Post-treatment technique for trivalent chromium plating film
The use of an aqueous solution with hydrogen peroxide and phosphorus compounds in cathodic electrolytic treatment addresses the corrosion resistance and color stability issues of trivalent chromium plating films, providing improved corrosion resistance and minimal color change.
Patent Information
- Application Number
- JP2023070823
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2043-04-24
Smart Images

Figure 2024156398000001 
Figure 2024156398000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a post-treatment technique for trivalent chromium plating film. [Background technology]
[0002] Chrome plating is used to provide excellent appearance and corrosion resistance as a final surface treatment for the interior and exterior parts of automobiles, plumbing parts, etc. Conventional chrome plating generally uses hexavalent chromium, but in recent years, the use of hexavalent chromium has begun to be restricted due to its harmful effects on the working environment.
[0003] Therefore, trivalent chromium plating has been developed as an alternative to hexavalent chromium plating. Depending on the bath composition, it is possible to obtain a film with a dark color tone (L* value of 70 or less in the L*a*b* color system) that cannot be obtained with hexavalent chromium plating, so trivalent chromium plating is currently widespread, especially for dark colors. However, trivalent chromium plating has inferior corrosion resistance compared to hexavalent chromium plating.
[0004] Therefore, in order to meet the strict standards for corrosion resistance, it is currently common to perform electrolytic chromating using hexavalent chromium as a post-treatment for trivalent chromium plating. Therefore, in reality, there is no process that does not use hexavalent chromium, and research is being conducted on post-treatment agents that do not use hexavalent chromium. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2005-097701 A Summary of the Invention [Problem to be solved by the invention]
[0006] Recently, there have been an increasing number of reports on various types of hexavalent chromium-free post-treatments, and products are also being developed. However, the actual corrosion resistance is not as good as that of hexavalent chromium electrolytic chromate, and the effect on corrosion resistance is particularly weak on dark-toned trivalent chromium plating films. Another issue is that the color tone changes due to post-treatment (especially the increase in the b* value in the L*a*b* color system) regardless of whether hexavalent chromium is present or not.
[0007] Patent Document 1 discloses a rust inhibitor that contains a phosphate, an oxidizing agent, and a nonionic surfactant, with the remainder being water. However, this rust inhibitor is insufficient in improving corrosion resistance.
[0008] An object of the present invention is to provide a technique for improving the corrosion resistance of trivalent chromium plating films while suppressing color change. [Means for solving the problem]
[0009] In view of the above problems, the present inventors have conducted intensive research and found that the above problems can be solved by an aqueous solution for cathodic electrolytic treatment of trivalent chromium plating films, which contains hydrogen peroxide and a phosphorus compound. Based on this finding, the present inventors have conducted further research and completed the present invention. That is, the present invention includes the following aspects.
[0010] Item 1. An aqueous solution containing hydrogen peroxide and a phosphorus compound for use in cathodic electrolytic treatment of trivalent chromium plating films.
[0011] Item 2. The aqueous solution according to Item 1, having a pH of 1.5 to 5.5.
[0012] Item 3. The aqueous solution according to Item 1, wherein the hydrogen peroxide content is 1 g / L or more.
[0013] Item 4. The aqueous solution according to Item 1, wherein the content of the phosphorus compound is 1 g / L or more.
[0014] Item 5. The aqueous solution according to Item 1, wherein the content of the hydrogen peroxide is 1 to 500 g / L and the content of the phosphorus compound is 1 to 200 g / L.
[0015] Item 6. The aqueous solution according to Item 1, wherein the phosphorus compound is at least one selected from the group consisting of phosphoric acid, dipotassium hydrogen phosphate, disodium hydrogen phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate, pyrophosphoric acid and salts thereof, tripolyphosphoric acid and salts thereof, etidronic acid and salts thereof, and aminotrimethylenephosphonic acid and salts thereof.
[0016] Item 7. A method for producing a corrosion-resistant trivalent chromium plating film, comprising cathodic electrolysis of a trivalent chromium plating film in the aqueous solution according to any one of Items 1 to 6.
[0017] Item 8. Cathode current density is 0.01 to 3 A / dm 2 Item 8. The method for producing according to Item 7,
[0018] Item 9. The method according to item 7, wherein the current application time is 30 to 1000 seconds.
[0019] Item 10. The method according to Item 7, wherein the bath temperature during cathodic electrolysis is 10 to 50°C.
[0020] Item 11. A method for post-treatment of a trivalent chromium plating film, comprising cathodic electrolysis of the trivalent chromium plating film in the aqueous solution according to any one of Items 1 to 6.
[0021] Item 12. A corrosion-resistant trivalent chromium plating film obtained by the manufacturing method according to item 7.
[0022] Item 13. An article comprising the corrosion-resistant chromium plating film according to item 12. Effect of the Invention
[0023] According to the present invention, it is possible to provide a technique for improving the corrosion resistance of a trivalent chromium plating film while suppressing color change. More specifically, according to the present invention, it is possible to provide an aqueous solution for use in cathodic electrolytic treatment of a trivalent chromium plating film, a method for producing a corrosion-resistant trivalent chromium plating film, a method for post-treatment of a trivalent chromium plating film, a corrosion-resistant trivalent chromium plating film, an article including the corrosion-resistant trivalent chromium plating film, and the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] In this specification, the expressions "contain" and "comprise" include the concepts of "contain", "include", "consist essentially of" and "consist only of".
[0025] 1.Aqueous solution In one aspect, the present invention relates to an aqueous solution for use in cathodic electrolytic treatment of a trivalent chromium plating film, the aqueous solution containing hydrogen peroxide and a phosphorus compound (also referred to as the "aqueous solution of the present invention" in this specification).
[0026] Hydrogen peroxide acts as an oxidizing agent in the aqueous solution of the present invention. Hydrogen peroxide can form an oxide film and / or a phosphate film together with phosphorus on the trivalent chromium plating film. Depending on the anode material, hydrogen peroxide can also suppress the dissolution of the anode.
[0027] The content of hydrogen peroxide is not particularly limited, but from the viewpoint of improving corrosion resistance and suppressing dissolution of the anode, it is preferably 1 g / L or more, more preferably 2 g / L or more, even more preferably 5 g / L or more, even more preferably 7 g / L or more, and particularly preferably 10 g / L or more. The upper limit of the content of hydrogen peroxide is not particularly limited, and is, for example, 500 g / L. From the viewpoint of cost, the upper limit is preferably 300 g / L, more preferably 200 g / L, even more preferably 150 g / L or more, and even more preferably 120 g / L. The range of the content of hydrogen peroxide can be any combination of the above lower limit and the above upper limit, and is, for example, 1 to 500 g / L, preferably 2 to 300 g / L, more preferably 5 to 200 g / L, and even more preferably 5 to 150 g / L.
[0028] The phosphorus compound can form a phosphate film on the outermost layer of the film formed on the trivalent chromium plating film, and can also suppress the decomposition of hydrogen peroxide.
[0029] The phosphorus compound is not particularly limited as long as it is a compound containing phosphorus, and any inorganic compound or organic compound that can be added to a plating post-treatment can be used. Preferred examples of inorganic phosphorus compounds include phosphoric acid, dipotassium hydrogen phosphate, disodium hydrogen phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate, pyrophosphoric acid and its salts (e.g., potassium pyrophosphate, sodium pyrophosphate, etc.), tripolyphosphoric acid and its salts (e.g., potassium tripolyphosphate, sodium tripolyphosphate, etc.), etc. Preferred examples of organic phosphorus compounds include etidronic acid and its salts, aminotrimethylenephosphonic acid and its salts, etc.
[0030] The phosphorus compounds may be used alone or in combination of two or more.
[0031] The content of the phosphorus compound is not particularly limited, but from the viewpoint of improving corrosion resistance, suppressing consumption of hydrogen peroxide, etc., it is preferably 1 g / L or more, more preferably 2 g / L or more, even more preferably 3 g / L or more, even more preferably 5 g / L or more, particularly preferably 7 g / L or more, and particularly preferably 10 g / L or more. The upper limit of the content of the phosphorus compound is not particularly limited, and is, for example, 200 g / L. From the viewpoint of suppressing attack on the anode, facilitating waste liquid treatment, etc., the upper limit is preferably 150 g / L, more preferably 100 g / L, and even more preferably 60 g / L, more preferably 80 g / L. The range of the content of the phosphorus compound can be any combination of the above lower limit and the above upper limit, and is, for example, 1 to 200 g / L, preferably 2 to 150 g / L, more preferably 3 to 100 g / L, and even more preferably 5 to 80 g / L.
[0032] By combining hydrogen peroxide and a phosphorus compound, the aqueous solution of the present invention can be subjected to cathodic electrolytic treatment described below, thereby making it possible to further improve the corrosion resistance of a trivalent chromium plating film while further suppressing color change.
[0033] The pH of the aqueous solution of the present invention is preferably 1.5 or more from the viewpoint of corrosion resistance. Also, the pH is preferably 5.5 or less from the viewpoint of inhibiting decomposition of hydrogen peroxide. From the above two viewpoints, the pH is preferably 1.5 to 5.5, more preferably 2.0 to 5.0.
[0034] The aqueous solution of the present invention may contain, for example, an organic acid for the purpose of functioning as a buffer. Preferred examples of the organic acid include citric acid, succinic acid, acetic acid, formic acid, and oxalic acid.
[0035] The organic acids can be used alone or in combination of two or more.
[0036] The content of the organic acid is, for example, 0 to 100 g / L, preferably 0 to 30 g / L.
[0037] The aqueous solution of the present invention can improve corrosion resistance without relying on metals. From this viewpoint, the content of metal ions in the aqueous solution of the present invention is, for example, 0 to 0.5 g / L, preferably 0 to 0.2 g / L, more preferably 0 to 0.1 g / L, even more preferably 0 to 0.01 g / L, still more preferably 0 to 0.001 g / L, and particularly preferably 0 g / L.
[0038] The aqueous solution of the present invention can improve corrosion resistance without relying on hexavalent chromium. From this viewpoint, the content of hexavalent chromium ions in the aqueous solution of the present invention is, for example, 0 to 0.1 g / L, preferably 0 to 0.05 g / L, more preferably 0 to 0.02 g / L, even more preferably 0 to 0.01 g / L, still more preferably 0 to 0.001 g / L, and particularly preferably 0 g / L.
[0039] The aqueous solution of the present invention is used for cathodic electrolysis of trivalent chromium plating film. Based on the new knowledge that the use of the aqueous solution of the present invention for cathodic electrolysis of trivalent chromium plating film can improve the corrosion resistance while suppressing the color change of the trivalent chromium plating film, the present inventors have found that the aqueous solution of the present invention is suitable for the above-mentioned use.
[0040] Therefore, in one aspect, the present invention relates to a method for producing a corrosion-resistant trivalent chromium plating film, which comprises cathodic electrolysis of a trivalent chromium plating film in the aqueous solution of the present invention, and a method for post-treatment of a trivalent chromium plating film, which comprises cathodic electrolysis of a trivalent chromium plating film in the aqueous solution of the present invention. These two methods are sometimes collectively referred to as the "method of the present invention."
[0041] The trivalent chromium plating film is a plating film obtained by a plating solution containing trivalent chromium ions, and is not particularly limited as long as it is a plating film mainly containing chromium as a metal, and includes so-called trivalent chromium alloy plating. In one aspect of the present invention, the chromium content in the trivalent chromium plating film can be, for example, 1 at% or more, 2 at% or more, 5 at% or more, 10 at% or more, 20 at% or more, 30 at% or more, 40 at% or more, or 45 at% or more, and can be 100 at% or less, 90 at% or less, 80 at% or less, 70 at% or less, 60 at% or less, or 50 at% or less, relative to 100 at% (atomic percent) of the metal. The upper and lower limits can be arbitrarily combined. The content can be measured by energy dispersive X-ray analysis (EDX). Examples of metals other than chromium in the trivalent chromium plating film include Co, Fe, Mn, Ni, Zn, and the like.
[0042] The plating solution for forming a trivalent chromium plating film preferably has a lower content of hexavalent chromium ions, and the content is, for example, 0 to 0.1 g / L, preferably 0 to 0.05 g / L, more preferably 0 to 0.02 g / L, even more preferably 0 to 0.01 g / L, still more preferably 0 to 0.001 g / L, and particularly preferably 0 g / L.
[0043] The trivalent chromium plating film can be either white (L* value of 70 or more in the L*a*b* color system) or black (L* value of 70 or less in the L*a*b* color system). According to the method of the present invention, a better effect on corrosion resistance can be exhibited even for black trivalent chromium plating films, for which the effect of improving corrosion resistance by conventional hexavalent chromium-free post-treatments is limited.
[0044] The objects on which the trivalent chromium plating film is formed are not particularly limited, and examples thereof include automobile parts, molding dies, various machine parts that are subject to wear, tools, rolls used in printing, papermaking, rolling, film processing, and steelmaking, plumbing fixtures, bicycle parts, fishing tackle, mobile phones, cameras, ornaments, miscellaneous goods, etc.
[0045] The trivalent chromium plating film can be formed according to or in accordance with a known method.
[0046] Cathodic electrolysis of a trivalent chromium plating film is carried out by immersing a trivalent chromium plating film as a cathode and an anode in the aqueous solution of the present invention, and performing electrolysis.
[0047] The anode is not particularly limited, and various insoluble or soluble anodes can be used.
[0048] Examples of insoluble anodes include carbon, Ti / Pt (Ti with a platinum-based coating), Ti / Ir oxide (Ti with an Ir oxide coating), Ti / Ru oxide (Ti with a Ru oxide coating), Ti / Ir oxide-Ru oxide (Ti with a mixed Ir oxide and Ru oxide coating), Ti / Ir oxide-Ta oxide (Ti with a mixed Ir oxide and Ta oxide coating), Ti / Pt / Ir oxide-Ru oxide (Ti / Pt with Ir oxide and Ta oxide coating), Examples of suitable electrodes include electrodes made of a mixture of Ru oxide and Ru oxide, Ti / Pt / Ir oxide-Ta oxide (Ti / Pt coated with a mixture of Ir oxide and Ta oxide), stainless steel, aluminum, lead alloys (Pb-Sn alloy, Pb-Ag alloy, Pb-Sb alloy), lead oxides (lead monoxide, lead dioxide, lead trioxide, trilead tetroxide), lead, tin oxide, carbon, diamond electrodes (diamond containing nitrogen or boron coated on a substrate such as silicon or niobium), and ITO electrodes (indium tin electrodes).
[0049] Soluble anodes include, for example, nickel, tin, cobalt, iron, and the like.
[0050] The anode is preferably made of nickel or stainless steel.
[0051] The bath temperature in the cathodic electrolysis is not particularly limited, but is preferably 10 to 50°C, more preferably 15 to 35°C, from the viewpoint of suppressing the decomposition of hydrogen peroxide, etc.
[0052] The cathode current density is not particularly limited, but from the viewpoint of improving corrosion resistance, anodic dissolution, etc., it is preferably 0.01 to 3 A / dm 2 , more preferably 0.1 to 1.5 A / dm 2 It is.
[0053] The current application time is not particularly limited, but from the viewpoints of improving corrosion resistance, cost, etc., it is preferably 30 to 1000 seconds, more preferably 60 to 600 seconds.
[0054] The method of the present invention provides a corrosion-resistant trivalent chromium plating film and an article including the corrosion-resistant trivalent chromium plating film. EXAMPLES
[0055] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples.
[0056] Test example 1. Post-treatment test of trivalent chromium plating film <Test Example 1-1. Formation of trivalent chromium plating film> On a 5cm x 10cm resin plate, a 20μm thick copper plating film, an 8μm thick semi-gloss Ni plating film, a 6μm thick gloss Ni plating film, and a 2μm thick microporous Ni plating film were formed in this order. Furthermore, a white trivalent chromium plating film or a black trivalent chromium plating film was formed on the outermost microporous Ni plating film. The white trivalent chromium plating film was formed using Top Fine Chrome (manufactured by Okuno Pharmaceutical Industries Co., Ltd.) as the plating solution, and the black trivalent chromium plating film was formed using Top Farbe BLB Plus (manufactured by Okuno Pharmaceutical Industries Co., Ltd.) as the plating solution.
[0057] <Test Example 1-2. Post-treatment of trivalent chromium plating film> Comparative Example 1 No post-treatment was performed on the trivalent chromium plating film obtained in Test Example 1-1.
[0058] Comparative Example 2 The trivalent chromium plating film obtained in Test Example 1-1 was immersed in a treatment solution (ECB-Y, manufactured by Okuno Chemical Industries, pH 3.5) and subjected to hexavalent chromium electrolytic chromate treatment (conditions: cathode current density 0.5 A / dm 2 The test was performed under the conditions of 1 min current application and 25°C bath temperature.
[0059] Comparative Example 3 The trivalent chromium plating film obtained in Test Example 1-1 was immersed in a treatment solution (Eleup CCS, manufactured by Okuno Chemical Industries, pH 3.5) and subjected to trivalent chromium electrolytic chromate treatment (conditions: cathode current density 0.5 A / dm 2 The test was performed under the conditions of 1 min current application and 25°C bath temperature.
[0060] Comparative Example 4 The trivalent chromium plating film obtained in Test Example 1-1 was immersed in a treatment solution (aqueous solution containing 20 g / L of hydrogen peroxide and 40 g / L of disodium hydrogen phosphate, pH 4.0) and left to stand for 5 minutes (bath temperature 25°C) without electrolytic treatment.
[0061] Comparative Example 5 The trivalent chromium plating film obtained in Test Example 1-1 was immersed in a treatment solution (aqueous solution containing 60 g / L of dipotassium hydrogen phosphate, not containing hydrogen peroxide, pH 4.0) and subjected to cathodic electrolysis of the plating film (conditions: cathodic current density 0.5 A / dm 2 The test was performed under the conditions of 25°C bath temperature and 3 minutes current application time.
[0062] Comparative Example 6 The trivalent chromium plating film obtained in Test Example 1-1 was immersed in a treatment solution (aqueous solution containing 20 g / L of hydrogen peroxide and no phosphorus compounds, pH 4.0) and subjected to cathodic electrolysis of the plating film (conditions: cathodic current density 0.5 A / dm 2 The test was performed under the conditions of 25°C bath temperature and 3 minutes current application time.
[0063] Example 1 The trivalent chromium plating film obtained in Test Example 1-1 was immersed in a treatment solution (aqueous solution containing 10 g / L of hydrogen peroxide and 30 g / L of sodium pyrophosphate, pH 4.0) and subjected to cathodic electrolysis of the plating film (conditions: cathodic current density 0.5 A / dm 2The test was performed under the conditions of 25°C bath temperature and 3 minutes current application time.
[0064] Example 2 The trivalent chromium plating film obtained in Test Example 1-1 was immersed in a treatment solution (aqueous solution containing 30 g / L of hydrogen peroxide and 50 g / L of potassium dihydrogen phosphate, pH 3.5) and subjected to cathodic electrolysis of the plating film (conditions: cathodic current density 0.2 A / dm 2 The test was performed under the conditions of 5 minutes of current application and 30°C bath temperature.
[0065] Example 3 The trivalent chromium plating film obtained in Test Example 1-1 was immersed in a treatment solution (aqueous solution containing 100 g / L of hydrogen peroxide and 10 g / L of etidronic acid, pH 4.5) and subjected to cathodic electrolysis of the plating film (conditions: cathodic current density 1 A / dm 2 The test was performed under the conditions of 2 minutes of current application and 20°C bath temperature.
[0066] Example 4 The trivalent chromium plating film obtained in Test Example 1-1 was immersed in a treatment solution (aqueous solution containing 80 g / L of hydrogen peroxide and 20 g / L of sodium tripolyphosphate, pH 3.0) and subjected to cathodic electrolysis of the plating film (conditions: cathodic current density 0.3 A / dm 2 The test was performed under the conditions of 10 minutes of current application and 35°C bath temperature.
[0067] Example 5 The trivalent chromium plating film obtained in Test Example 1-1 was immersed in a treatment solution (aqueous solution containing 50 g / L of hydrogen peroxide and 35 g / L of disodium hydrogen phosphate, pH 2.0) and subjected to cathodic electrolysis of the plating film (conditions: cathodic current density 0.1 A / dm 2 The test was performed under the conditions of 8 minutes of current application and 40°C bath temperature.
[0068] Example 6 The trivalent chromium plating film obtained in Test Example 1-1 was immersed in a treatment solution (aqueous solution containing 150 g / L of hydrogen peroxide and 55 g / L of sodium dihydrogen phosphate, pH 5.0) and subjected to cathodic electrolysis of the plating film (conditions: cathodic current density 1.5 A / dm 2 The test was performed under the conditions of 4 minutes of current application and 15°C bath temperature.
[0069] <Test Example 1-3. Corrosion resistance evaluation> The corrosion resistance of the plating film (test piece) after post-treatment obtained in Test Example 1-2 was evaluated by CASS test. Specifically, the test piece was placed in a test tank at 50°C, and a solution containing 50g / L of sodium chloride and 0.205g / L of copper chloride and adjusted to pH 3.0 with acetic acid was sprayed onto it, and the degree of corrosion was checked at regular intervals. Evaluation was performed according to the following evaluation criteria. ○: The corroded area of the test piece 48 hours after the start of the test is less than 1%. △: The corroded area of the test piece 48 hours after the start of the test was 1% or more and less than 10%. ×: The corroded area of the test piece 48 hours after the start of the test is 10% or more.
[0070] <Test Example 1-4. Evaluation of color change> The color of the surface of the trivalent chromium plating film obtained in Test Example 1-1 and the surface of the plating film after post-treatment obtained in Test Example 1-2 were measured with a color difference meter (product name: CM-3700A, manufactured by Konica Minolta, Inc., measurement conditions: SCI). The change in b* value before and after post-treatment in the L*a*b* color system (= b* value of the plating film after post-treatment obtained in Test Example 1-2 - b* value of the trivalent chromium plating film obtained in Test Example 1-1) was calculated and evaluated according to the following evaluation criteria. The L* value of the surface of the trivalent chromium plating film obtained in Test Example 1-1 was 83.5 for the white system and 58.4 for the black system. ○: The change in b* value before and after post-processing is less than 0.1. △: The change in b* value before and after post-processing is 0.1 or more and less than 0.3. ×: The change in b* value before and after post-processing is 0.3 or more.
[0071] <Result> The results are shown in Tables 1 and 2.
[0072] [Table 1]
[0073] [Table 2]
[0074] It has been found that cathodic electrolytic treatment of trivalent chromium plating film in an aqueous solution containing hydrogen peroxide and a phosphorus compound can improve corrosion resistance while further suppressing color change.
Claims
1. An aqueous solution containing hydrogen peroxide and a phosphorus compound for use in cathodic electrolysis of trivalent chromium plating films.
2. 2. The aqueous solution according to claim 1, having a pH of 1.5 to 5.
5.
3. 2. The aqueous solution according to claim 1, wherein the hydrogen peroxide content is 1 g / L or more.
4. 2. The aqueous solution according to claim 1, wherein the content of the phosphorus compound is 1 g / L or more.
5. 2. The aqueous solution according to claim 1, wherein the content of the hydrogen peroxide is 1 to 500 g / L and the content of the phosphorus compound is 1 to 200 g / L.
6. 2. The aqueous solution according to claim 1, wherein the phosphorus compound is at least one selected from the group consisting of phosphoric acid, dipotassium hydrogen phosphate, disodium hydrogen phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate, pyrophosphoric acid and its salts, tripolyphosphoric acid and its salts, etidronic acid and its salts, and aminotrimethylenephosphonic acid and its salts.
7. A method for producing a corrosion-resistant trivalent chromium plating film, comprising cathodic electrolysis of a trivalent chromium plating film in the aqueous solution according to any one of claims 1 to 6.
8. Cathode current density is 0.01 to 3 A / dm 2 The method according to claim 7, wherein
9. The method according to claim 7, wherein the current application time is 30 to 1000 seconds.
10. The method according to claim 7, wherein the bath temperature during cathodic electrolysis is 10 to 50°C.
11. A method for post-treatment of a trivalent chromium plating film, comprising cathodic electrolysis of the trivalent chromium plating film in the aqueous solution according to any one of claims 1 to 6.
12. A corrosion-resistant trivalent chromium plating film obtained by the manufacturing method according to claim 7.
13. 13. An article comprising the corrosion-resistant chromium plating film of claim 12.
Citation Information
Patent Citations
Antirust
JP2005097701A
Chromium plated product, and production method and testing method therefor
JP2005232529A
Method for manufacturing tin-plated steel sheet
JP2008111155A
Chrome finish surface treatment method
JP2019529715A
Method for improving corrosion resistance by electrolytic passivation of outermost chromium layer or outermost chromium alloy layer
JP2020506292A