be analyzed. [Brief description of the drawings]

[0007] [Figure 1] 1 is a graph showing the relationship between temperature and weight retention in thermogravimetry for an uncrosslinked rubber composition A, a completely crosslinked product B, and a peroxide-crosslinked rubber X. [Figure 2A] 1 is a graph showing the relationship between time and weight retention in thermogravimetry for an uncrosslinked rubber composition A and a completely crosslinked product B. [Figure 2B] 1 is a graph showing the relationship between time and weight retention in thermogravimetry for an uncrosslinked rubber composition A and a peroxide-crosslinked rubber X. [Figure 3A] 1 is a graph showing the relationship between the degree of crosslinking and the 100% tensile stress of the completely crosslinked product B and the peroxide-crosslinked rubbers X1 to X5 calculated by the first analysis method. [Figure 3B] 1 is a graph showing the relationship between the degree of crosslinking and the 100% tensile stress of the completely crosslinked product B and the peroxide-crosslinked rubbers X1 to X5 calculated by the second analysis method. [Figure 4] 1 is a graph showing the relationship between the degree of crosslinking calculated by a first analysis method and the degree of crosslinking calculated by a second analysis method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The following describes the embodiments.

[0009] In the method for analyzing the crosslinking degree of peroxide-crosslinked rubber X according to the embodiment, the peroxide-crosslinked rubber X to be analyzed is a crosslinked rubber composition obtained from an uncrosslinked rubber composition A having a known formulation containing a rubber component and a peroxide crosslinking agent.

[0010] Examples of the peroxide crosslinkable rubber component in the uncrosslinked rubber composition A include natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), ethylene-propylene-diene copolymer rubber (EPDM), ethylene-propylene copolymer rubber (EPM), nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), chloroprene rubber (CR), chlorosulfonated polyethylene rubber (CSM), silicone rubber (Q), fluororubber (F), etc. The rubber component preferably contains one or more of these.

[0011] Examples of peroxides for the crosslinking agent include dialkyl peroxides such as dicumyl peroxide, 1,3-di(t-butylperoxy)diisopropylbenzene, 1,4-di(t-butylperoxy)diisopropylbenzene, t-butylcumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane-3; peroxyketals such as 1,1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, and n-butyl-4,4-di(t-butylperoxy)valerate; and peroxyesters such as 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-hexylperoxybenzoate, and t-butylperoxybenzoate. The peroxide preferably contains one or more of these. The amount of the peroxide mixed in the uncrosslinked rubber composition A is, for example, 0.5 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the rubber component.

[0012] The uncrosslinked rubber composition A may contain reinforcing agents such as carbon black, fillers, processing aids, antioxidants, plasticizers, vulcanization accelerators, vulcanization acceleration aids, and the like.

[0013] In the method for analyzing the degree of crosslinking of peroxide-crosslinked rubber X according to the embodiment, first, thermogravimetry is performed on each of the uncrosslinked rubber composition A, the completely crosslinked product B of the uncrosslinked rubber composition A, and the peroxide-crosslinked rubber X to be analyzed.

[0014] Here, the term "completely crosslinked product B" in the present application refers to a product obtained by crosslinking an uncrosslinked rubber composition A by heating it at a predetermined crosslinking temperature for a 100% crosslinking time tc(100) determined in accordance with JIS K6300-2:2001 using a Curastometer (registered trademark).

[0015] From the viewpoint of improving analytical accuracy, the thermogravimetric measurement of the completely crosslinked product B and the peroxide crosslinked rubber X is preferably carried out after the primary crosslinking in which heating is performed by press molding or the like and before the secondary crosslinking in which heating is performed in an oven or the like.

[0016] The thermogravimetric measurement is preferably carried out in an atmosphere in which an inert gas such as nitrogen flows. The flow rate of the inert gas is, for example, 300 ml / min to 1000 ml / min.

[0017] The heating rate in thermogravimetry is preferably 1°C / min or more from the viewpoint of avoiding long measurement times, and is preferably 10°C / min or less, more preferably 5°C / min or less, and even more preferably 2°C / min or less, from the viewpoint of tracking the temperature rise of the sample and improving measurement accuracy.

[0018] In the results of the thermogravimetry, the difference P in the weight retention rate between the uncrosslinked rubber composition A and the completely crosslinked product B at the temperature T shown in Fig. 1 corresponds to the difference in the weight loss rate between the uncrosslinked rubber composition A and the completely crosslinked product B, and therefore can be regarded as the consumption amount of the peroxide crosslinking agent consumed when the completely crosslinked product B is obtained by heating and crosslinking the uncrosslinked rubber composition A. Similarly, the difference Q in the weight retention rate between the uncrosslinked rubber composition A and the peroxide crosslinked rubber X at the temperature T shown in Fig. 1 corresponds to the difference in the weight loss rate between the uncrosslinked rubber composition A and the peroxide crosslinked rubber X, and therefore can be regarded as the consumption amount of the peroxide crosslinking agent consumed when the peroxide crosslinked rubber X is obtained by heating and crosslinking the uncrosslinked rubber composition A.

[0019] From the above, in the method for analyzing the degree of crosslinking of the peroxide crosslinked rubber X according to the embodiment, the difference P in the weight retention rate between the uncrosslinked rubber composition A and the completely crosslinked product B at temperature T, i.e., the difference in the weight loss rate, is regarded as the consumption amount of the peroxide crosslinking agent consumed when obtaining the completely crosslinked product B from the uncrosslinked rubber composition A, and the difference Q in the weight retention rate between the uncrosslinked rubber composition A and the peroxide crosslinked rubber X at temperature T, i.e., the difference in the weight loss rate, is regarded as the consumption amount of the peroxide crosslinking agent consumed when obtaining the peroxide crosslinked rubber X from the uncrosslinked rubber composition A, and the degree of crosslinking of the peroxide crosslinked rubber X is calculated based on the difference Q. Specific analysis methods include the following first and second analysis methods.

[0020] <First analysis method> In the first analysis method, as shown in Fig. 1, the difference P in the weight loss rate between the uncrosslinked rubber composition A and the completely crosslinked product B and the difference Q in the weight loss rate between the uncrosslinked rubber composition A and the peroxide crosslinked rubber X are obtained from the results of thermogravimetry at a predetermined analysis temperature T at which most of the peroxide in the crosslinking agent decomposes. Then, the ratio of the difference Q in the weight loss rate between the uncrosslinked rubber composition A and the peroxide crosslinked rubber X to the difference P in the weight loss rate between the uncrosslinked rubber composition A and the completely crosslinked product B is calculated as the crosslinking degree of the peroxide crosslinked rubber X.

[0021] The analysis temperature T is preferably 200° C. or higher and 250° C. or lower, more preferably 220° C., from the viewpoint of detecting the decomposition of as much peroxide as possible to increase the analytical accuracy while reducing the influence of high-temperature decomposition components other than peroxide on the weight loss. This analysis temperature T can be set by confirming the decomposition of peroxide from a DTG curve obtained by differential thermogravimetry (DTG) of the uncrosslinked rubber composition A.

[0022] This first analysis method is a simple method suitable for cases in which the uncrosslinked rubber composition A has a relatively simple compounding.

[0023] <Second analysis method> In the second analysis method, the difference P in the weight retention rate between the uncrosslinked rubber composition A and the completely crosslinked product B is integrated over time from the lower limit temperature Tmin to the upper limit temperature Tmax of a predetermined peroxide decomposition temperature range, and the peroxide consumption parameter S is calculated based on the results of the thermogravimetric analysis. I (=∫Pdt) is calculated. This peroxide consumption parameter S I is an index of the consumption amount of peroxide of the crosslinking agent consumed when obtaining a completely crosslinked product B from an uncrosslinked rubber composition A, and is the maximum value of the index.

[0024] As shown in FIG. 2B, the difference Q in the weight retention rate between the uncrosslinked rubber composition A and the peroxide-crosslinked rubber X is integrated over time from the lower limit temperature Tmin to the upper limit temperature Tmax of a predetermined peroxide decomposition temperature range to obtain a peroxide consumption parameter S II (=∫Qdt) is calculated. This peroxide consumption parameter S II is an index of the amount of peroxide consumed as a crosslinking agent when obtaining peroxide-crosslinked rubber X from an uncrosslinked rubber composition A.

[0025] and the peroxide consumption parameter S I Peroxide consumption parameter S II The ratio is calculated as the degree of crosslinking of the peroxide crosslinked rubber X.

[0026] Here, the peroxide decomposition temperature range is a temperature range for detecting weight loss mainly caused by the decomposition of the peroxide of the crosslinking agent by thermogravimetry (TGA). This peroxide decomposition temperature range can be set by confirming the decomposition of the peroxide from a DTG curve obtained by differential thermogravimetry (DTG) of the uncrosslinked rubber composition A.

[0027] The lower limit temperature Tmin of the peroxide decomposition temperature range is preferably set to a temperature of 80° C. or more and 120° C. or less, from the viewpoint of detecting the decomposition of as much peroxide as possible while minimizing the effect of dissipation of low-volatile components on weight loss, and more preferably set to 100° C., particularly from the viewpoint of eliminating the effect of dissipation of moisture on weight loss. The upper limit temperature Tmax of the peroxide decomposition temperature range is preferably set to a temperature of 200° C. or more and 250° C. or less, and more preferably set to 220° C., from the viewpoint of detecting the decomposition of as much peroxide as possible to increase analytical accuracy while minimizing the effect of high-temperature decomposition components other than peroxide on weight loss.

[0028] Peroxide consumption parameter S I ,S II is a tangible indication of the consumption amount of peroxide of the crosslinking agent consumed when obtaining a completely crosslinked product B or a peroxide-crosslinked rubber X from an uncrosslinked rubber composition A. Therefore, this second analytical method can also be used in cases where the uncrosslinked rubber composition A has a complicated blend containing a wide variety of components.

[0029] According to the above-mentioned method for analyzing the degree of crosslinking of peroxide-crosslinked rubber X, the degree of crosslinking of the peroxide-crosslinked rubber X can be analyzed by using the results of thermogravimetry of the uncrosslinked rubber composition A, the completely crosslinked product B thereof, and the peroxide-crosslinked rubber X to be analyzed. Moreover, since a minute amount of the sample of the peroxide-crosslinked rubber X is sufficient for the thermogravimetry, for example, if only a small part of a rubber product can be collected as a sample, the degree of crosslinking of the rubber product can be analyzed. Therefore, the method for analyzing the degree of crosslinking of the peroxide-crosslinked rubber X according to the embodiment can be used as a process inspection or product inspection to analyze the degree of crosslinking of the sample of the peroxide-crosslinked rubber X collected from a semi-finished product or a finished product, by carrying out the thermogravimetry of the uncrosslinked rubber composition A and the completely crosslinked product B thereof in advance and storing the results in a database. EXAMPLES

[0030] (Uncrosslinked rubber composition A and completely crosslinked product B) Hydrogenated nitrile rubber (HNBR) was used as the rubber component, and 2.4 parts by mass of 1,3-di(t-butylperoxy)diisopropylbenzene, which is a peroxide crosslinking agent, and 30 parts by mass of carbon black were blended and kneaded with 100 parts by mass of this rubber component to prepare an uncrosslinked rubber composition A.

[0031] The 100% crosslinking time tc(100) of this uncrosslinked rubber composition A was measured at 175°C using a Curastometer (registered trademark) in accordance with JIS K6300-2:2001, and was found to be 15 minutes. From this, the uncrosslinked rubber composition A was crosslinked at a crosslinking temperature of 175°C for a crosslinking time of 15 minutes to be a completely crosslinked product B.

[0032] (Peroxide cross-linked rubber X) The uncrosslinked rubber composition A was crosslinked at a crosslinking temperature of 175°C for a crosslinking time of 7 minutes to obtain a peroxide crosslinked rubber X1. The peroxide crosslinked rubbers X2 to X5 were the same as the peroxide crosslinked rubber X1 except that the crosslinking temperatures were 170°C, 165°C, 160°C, and 155°C.

[0033] (Thermogravimetric measurement) Thermogravimetry was carried out for each of the uncrosslinked rubber composition A, the completely crosslinked product B, and the peroxide crosslinked rubbers X1 to X5. The thermogravimetry was carried out under the following temperature history: the chamber in which the sample was placed was circulated with nitrogen at a flow rate of 500 ml / min, the temperature was raised from 30°C to 50°C at a heating rate of 10°C / min, the temperature was held for 5 minutes, the temperature was then raised from 50°C to 80°C at a heating rate of 10°C / min, and the temperature was then raised from 80°C to 220°C at a heating rate of 2°C / min.

[0034] (Degree of cross-linking) <First analysis method> For each of the peroxide-crosslinked rubbers X1 to X5, the degree of crosslinking was calculated by the first analysis method of the above embodiment at an analysis temperature T of 220° C. The results are shown in Table 1.

[0035] [Table 1]

[0036] <Second analysis method> For each of the peroxide-crosslinked rubbers X1 to X5, the degree of crosslinking was calculated by the second analysis method of the above embodiment, with the peroxide decomposition temperature range being set to a lower limit temperature Tmin of 100° C. and an upper limit temperature Tmax of 220° C. The results are shown in Table 2.

[0037] [Table 2]

[0038] (Tensile stress at 100% elongation) The tensile stress at 100% elongation was measured for each of the completely crosslinked product B and the peroxide crosslinked rubbers X1 to X5 based on JIS K6251: 2010. It can be said that the tensile stress at 100% elongation is a physical property that reflects the actual degree of crosslinking of the completely crosslinked product B and the peroxide crosslinked rubbers X1 to X5.

[0039] Fig. 3A shows the relationship between the degree of crosslinking of the completely crosslinked product B and the peroxide crosslinked rubbers X1 to X5 calculated by the first analysis method and the 100% tensile stress. Fig. 3B shows the relationship between the degree of crosslinking of the completely crosslinked product B and the peroxide crosslinked rubbers X1 to X5 calculated by the second analysis method and the 100% tensile stress. Fig. 4 shows the relationship between the degree of crosslinking calculated by the first analysis method and the degree of crosslinking calculated by the second analysis method.

[0040] 3A and 3B show that the degree of crosslinking calculated by both the first and second analytical methods has a strong correlation with the tensile stress at 100% elongation, and FIG 4 shows that there is no significant difference between the degree of crosslinking calculated by both the first and second analytical methods. [Industrial Applicability]

[0041] The present invention is useful in the technical field of a method for analyzing the degree of crosslinking of peroxide-crosslinked rubber.

Claims

1. A method for analyzing a crosslinking degree of a peroxide-crosslinked rubber obtained from an uncrosslinked rubber composition containing a rubber component and a peroxide crosslinking agent, comprising the steps of: Thermogravimetry is performed on each of the uncrosslinked rubber composition, the completely crosslinked product of the uncrosslinked rubber composition, and the peroxide-crosslinked rubber to be analyzed; A method for analyzing the degree of crosslinking of a peroxide-crosslinked rubber, in which the difference in the weight loss rate between the uncrosslinked rubber composition and the completely crosslinked product from the results of the thermogravimetry is regarded as the consumption amount of peroxide of the crosslinking agent consumed when obtaining the completely crosslinked product from the uncrosslinked rubber composition, and the difference in the weight loss rate between the uncrosslinked rubber composition and the peroxide-crosslinked rubber is regarded as the consumption amount of peroxide of the crosslinking agent consumed when obtaining the peroxide-crosslinked rubber from the uncrosslinked rubber composition, and the degree of crosslinking of the peroxide-crosslinked rubber is calculated.

2. The method for analyzing a crosslinking degree according to claim 1, A crosslinking degree analysis method in which a ratio of the difference in weight loss rate between the uncrosslinked rubber composition and the peroxide-crosslinked rubber to the difference in weight loss rate between the uncrosslinked rubber composition and the completely crosslinked product at a specified analysis temperature is calculated from the results of the thermogravimetry as the crosslinking degree of the peroxide-crosslinked rubber.

3. The method for analyzing the degree of crosslinking according to claim 2, The method for analyzing a degree of crosslinking, wherein the analysis temperature is 200° C. or higher and 250° C. or lower.

4. The method for analyzing a crosslinking degree according to claim 1, A crosslinking degree analysis method, which calculates the degree of crosslinking of the peroxide-crosslinked rubber from the results of the thermogravimetry by calculating a ratio of a peroxide consumption parameter obtained by time-integrating the difference in the weight loss rates of the uncrosslinked rubber composition and the completely crosslinked product in a specified peroxide decomposition temperature range to a peroxide consumption parameter obtained by time-integrating the difference in the weight loss rates of the uncrosslinked rubber composition and the peroxide-crosslinked rubber.

5. The method for analyzing a crosslinking degree according to claim 4, The method for analyzing a degree of crosslinking, wherein the lower limit temperature of the peroxide decomposition temperature range is 100°C.

6. The method for analyzing the degree of crosslinking according to claim 4 or 5, The method for analyzing a degree of crosslinking, wherein the upper limit temperature of the peroxide decomposition temperature range is a temperature of 200° C. or higher and 250° C. or lower.

Citation Information

Patent Citations

  • Method for crosslinking power cable semiconductive layer

    JP1992311729A

  • Production of elastomer composition

    JP2000103909A

  • Photosensitive siloxane composition, cured film formed from the same and element having cured film

    JP2008020898A

  • Method for accelerating curing of mixture and method for accelerating curing of adhesive composition

    JP2008156513A

  • Resin composition for solar cell sealing material, solar cell sealing material arranged by use thereof, and solar battery module

    JP2015211189A