Method for specifying composition and structure of crystal grain of compound of rubber and metal

The method accurately determines the composition and structure of crystal grains at the rubber-metal interface using a scanning transmission electron microscope and Fourier transform, enhancing adhesion properties.

JP2024156329APending Publication Date: 2024-11-06THE YOKOHAMA RUBBER CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023070701
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-06

AI Technical Summary

Technical Problem

Existing methods cannot accurately identify the composition and structure of crystal grains at the adhesive interface between vulcanized rubber and metal, which affects the adhesion properties.

Method used

A method using a scanning transmission electron microscope to obtain image data, applying fast Fourier transform to diffraction patterns, and calculating distances and angles to determine the composition and structure of crystal grains through a combination of interplanar spacing and plane angles.

Benefits of technology

Enables precise identification of crystal grain composition and structure, enhancing the understanding of adhesion mechanisms and improving adhesive properties between rubber and metal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156329000001_ABST
    Figure 2024156329000001_ABST
Patent Text Reader

Abstract

To provide a method for specifying a composition and structure of a crystal grain of a compound of a rubber and a metal capable of precisely specifying the composition and structure of the crystal grain of the compound formed on a boundary between the vulcanized rubber and the metal.SOLUTION: Image data 20 of a specimen 10 is acquired by a scanning type transmission electron microscope 2, and a region selected from the acquired image data 20 is subjected to a fast Fourier transform by a computing device 3 to acquire diffraction pattern data (24-26). Distances (L1-L4) from the center O of each diffraction spot to each of object spots (A-D) and intersection angles (θ1-θ3) formed by line segments connecting the center O and each of the object spots (A-D) are calculated. The combination of each calculated distance and intersection angle is used to specify a composition and structure of crystal grains.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for identifying the composition and structure of crystal grains of a compound of rubber and metal, and more particularly to a method for identifying the composition and structure of crystal grains of a compound formed at the boundary between vulcanized rubber and metal with high accuracy. [Background technology]

[0002] Rubber products such as tires use metal materials such as steel cords. During the vulcanization process of rubber products, sulfur in unvulcanized rubber reacts with brass in brass-plated steel cords, and the vulcanized rubber and metal are bonded together by an adhesive interface layer formed at the boundary between them. In order to improve the adhesion between rubber and brass, it has been proposed to form a needle-shaped Cu-S-based reaction product at the adhesive interface between the brass and rubber (see Patent Document 1).

[0003] It is believed that the mechanism of adhesion by this adhesive interface layer is influenced by the composition and structure of the crystal grains of the metal compound derived from the brass that constitutes the adhesive interface layer. Therefore, if the composition and structure of this metal compound can be clearly identified, it is expected to contribute in various ways, such as elucidating the formation process of the metal compound during the vulcanization process and improving adhesion. Although the image data of the adhesive interface layer obtained by a scanning electron microscope can identify the approximate distribution of the metal elements, it cannot identify the composition and structure of the crystal grains of the metal compound. Therefore, various ingenuity is required to accurately identify the composition and structure of the crystal grains of the metal compound formed at the boundary between the vulcanized rubber and the metal. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-263336 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a method for accurately identifying the composition and structure of crystal grains of a metal compound formed at the boundary between vulcanized rubber and a metal. [Means for solving the problem]

[0006] The present invention, which achieves the above object, provides a method for identifying the composition and structure of crystal grains of a rubber-metal compound, which involves obtaining image data of a thin specimen including an adhesive interface layer formed at the boundary between vulcanized rubber and metal using a scanning transmission electron microscope, and using the image data to identify the composition and structure of crystal grains of a metal compound derived from the metal present in the adhesive interface layer. The method is characterized in that a region selected from the image data is fast Fourier transformed by a computing device to obtain diffraction pattern data showing the structure of the crystal grains, and a plurality of diffraction spots that are asymmetrical to each other and selected from a large number of diffraction spots present in the obtained diffraction pattern data are used as target spots, and the distance from the center of each of the diffraction spots to each of the target spots and the intersection angle between the line segments connecting the center and each of the target spots are calculated, and the composition and structure of the crystal grains are identified using a combination of the calculated distances and the calculated intersection angles. Effect of the Invention

[0007] According to the present invention, the combination of each of the distances and each of the crossing angles calculated based on the diffraction pattern data can be regarded as the interplanar spacing of a plurality of crystal lattice planes having different plane orientations in the crystal grains and the interplanar angles between the respective crystal lattice planes. Since each interplanar spacing and interplanar angle is a unique value between crystal grains having the same composition and structure, the composition and structure of the crystal grains of the actual metal compound present in the adhesive interface layer at the boundary between the vulcanized rubber and the metal can be accurately identified by using the combination. [Brief description of the drawings]

[0008] [Figure 1]FIG. 1 is an explanatory diagram illustrating an observation system. [Diagram 2] FIG. 1 is an explanatory diagram illustrating a scanning transmission electron microscope. [Diagram 3] FIG. 1 is a flow diagram illustrating the steps of an embodiment of a method for identifying the composition and structure of grains of a rubber-metal compound. [Figure 4] FIG. 2 is an explanatory diagram illustrating an example of image data. [Diagram 5] 5 is an enlarged view showing an example of regional image data obtained by enlarging a portion of FIG. 4; FIG. [Figure 6] 5 is an enlarged view showing an example of regional image data obtained by enlarging a portion of FIG. 4; FIG. [Figure 7] 5 is an enlarged view showing an example of regional image data obtained by enlarging a portion of FIG. 4; FIG. [Figure 8] FIG. 6 is an explanatory diagram illustrating diffraction pattern data for the region in FIG. 5. [Figure 9] FIG. 7 is an explanatory diagram illustrating diffraction pattern data for the region of FIG. 6. [Figure 10] FIG. 8 is an explanatory diagram illustrating diffraction pattern data for the region of FIG. 7. [Figure 11] FIG. 10 is an explanatory diagram showing a schematic representation of the diffraction pattern data of FIG. [Figure 12] FIG. 2 is an explanatory diagram illustrating a part of a database. [Figure 13] FIG. 2 is an explanatory diagram illustrating a part of a database. [Figure 14] FIG. 1 is an explanatory diagram illustrating image data; [Figure 15] FIG. 11 is a flow diagram illustrating a procedure of the first modified example. [Figure 16] 6 is an explanatory diagram illustrating model data of crystal grains present in the region of FIG. 5. [Figure 17] FIG. 7 is an explanatory diagram illustrating model data of crystal grains present in the region of FIG. 6. [Figure 18] FIG. 8 is an explanatory diagram illustrating model data of crystal grains present in the region of FIG. 7. [Figure 19] 6 is an explanatory diagram illustrating comparison data for the regional image data of FIG. 5; [Figure 20] 7 is an explanatory diagram illustrating comparison data for the regional image data of FIG. 6; [Figure 21] 8 is an explanatory diagram illustrating comparison data for the regional image data of FIG. 7; [Figure 22] FIG. 11 is a flow diagram illustrating a procedure of Modification Example 2. [Figure 23] 6 is an explanatory diagram illustrating comparison data for the regional image data of FIG. 5; [Figure 24] 7 is an explanatory diagram illustrating comparison data for the regional image data of FIG. 6; [Diagram 25] 8 is an explanatory diagram illustrating comparison data for the regional image data of FIG. 7; [Figure 26] FIG. 1 is an explanatory diagram illustrating a crystal plane database. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the method for identifying the composition and structure of crystal grains of a rubber-metal compound of the present invention will be described based on the embodiment shown in the drawings.

[0010] The observation system 1 illustrated in Fig. 1 is used to carry out the identification method of the present invention. In this identification method, first, a scanning transmission electron microscope 2 (hereinafter referred to as microscope 2) is used to acquire image data 20 illustrated in Fig. 4, which will be described later, using a thin specimen 10. Next, the composition and structure of the crystal grains of the metal compound present in the adhesive interface layer of the specimen 10 are identified by a computing device 3 using the acquired image data 20.

[0011] First, the observation system 1 will be described.

[0012] The observation system 1 includes a microscope 2 and a computing device 3. Various data are input and stored in the computing device 3, which processes the data using the input data. The computing device 3 may be any of various known computers. The computing device 3 includes a central processing unit (CPU), a main storage unit (memory), an auxiliary storage unit (e.g., HDD), an input unit (keyboard, mouse), and an output unit (display).

[0013] 2 irradiates an electron beam onto a specimen 10, and acquires image data such as dark-field image (HAADF-STEM image, LAADF-STEM image) data and bright-field image (BF-STEM image) data, which enable observation of the spatial distribution of electron transmittance inside the specimen 10 from the intensity of the transmitted electron beam. In addition to acquiring this image data, the microscope 2 also acquires element mapping data, which enables observation of the distribution of elements present in the image data. The image data 20 generated by the computing device 3 by superimposing (combining) either the dark-field image data or the bright-field image data acquired by the microscope 2 with the element mapping data is stored in the auxiliary storage unit of the computing device 3.

[0014] The microscope 2 may be any of various known scanning transmission electron microscopes, but is preferably one incorporating a spherical aberration corrector 6. Specifically, the microscope 2 has an electron gun 4, a condenser lens 5, a spherical aberration corrector (concave lens) 6, an objective lens (convex lens) 7, and various detectors. The detectors include a DF (dark field) detector 8a, a BF (bright field) detector 8b, an EDS (energy dispersive X-ray spectroscopy) detector 9a, and an EELS (electron energy loss spectroscopy) detector 9b. The microscope 2 having the spherical aberration corrector 6 can achieve a smaller resolution, which is advantageous for identifying structures at the single-atom level and improving the accuracy of identifying elements.

[0015] As the detector, it is sufficient to have either the DF detector 8a or the BF detector 8b, and either the EDS detector 9a or the EELS detector 9b, and it is not necessary to have all the detectors. However, if all the detectors are included, multiple types of data can be obtained, and analysis can be performed from multiple angles.

[0016] The DF detector 8a has a circular ring shape in a top view and detects electrons scattered at a high angle. The acceptance angle of the DF detector 8a (the scattering angle of detectable electrons) is, for example, more than 20 mrad and not more than 200 mrad. The DF detector 8a can also be composed of two circular ring-shaped detectors, one large and one small, in which case the larger diameter detector is placed above the smaller diameter detector. The acceptance angle of the larger diameter detector placed at the top is, for example, more than 90 mrad and not more than 200 mrad, and the acceptance angle of the smaller diameter detector placed at the bottom is, for example, more than 20 mrad and not more than 90 mrad.

[0017] The BF detector 8b has a circular ring shape in a top view, and detects electrons that have passed through the specimen 10 and electrons that have been scattered at small angles. The acceptance angle of the BF detector 8b is, for example, 20 mrad or less. The BF detector 8b can also be configured with two circular ring-shaped detectors, one large and one small, in which case the acceptance angle of the larger diameter detector is, for example, more than 10 mrad and 20 mrad or less, and the acceptance angle of the smaller diameter detector is, for example, 10 mrad or less.

[0018] The EDS detector 9a and the EELS detector 9b analyze the distribution of elements in the specimen 10 by utilizing the inelastic scattering process of electrons accompanying the excitation of inner-shell electrons of atoms caused by irradiation with an electron beam. The EDS detector 9a analyzes the spectrum of characteristic X-rays generated from atoms present in the specimen 10 by irradiation with an electron beam. The EELS detector 9b analyzes the spectrum of energy lost due to the interaction between the electron beam and atoms present in the specimen 10.

[0019] Next, the specimen 10 will be described.

[0020] The specimen 10 is a metal-rubber composite material produced by vulcanizing unvulcanized rubber containing a metal. The metal preferably contains at least one of copper and zinc, and may contain both copper and zinc. Examples of this metal include brass or brass-plated metal plates and wires, and brass powder. Since a magnetic metal deflects the electron beam of the microscope 2, making high-resolution observation difficult, it is preferable that the metal is not magnetic.

[0021] Unvulcanized rubber may be any rubber component (polymer) that can be crosslinked by a crosslinking agent containing sulfur, such as natural rubber (NR) or synthetic rubbers such as styrene-butadiene rubber (SBR), butadiene rubber (BR), and isoprene rubber (IR). The crosslinking agent may contain at least sulfur, and may be used in combination with an organic peroxide such as peroxide. Unvulcanized rubber may contain additives other than the crosslinking agent, such as crosslinking accelerators (vulcanization accelerators), fillers (silica, carbon black, etc.), antioxidants, flame retardants, reinforcing materials, and colorants.

[0022] The degree of vulcanization of the specimen 10 is not particularly limited as long as an adhesive interface layer is formed at the boundary between the metal and the vulcanized rubber. In the adhesive interface layer, crystal grains of metal compounds (metal sulfides) derived from the surrounding metals are present.

[0023] The specimen 10 is a thin piece whose thickness falls within a preset thickness standard range. In the method for producing the specimen 10, first, the metal-rubber composite material is sliced ​​so as to cross the adhesive interface layer formed inside the metal-rubber composite material. Next, the sliced ​​thin section of the metal-rubber composite material is polished to expose the adhesive interface layer more and to have a thickness within a preset thickness standard range. For slicing, for example, a known ultramicrotome is used. For polishing, for example, a known mechanical polishing method or ion milling method is used. For polishing the thin section of the metal-rubber composite material, it is preferable to use both the mechanical polishing method and the ion milling method, and it is preferable to polish the thin section by the mechanical polishing method and then by the ion milling method. The thickness standard range is set so that the clarity of the crystal grains of the metal compound present in the adhesive interface layer in the image data 20 illustrated in FIG. 4 described later is within an acceptable range.

[0024] The clarity of the crystal grains in the image data 20 is the degree of clarity of the atoms that affects the visibility of the crystal grain structure (suitability for observation). In order to specify the structure of the crystal grains, a region in the image data 20 where the crystal grains of the metal compound can be clearly observed is required. In the image data 20 acquired by the microscope 2, the metals and metal compounds are expressed by contrast (difference in light and dark) that indicates the difference in the atoms that compose them. In the image data 20, if the density of each atom is high, the contrast due to the atoms becomes less clear, and if the density of the atoms is low, the contrast becomes clearer. In the image data 20, the greater the thickness of the specimen 10, the higher the density of each atom. Therefore, the greater the thickness of the specimen 10, the lower the clarity of the atoms in the image data 20, making it unsuitable for observing the crystal grains of the metal compound. On the other hand, the thinner the thickness of the specimen 10, the higher the clarity of the atoms in the image data 20, making it suitable for observation. The thickness reference range is appropriately set based on the results of many tests, and is set so as to exclude images that cause the contrast in the image data 20 to become unclear. Therefore, when this degree of clarity is within an acceptable range, the density of each atom is appropriately low, and the contrast in the image data 20 is clear.

[0025] The optimal thickness standard range varies slightly depending on the type of metal and unvulcanized rubber that make up the metal-rubber composite material, but considering the test results, the following range is considered to be effective for most types of metal-rubber composite materials. Therefore, the thickness standard range should be 1 nm or more and 100 nm or less, but 1 nm or more and 50 nm or less is preferable, and 1 nm or more and 20 nm or less is more preferable.

[0026] Next, the method of specification will be described.

[0027] FIG. 3 shows an example of the procedure of an embodiment of the identification method. In this identification method, the above-mentioned specimen 10 is used. For example, the metal-rubber composite material used for the specimen 10 is a brass plate having a thickness of 10 μm to 100 μm, which is sandwiched between unvulcanized rubber containing sulfur as a crosslinking agent and then vulcanized. The thickness of the specimen 10 may be 1 nm to 50 nm, which is considered to be effective for most types of metal-rubber composite materials. That is, in this identification method, the metal-rubber composite material is sliced ​​to a thickness of 1 nm to 50 nm, polished, and used as the specimen 10 including an adhesive interface layer between the metal and the vulcanized rubber.

[0028] First, image data 20 of the specimen 10 is acquired using the microscope 2 (S110). Next, a region in which crystal grains of a desired metal compound are present is selected from the acquired image data 20, and diffraction pattern data of that region (diffraction pattern data 24-26 illustrated in Figs. 8-10 described later) is acquired using the microscope 2 (S120, S130). Next, a predetermined program is executed, and each data processing is performed by the arithmetic unit 3 (S140, S150). The contents of each step (S110-S150) are described in detail below.

[0029] In step (S110), the specimen 10 is set on the microscope 2, and image data 20 of the specimen 10 is acquired by the microscope 2. The image data 20 is created by superimposing (combining) the dark-field image data or the bright-field image data with the element mapping data. With only one of the image data, the dark-field image data or the bright-field image data, it may be possible to identify the region in which the desired crystal grains of the metal compound exist from the shape of the adhesive interface layer and the position of the crystal grains in the adhesive interface layer shown in the image data. On the other hand, by acquiring the image data 20 in which the element mapping data is superimposed on the image data, the distribution of elements in the image data 20 can be grasped in more detail. Therefore, even if a new metal-rubber composite material in which the combination of metal and unvulcanized rubber is not already known is used as a sample, the region in which the crystal grains of the metal compound exist can be identified. To create the element mapping data, it is sufficient to use either the EDS detector 9a or the EELS detector 9b, but to identify the composition and structure of the crystal grains of the metal compound, it is preferable to use the EDS detector 9a, which is suitable for analyzing heavy elements.

[0030] In step (S120), a region in which crystal grains of a desired metal compound exist is selected from the image data 20. The region in which the desired crystal grains exist is selected by utilizing the distribution of elements in the element mapping data.

[0031] The image data 20 shown in Fig. 4 is created by superimposing dark-field image data (HAADF-STEM image: high-angle scattering annular dark-field image) detected by the DF detector 8a and element mapping data detected by the EDS detector 9a. In each image data 20, the white parts represent metals and metal compounds, and the black parts represent vulcanized rubber. The area near the boundary where the white and black parts in the image data 20 are adjacent is the adhesive interface layer.

[0032] Although not shown in FIG. 4, in the actual image data 20, the element mapping data is color-coded for each of a plurality of elements, and the distribution of metal compounds in the adhesive interface layer can be understood from the distribution of elements shown in the element mapping data. The element mapping data shows the distribution of four elements, for example, Cu, Zn, S, and O. Therefore, in the adhesive interface layer shown in FIG. 4, the metal compounds are mainly Cu, in the order from the vulcanized rubber on the top to the metal on the bottom. x S(Cu 1.75 The layer where the ZnS or CuS exists, the layer where the ZnO exists, and the layer where the ZnO exists can be identified. The element mapping data may further show the distribution of carbon element C, which is a main component of vulcanized rubber, in order to understand the adhesive interface layer in more detail.

[0033] 4, three regions (21 to 23) are selected as regions in which desired crystal grains exist. Hereinafter, the image data 20 indicating the regions 21, 22, 23 will be referred to as region image data 21, 22, 23, respectively.

[0034] In each of the area image data 21, 22, and 23 shown in Fig. 5, Fig. 6, and Fig. 7, a pattern like dots or lines appears in the white parts, and it can be seen that the distribution of elements is visualized by the element mapping data. In the actual area image data 21, 22, and 23, it can be confirmed from the element mapping data that Cu and S are distributed in large amounts. Therefore, it is believed that the metal compounds present in each area are Cu. x S. However, Cu x The composition of S ( x However, it has not yet been possible to determine the value of

[0035] In step (S130), the selected regions 21, 22, 23 are subjected to a fast Fourier transform (FFT) by the arithmetic unit 3, and data processing is executed to obtain diffraction pattern data (24, 25, 26) showing the structure of the crystal grains as exemplified in Figs. 8, 9, and 10. Since the imaging system using the lenses of the microscope 2 can be treated as Fraunhofer diffraction, the series of processes from the scattered waves by the specimen 10 to the acquisition of the image data 20 can be said to be a repetition of Fourier transform and inverse Fourier transform. Thus, by processing the data using the fast Fourier transform, diffraction pattern data (24 to 26) is obtained in which the periodicity of each crystal lattice plane of the crystal grains appears as a diffraction spot at the position of the spatial frequency corresponding to the period and direction (periodic arrangement) of the crystal grain structure.

[0036] In the diffraction pattern data 24, 25, and 26 shown in Figures 8, 9, and 10, the diffraction spots appear as white dots. The three-digit numbers such as (011) (some of which are marked with an overscore " ̄") around the diffraction spots in Figures 8 to 10 indicate the Miller indices of the respective crystal lattice planes.

[0037] In step (S140), the arithmetic unit 3 executes data processing to calculate the distances (L1 to L4) from the center O of each diffraction spot to each target spot (A to D) and the intersection angles (θ1 to θ3) between the line segments connecting the center O and each target spot (A to D) shown in FIG. 11 described later. Among the many diffraction spots present in the diffraction pattern data (24 to 26), there are diffraction spots that are line-symmetric to each other due to the translational symmetry of the crystal grain structure. Since the diffraction spots that are line-symmetric to each other have the same characteristics in the periodicity of the crystal lattice plane, diffraction spots with the same characteristics are not selected as the target spots. Therefore, a plurality of diffraction spots that are asymmetric to each other are selected as the target spots. The number of target spots is not particularly limited as long as it is two or more, but it is preferable to select all diffraction spots that are asymmetric to each other from the many diffraction spots as the target spots.

[0038] FIG. 11 is a schematic diagram of the diffraction pattern data 25 shown in FIG. 9. In FIG. 11, white circles indicate diffraction spots. There are eight diffraction spots in the diffraction pattern data 25, and four of the eight diffraction spots are asymmetrical to each other. The center O is the center of the eight diffraction spots. The target spots A to D are asymmetrical to each other. The respective distances L1 to L4 are the distances from the center O to the respective target spots A to D. The respective intersection angles θ1 to θ3 are the angles between the line segments connecting the center O to the respective target spots A to D. For example, the intersection angle θ1 is "the angle between the line segment connecting the center O to the target spot A and the line segment connecting the center O to the target spot B." Other crossing angles besides the crossing angles θ1 to θ3 include "the angle between the line segment connecting the center O and the target spot A and the line segment connecting the center O and the target spot D" and "the angle between the line segment connecting the center O and the target spot A and the line segment connecting the center O and the target spot C." These other crossing angles can be calculated using the crossing angles (θ1 to θ3) described above. Therefore, in step (S130), it is sufficient to calculate the crossing angle between adjacent line segments in the circumferential direction around the center O.

[0039] In step (S150), the composition and structure of the crystal grains of the metal compound present in the adhesive interface layer are identified using combinations of the calculated distances (L1 to L4) and the crossing angles (θ1 to θ3). The combinations of the distances (L1 to L4) and the crossing angles (θ1 to θ3) can be regarded as the interplanar spacing of a plurality of crystal lattice planes of the crystal grains having different plane orientations and the interplanar angles between the crystal lattice planes. The interplanar spacing and the interplanar angle are unique values ​​between crystal grains of the same composition and crystal structure. Therefore, it is possible to identify the composition and crystal structure of the crystal grains (type of crystal system or Brapais lattice) based on the combination. By identifying the composition and crystal structure of the crystal grains, the three-dimensional arrangement of atoms in the crystal grains can be grasped. In this way, the combinations of the distances (L1 to L4) and the crossing angles (θ1 to θ3) can be used as indicators for identifying the composition and structure of the crystal grains.

[0040] Specifically, to identify the composition and crystal structure of the crystal grains, the calculation device 3 selects the relevant crystal grains of a known metal compound from the database D1 based on a combination of each distance (L1-L4) and each crossing angle (θ1-θ3), and executes data processing to identify the composition of the selected crystal grains of the known metal compound as the composition of the crystal grain to be observed. The database D1 is desirably stored in advance in the auxiliary storage unit of the calculation device 3, but may also be stored in the auxiliary storage unit of a computer external to the calculation device 3, such as a data server.

[0041] In a part of the database D1 shown in Figs. 12 and 13, the plane spacings and plane angles of the crystal grains of Cu2S are accumulated. In the actual database D1, the compositions of crystal grains of many kinds of known metal compounds including the crystal grains of Cu2S shown as an example, the plane spacings of a plurality of crystal lattice planes having different plane orientations, and the plane angles between the respective crystal lattice planes are accumulated. The crystal grains of known metal compounds include, for example, CuS, Cu 1.96 S, Cu 1.94 S, Cu 1.75 S, Cu 1.80 The database D1 is made up of crystal grains of S, Cu2S, ZnS, ZnO, etc., and is prepared by utilizing various known documents and databases available via the Internet. In known documents and databases, the plane spacing and Miller indices of the crystal lattice planes are disclosed, but the plane angles between the respective crystal lattice planes are often not disclosed. Therefore, the respective plane angles in the database D1 are calculated using the Miller indices of the respective crystal lattice planes that are disclosed. The database D1 may include the crystal system of the crystal grains that exhibit the crystal structure and the type of Brappais lattice.

[0042] In step (S150), the calculation device 3 regards the calculated combination as the interplanar spacing and interplanar angle of each crystal grain, and selects from the database D1 crystal grains of a known metal compound whose interplanar spacing and interplanar angle are similar to the calculated combination. To determine whether or not they are similar, the calculated combination may be compared with the interplanar spacing and interplanar angle in the database D1 to determine whether or not they are within a set allowable range. The allowable range may be set arbitrarily, and may be, for example, a range of about ±5% of the interplanar spacing and interplanar angle values ​​in the database D1. In addition, to determine whether or not they are similar, the ratio of each distance and the ratio of each intersection angle in the calculated combination may be compared with the ratio of each interplanar spacing and the ratio of each interplanar angle in the database D1.

[0043] By data processing using the database D1, the crystal grains shown in the diffraction pattern data 24 of FIG. 8 are identified as having a composition of Cu2S. Similarly, the crystal grains shown in the diffraction pattern data 25 of FIG. 9 are identified as having a composition of Cu 1.75 S, and the crystal grains shown in the diffraction pattern data 26 of Fig. 10 are identified as having a composition of CuS. If each crystal grain whose composition has been identified is not a polymorph, the crystal system and type of Bragg lattice are also identified along with the composition identification. In this way, by comparing each calculated combination of distance and crossing angle with the database D1, the composition and crystal structure of the crystal grains to be observed can be identified.

[0044] As described above, according to this embodiment, the combination of each calculated distance (L1 to L4) and each crossing angle (θ1 to θ3) can be regarded as the interplanar spacing of each of a plurality of crystal lattice planes having different plane orientations in the crystal grain and the interplanar angle between each of the crystal lattice planes. In other words, by using the combination as an index, the composition and crystal structure of the crystal grain observed in the image data 20 can be identified. Thus, according to this embodiment, the composition and structure of the crystal grain of the actual metal compound present in the adhesive interface layer at the boundary between the vulcanized rubber and the metal can be accurately identified.

[0045] The image data 20 illustrated in FIG. 14 shows the distribution of crystal grains identified by the above-mentioned identification method using the same specimen 10 as in the embodiment. In the image data 20 in FIG. 14, the area surrounded by a white line shows the distribution of CuS crystal grains, and the area surrounded by a black line shows the distribution of Cu2S crystal grains. 1.75 The crystal grains of S are not shown because their abundance is small compared to Cu2S and CuS. Three crystalline solids of Cu2S (aggregates of many crystal grains) and eight crystalline solids of CuS can be confirmed in Fig. 14.

[0046] In Figure 14, it can be seen that crystalline solids of Cu2S and CuS are formed on the vulcanized rubber side of the adhesive interface layer. The vulcanized rubber side of the adhesive interface layer has a higher sulfur content than the metal side. Therefore, it can be inferred that crystalline solids of Cu2S and CuS, which have a higher sulfur composition ratio, are formed in large amounts on the vulcanized rubber side of the adhesive interface layer.

[0047] When the shapes of the crystalline solids of Cu2S and CuS in the image data 20 are approximated to an ellipse, the aspect ratio of the long axis and the short axis of the approximated ellipse in the crystalline solid of Cu2S is 1.6±0.6, and the shape of the crystalline solid of Cu2S is approximated to a sphere. Since the surface density of S atoms is similar in each crystal face of the crystalline solid of Cu2S, the interfacial energy between each crystal face and the vulcanized rubber is roughly the same. Therefore, it can be inferred that the growth rate is similar in each crystal face and that the shape of the crystalline solid of Cu2S is isotropic. The aspect ratio of the crystalline solid of CuS is 2.6±0.9, and the shape of the crystalline solid of CuS is approximated to an elongated shape. Since the surface density of S atoms is significantly different in each crystal face of the crystalline solid of CuS, the interfacial energy between each crystal face and the vulcanized rubber is also different. Therefore, it can be inferred that the growth rate is different in each crystal face and that the shape of the crystalline solid of CuS is anisotropic.

[0048] The higher the surface density of the crystal planes, and the larger the area of ​​the crystal planes in contact with the vulcanized rubber, the more covalent bonds with the vulcanized rubber will be formed. Therefore, it can be inferred that the crystalline solids of CuS, which have anisotropic shapes and penetrate deeper into the vulcanized rubber, have a large contact area with the vulcanized rubber, and therefore have a high affinity with the vulcanized rubber. It can be inferred that the crystalline solids of Cu2S, which have a higher surface density of crystal planes than the crystalline solids of CuS, have a small contact area with the vulcanized rubber, but have a high affinity with the vulcanized rubber due to their high surface density. In this way, the distribution and shape of the crystalline solids of the metal compound present in the adhesive interface layer are important factors in elucidating the mechanism of adhesion at the adhesive interface layer. Therefore, according to this embodiment, the distribution and shape of the crystalline solids of the metal compound can be accurately grasped along with the identification of the composition and structure of the crystal grains of the metal compound, which greatly contributes to elucidating the mechanism of adhesion at the adhesive interface layer.

[0049] Next, a first modified example of the embodiment of the identification method shown in FIG. 15 will be described.

[0050] In the first modification, steps S160 and S170 are added to the procedure of FIG. 3 described above. That is, in the procedure of the first modification, after the composition and structure of the crystal grains are specified (S150), the calculation device 3 checks whether the specified composition and structure of the crystal grains are correct (S160, S170). Therefore, in the first modification, errors caused by measurement errors and the like are corrected. Also, in the process of checking the correctness, in addition to the composition and crystal structure of the crystal grains to be observed, the direction of the crystal axis is specified, and the three-dimensional arrangement of atoms of the crystal grains of the metal compound in the image data 20 is grasped. Note that the image data 20 of the first modification uses image data of either the dark-field image data or the bright-field image data superimposed (combined) with element mapping data.

[0051] In step (S160), the calculation device 3 executes data processing to create model data (model data 27, 28, 29 shown in Figs. 16, 17, 18 to be described later) that models the identified crystal grains based on their composition and structure. For modeling the crystal grains, various known drawing software capable of creating model data from the composition and crystal structure of the crystal grains can be used. This drawing software is preferably capable of simulating a diffraction pattern from the created model data, and more preferably capable of mutually simulating the created model data and the diffraction pattern.

[0052] The model data 27, 28, 29 illustrated in each of Figs. 16, 17, 18 are modeled crystal grains present in each of the area image data 21, 22, 23. In Figs. 16 to 18, black balls represent Cu, and white balls represent S. The a-axis, b-axis, and c-axis, which are crystal axes, are specified using a simulation by drawing software. Specifically, each of the model data 27, 28, 29 is three-dimensionally rotated to specify the diffraction patterns generated from the model data 27, 28, 29 created by the simulation of the drawing software so that they match the diffraction pattern data 24, 25, 26 of Figs. 8 to 10 described above. For example, each diffraction spot in the diffraction pattern generated by the model data 27 in Fig. 16 by the simulation of the drawing software generally matches each diffraction spot in the diffraction pattern data 24 of Fig. 8 described above. The orientation (directions of the a-axis, b-axis, and c-axis) of the model data 27 when they match can be regarded as the orientation of the crystal grain to be observed in the area image data 21. Note that the crossing angles and lengths of the a-axis, b-axis, and c-axis crystal axes differ for each crystal system.

[0053] By creating each of the model data 27, 28, 29, the composition and crystal structure of the crystal grains (such as the crystal system and the type of Braphey lattice) as well as the direction of the crystal axis (arrangement of the crystal grains) are specified. Therefore, the model data 27, 28, 29 accurately represent the structure of the actual crystal grains. In the adhesive interface layer, even if the composition is the same, there are crystalline solids whose constituent crystal grains have different crystal axis directions. The characteristics of the crystalline solids whose crystal grains have different crystal axis directions are different. Therefore, by creating the model data 27, 28, 29 and specifying the crystal axis direction of the crystal grains, it is possible to individually distinguish between crystalline solids whose crystal grains have different crystal axis directions, which is advantageous for elucidating the mechanism of adhesion in the adhesive interface layer. Note that, when the crystal grains of the metal compound to be observed are polymorphic, in addition to the composition and the direction of the crystal axis, it is necessary to specify the crystal system or the type of Braphey lattice. As an example of the crystal grains of a polymorphic metal compound, there is iron disulfide, which has an equiaxial crystal system and an orthorhombic crystal system. For such polymorphic metal compounds, the type of crystal system or Brabham lattice can be identified in the process of creating model data.

[0054] In step (S170), the calculation device 3 performs data processing to compare the created model data 27, 28, 29 with the area image data 21, 22, 23 to confirm whether the composition and structure of the identified crystal grains are correct. Specifically, the calculation device 3 creates comparison data (comparison data 31, 32, 33 illustrated in Figs. 19, 20, 21 described later). The comparison data is created, for example, by arranging a large number of model data 27 corresponding to the area image data 21 in a predetermined range of the area image data 21. Next, the calculation device 3 compares the three-dimensional arrangement of atoms indicated by the many arranged model data 27 with the distribution of elements indicated by the element mapping data in the area image data 21, and if they match, it determines that the composition and structure of the identified crystal grains are correct, and if they do not match, it determines that the composition and structure of the identified crystal grains are incorrect. If the identified composition and structure of the crystal grains are incorrect, another region is selected again (return to S120), or the composition and structure of the crystal grains are identified again based on the calculated combination (return to S150).

[0055] In the comparative data 31, 32, and 33 illustrated in Figures 19, 20, and 21, the black spheres representing Cu in the model data 27, 28, and 29 match the points representing Cu in the element mapping data, and the white spheres representing S in the model data 27, 28, and 29 roughly match the points representing S in the element mapping data. In this way, the fact that the data roughly match means that the composition and structure of the identified crystal grains are correct. Also, the fact that the data clearly do not match means that the composition and structure of the identified crystal grains are incorrect.

[0056] In this step (S170), the determination of whether or not there is a match can be made using various known image similarity determination methods, etc. For example, the color coding of each element in the model data 27, 28, 29 is made the same as the color coding of the elements in the element mapping data, and the similarity between the comparison data 31, 32, 33 and the original regional image data 21, 22, 23 without the model data superimposed is calculated, and whether or not there is a match is determined based on the calculated similarity.

[0057] In this step (S170), by gradually expanding the predetermined range in which the multiple model data 27, 28, 29 are arranged, or by setting multiple predetermined ranges in the region image data 21, 22, 23, it is possible to grasp various boundaries such as the boundary between the crystalline solid and the vulcanized rubber in the region image data 21, 22, 23, the boundary between the crystalline solids, and the grain boundary in the same crystalline solid. For example, when multiple predetermined ranges are set in the comparison data 31 and there are predetermined ranges in each predetermined range with different degrees of agreement, the boundary between the crystalline solid and the vulcanized rubber, the boundary between the crystalline solids, and the grain boundary are present in the predetermined range. In this way, by determining the degree of agreement using the comparison data 31, 32, 33 over the entire region image data 21, 22, 23, it is possible to identify various boundaries such as the boundary between the crystalline solid and the vulcanized rubber, the boundary between the crystalline solids, and the grain boundary.

[0058] As described above, according to the first modification, by checking the correctness of the identified composition and structure of the crystal grains, the degree of influence on the adhesion between the metal and the vulcanized rubber can be observed using the composition and structure of the crystal grains that are more likely to be correct. In addition, in the process of checking the correctness, the direction of the crystal axis can be grasped in addition to the composition and crystal structure of the crystal grains. Therefore, it is advantageous for grasping the structure of the crystal grains with high accuracy. Furthermore, various boundaries such as the boundary between the crystalline solid and the vulcanized rubber, the boundary between crystalline solids, and the grain boundary in the same crystalline solid can be identified, and the distribution and shape of the irregular metal compound in the actual adhesive interface layer (the growth state of the crystalline solid of the metal compound) can be grasped more faithfully.

[0059] Next, a second modification of the embodiment of the identification method shown in FIG. 22 will be described.

[0060] In the second modification, another step S180 is added to the procedure of Fig. 15 described above. That is, in the procedure of the second modification, after the correctness of the composition and structure of the identified crystal grains is confirmed (S170), the calculation device 3 identifies the crystal plane of the crystal grain that comes into contact with the vulcanized rubber (S180). Therefore, in the second modification, the affinity acting between the crystal grains and the vulcanized rubber is quantified using the amount of sulfur per unit area on the identified crystal plane as an index.

[0061] In step (S180), the calculation device 3 executes data processing to identify the crystal plane of the crystal grain in contact with the vulcanized rubber based on the model data 27, 28, 29. Specifically, the calculation device 3 identifies the Miller indices of the crystal plane in contact with the vulcanized rubber using the comparison data 31, 32, 33 in the above-mentioned Figs. 19, 20, 21. By extending a predetermined range of the comparison data 31, 32, 33 to the boundary of the vulcanized rubber, the crystal plane of the boundary can be identified based on the three-dimensional arrangement of atoms in the model data 27, 28, 29.

[0062] In the comparative data 31, 32, and 33 shown in Figures 23, 24, and 25, the white lines in each figure indicate the crystal planes facing the vulcanized rubber. The three-digit white letters in parentheses around the white lines indicate the Miller indices of the crystal planes. Some Miller indices are marked with an overbar " ̄", which indicates "-" (negative value). The crystal planes indicated by the white lines are the surfaces that contact the vulcanized rubber among the surfaces that form the surface of a minute crystalline solid composed of a large number of crystal grains. In this way, by identifying the Miller indices of the crystal planes that contact the vulcanized rubber, the degree of influence of the metal compounds present in the adhesive interface layer on the adhesion between the metal and the vulcanized rubber can be observed.

[0063] When the crystal plane in contact with the vulcanized rubber is identified, the amount of sulfur (atomic weight or number of atoms) per unit area on the identified crystal plane can be calculated. Either the atomic weight or the number of atoms may be used for the amount of sulfur per unit area. Specifically, the calculation device 3 calculates the amount of sulfur per unit area on the identified crystal plane using a crystal plane database D2 illustrated in FIG. 26, which will be described later.

[0064] The crystal plane database D2 illustrated in FIG. 26 contains the Miller indices, area, sulfur content (number of atoms), and unit area [Å] for each crystal plane of a crystal grain of a metal compound. 2 The crystal plane database D2, like the database D1, was created by referring to various known documents and various databases available on the Internet.

[0065] From the crystal plane database D2, we can see that the lower the index plane (the crystal plane with a lower sum of Miller indices), the greater the amount of sulfur per unit area. Assuming that chemical bonds are also formed between the S atoms on the crystal plane of the metal compound and the vulcanized rubber, low-index planes, which have a greater amount of sulfur per unit area, are more stable (have higher adhesion) than high-index planes because they can form more bonds. Therefore, for example, the amount of sulfur per unit area on the low-index planes of CuS and Cu2S is about 6 to 7 [atoms / Å]. 2], but Cu2S has a higher affinity with vulcanized rubber than CuS because all of its crystal faces are low-index faces. Based on this knowledge, the amount of sulfur per unit area of ​​the crystal faces of a metal compound that come into contact with vulcanized rubber can be used as an index to evaluate the adhesion between the metal and vulcanized rubber.

[0066] In the above-described embodiment and modified examples 1 and 2, the area image data 21, 22, and 23 are mainly Cu. x Although we used a layer containing S, the same method can also be applied to layers containing ZnS or ZnO, and the composition and structure of the crystal grains in those layers can also be identified. x The composition and structure of ZnS and ZnO crystal grains in the S-containing layer can also be identified.

[0067] The present invention is not limited to a specific embodiment, and various modifications and variations are possible within the scope of the gist of the present invention. [Explanation of symbols]

[0068] 1 Observation System 2. Scanning Transmission Electron Microscopy 3 Computing device 10. Observation specimens 20 Image data 21, 22, 23 Area image data 24, 25, 26 Diffraction pattern data 27, 28, 29 Model data 31, 32, 33 Comparison data D1 Database D2 Crystallographic Plane Database

Claims

1. A method for identifying the composition and structure of crystal grains of a rubber-metal compound, comprising obtaining image data of a thin specimen including an adhesive interface layer formed at the boundary between vulcanized rubber and a metal by a scanning transmission electron microscope, and using the image data to identify the composition and structure of crystal grains of a metal compound originating from the metal present in the adhesive interface layer, comprising: A method for identifying the composition and structure of crystal grains of a rubber and metal compound, in which a region selected from the image data is subjected to a fast Fourier transform by an arithmetic device to obtain diffraction pattern data showing the structure of the crystal grains, and a plurality of diffraction spots that are asymmetric with respect to each other and selected from a large number of diffraction spots present in the obtained diffraction pattern data are used as target spots, the distance from the center of each of the diffraction spots to each of the target spots and the intersection angle between the line segments connecting the center and each of the target spots are calculated, and the composition and structure of the crystal grains are identified using a combination of each of the calculated distances and each of the calculated intersection angles.

2. A method for identifying the composition and structure of crystal grains of a rubber and metal compound as described in claim 1, wherein a database is used that accumulates the composition, the interplanar spacings of a plurality of crystal lattice planes having different interplanar orientations, and the interplanar angles formed by each of the crystal lattice planes for crystal grains of a large number of types of known metal compounds, and the calculation device regards the combinations as the interplanar spacings and the interplanar angles, and selects from the database crystal grains of the known metal compounds whose interplanar spacings and interplanar angles are close to those of the combinations, and identifies the composition and structure of the crystal grains based on the composition of the selected crystal grains of the known metal compounds.

3. the image data includes dark-field image data or bright-field image data superimposed on elemental mapping data showing a distribution of elements constituting the metal compound, 3. A method for identifying the composition and structure of crystal grains of a rubber and metal compound as described in claim 1 or 2, further comprising the steps of: creating model data of the crystal grains by the computing device based on the identified composition and structure of the crystal grains; and comparing the created model data with the element mapping data to determine whether the identified composition and structure of the crystal grains are correct.

4. The method for identifying the composition and structure of crystal grains of a rubber-metal compound according to claim 3, wherein the crystal faces of the crystal grains that come into contact with the vulcanized rubber are identified by the computing device based on the model data.

5. 5. A method for identifying the composition and structure of crystal grains of a rubber-metal compound according to claim 4, wherein the adhesion of the adhesive interface layer is evaluated using the amount of sulfur per unit area on the identified crystal plane as an index.

Citation Information

Patent Citations

  • Rubber-bonded brass conjugate

    JP2004263336A