Optical film, display device, and composition for forming ultraviolet absorbing layer
The optical film with a specific active energy ray-curable resin and structural units addresses adhesion issues in ultraviolet absorbing layers, ensuring high adhesion and effective ultraviolet shielding while maintaining light resistance.
Patent Information
- Application Number
- JP2023070822
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
AI Technical Summary
Conventional methods for forming ultraviolet absorbing layers in optical films face challenges with adhesion issues between the ultraviolet absorbing layer and the resin layer, leading to decreased adhesion and increased stress due to higher exposure amounts of initiators, which results in volumetric contraction and stress.
An optical film comprising a transparent base material, a hard coat layer, and an ultraviolet absorbing layer containing an active energy ray-curable resin with specific structural units and a copolymer, which enhances adhesion and includes additives for antistatic, antifouling, and antiglare properties, achieving a high ultraviolet shielding rate and pencil hardness.
The solution provides an optical film with high adhesion, excellent ultraviolet shielding, and improved light resistance, maintaining optical properties even after exposure to outdoor conditions.
Smart Images

Figure 2024156397000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical film. The present invention also relates to a display device using the optical film and a composition for forming an ultraviolet absorbing layer related to the optical film. [Background technology]
[0002] Hard coat films are widely used to protect display screens of displays, touch panels, mobile phones, and the like. Mobile products such as mobile phones and smartphones are increasingly being used outdoors. Hard coat films for such outdoor applications are required to have excellent light resistance, such as not turning yellow even when exposed to ultraviolet light for a long period of time and not causing peeling between the hard coat layer and the base film.
[0003] Patent Document 1 proposes adding an ultraviolet absorber and a light stabilizer to the hard coat layer for the purpose of imparting weather resistance. Patent Document 2 proposes a method of preventing photodegradation of not only the substrate but also colorable layers by using a hard coat layer containing an ultraviolet absorbent together with a primer layer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-157315 [Patent Document 2] International Publication No. 2019 / 065833 Summary of the Invention [Problem to be solved by the invention]
[0005] It is generally known that when a photocured layer (ultraviolet absorbing layer) containing an ultraviolet absorber is formed, the adhesion with the resin layer in contact is poor. It is thought that the photocured layer containing an ultraviolet absorber needs to increase the exposure dose and initiator in order to increase the hardness, and this causes volume shrinkage and stress stronger than usual, resulting in poor adhesion. To address this issue, conventional countermeasures have been taken, such as changing the formula of the underlayer that serves as the base when applying the UV-absorbing layer, adjusting the surface condition and flexibility, applying a surface treatment to the underlayer, applying a primer layer to the underlayer and curing it together with the UV-absorbing layer, etc. However, depending on the type of UV-absorbing layer and underlayer, this may not lead to an improvement in adhesion, and therefore a UV-absorbing layer with good adhesion is required from the perspective of reducing the number of processes.
[0006] In view of the above circumstances, an object of the present invention is to provide an optical film in which an ultraviolet absorbing layer has high adhesion. Another object of the present invention is to provide a composition for forming an ultraviolet absorbing layer, which is capable of forming an ultraviolet absorbing layer having high adhesion. [Means for solving the problem]
[0007] A first aspect of the present invention is an optical film comprising a first functional layer, an ultraviolet absorbing layer located on a first surface of the first functional layer, and a transparent substrate located on a second surface of the first functional layer. The ultraviolet absorbing layer contains an active energy ray curable resin and an ultraviolet absorbing agent. The active energy ray-curable resin contains a copolymer of a structural unit represented by the following formula (i) and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit. This optical film has an ultraviolet ray shielding rate of 90% or more as measured in accordance with JIS L1925, and the pencil hardness of the surface on the first side under a load of 500 g is H or more. [ka] [In formula (i), R 1 represents a hydrogen atom, a halogen atom, a carboxyl group, a sulfo group, a cyano group, a hydroxy group, an alkyl group having 10 or less carbon atoms, an alkoxycarbonyl group having 10 or less carbon atoms, an alkylsulfonylaminocarbonyl group having 10 or less carbon atoms, an arylsulfonylaminocarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, an acylaminosulfonyl group having 10 or less carbon atoms, an alkoxy group having 10 or less carbon atoms, an alkylthio group having 10 or less carbon atoms, an aryloxy group having 10 or less carbon atoms, a nitro group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an acyloxy group having 10 or less carbon atoms, an acyl group having 10 or less carbon atoms, a carbamoyl group, a sulfamoyl group, an aryl group having 10 or less carbon atoms, a substituted amino group, a substituted ureido group, a substituted phosphono group, or a heterocyclic group; R 2 represents a hydrogen atom or an alkyl group having 30 or less carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or less carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by combining these, any of which may contain a spirodioxane ring.]
[0008] A second aspect of the present invention is a display device comprising the optical film according to the first aspect.
[0009] A third aspect of the present invention is a composition for forming an ultraviolet absorbing layer, which contains an ultraviolet absorber, an active energy ray curable resin, a photopolymerization initiator, and a solvent. The active energy ray-curable resin contains a copolymer of a structural unit represented by the above formula (i) and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit. When this composition is used to form a film having a thickness of 5 μm, the film has an ultraviolet ray shielding rate of 90% or more as measured according to the method described in JIS L1925. Effect of the Invention
[0010] According to the present invention, an optical film having an ultraviolet absorbing layer with high adhesion can be provided. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic cross-sectional view of an optical film according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of an optical film according to a second embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic cross-sectional view of an optical film according to a third embodiment of the present invention. [Figure 4] FIG. 11 is a schematic cross-sectional view of an optical film according to a fourth embodiment of the present invention. [Diagram 5] 1 is a graph showing the spectrum of a white display output through an organic EL light source and a color filter in an example. [Figure 6] 11 is a graph showing the spectra of red, green, and blue colors output through an organic EL light source and a color filter in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] A first embodiment of the present invention will be described with reference to FIG.
[0013] [Optical film] FIG. 1 is a schematic cross-sectional view of an optical film 1 according to a first embodiment of the present invention. 1, the optical film 1 includes a transparent substrate 10, a hard coat layer (first functional layer) 20, and an ultraviolet absorbing layer 30, and is a laminate in which the hard coat layer 20 and the ultraviolet absorbing layer 30 are laminated in this order on the transparent substrate 10. That is, the ultraviolet absorbing layer 30 is located on one surface (first surface) of the hard coat layer 20, and the transparent substrate 10 is located on the other surface (second surface).
[0014] The thickness of the optical film 1 is, for example, preferably 10 to 140 μm, more preferably 15 to 120 μm, and even more preferably 20 to 100 μm. When the thickness of the optical film 1 is equal to or more than the above lower limit, the strength of the optical film 1 can be further increased. When the thickness of the optical film 1 is equal to or less than the above upper limit, not only can the optical film 1 be made lighter, but also it is advantageous for making the display device thinner. Each layer constituting the optical film 1 will now be described.
[0015] ≪Transparent base material≫ The transparent substrate 10 is a sheet-like member. The material of the transparent substrate 10 may be a resin film having light transmissibility. The material for forming the transparent substrate 10 may be a transparent resin or inorganic glass. Examples of the transparent resin include polyolefin, polyester, polyacrylate, polyamide, polyimide, polyarylate, polycarbonate, triacetyl cellulose, polyvinyl alcohol, polyvinyl chloride, cycloolefin copolymer, norbornene-containing resin, polyethersulfone, polysulfone, and the like. Examples of the polyolefin include polyethylene and polypropylene. Examples of the polyester include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of the polyacrylate include polymethyl methacrylate, and the like. Examples of the polyamide include nylon 6 and nylon 66. Among these, a film made of polyethylene terephthalate (PET), a film made of triacetyl cellulose (TAC), a film made of polymethyl methacrylate (PMMA), and a film made of polyester other than PET may be suitably used. The thickness of the transparent substrate 10 is not particularly limited, but is preferably, for example, 10 to 100 μm. The transmittance of the transparent substrate 10 is preferably, for example, 90% or more.
[0016] The transparent substrate 10 may be provided with ultraviolet ray absorbing ability. The transparent substrate 10 can be provided with ultraviolet ray absorbing ability by adding an ultraviolet ray absorbing agent to the resin that is the raw material of the transparent substrate 10.
[0017] Examples of the ultraviolet absorbing agent include salicylic acid ester-based ultraviolet absorbing agents, benzophenone-based ultraviolet absorbing agents, benzotriazole-based ultraviolet absorbing agents, benzotriazine-based ultraviolet absorbing agents, and cyanoacrylate-based ultraviolet absorbing agents. These ultraviolet absorbents may be used alone or in combination of two or more.
[0018] When the transparent substrate 10 is provided with ultraviolet absorbing ability, the ultraviolet ray shielding rate is preferably 85% or more. Here, the ultraviolet ray shielding rate is a value measured in accordance with JIS L1925, and is calculated by the following formula. UV blocking rate (%) = 100 - average transmittance of UV rays with wavelengths of 290 to 400 nm (%)
[0019] <Hard coat layer> The hard coat layer 20 is formed on the transparent substrate 10 and is in contact with the transparent substrate 10. The hard coat layer 20 functions as a reinforcing layer that suppresses scratches and the like in the optical film 1. Examples of the hard coat layer 20 include a layer formed of a hard coat agent containing a monofunctional, bifunctional, trifunctional or higher functional (meth)acrylate or a urethane (meth)acrylate. In this specification, "(meth)acrylate" means both or either one of "acrylate" and "methacrylate".
[0020] <Ultraviolet absorbing layer> The ultraviolet absorbing layer 30 is formed on the hard coat layer 20 and is in contact with the hard coat layer 20 . The ultraviolet absorbing layer 30 contains an active energy ray curable resin and an ultraviolet absorbing agent.
[0021] The active energy ray curable resin is a resin that is polymerized and cured by irradiation with active energy rays such as ultraviolet rays and electron beams. The active energy ray-curable resin according to this embodiment contains a copolymer of a radical scavenger and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit.
[0022] The radical scavenger according to this embodiment is an amine structure-containing polymer having radical scavenging ability, and contains a structural unit represented by the following formula (i).
[0023] [ka]
[0024] In the above formula (i), R 1 represents a hydrogen atom, a halogen atom, a carboxyl group, a sulfo group, a cyano group, a hydroxy group, an alkyl group having 10 or less carbon atoms, an alkoxycarbonyl group having 10 or less carbon atoms, an alkylsulfonylaminocarbonyl group having 10 or less carbon atoms, an arylsulfonylaminocarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, an acylaminosulfonyl group having 10 or less carbon atoms, an alkoxy group having 10 or less carbon atoms, an alkylthio group having 10 or less carbon atoms, an aryloxy group having 10 or less carbon atoms, a nitro group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an acyloxy group having 10 or less carbon atoms, an acyl group having 10 or less carbon atoms, a carbamoyl group, a sulfamoyl group, an aryl group having 10 or less carbon atoms, a substituted amino group, a substituted ureido group, a substituted phosphono group, or a heterocyclic group; R 2 represents a hydrogen atom or an alkyl group having 30 or less carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or less carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by combining these, any of which may contain a spirodioxane ring.
[0025] R 1is preferably a hydrogen atom, a hydroxyl group, or an alkyl group having no more than 10 carbon atoms. The alkyl group preferably has 1 to 6 carbon atoms, and more preferably has 1 to 3 carbon atoms. R 2 is preferably a hydrogen atom or an alkyl group having 10 or less carbon atoms. The alkyl group preferably has 1 to 6 carbon atoms, and more preferably has 1 to 3 carbon atoms. X is preferably a single bond or an aliphatic alkyl chain having up to 30 carbon atoms. The aliphatic alkyl chain preferably has up to 10 carbon atoms, more preferably 1 to 6 carbon atoms, and even more preferably 2 to 4 carbon atoms.
[0026] The molecular weight of the structural unit represented by formula (i) is preferably 2000 or more. When the molecular weight is 2000 or more, the deterioration suppression effect of the ultraviolet absorber is improved. This is believed to be because more molecules remain in the ultraviolet absorbing layer 30, and a sufficient deterioration suppression effect is obtained. The upper limit of the molecular weight of the structural unit represented by formula (i) is not particularly limited, but can be, for example, about 100,000 or more. In this specification, "molecular weight" refers to the "weight average molecular weight" measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.
[0027] Examples of the repeating unit of the copolymer include a (meth)acrylate repeating unit, an olefin repeating unit, a halogen atom-containing repeating unit, a styrene repeating unit, a vinyl acetate repeating unit, and a vinyl alcohol repeating unit.
[0028] Examples of the (meth)acrylate repeating unit include a repeating unit derived from a (meth)acrylate monomer having a linear or branched alkyl group on the side chain, and a repeating unit derived from a (meth)acrylate monomer having a hydroxyl group on the side chain.
[0029] Examples of the repeating units derived from a (meth)acrylate monomer having a linear or branched alkyl group on the side chain include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, and isopropyl (meth)acrylate. Examples of monomer-derived components include octyl, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, myristyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, and octadecyl (meth)acrylate. These may be used alone or in combination of two or more. Among the above, (meth)acrylate-based repeating units having a linear or branched alkyl group having a carbon number of 1 to 4 in the side chain can be preferably used.
[0030] Examples of the repeating units derived from a (meth)acrylic monomer having a hydroxyl group in the side chain include monomer-derived components such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, hydroxyphenyl (meth)acrylate, etc. These may be used alone or in combination of two or more.
[0031] Examples of the olefin repeating unit include components derived from olefin monomers such as ethylene, propylene, isoprene, butadiene, etc. These may be used alone or in combination of two or more.
[0032] Examples of the halogen atom-containing repeating unit include monomer-derived components such as vinyl chloride, vinylidene chloride, etc. These may be used alone or in combination of two or more.
[0033] Examples of the styrene-based repeating unit include components derived from styrene-based monomers such as styrene, α-methylstyrene, vinyltoluene, etc. These may be used alone or in combination of two or more. Examples of the vinyl acetate repeating unit include esters of saturated carboxylic acids and vinyl alcohol, such as vinyl acetate and vinyl propionate, which may be used alone or in combination of two or more. An example of the vinyl alcohol repeating unit is vinyl alcohol, which may have a 1,2-glycol bond in the side chain.
[0034] The copolymer may have any structure of a random copolymer, an alternating copolymer, a block copolymer, or a graft copolymer. If the copolymer has a random structure, the manufacturing process and preparation with other components are easy. Therefore, a random copolymer is more preferable than other copolymers.
[0035] Radical polymerization can be used as a polymerization method for obtaining the copolymer. Radical polymerization is preferred because it is easy to produce industrially. Radical polymerization may be a solution polymerization method, an emulsion polymerization method, a bulk polymerization method, a suspension polymerization method, or the like. For radical polymerization, it is preferred to use a solution polymerization method. By using the solution polymerization method, it is easy to control the molecular weight of the copolymer.
[0036] In the radical polymerization, the above-mentioned monomer may be diluted with a polymerization solvent, and then a polymerization initiator may be added to polymerize the monomer. The polymerization solvent may be, for example, an ester-based solvent, an alcohol ether-based solvent, a ketone-based solvent, an aromatic solvent, an amide-based solvent, and an alcohol-based solvent. The ester-based solvent may be, for example, methyl acetate, ethyl acetate, n-butyl acetate, isobutyl acetate, t-butyl acetate, methyl lactate, and ethyl lactate. The alcohol ether-based solvent may be, for example, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether, 3-methoxy-1-butanol, and 3-methoxy-3-methyl-1-butanol. The ketone-based solvent may be, for example, acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. The aromatic solvent may be, for example, benzene, toluene, and xylene. The amide-based solvent may be, for example, formamide and dimethylformamide. The alcohol-based solvent may be, for example, methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, s-butanol, t-butanol, diacetone alcohol, 2-methyl-2-butanol, etc. Among the above-mentioned polymerization solvents, one type may be used alone, or two or more types may be mixed and used.
[0037] The radical polymerization initiator may be, for example, a peroxide or an azo compound. The peroxide may be, for example, benzoyl peroxide, t-butyl peroxyacetate, t-butyl peroxybenzoate, and di-t-butyl peroxide. The azo compound may be, for example, azobisisobutyronitrile, azobisamidinopropane salt, azobiscyanovaleric acid (salt), and 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide].
[0038] The amount of radical polymerization initiator used is preferably 0.0001 parts by mass or more and 20 parts by mass or less, more preferably 0.001 parts by mass or more and 15 parts by mass or less, and even more preferably 0.005 parts by mass or more and 10 parts by mass or less, when the total amount of monomers is set to 100 parts by mass. The radical polymerization initiator may be added to the monomer and polymerization solvent before the start of polymerization, or may be dropped into the polymerization reaction system. Dropping the radical polymerization initiator into the polymerization reaction system for the monomer and polymerization solvent is preferable in that heat generation due to polymerization can be suppressed.
[0039] The reaction temperature of the radical polymerization is appropriately selected depending on the type of radical polymerization initiator and polymerization solvent. From the viewpoint of ease of production and reaction controllability, the reaction temperature is preferably 60° C. or more and 110° C. or less.
[0040] The content of the radical scavenger represented by formula (i) is preferably from 1 to 95 mol %, and more preferably from 10 to 90 mol %, based on the total molar amount of monomers constituting the active energy ray-curable resin.
[0041] As the ultraviolet absorbing agent, the same ones as those exemplified in the explanation of the transparent substrate can be used.
[0042] The optical film 1 of the present embodiment having the above configuration exhibits sufficient ultraviolet shielding ability with an ultraviolet shielding rate of 90% or more measured in accordance with JIS L1925 due to the ultraviolet absorbing layer 30, and also provides sufficient adhesion between the ultraviolet absorbing layer 30 and the hard coat layer 20. The copolymer contained in the active energy ray-curable resin improves the adhesion between the ultraviolet absorbing layer 30 and the hard coat layer 20, and the radical scavenger represented by formula (i) suppresses deterioration of the ultraviolet absorber and improves light resistance. In the optical film 1, the ultraviolet absorbing layer 30 has good adhesion even without performing surface treatment or forming a primer layer on the surface in contact with the ultraviolet absorbing layer 30. Furthermore, due to the hardness of the hard coat layer 20 and the active energy ray curable resin after curing, the ultraviolet absorbing layer 30 side has a sufficient surface hardness of H or more in a pencil hardness test with a load of 500 g in accordance with JIS-K5400-1990.
[0043] In the ultraviolet absorbing layer 30 according to the present invention, antistatic properties, antifouling properties, antiglare properties, etc. may be imparted by adding a specific substance. Examples of additives for imparting antistatic properties include various antistatic agents such as metal oxide fine particles such as antimony-doped tin oxide (ATO) and tin-doped indium oxide (ITO), polymer-type conductive compositions, and quaternary ammonium salts. Examples of additives for imparting antifouling properties include various antifouling agents such as silicon oxides, fluorine-containing silane compounds, fluoroalkylsilazanes, fluoroalkylsilanes, fluorine-containing silicon compounds, and perfluoropolyether group-containing silane coupling agents.
[0044] As an additive for imparting antiglare properties, organic fine particles or inorganic fine particles can be used. The organic fine particles are materials that form fine irregularities on the surface and impart a function of scattering external light. Examples of the organic fine particles include resin particles made of light-transmitting resin materials such as acrylic resin, polystyrene resin, styrene-(meth)acrylic acid ester copolymer, polyethylene resin, epoxy resin, silicone resin, polyvinylidene fluoride, and polyethylene fluoride resin. In order to adjust the refractive index and dispersibility of the resin particles, two or more types of resin particles with different materials (refractive index) may be mixed and used. Inorganic fine particles are materials that adjust the precipitation and aggregation of organic fine particles. Examples of inorganic fine particles that can be used include silica fine particles, metal oxide fine particles, and various mineral fine particles. Examples of silica fine particles that can be used include colloidal silica and silica fine particles surface-modified with reactive functional groups such as (meth)acryloyl groups. Examples of metal oxide fine particles that can be used include alumina (aluminum oxide), zinc oxide, tin oxide, antimony oxide, indium oxide, titania (titanium dioxide), and zirconia (zirconium dioxide). Examples of mineral fine particles that can be used include mica, synthetic mica, vermiculite, montmorillonite, iron montmorillonite, bentonite, beidellite, saponite, hectorite, stevensite, nontronite, magadiite, ilealite, kanemite, layered titanic acid, smectite, synthetic smectite, and the like. The mineral fine particles may be either natural or synthetic (including substituted or derivative), or a mixture of both may be used. Among mineral fine particles, layered organic clay is more preferred. Layered organic clay refers to an organic onium ion introduced between layers of swelling clay. The organic onium ion is not limited as long as it can be made organic by utilizing the cation exchange property of swelling clay. When layered organic clay mineral is used as mineral fine particles, the above-mentioned synthetic smectite can be preferably used.
[0045] A second embodiment of the present invention will be described with reference to Fig. 2. In the following description, configurations common to those already described will be given the same reference numerals and duplicated description will be omitted.
[0046] 2 is a schematic cross-sectional view of an optical film 2 according to this embodiment. The optical film 2 has a second functional layer 40 formed on an ultraviolet absorbing layer 30.
[0047] The function exhibited by the second functional layer 40 can be changed in various ways depending on the application of the optical film, etc. Specific examples of the second functional layer include a low refractive index layer, an antiglare layer, an antistatic layer, an antifouling layer, etc., and the second functional layer may have two or more functions. The antistatic layer, antifouling layer and antiglare layer can be formed using a composition in which the above-mentioned various additives are added to the base resin constituting the layer.
[0048] When the second functional layer 40 is a low refractive index layer, the refractive index can be, for example, 1.20 to 1.55. Examples of additives used to adjust the refractive index include fine particles of lithium fluoride (LiF), magnesium fluoride (MgF2), sodium hexafluoroaluminum (cryolite, cryolite, 3NaF·AlF3, Na3AlF6), aluminum fluoride (AlF3), and silica fine particles. As the silica fine particles, those having voids inside the particles, such as porous silica fine particles and hollow silica fine particles, are suitable.
[0049] There is no limitation on the method for forming the low refractive index layer, and a method of applying a composition for forming a low refractive index layer to the ultraviolet absorbing layer 30 and curing it by irradiating it with active energy rays, a vacuum deposition method, a sputtering method, an ion plating method, an ion beam method, a plasma vapor phase growth method, or the like can be used. The thickness of the low refractive index layer is not particularly limited, but is preferably, for example, 40 nm to 1 μm. By providing the low refractive index layer, the optical film 2 exhibits an anti-reflection function.
[0050] A third embodiment of the present invention will be described with reference to FIG. 3 is a schematic cross-sectional view of an optical film 3 according to this embodiment. The optical film 3 has a configuration in which a colored layer 50 is provided in place of the hard coat layer 20 of the optical film 1.
[0051] The colored layer 50, which is the first functional layer, is a cured product of a colored layer-forming composition, and contains a dye (A), an active energy ray-curable resin (B), and a photopolymerization initiator (C). The thickness of the colored layer 50 is preferably, for example, 0.5 to 10 μm. When the thickness of the colored layer 50 is equal to or greater than the lower limit, the colored layer 50 can contain a dye without causing abnormalities in the appearance of the colored layer 50, and the light absorption properties of the dye can improve the reflectivity and color reproducibility. When the thickness of the colored layer 50 is equal to or less than the upper limit, it is advantageous for making the display device thinner. The thickness of the colored layer 50 can be determined by observing a cross section of the optical film in the thickness direction with a microscope or the like.
[0052] <Dye (A)> The colorant (A) contains at least one of a first coloring material, a second coloring material, and a third coloring material described below. The first coloring material has a maximum absorption wavelength in the range of 470 nm to 530 nm, and a half-width of the absorption spectrum in the range of 15 nm to 45 nm. If the maximum absorption wavelength is less than the lower limit, the luminance efficiency of blue light emission is likely to decrease, and if it exceeds the upper limit, the luminance efficiency of green light emission is likely to decrease. If the half-width of the absorption spectrum is less than the lower limit, the effect of suppressing the reflection characteristics to external light is small, and if it exceeds the upper limit, the reflection characteristics to external light are likely to be improved, but the luminance efficiency is likely to decrease.
[0053] The second coloring material has a maximum absorption wavelength in the range of 560 nm to 620 nm, and a half-width of the absorption spectrum in the range of 15 nm to 55 nm. If the maximum absorption wavelength is less than the lower limit, the luminance efficiency of green light emission is likely to decrease, and if it exceeds the upper limit, the luminance efficiency of red light emission is likely to decrease. If the half-width of the absorption spectrum is less than the lower limit, the suppression effect on the reflection characteristics to external light is small, and if it exceeds the upper limit, the reflection characteristics to external light are likely to be improved, but the luminance efficiency is likely to decrease.
[0054] The third coloring material has a wavelength of 380 to 780 nm at which the transmittance is lowest in the range of 650 to 780 nm. If the wavelength of the third coloring material at which the transmittance is lowest in the range of 400 to 780 nm is less than the lower limit, the luminance efficiency of red light emission is likely to decrease, whereas if it exceeds the upper limit, the effect of suppressing the reflection characteristics against external light is reduced.
[0055] The dye (A) preferably contains a compound having any one of a porphyrin structure, a merocyanine structure, a phthalocyanine structure, an azo structure, a cyanine structure, a squarylium structure, a coumarin structure, a polyene structure, a quinone structure, a tetradiporphyrin structure, a pyrromethene structure, and an indigo structure, or a metal complex thereof. In particular, it is more preferable to use a metal complex having a porphyrin structure, a pyrromethene structure, or a phthalocyanine structure, or a compound having a squarylium structure, because of its excellent reliability. The dye (A) may contain one of these compounds or metal complexes thereof alone, or may contain two or more of them. These compounds or metal complexes thereof may be contained in the first coloring material, the second coloring material, the third coloring material, or two or more of these coloring materials.
[0056] <Energy ray curable compound (B)> The energy ray curable compound (B) is a resin that is polymerized and cured by irradiation with active energy rays such as ultraviolet rays, electron beams, etc. For example, monofunctional, difunctional or trifunctional or higher functional (meth)acrylate monomers, urethane (meth)acrylates, etc. can be used.
[0057] Examples of monofunctional (meth)acrylate compounds that can be contained in the energy ray curable compound (B) include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, glycidyl (meth)acrylate, acryloylmorpholine, N-vinylpyrrolidone, tetrahydrofurfuryl acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and the like. Acrylate, isobornyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phosphate (meth)acrylate, ethylene oxide modified phosphate (meth)acrylate, phenoxy (meth)acrylate, ethylene oxide modified phenoxy (meth)acrylate ) acrylate, propylene oxide modified phenoxy (meth)acrylate, nonylphenol (meth)acrylate, ethylene oxide modified nonylphenol (meth)acrylate, propylene oxide modified nonylphenol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxy-3-phenoxypropyl (meth ) acrylate, 2-(meth)acryloyloxyethyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hexahydrohydrogen phthalate, 2-(meth)acryloyloxypropyl tetrahydrohydrogen phthalate, dimethylaminoethyl (meth)acrylate, trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropropyl (meth)acrylate,Examples of the mono(meth)acrylate include adamantane derivative mono(meth)acrylates such as adamantyl acrylate having a monovalent mono(meth)acrylate derived from 2-adamantane and adamantanediol. Here, "(meth)acryloyl" means both or either one of "acryloyl" and "methacryloyl".
[0058] Examples of bifunctional (meth)acrylate compounds that can be contained in the energy ray curable compound (B) include di(meth)acrylates such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, ethoxylated hexanediol di(meth)acrylate, propoxylated hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and hydroxypivalic acid neopentyl glycol di(meth)acrylate.
[0059] Examples of trifunctional or higher (meth)acrylate compounds that can be contained in the energy ray curable compound (B) include tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, and glycerin tri(meth)acrylate, trifunctional (meth)acrylates such as pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and ditrimethylolpropane tri(meth)acrylate. Examples of the (meth)acrylate compound include trifunctional or higher polyfunctional (meth)acrylate compounds such as pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and ditrimethylolpropane hexa(meth)acrylate, as well as polyfunctional (meth)acrylate compounds in which a portion of these (meth)acrylates is substituted with an alkyl group or ε-caprolactone.
[0060] In addition, urethane (meth)acrylate can also be used as a resin that can be contained in the energy ray curable compound (B). For example, the urethane (meth)acrylate can be obtained by reacting a product obtained by reacting a polyester polyol with an isocyanate monomer or a prepolymer with a (meth)acrylate monomer having a hydroxyl group.
[0061] Examples of urethane (meth)acrylates include pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate toluene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate toluene diisocyanate urethane prepolymer, pentaerythritol triacrylate isophorone diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate isophorone diisocyanate urethane prepolymer, and the like.
[0062] The monofunctional, bifunctional, trifunctional or higher functional (meth)acrylate monomers, urethane (meth)acrylates, etc. that can be contained in the other energy ray curable compound (B) may be used alone or in combination of two or more kinds. They may also be partially polymerized oligomers. Copolymers containing various repeating units used in the ultraviolet absorbing layer 30 can also be included in the energy ray curable compound (B).
[0063] The content of the energy ray curable compound (B) is preferably 20 to 80 mass %, more preferably 30 to 70 mass %, based on the total mass of the colored layer forming composition. When the content of the energy ray curable compound (B) is equal to or more than the above lower limit, the color fading suppression effect can be further improved. When the content of the energy ray curable compound (B) is equal to or less than the above upper limit, the handleability of the colored layer forming composition can be further improved.
[0064] <Photopolymerization initiator (C)> When ultraviolet rays are used as the active energy rays, the photopolymerization initiator (C) generates radicals when irradiated with ultraviolet rays. Examples of the photopolymerization initiator (C) include benzoins (benzoin alkyl ethers such as benzoin, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether), phenyl ketones [for example, acetophenones (for example, acetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, and 1,1-dichloroacetophenone), alkyl phenyl ketones such as 2-hydroxy-2-methylpropiophenone, and cycloalkyl phenyl ketones such as 1-hydroxycyclohexyl phenyl ketone], aminoacetophenones {2-methyl-1-[4-(methylthio)phenyl Examples of the photopolymerization initiator include 2-methyl-2-morpholinoaminopropanone-1, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, etc.}, anthraquinones (anthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-t-butylanthraquinone, 1-chloroanthraquinone, etc.), thioxanthones (2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone, etc.), ketals (acetophenone dimethyl ketal, benzyl dimethyl ketal, etc.), benzophenones (benzophenone, etc.), xanthones, phosphine oxides (for example, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, etc.), etc. These photopolymerization initiators may be used alone or in combination of two or more.
[0065] The content of the photopolymerization initiator (C) is preferably 0.01 to 20 mass % and more preferably 0.01 to 5 mass % based on the solid content of the color layer forming composition. If the content of the photopolymerization initiator (C) is less than the lower limit, the curability is insufficient. If the content of the photopolymerization initiator (C) is more than the upper limit, unreacted photopolymerization initiator (C) remains, and reliability such as heat resistance is deteriorated.
[0066] The colored layer 10 may contain a solvent (D) and an additive (E). These will be described in detail below. <Solvent (D)> The solvent (D) is necessary when forming the colored layer. Most of it disappears from the colored layer by volatilization during drying after coating, but some remains in the colored layer, so its components are described below. Examples of the solvent (D) include ethers, ketones, esters, and cellosolves. Examples of the ethers include dibutyl ether, dimethoxymethane, dimethoxyethane, diethoxyethane, propylene oxide, 1,4-dioxane, 1,3-dioxolane, 1,3,5-trioxane, tetrahydrofuran, anisole, and phenetole. Examples of the ketones include acetone, methyl ethyl ketone, diethyl ketone, dipropyl ketone, diisobutyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methylcyclohexanone, and ethylcyclohexanone. Examples of the esters include ethyl formate, propyl formate, n-pentyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, n-pentyl acetate, and γ-butyrolactone. Examples of cellosolves include methyl cellosolve, cellosolve (ethyl cellosolve), butyl cellosolve, cellosolve acetate, etc. The solvent (D) may be used alone or in combination of two or more kinds.
[0067] The content of the solvent (D) is preferably 20 to 80 mass %, more preferably 30 to 70 mass %, based on the total mass of the colored layer forming composition including the above (A) to (C). When the content of the solvent (D) is equal to or more than the lower limit, the handleability of the colored layer forming composition can be improved. When the content of the solvent (D) is equal to or less than the upper limit, the time required to form the colored layer can be shortened.
[0068] <Additives (E)> Examples of additive (E) include a compound having at least the structure represented by the following formula (ii) (hereinafter referred to as "compound A"), a radical scavenger, a singlet oxygen quencher, a peroxide decomposer, and the like.
[0069] [ka]
[0070] In formula (ii), R 1 each independently represents an alkyl group, an alkenyl group, an aryl group, a heterocyclic group, R 9 CO-, R 10 SO2-, and R 11 NHCO- (R 9 , R 10 , R 11 Each of R is independently an alkyl group, an alkenyl group, an aryl group, or a heterocyclic group. 2 and R 3 R is independently any one of a hydrogen atom, a halogen atom, an alkyl group, an alkenyl group, an alkoxy group, and an alkenyloxy group. 4 ~R 8 are each independently a hydrogen atom, an alkyl group, an alkenyl group, or an aryl group.
[0071] Examples of radical scavengers include hindered amine-based light stabilizers such as 4-isopropylaminodiphenylamine, N-phenyl-1-naphthylamine, and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, and phenol-based antioxidants such as 2,6-di-t-butyl-p-cresol and 6,6'-di-t-butyl-4,4'-butylidene-m-cresol.
[0072] Examples of singlet oxygen quenchers include transition metal complexes, dyes, amines, phenols, and sulfides. Particularly preferred materials include transition metal complexes of dialkyldithiophosphates, dialkyldithiocarbanates, benzenedithiol, or similar dithiols, and nickel, zinc, copper, or cobalt is preferably used as the central metal of these transition metal complexes.
[0073] Peroxide decomposers have the function of decomposing the peroxides generated when the dye is oxidized and deteriorated, stopping the autoxidation cycle and suppressing dye deterioration (fading). Phosphorus-based antioxidants and sulfur-based antioxidants can be used as peroxide decomposers.
[0074] Examples of phosphorus-based antioxidants include 2,2'-methylenebis(4,6-di-t-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphorus, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, and 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenz[d,f][1,3,2]dioxaphosphepine.
[0075] Examples of sulfur-based antioxidants include 2,2-bis({[3-(dodecylthio)propionyl]oxy}methyl)-1,3-propanediyl-bis[3-(dodecylthio)propionate], 2-mercaptobenzimidazole, dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, pentaerythrityl-tetrakis(3-laurylthiopropionate), and 2-mercaptobenzothiazole.
[0076] By incorporating these additives in the colored layer 50, the light resistance and heat resistance of the dye (A) can be improved.
[0077] The additive (E) may contain other additives such as a leveling agent, an antifoaming agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a photosensitizer, and a conductive material.
[0078] The optical film 3 according to this embodiment includes the colored layer 50, and when attached to various display devices, it can achieve both reflection suppression and luminance efficiency, thereby contributing to improving display quality. In addition, when the ultraviolet absorbing layer 30 is positioned on the side where external light enters, deterioration of the colored layer can be suppressed, and the effect can be maintained for a long period of time.
[0079] A fourth embodiment of the present invention will be described with reference to FIG. 4 is a schematic cross-sectional view of an optical film 4 according to this embodiment. The optical film 4 has a configuration similar to that of the optical film 3, except that an oxygen barrier layer (second functional layer) 60 is provided between the ultraviolet absorbing layer 30 and the colored layer 50.
[0080] The oxygen barrier layer 60 is a transparent layer having optical transparency, and is one embodiment of the second functional layer. The oxygen permeability of the oxygen barrier layer 60 is 10 cm 3 / m 2 ·day·atm or less, 5cm 3 / (m 2 It is more preferable that the temperature is 1 cm 3 / (m 2 When the oxygen permeability of the oxygen barrier layer 60 is equal to or less than the above upper limit, sufficient oxygen barrier properties can be exhibited. The lower limit of the oxygen permeability of the oxygen barrier layer 60 is not particularly limited, and is preferably 0 cm 3 / (m 2 ·day·atm). The material for forming the oxygen barrier layer 60 preferably contains polyvinyl alcohol (PVA), ethylene-vinyl alcohol copolymer (EVOH), vinylidene chloride, siloxane resin, etc., and examples of materials that can be used include Maxive (registered trademark) manufactured by Mitsubishi Gas Chemical Company, Inc., EVAL manufactured by Kuraray Co., Ltd., Saran Latex and Saran Resin manufactured by Asahi Kasei Corp. The thickness of the oxygen barrier layer 60 is not particularly limited, and may be any thickness that provides the desired oxygen barrier properties. In this specification, the oxygen permeability of the oxygen barrier layer 60 is a value measured using an oxygen permeability measuring device under conditions of 30° C. and a relative humidity of 60%.
[0081] In addition, inorganic particles (particles made of an inorganic compound) may be dispersed in the oxygen barrier layer 60. The inorganic particles can reduce oxygen permeability and further suppress oxidation deterioration (discoloration) of the colored layer 50. The size and content of the inorganic particles are not particularly limited and may be appropriately set according to the thickness of the oxygen barrier layer 60 and the like. The size (maximum length) of the inorganic particles dispersed in the oxygen barrier layer 60 is preferably less than the thickness of the oxygen barrier layer 60, and the smaller the size, the more advantageous it is. The size of the inorganic particles dispersed in the oxygen barrier layer 60 may be uniform or non-uniform. Specific examples of the inorganic particles dispersed in the oxygen barrier layer 60 include silica particles, alumina particles, silver particles, copper particles, titanium particles, zirconia particles, tin particles, and the like.
[0082] The optical film 4 according to this embodiment includes an oxygen barrier layer 60. Therefore, by attaching the oxygen barrier layer 60 to a display device so that it is closer to a viewer than the colored layer 50, oxygen contained in the outside air does not reach the colored layer 50 unless it passes through the oxygen barrier layer 60. As a result, deterioration of the color material contained in the colored layer 50 due to oxygen is suppressed, and the color correction function can be maintained for a longer period of time. In this embodiment, the number and positions of the oxygen barrier layers 60 can be set appropriately.
[0083] [Method of manufacturing optical film] The optical film according to each embodiment of the present invention can be produced by a conventionally known method. For example, in the case of the optical film 1, first, a hard coat agent is applied to one surface of the transparent substrate 10 and cured to form the hard coat layer 20. Thereafter, a composition for forming an ultraviolet absorbing layer is applied and cured by irradiation with active energy rays, thereby obtaining the ultraviolet absorbing layer 30.
[0084] The ultraviolet absorbing layer forming composition according to the present invention contains an ultraviolet absorber, an active energy ray curable resin, a photopolymerization initiator, and a solvent. The active energy ray curable resin contains a copolymer of a structural unit represented by formula (i) and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit. As the photopolymerization initiator, those described above as the photopolymerization initiator (C) can be used. The light source for forming the ultraviolet absorbing layer 30 can be any light source that generates active energy rays. As the active energy rays, light energy rays such as radiation (gamma rays, X-rays, etc.), ultraviolet rays, visible light, and electron beams (EB) can be used, and usually, ultraviolet rays and electron beams are used in many cases. For example, as lamps that radiate ultraviolet rays, low pressure mercury lamps, medium pressure mercury lamps, high pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, electrodeless discharge tubes, etc. can be used. As irradiation conditions, the ultraviolet ray irradiation amount is usually 100 to 1000 mJ / cm. 2 It is. A film having a thickness of 5 μm formed from this composition for forming an ultraviolet absorbing layer has an ultraviolet shielding rate of 90% or more as measured according to the method described in JIS L1925.
[0085] [Display device] The display device of the present invention includes the optical film of the present invention. Specific examples of the display device include televisions, monitors, mobile phones, portable game devices, personal digital assistants, personal computers, electronic books, video cameras, digital still cameras, head-mounted displays, navigation systems, audio playback devices (car audio, digital audio players, etc.), copiers, facsimiles, printers, printer-combinations, vending machines, automated teller machines (ATMs), personal authentication devices, optical communication devices, IC cards, etc. Among these, the optical film of the present invention is preferably used for display devices including self-luminous elements such as LEDs, organic electroluminescence (EL), inorganic phosphors, and quantum dots that are susceptible to the influence of external light reflection due to metal electrodes and wiring.
[0086] Although each embodiment of the present invention has been described in detail above with reference to the drawings, the specific configuration is not limited to this embodiment, and configuration changes, combinations, etc. are also included within the scope that does not deviate from the gist of the present invention. EXAMPLES
[0087] The present invention will be described in more detail below with reference to examples. The technical scope of the present invention is not limited in any way solely to the specific contents of these examples.
[0088] [Examples 1 to 13, Comparative Examples 1 to 5] In the following Examples and Comparative Examples, optical films A to R were prepared having the layer structures shown in Tables 1 and 2. In the tables, "-" indicates that the corresponding layer was not present.
[0089] [Table 1]
[0090] [Table 2]
[0091] Tables 3 and 4 show the layer configurations for each example.
[0092] [Table 3]
[0093] [Table 4]
[0094] <Production of optical film> Each layer constituting the optical film will be described in detail below.
[0095] <Transparent base material> Details of the materials listed in Tables 1 and 2 are shown below. TAC: Triacetyl cellulose film (FUJIFILM Corporation, TG60UL, substrate thickness 60μm, UV shielding rate 92.9%) PMMA: Polymethyl methacrylate film (Sumitomo Chemical Co., Ltd., W002N80, substrate thickness 80 μm, UV shielding rate 13.9%)
[0096] <Hard Coat Layer and UV Absorbing Layer> Details of the materials listed in Table 3 are given below. ·Active energy ray curable resin Resin 1: A polymer containing a structural unit represented by formula (i), R 1 is CH3, R 2 is a resin (molecular weight 120,000) having an amine structure in which CH3 and X are single bonds. UA-306H: Pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer (Kyoeisha Chemical Co., Ltd., UA-306H) DPHA: Dipentaerythritol hexaacrylate PETA: Pentaerythritol triacrylate (Resin 1 manufacturing example) 2.4g of 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate (Showa Denko Materials Co., Ltd., FA-711MM), 5.6g of methyl methacrylate (Kanto Chemical Co., Ltd.), 31g of cyclohexanone (Kanto Chemical Co., Ltd.), and 0.11g of 2,2'-azobis(isobutyronitrile) (Fujifilm Wako Pure Chemical Co., Ltd.) were placed in a reaction vessel and heated and stirred at 70°C for 8 hours under a nitrogen gas atmosphere. After that, the mixture was heated and stirred at 100°C for 1 hour to obtain a polymer solution. This polymer solution was poured into 400mL of methanol (Kanto Chemical Co., Ltd.) to obtain a precipitate, which was filtered and dried to obtain resin 1 copolymerized with 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate:methyl methacrylate = 15:85 [mol%]. Photopolymerization initiator Omnirad 819: Acylphosphine oxide photoinitiator (manufactured by IGM Resins BV). Ultraviolet (UV) absorbers Tinuvin 477: Hydroxyphenyltriazine ultraviolet absorber, Tinuvin (registered trademark) 477 (manufactured by BASF Japan Ltd.). Tinuvin 479: Hydroxyphenyltriazine ultraviolet absorber, Tinuvin (registered trademark) 479 (manufactured by BASF Japan Ltd.). Tinuvin 970: Hydroxyphenyltriazine ultraviolet absorber, Tinuvin (registered trademark) 970 (manufactured by BASF Japan Ltd.). Additives (Anti-stain agent) OPTOOL (registered trademark) AR-110 (manufactured by Daikin Industries, Ltd., solid content 15%, solvent: methyl isobutyl ketone) (HALS agents (hindered amine light stabilizers)) Adeka STAB LA-82 (ADEKA Corporation, molecular weight 239) Anti-glare particles (Resin particles) Styrene-methyl methacrylate copolymer particles (refractive index 1.515, average particle size 2.0 μm) (Inorganic fine particles) Inorganic particles 1: Synthetic smectite Inorganic fine particles 2: Alumina nanoparticles (average particle size 40 nm) ·solvent MEK: Methyl ethyl ketone Methyl acetate: Methyl acetate Toluene:Toluene IPA: Isopropyl alcohol
[0097] [Formation of hard coat layer and UV absorbing layer] In each example, a composition for forming a hard coat layer or an ultraviolet absorbing layer having the composition shown in Table 3 was applied onto the corresponding layer and dried in an oven at 80° C. for 60 seconds. Then, an ultraviolet irradiation device was used to irradiate the layer with an irradiation dose of 150 mJ / cm 2 . 2The coating was cured by irradiating it with ultraviolet light (H bulb, light source, manufactured by Fusion UV Systems Japan Co., Ltd.), and a hard coat layer and an ultraviolet absorbing layer were formed so that the film thickness after curing was 5.0 μm. The amounts added in Table 3 are mass ratios (mass %), and "-" indicates that the component is not contained.
[0098] <Low refractive index layer> Details of the composition for forming the low refractive index layer are shown below. Refractive index adjuster Porous silica fine particles (average particle size 75 nm, solid content 20%) methyl isobutyl ketone dispersion 8.5 parts by mass ·Anti-fouling agent OPTOOL (registered trademark) AR-110 5.6 parts by weight ·Active energy ray curable resin PETA 0.4 parts by mass Photopolymerization initiator Omnirad TPO (manufactured by IGM Resins BV) 0.07 parts by mass Leveling agent RS-77 (manufactured by DIC Corporation) 1.7 parts by mass ·solvent Methyl isobutyl ketone 83.73 parts by mass
[0099] [Formation of low refractive index layer] The composition for forming a low refractive index layer was applied onto the ultraviolet absorbing layer and dried in an oven at 80° C. for 60 seconds. Thereafter, the composition was exposed to an ultraviolet ray irradiation device at a dose of 200 mJ / cm 2 . 2 The coating was cured by irradiating it with ultraviolet light (light source H bulb, manufactured by Fusion UV Systems Japan Co., Ltd.), to form a low refractive index layer having a thickness of 100 nm after curing.
[0100] <Anti-glare layer> Details of the composition for forming the antiglare layer are shown below. ·Active energy ray curable resin Pentaerythritol triacrylate, Light Acrylate PE-3A (manufactured by Kyoeisha Chemical Co., Ltd., refractive index 1.52) 43.7 parts by mass Photopolymerization initiator Omnirad TPO 4.55 parts by mass Resin particles Styrene-methyl methacrylate copolymer particles (refractive index 1.515, average particle size 2.0 μm) 0.5 parts by mass ·Inorganic fine particles Synthetic smectite 0.25 parts by weight. Alumina nanoparticles (average particle size 40nm) 1.0 parts by mass ·solvent Toluene 15 parts by mass Isopropyl alcohol 35 parts by weight [Formation of anti-glare layer] In the corresponding example, the antiglare layer-forming composition was applied onto the ultraviolet absorbing layer and dried in an oven at 80° C. for 60 seconds. Thereafter, the composition was exposed to an ultraviolet ray irradiation device at a dose of 150 mJ / cm 2 . 2 The coating was cured by irradiating it with ultraviolet light (H bulb, light source, manufactured by Fusion UV Systems Japan Co., Ltd.) to form an antiglare layer having a thickness of 5.0 μm after curing.
[0101] <Antistatic and stain-resistant layer> Details of the composition for forming the antistatic and antifouling layer are shown below. ·Anti-fouling agent 5.6 parts by weight of Optool (registered trademark) AR-110. ·Active energy ray curable resin PETA 0.4 parts by mass. Photopolymerization initiator Omnirad TPO 0.07 parts by mass. Leveling agent RS-77 1.7 parts by mass. ·solvent Methyl isobutyl ketone 91.6 parts by weight. [Formation of antistatic and antifouling layer] In the corresponding example, the above-mentioned antistatic and antifouling layer-forming composition was applied onto the ultraviolet absorbing layer and dried in an oven at 80° C. for 60 seconds. Thereafter, the composition was exposed to an ultraviolet ray irradiation device at a dose of 200 mJ / cm 2 . 2The ultraviolet rays were irradiated using a light source H bulb (manufactured by Fusion UV Systems Japan Co., Ltd.) to cure the coating film, and an antistatic and antifouling layer with a film thickness of 100 nm after curing was formed.
[0102] <Oxygen barrier layer> As a composition for forming an oxygen barrier layer, an 80% by mass aqueous solution of PVA (Kuraray Poval (registered trademark) PVA-117 (manufactured by Kuraray Co., Ltd.)) was used. In the corresponding example, this was applied onto the colored layer and dried to form an oxygen barrier layer with an oxygen permeability of 1 cm 3 / (m 2 ·day·atm).
[0103] <Colored layer> Details of the materials used for the colored layer are shown below. The maximum absorption wavelength, half-value width, and minimum transmittance wavelength in the specified wavelength range of the colorant are values for a cured coating film with a thickness of 5 μm. <Dye (A)> ·First colorant Dye-1: Pyromethene cobalt complex dye (maximum absorption wavelength 493 nm, half-value width 26 nm) <Production example of Dye-1> Ethyl 5-formyl-2,4-dimethyl-1H-pyrrole-3-carboxylate (2.5 g) was enclosed in a reaction vessel, dissolved in methanol (50 mL), and then 47% hydrobromic acid (45 g) was added, followed by refluxing for 1 hour. The precipitated solid was filtered off to obtain 3,3’,5,5’-tetramethyl-4,4’-di-ethoxycarbonyl-2,2’-dipyrromethene hydrobromide (2.6 g). 3,3’,5,5’-tetramethyl-4,4’-di-ethoxycarbonyl-2,2’-dipyrromethene hydrobromide (0.6 g) was enclosed in a reaction vessel, and methanol (5 mL), triethylamine (0.17 g), and cobalt acetate tetrahydrate (0.18 g) were added, followed by refluxing for 2 hours. The precipitated solid was filtered off to obtain Dye-1 (0.42 g). ·Second colorant Dye-2: Tetraazaporphyrin copper complex dye (Yamamoto Chemical Industries, Ltd., PD-311S, maximum absorption wavelength 586 nm, half-width 22 nm) Dye-3: Tetraazaporphyrin copper complex dye (Yamada Chemical Co., Ltd., FDG-007, maximum absorption wavelength 595 nm, half-width 22 nm) Third colorant Dye-4: Phthalocyanine copper complex dye (Yamada Chemical Industry Co., Ltd., FDN-002, minimum transmittance wavelength 780 nm in the range of 400 to 780 nm)
[0104] <Energy ray curable compound (B)> Resin 1: Same as that used for the UV absorbing layer ·UA-306H ·DPHA PETA <Photopolymerization initiator (C)> Omnirad 819 <Solvent (D)> MEK: Methyl ethyl ketone Methyl acetate <Additives (E)> D1781: Singlet oxygen quencher (bis(dibutyldithiocarbamate)nickel(II), manufactured by Tokyo Chemical Industry Co., Ltd.)
[0105] [Formation of colored layer] In the corresponding example, the color layer-forming composition was applied onto a transparent substrate and dried in an oven at 80° C. for 60 seconds. Thereafter, the composition was irradiated with a UV light at a dose of 150 mJ / cm 2 using an ultraviolet irradiator. 2 The coating was cured by irradiating it with ultraviolet light (Fusion UV Systems Japan, Inc., light source H bulb), forming an antistatic and antifouling layer with a cured thickness of 5.0 nm.
[0106] The optical films according to the respective examples were evaluated as follows. [Film characteristic evaluation] <UV shielding rate of UV absorbing layer> A layer structure of a layer above the first functional layer in each example was formed on a glass substrate, and peeled off using cellophane tape conforming to the JIS-K5600 adhesion test. The transmittance of the peeled cellophane tape was measured using an automatic spectrophotometer (U-4100, manufactured by Hitachi, Ltd.), and the transmittance was measured using the cellophane tape alone as a reference. Using the obtained transmittance, the average transmittance [%] in the ultraviolet range (290 nm to 400 nm) was calculated, and the ultraviolet shielding rate [%] was calculated as a value obtained by subtracting the average transmittance [%] in the ultraviolet range (290 nm to 400 nm) from 100%. The ultraviolet shielding rate is preferably 90% or more, more preferably 95% or more, and may be 100%.
[0107] <Adhesion test> In accordance with JIS K-5600 5-6:1999, 10x10 cross cuts were made at 1mm intervals on the surface of the first side (the side on which the functional layer is provided) of the optical film according to each example, and then an adhesive tape adhesion test was performed to visually evaluate the remaining rate of the coating film. The results were recorded as "○ (pass)" when the results corresponded to the JIS classifications 0, 1, and 2, and as "× (fail)" when the results corresponded to the JIS classifications 3, 4, and 5.
[0108] <Pencil hardness test> A pencil hardness test was carried out on the first surface of the optical film according to each example using a Clemens scratch hardness tester (HA-301, Tester Sangyo Co., Ltd.) in accordance with JIS-K5600-5-4:1999, using a pencil (UNI, pencil hardness H, manufactured by Mitsubishi Pencil Co., Ltd.) with a load of 500 gf (4.9 N). The change in appearance due to scratches was evaluated visually, and the case where no scratches were observed was rated as "○ (pass)", and the case where scratches were observed was rated as "× (fail)".
[0109] <Light resistance test> The light resistance of the obtained optical film was tested using a xenon weather meter tester (X75, manufactured by Suga Test Instruments Co., Ltd.) with a xenon lamp illuminance of 60 W / m 2The test was conducted for 120 hours under conditions of 45°C temperature and 50% RH inside the tester (300nm~400nm), and the transmittance was measured before and after the test using an automatic spectrophotometer (U-4100, manufactured by Hitachi, Ltd.), and the difference in UV shielding rate ΔT(290-400nm) before and after the test was calculated. The closer to zero the UV shielding rate difference is, the better, and |ΔT(290-400nm)|≦10 is preferable, and |ΔT(290-400nm)|≦5 is even more preferable. For the examples and comparative examples including a colored layer, the transmittance difference ΔTλ1 before and after the test at the wavelength λ1 showing the minimum transmittance before the test in the wavelength range of 470 nm to 530 nm, and the transmittance difference ΔTλ2 before and after the test at the wavelength λ2 showing the minimum transmittance before the test in the wavelength range of 560 nm to 620 nm were also calculated. The transmittance difference is better when it is close to zero, and it is preferable that |ΔTλN|≦20 (N=1 to 2), and more preferably that |ΔTλN|≦10 (N=1 to 2).
[0110] [Display device characteristic evaluation] <White display transmission characteristics> The transmittance of the obtained optical film was measured using an automatic spectrophotometer (U-4100, manufactured by Hitachi, Ltd.), and the efficiency of light transmitted through the optical film during white display was calculated using this transmittance, which was evaluated as the white display transmittance characteristic. As a standard, the efficiency of the spectrum during white display output through a white organic EL light source and a color filter, whose spectrum is shown in Figure 5, was set to 100. The closer to 100, the higher the white display transmittance and the more excellent the luminance efficiency. <Display device reflection characteristics> The transmittance T(λ) and surface reflectance R2(λ) of the obtained optical film were measured using an automatic spectrophotometer (U-4100). For the measurement of surface reflectance R2(λ), a matte black dye was applied to the surface of the transparent substrate on which no ultraviolet absorbing layer or the like was formed to perform an anti-reflection treatment, and the spectral reflectance at an incident angle of 5° was measured to obtain the surface reflectance R2(λ). Electrode reflectance R EThe relative reflectance value was calculated based on the following formulas (1) to (4) when the reflectance value of the display device for the D65 light source (CIE (International Commission on Illumination) standard light source D65) without the optical film was taken as 100, and the surface reflectance R(λ) of the outermost layer on the observer side was used to evaluate the reflectance characteristics of the display device. The lower the reflectance characteristic value of the display device, the more the external light reflection can be reduced and the more excellent the reflectance characteristics. In formulas (1) to (4), R1(λ) represents the internal reflection component, Y represents one of the three stimulus values at the white point of the D65 light source, and P D65 (λ) represents the spectrum of the D65 illuminant, and the overline y(λ) represents the CIE1931 color matching function.
[0111]
number
number
number
number
[0112] For the examples and comparative examples having a colored layer, color reproducibility was further evaluated by the following procedure. <Color reproducibility> The transmittance of the obtained optical film was measured using an automatic spectrophotometer (U-4100), and the red, green, and blue display spectra in FIG. 6, which were output through a white EL light source and a color filter, of the spectrum shown in FIG. 5, were measured. The vertical axis of the graphs in FIG. 5 and FIG. 6 represents the emission intensity [au] (arbitrary unit). The NTSC (National Television System Committee) ratio was calculated from the CIE1931 chromaticity value calculated using the measured transmittance and the red, green, and blue display spectra in FIG. 6, and the NTSC ratio was evaluated as an index of color reproducibility. The higher the NTSC ratio, the better the color reproducibility.
[0113] The results are shown in Tables 5 to 9. The white display transmission characteristics and the display device reflection characteristics are also shown as a ratio with Comparative Example 1, which does not have a colored layer, taken as the standard (100%).
[0114] [Table 5]
[0115] [Table 6]
[0116] [Table 7]
[0117] [Table 8]
[0118] [Table 9]
[0119] The results of Example 2, Comparative Example 1, and Comparative Example 2 show that the inclusion of a structural unit represented by formula (i) improves adhesion. The results of Example 2 and Comparative Example 3 show that sufficient photopolymerization is necessary for the optical film to have sufficient surface hardness. The results of Examples 2 and 3 show that it is possible to impart antistatic properties, antifouling properties, and antiglare properties to the ultraviolet absorbing layer while maintaining the physical properties. The results of Examples 4 to 13 show that the physical properties can be satisfied even if a second functional layer such as a low refractive index layer, an antistatic / antifouling layer, or an antiglare layer is provided in addition to the ultraviolet absorbing layer. The results of Example 8, Comparative Example 4, and Comparative Example 5 show that an optical film having an ultraviolet absorbing layer containing a structural unit represented by formula (i) can most improve the light resistance of a colored layer. This was thought to be because the ultraviolet absorbing layer of Comparative Example 5, which does not contain a structural unit represented by formula (i), deteriorated faster than that of Example 8. The results of Examples 8 and 10 show that the light resistance of the colored layer is further improved by providing an oxygen barrier layer as a second functional layer. The results of Examples 8, 11, and 12 show that the light resistance of the colored layer is improved by including a radical scavenger or a singlet oxygen quencher in the colored layer. The results of Examples 2 and 13 demonstrate that optical films that satisfy the required physical and optical properties can be produced using transparent substrates other than TAC.
[0120] In displays employing the optical films of Examples 7 to 9, which have a colored layer as a first functional layer, the reflection characteristics were significantly improved compared to a display employing the optical film of Comparative Example 1, which does not have a colored layer. It is generally said that the transmittance is halved in a display device equipped with a circular polarizing plate, whereas the display device using the optical films of Examples 7 to 9 had excellent luminance efficiency, as shown by the evaluation value of white display transmittance, and also had improved color reproducibility. From the results of Examples 7 to 9, it was found that the wider the absorption wavelength band, the more excellent the reflection characteristics tend to be. [Explanation of symbols]
[0121] 1, 2, 3, 4 Optical Film 10 Transparent base material 20 Hard coat layer (first functional layer) 30 UV absorbing layer 40 Second functional layer 50 Colored layer (first functional layer)
Claims
1. A first functional layer; an ultraviolet absorbing layer located on a first surface of the first functional layer; A transparent substrate located on the second surface of the first functional layer; Equipped with The ultraviolet absorbing layer is an active energy ray-curable resin; An ultraviolet absorber, the active energy ray-curable resin contains a copolymer of a structural unit represented by the following formula (i) and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit, The ultraviolet ray shielding rate measured in accordance with JIS L1925 is 90% or more, and the pencil hardness of the surface on the first side under a load of 500 g is H or more. Optical film. 【Chemistry 1】 [In formula (i), R 1 represents a hydrogen atom, a halogen atom, a carboxyl group, a sulfo group, a cyano group, a hydroxy group, an alkyl group having 10 or less carbon atoms, an alkoxycarbonyl group having 10 or less carbon atoms, an alkylsulfonylaminocarbonyl group having 10 or less carbon atoms, an arylsulfonylaminocarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, an acylaminosulfonyl group having 10 or less carbon atoms, an alkoxy group having 10 or less carbon atoms, an alkylthio group having 10 or less carbon atoms, an aryloxy group having 10 or less carbon atoms, a nitro group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an acyloxy group having 10 or less carbon atoms, an acyl group having 10 or less carbon atoms, a carbamoyl group, a sulfamoyl group, an aryl group having 10 or less carbon atoms, a substituted amino group, a substituted ureido group, a substituted phosphono group, or a heterocyclic group; R 2 represents a hydrogen atom or an alkyl group having 30 or less carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or less carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by combining these, any of which may contain a spirodioxane ring.
2. The ultraviolet absorbing layer has one or more functions of antistatic property, antifouling property, and antiglare property. The optical film according to claim 1 .
3. Further comprising a second functional layer provided on the first surface side of the first functional layer and having a function different from that of the first functional layer. The optical film according to claim 1 .
4. The second functional layer has at least one of an anti-reflection function and an anti-glare function. The optical film according to claim 3 .
5. The second functional layer is an antistatic layer or an antifouling layer. The optical film according to claim 3 .
6. The second functional layer has an oxygen permeability of 10 cm 3 / (m 2 .day.atm) or less of oxygen barrier layer, The optical film according to claim 3 .
7. the first functional layer contains at least one of a first color material, a second color material, and a third color material; the first coloring material has an absorption maximum wavelength in the range of 470 to 530 nm and a half-width of an absorption spectrum of 15 to 45 nm; the second coloring material has an absorption maximum wavelength in the range of 560 to 620 nm and a half-width of an absorption spectrum of 15 to 55 nm; the third coloring material has a wavelength having the lowest transmittance in the range of 380 to 780 nm, the wavelength being in the range of 650 to 780 nm; The optical film according to claim 1 .
8. the first functional layer contains a copolymer of a structural unit represented by formula (i) and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit; The optical film according to claim 7.
9. The first functional layer contains at least one of a radical scavenger, a peroxide decomposer, and a singlet oxygen quencher; The optical film according to claim 7.
10. The singlet oxygen quencher contains any one of dialkyl phosphate, dialkyl dithiocarbamate, benzene dithiol, and transition metal complexes thereof; The optical film according to claim 9 .
11. At least one of the first color material, the second color material, and the third color material contained in the first functional layer contains at least one compound selected from the group consisting of compounds having any one of a porphyrin structure, a merocyanine structure, a phthalocyanine structure, an azo structure, a cyanine structure, a squarylium structure, a coumarin structure, a polyene structure, a quinone structure, a tetradiporphyrin structure, a pyrromethene structure, and an indigo structure, and metal complexes thereof; The optical film according to claim 7.
12. The optical film according to any one of claims 1 to 11, Display device.
13. Contains an ultraviolet absorber, an active energy ray curable resin, a photopolymerization initiator, and a solvent; The active energy ray-curable resin contains a copolymer of a structural unit represented by formula (i) and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit, When a film having a thickness of 5 μm is formed, the film has an ultraviolet ray shielding rate of 90% or more as measured in accordance with the method described in JIS L1925. A composition for forming an ultraviolet absorbing layer. 【Chemistry 2】 [In formula (i), R 1 represents a hydrogen atom, a halogen atom, a carboxyl group, a sulfo group, a cyano group, a hydroxy group, an alkyl group having 10 or less carbon atoms, an alkoxycarbonyl group having 10 or less carbon atoms, an alkylsulfonylaminocarbonyl group having 10 or less carbon atoms, an arylsulfonylaminocarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, an acylaminosulfonyl group having 10 or less carbon atoms, an alkoxy group having 10 or less carbon atoms, an alkylthio group having 10 or less carbon atoms, an aryloxy group having 10 or less carbon atoms, a nitro group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an acyloxy group having 10 or less carbon atoms, an acyl group having 10 or less carbon atoms, a carbamoyl group, a sulfamoyl group, an aryl group having 10 or less carbon atoms, a substituted amino group, a substituted ureido group, a substituted phosphono group, or a heterocyclic group; R 2 represents a hydrogen atom or an alkyl group having 30 or less carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or less carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by combining these, any of which may contain a spirodioxane ring.
Citation Information
Patent Citations
Ultraviolet-curable resin raw material composition, resin molding surface-modified therewith, and production of the molding
JP1997157315A
Hard coating film and laminate
WO2019065833A1
Cited By
Optical laminate and display device using same