Flux, solder paste, and method for producing conjugant

A flux composition with triol solvent and monoamide thixotropic agent addresses void generation in soldering, improving bonding quality and thermal conductivity in power semiconductor packaging.

JP2024156522APending Publication Date: 2024-11-06SENJU METAL IND CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023071059
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-06

AI Technical Summary

Technical Problem

In the packaging of power semiconductors, the generation of voids during soldering is a significant challenge, particularly due to the incorporation of gasified flux components into molten solder, which affects bonding quality and thermal conductivity.

Method used

A flux composition containing a triol solvent, monoamide thixotropic agent, and specific solvents is used, with controlled proportions to enhance thixotropy and suppress void generation, suitable for reflow soldering in a reducing gas atmosphere.

Benefits of technology

The proposed flux composition significantly reduces void formation during soldering, improves thixotropy, and minimizes residue, enhancing the bonding process and thermal conductivity of soldered components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156522000005
    Figure 2024156522000005
  • Figure 2024156522000006
    Figure 2024156522000006
  • Figure 2024156522000001
    Figure 2024156522000001
Patent Text Reader

Abstract

To provide a flux that suppresses the generation of voids during soldering, a solder paste, and a method for producing a conjugant.SOLUTION: This flux contains: a triol solvent (S1); a monoamide thixotropic agent; and at least one type of solvent (S2) selected from the group consisting of a monovalent solvent and a divalent solvent. A content of the monoamide thixotropic agent is 0.5-15 mass% of a total mass of the flux, and a content of the solvent (S2) is 50 mass% or more of the total mass of the flux. The method for producing the conjugant comprises a step of providing the conjugant by soldering components and a substrate. During the soldering, reflowing is performed in a reductive gas atmosphere by using solder paste containing solder alloy powder and the flux of the present invention.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a flux, a solder paste, and a method for producing a joint. [Background technology]

[0002] In manufacturing electronic components, components are fixed to a substrate and electrically connected to the substrate by soldering, which uses flux, solder powder, and a solder paste made of a mixture of flux and solder powder. Flux has the effect of chemically removing metal oxides that exist in the solder and in the metal surface of the objects to be soldered, enabling the movement of metal elements at the interface between the two. Therefore, by using flux for soldering, an intermetallic compound is formed between the two, resulting in a strong bond.

[0003] In soldering using solder paste, the solder paste is first printed on a board, components are then mounted on the board, and the board with the components mounted is heated in a heating furnace called a reflow furnace. This melts the solder powder contained in the solder paste, and the components are soldered to the board. The flux used in this reflow soldering generally contains a resin component, a solvent, an activator, a thixotropic agent, etc.

[0004] In the packaging of power semiconductors that control large currents, solder materials are used in die bonding portions and heat sink bonding portions. Such packaging applications require bonding that suppresses the generation of voids. It is believed that the cause of voids that occur during reflow soldering is the phenomenon in which gasified flux components are incorporated into the molten solder. As a method for satisfying such requirements, there is a method of performing reflow in a reducing gas atmosphere such as formic acid. By performing reflow in a reducing gas atmosphere, a fluxless method can be realized by making the reducing gas itself act as a flux, and the cause of voids can be eliminated. In addition, in the reflow in a reducing gas atmosphere, since the reducing gas itself does not remain as a residue, a cleaning-less joining process can be realized.

[0005] In the fluxless method, it is assumed that a solder preform is used as a solder material, but on the other hand, from the viewpoint of ease of handling by users and automation, there is a demand for using a solder paste even in the reflow process performed in a reducing gas atmosphere. For example, Patent Document 1 proposes a method for producing a soldered product in which reflow soldering is performed in a reducing atmosphere containing a reducing gas, and a solder paste used therefor. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 6706000 Summary of the Invention [Problem to be solved by the invention]

[0007] In the packaging of power semiconductors, mainly from the viewpoint of heat dissipation, bonding that suppresses the occurrence of voids to an extremely high degree is required. The present invention has been made in view of the above circumstances, and provides a flux, a solder paste, and a method for producing a joint body in which the generation of voids during soldering is further suppressed. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention employs the following configuration.

[0009] [1] A flux containing a triol solvent (S1), a monoamide-based thixotropic agent, and at least one solvent (S2) selected from the group consisting of monohydric solvents and dihydric solvents, wherein the content of the monoamide-based thixotropic agent is 0.5 mass% or more and less than 15 mass% with respect to the total mass of the flux, and the content of the solvent (S2) is 50 mass% or more with respect to the total mass of the flux.

[0010] [2] The flux according to [1], wherein the content of the triol solvent (S1) is 1 mass % or more and 15 mass % or less based on the total mass of the flux.

[0011] [3] The flux according to [1] or [2], wherein the triol solvent (S1) is a triol compound in which three hydroxy groups are bonded to a chain hydrocarbon group having 3 to 6 carbon atoms. [4] The flux according to [3], wherein the triol solvent (S1) is at least one selected from the group consisting of 3-methylbutane-1,2,3-triol, 2-methylbutane-1,2,4-triol, 1,2,6-hexanetriol, glycerin, and 1,2,4-butanetriol.

[0012] [5] The flux according to [4], wherein the triol solvent (S1) is a combination of a first triol solvent selected from the group consisting of 3-methylbutane-1,2,3-triol and 2-methylbutane-1,2,4-triol, and a second triol solvent selected from the group consisting of 1,2,6-hexanetriol, glycerin, and 1,2,4-butanetriol. [6] The flux according to [5], wherein a mixing ratio of the first triol solvent to the second triol solvent is 1 to 10, expressed as a mass ratio of the first triol solvent / the second triol solvent.

[0013] [7] The flux according to any one of [1] to [6], wherein the solvent (S2) contains the monovalent solvent. [8] The flux according to [7], wherein the monohydric solvent is a branched aliphatic monohydric alcohol having 16 to 20 carbon atoms.

[0014] [9] The flux according to any one of [1] to [8], wherein a mixing ratio of the solvent (S2) to the triol solvent (S1) is 7 to 31 as a mass ratio expressed as solvent (S2) / triol solvent (S1).

[0015]

[10] The flux according to any one of [1] to [9], wherein the monoamide-based thixotropic agent is a combination of an aromatic amide and a fatty acid amide.

[0016]

[11] The flux according to any one of [1] to

[10] , further comprising an activator, the content of the activator being more than 0 mass % and 5 mass % or less with respect to the total mass of the flux.

[0017]

[12] The flux according to any one of [1] to

[11] , which does not contain a rosin-based resin.

[13] The flux according to any one of [1] to

[10] and

[12] , which does not contain an activator.

[0018]

[14] A solder paste comprising a solder alloy powder and the flux according to any one of [1] to

[13] .

[0019]

[15] A method for producing a bonded body, comprising: a step of obtaining a bonded body by soldering a component and a substrate, wherein the soldering is performed by reflow in a reducing gas atmosphere using the solder paste according to

[14] . Effect of the Invention

[0020] According to the present invention, it is possible to provide a flux in which the generation of voids during soldering is further suppressed, a solder paste using the flux, and a method for producing a bonded body using the solder paste. [Brief description of the drawings]

[0021] [Figure 1] FIG. 13 is a diagram showing a reflow profile in the evaluation of the void generation suppression ability. [Diagram 2] FIG. 1 is a schematic diagram showing pattern holes of I in the evaluation of heat sagging suppression ability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] (Flux) One embodiment of the flux according to the first aspect contains a triol solvent (S1), a monoamide-based thixotropic agent, and at least one solvent (S2) selected from the group consisting of monohydric solvents and dihydric solvents. In the flux of this embodiment, the content of the monoamide-based thixotropic agent is 0.5 mass% or more and less than 15 mass% with respect to the total mass of the flux, and the content of the solvent (S2) is 50 mass% or more with respect to the total mass of the flux. The flux of this embodiment is suitable for use in reflow soldering, and is capable of further suppressing the occurrence of voids compared to conventional fluxes.

[0023] <Triol Solvent (S1)> In the flux of the present embodiment, the triol solvent is contained, so that the occurrence of voids during soldering is further suppressed. The term "triol solvent" refers to a solvent having three hydroxy groups. An example of the triol solvent is a triol compound having three hydroxy groups and a boiling point of 170 to 330° C. Alternatively, an example of the triol solvent is a triol compound in which three hydroxy groups are bonded to a chain hydrocarbon group, and a preferred example is a triol compound in which three hydroxy groups are bonded to a chain hydrocarbon group having 3 to 6 carbon atoms. This chain hydrocarbon group may be either linear or branched, with branched groups being preferred.

[0024] Specific examples of triol solvents include 3-methylbutane-1,2,3-triol, 2-methylbutane-1,2,4-triol, 1,2,6-hexanetriol, glycerin, 1,2,4-butanetriol, and 1,2,3-butanetriol.

[0025] The triol solvent may be used alone or in combination of two or more. Among the above, the triol solvent is preferably a triol compound having three hydroxy groups bonded to a chain hydrocarbon group having 3 to 6 carbon atoms, from the viewpoint of easily enhancing the ability to suppress the generation of voids, more preferably at least one selected from the group consisting of 3-methylbutane-1,2,3-triol, 2-methylbutane-1,2,4-triol, 1,2,6-hexanetriol, glycerin and 1,2,4-butanetriol, and even more preferably includes at least one selected from the group consisting of 3-methylbutane-1,2,3-triol and 2-methylbutane-1,2,4-triol. Alternatively, among the above, at least one triol solvent selected from the group consisting of 1,2,6-hexanetriol, glycerin, and 1,2,4-butanetriol is more preferable, since it is likely to increase the thixotropy of the solder paste and to improve the ability to suppress heat dripping when made into a solder paste.

[0026] In addition to suppressing the generation of voids, the triol solvent is likely to increase the thixotropy of the solder paste and is likely to improve the ability to suppress heat dripping when made into a solder paste. Therefore, it is preferable that the triol solvent is a combination of a first triol solvent selected from the group consisting of 3-methylbutane-1,2,3-triol and 2-methylbutane-1,2,4-triol and a second triol solvent selected from the group consisting of 1,2,6-hexanetriol, glycerin and 1,2,4-butanetriol. It is more preferable that 1,2,3-triol is used in combination with a second triol solvent selected from the group consisting of 1,2,6-hexanetriol, glycerin, and 1,2,4-butanetriol, it is even more preferable that 3-methylbutane-1,2,3-triol is used in combination with a second triol solvent selected from the group consisting of glycerin and 1,2,4-butanetriol, and it is particularly preferable that 3-methylbutane-1,2,3-triol is used in combination with glycerin.

[0027] The content of the triol solvent in the flux of the present embodiment is preferably 1 mass % or more and 15 mass % or less, more preferably 1.5 mass % or more and 12 mass % or less, and even more preferably 2 mass % or more and 11 mass % or less, relative to the total amount of the flux (100 mass %). When the content of the triol solvent is equal to or greater than the lower limit of the above-mentioned preferred range, the generation of voids during soldering is easily suppressed, whereas when the content is equal to or less than the upper limit of the above-mentioned preferred range, the thixotropy of the solder paste is easily enhanced, and the ability to suppress heat dripping when made into a solder paste is also easily improved.

[0028] Regarding the triol solvent, when the first triol solvent and the second triol solvent are used in combination, the mixing ratio of the two, expressed as a mass ratio of the first triol solvent / the second triol solvent, is preferably 1 to 10, more preferably 2 to 10, and further preferably 3 to 10. When the mixing ratio of the two is equal to or greater than the lower limit of the above-mentioned preferred range, the generation of voids during soldering is easily suppressed. On the other hand, when the mixing ratio is equal to or less than the upper limit of the above-mentioned preferred range, the ability to suppress the generation of voids, the thixotropy of the solder paste, and the ability to suppress heat dripping when made into a solder paste are all easily improved.

[0029] <Monoamide thixotropic agent> In the flux of the present embodiment, the inclusion of a monoamide-based thixotropic agent imparts thixotropy to the solder paste, improving the printability of the solder paste. Examples of monoamide-based thixotropic agents include saturated fatty acid amides, unsaturated fatty acid amides (collectively referred to simply as "fatty acid amides"); and aromatic amides, such as acetamide, propionic acid amide, butanoic acid amide, isobutanoic acid amide, hexanoic acid amide, octanoic acid amide, 2-ethylhexanoic acid amide, lauric acid amide, palmitic acid amide, stearic acid amide, oleic acid amide, behenic acid amide, erucic acid amide, hydroxystearic acid amide, hexamethylenehydroxystearic acid amide, methylolstearic acid amide, methylol amide, fatty acid ester amide, benzamide, 2-phenylacetamide, and p-toluamide.

[0030] The monoamide-based thixotropic agent may be used alone or in combination of two or more kinds. Among the above, the monoamide-based thixotropic agent is preferably at least one selected from the group consisting of fatty acid amides and aromatic amides, and more preferably at least one selected from the group consisting of saturated fatty acid amides and aromatic amides. For example, the monoamide-based thixotropic agent may be a combination of fatty acid amide and aromatic amide, or a combination of saturated fatty acid amide and aromatic amide, and a combination of stearic acid amide and p-toluamide is preferred.

[0031] The content of the monoamide-based thixotropic agent in the flux of this embodiment is 0.5 mass% or more and less than 15 mass%, preferably 1 mass% or more and 10 mass% or less, and more preferably 2 mass% or more and 8 mass% or less, relative to the total amount of the flux (100 mass%). When the content of the monoamide-based thixotropic agent is less than the upper limit of the above range, the generation of voids during soldering is easily suppressed, whereas when the content is equal to or greater than the lower limit of the above range, the thixotropy of the solder paste is easily enhanced, and the ability to suppress heat dripping when made into a solder paste is also improved.

[0032] Regarding the monoamide-based thixotropic agent, when a fatty acid amide and an aromatic amide are used in combination, the mixing ratio of the two, expressed as a mass ratio of aromatic amide / fatty acid amide, is preferably 5 / 5 or more and 9 / 1 or less, more preferably more than 5 / 5 and 8 / 2 or less, and even more preferably more than 5 / 5 and 7 / 3 or less.

[0033] <Solvent (S2)> The flux of this embodiment contains at least one solvent (S2) selected from the group consisting of monohydric solvents and dihydric solvents in an amount of 50 mass% or more based on the total mass of the flux, which makes it easier to suppress the generation of voids during soldering and also makes it easier to prepare a flux with low residue. The flux of the present embodiment preferably contains a solvent (S2) containing a monovalent solvent, and more preferably contains a monovalent solvent as the base solvent of the entire flux. The monovalent solvent has a high interaction with the triol solvent (S1), and when the monovalent solvent is contained, the combined effect of the first triol solvent and the second triol solvent is particularly enhanced, resulting in good void generation suppression ability and improved thixotropy of the solder paste and heat drip suppression ability. A "monohydric solvent" is a solvent that has one hydroxyl group. A "dihydric solvent" is a solvent that has two hydroxyl groups.

[0034] <Monovalent solvent> Examples of the monohydric solvent include alcohol-based solvents, glycol ether-based solvents, and terpineols.

[0035] The alcohol-based solvent is preferably a branched aliphatic monohydric alcohol, and suitable examples thereof include branched aliphatic monohydric alcohols having 16 to 20 carbon atoms, such as isohexadecanol, isoheptadecanol, isooctadecanol, isononadecanol, and isoeicosanol. Examples of isohexadecanol include 2-hexyl-1-decanol and 2-pentyl-1-undecanol. Examples of isoheptadecanol include 2-hexyl-1-undecanol and 2-heptyl-1-decanol. Examples of isooctadecanol include 5,7,7-trimethyl-2-(1,3,3-trimethylbutyl)-1-octanol, 2-nonyl-1-nonal, 8-methyl-2-(4-methylhexyl)-1-decanol, 2-octyl-1-decanol, 2-heptyl-1-undecanol, and 2-hexyl-1-dodecanol. An example of isononadecanol is 2-hexyl-1-tridecanol. An example of isoeicosanol is 5,9-dimethyl-2-(1,5-dimethylhexyl)-1-decanol.

[0036] Examples of glycol ether solvents include ethylene glycol monophenyl ether, diethylene glycol monobutyl ether, diethylene glycol monohexyl ether (hexyl diglycol), diethylene glycol mono 2-ethylhexyl ether, propylene glycol monophenyl ether, triethylene glycol monobutyl ether, tripropylene glycol monomethyl ether, and tri(propylene glycol) n-butyl ether.

[0037] Among the above, the monohydric solvent is preferably an alcohol-based solvent, more preferably a branched aliphatic monohydric alcohol, and among these, a branched aliphatic monohydric alcohol having 16 to 20 carbon atoms is even more preferable from the viewpoints of void generation suppression ability and thixotropy of the solder paste.

[0038] <Dihydric solvent> Examples of the dihydric solvent include ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, neopentyl glycol; 2-ethyl-2-hydroxymethyl-1,3-propanediol, 2-ethyl-2-methyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-ethyl-2-propyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, and 2,5-dimethylhexane-2,5-diol.

[0039] The solvent (S2) may be used alone or in combination of two or more kinds. The solvent (S2) is at least one selected from the group consisting of monohydric solvents and dihydric solvents, and among the above, those containing a monohydric solvent are preferred. As the monohydric solvent here, it is more preferable to use an alcohol-based solvent, and it is even more preferable to use a branched aliphatic monohydric alcohol having 16 to 20 carbon atoms.

[0040] The content of the solvent (2) in the flux of the present embodiment is 50 mass % or more, 70 mass % or more, 80 mass % or more, 98.5 mass % or less, or 95 mass % or less, relative to the total amount (100 mass %) of the flux. In the flux of the present embodiment, the content of the solvent (2) may be the remainder that adjusts the total of all components (including the solvent (2)) blended in the flux to 100 mass %.

[0041] In the flux of the present embodiment, the mixing ratio of the solvent (S2) to the triol solvent (S1), expressed as a mass ratio represented by solvent (S2) / triol solvent (S1), is preferably 7 to 31, more preferably 7 to 25, and further preferably 7.5 to 20. When the ratio of the solvent (S2) / triol solvent (S1) is within the above-mentioned preferred range, the void generation suppression ability, the thixotropy of the solder paste, and the heat drip suppression ability when the solder paste is made are all likely to be improved. In particular, when the ratio is equal to or less than the upper limit of the above-mentioned preferred range, the generation of voids during soldering is likely to be suppressed.

[0042] <Other ingredients> The flux of the present embodiment may contain other components as necessary in addition to the triol solvent, the monoamide-based thixotropic agent, the monohydric solvent, and the dihydric solvent. Other components include activators such as organic acids, amines, and halogen compounds; resin components such as rosin; thixotropic agents other than monoamide-based thixotropic agents; solvents other than triol solvents, monohydric solvents, and dihydric solvents; surfactants, metal deactivators, antioxidants, silane coupling agents, colorants, and the like.

[0043] <Stimulant> The flux of the present embodiment may contain an activator such as an organic acid, an amine, or a halogen compound.

[0044] The organic acid includes, for example, a carboxylic acid and an organic sulfonic acid. Examples of the carboxylic acid include an aliphatic carboxylic acid and an aromatic carboxylic acid. Examples of aliphatic carboxylic acids include aliphatic monocarboxylic acids and aliphatic dicarboxylic acids. Examples of aliphatic monocarboxylic acids include caproic acid, enanthic acid, caprylic acid, pelargonic acid, isopelargonic acid, capric acid, caproleic acid, lauric acid (dodecanoic acid), undecanoic acid, Linderic acid, tridecanoic acid, myristoleic acid, pentadecanoic acid, isopalmitic acid, palmitoleic acid, hiragonic acid, hydnocarpic acid, margaric acid, isostearic acid, elaidic acid, petroselinic acid, moroctic acid, eleostearic acid, talic acid, vaccenic acid, riminoleic acid, vernolic acid, sterculic acid, nonadecanoic acid, eicosanoic acid, stearic acid, 12-hydroxystearic acid, oleic acid, linoleic acid, linolenic acid, myristic acid, etc. Examples of aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, eicosanedioic acid, tartaric acid, 2,4-diethylglutaric acid, diglycolic acid, 2-methylnonanedioic acid, 4-(methoxycarbonyl)-2,4-dimethylundecanedioic acid, 4,6-bis(methoxycarbonyl)-2,4,6-trimethyltridecanedioic acid, and 8,9-bis(methoxycarbonyl)-8,9-dimethylhexadecanedioic acid. Examples of aromatic carboxylic acids include salicylic acid, dibutylaniline diglycolic acid, terephthalic acid, parahydroxyphenylacetic acid, phenylsuccinic acid, phthalic acid, benzoic acid, 2,3-dihydroxybenzoic acid, 2-quinolinecarboxylic acid, 3-hydroxybenzoic acid, and p-anisic acid.

[0045] Further, examples of the carboxylic acid include tris(2-carboxyethyl) isocyanurate, 1,3-cyclohexanedicarboxylic acid; hydroxycarboxylic acids such as 2,2-bis(hydroxymethyl)propionic acid, 2,2-bis(hydroxymethyl)butanoic acid, citric acid, isocitrate, malic acid, and tartaric acid; dimer acid, trimer acid, hydrogenated dimer acid obtained by adding hydrogen to dimer acid, and hydrogenated trimer acid obtained by adding hydrogen to trimer acid; picolinic acid, dipicolinic acid, and 3-hydroxypicolinic acid.

[0046] The organic sulfonic acid includes aliphatic sulfonic acids and aromatic sulfonic acids. Examples of the aliphatic sulfonic acid include alkane sulfonic acid and alkanol sulfonic acid. Examples of the alkane sulfonic acid include methane sulfonic acid, ethane sulfonic acid, 1-propane sulfonic acid, 2-propane sulfonic acid, 1-butane sulfonic acid, 2-butane sulfonic acid, pentane sulfonic acid, hexane sulfonic acid, decane sulfonic acid, and dodecane sulfonic acid. Examples of the alkanol sulfonic acid include 2-hydroxyethane-1-sulfonic acid, 2-hydroxypropane-1-sulfonic acid, 2-hydroxybutane-1-sulfonic acid, 2-hydroxypentane-1-sulfonic acid, 1-hydroxypropane-2-sulfonic acid, 3-hydroxypropane-1-sulfonic acid, 4-hydroxybutane-1-sulfonic acid, 2-hydroxyhexane-1-sulfonic acid, 2-hydroxydecane-1-sulfonic acid, and 2-hydroxydodecane-1-sulfonic acid. Examples of aromatic sulfonic acids include 1-naphthalenesulfonic acid, 2-naphthalenesulfonic acid, p-toluenesulfonic acid, xylenesulfonic acid, p-phenolsulfonic acid, cresolsulfonic acid, sulfosalicylic acid, nitrobenzenesulfonic acid, sulfobenzoic acid, and diphenylamine-4-sulfonic acid.

[0047] Examples of the amine include azoles, guanidines, amino alcohols, alkylamine compounds, and amine polyoxyalkylene adducts. Examples of halogen compounds include amine hydrohalides, halogenated aliphatic alcohols, halogenated heterocyclic compounds, etc. Amine hydrohalides are compounds obtained by reacting an amine with hydrogen halide.

[0048] The activator may be used alone or in combination of two or more kinds. In the flux of this embodiment, if it further contains an activator, the content of the activator in the flux is preferably more than 0 mass% and not more than 5 mass% with respect to the total amount of the flux (100 mass%), from the viewpoint of suppressing the occurrence of voids during soldering.

[0049] Alternatively, when a solder paste containing the flux of the present embodiment is used for soldering in a reflow atmosphere in a reducing gas atmosphere, the flux may not contain an activator. In particular, the flux of the present embodiment, which does not contain an activator, is suitable for soldering applications in which a reflow method in a reducing gas atmosphere of formic acid is combined with a solder paste.

[0050] <Resin component> The flux of the present embodiment may contain a resin component such as a rosin-based resin. However, since the flux of the present embodiment contains a triol solvent and a monoamide-based thixotropic agent, the resin component such as rosin may be used optionally, and it is preferable that the flux does not contain a rosin-based resin from the viewpoint of reducing the amount of flux residue during soldering.

[0051] The rosin-based resin referred to here includes natural resins containing abietic acid as the main component or a mixture of abietic acid and its isomers, as well as chemically modified natural resins (hereinafter referred to as "rosin derivatives"). Examples of rosin derivatives include purified rosin and modified rosin. Examples of modified rosins include hydrogenated rosin, polymerized rosin, polymerized hydrogenated rosin, disproportionated rosin, acid-modified rosin, rosin ester, acid-modified hydrogenated rosin, acid anhydride-modified hydrogenated rosin, acid-modified disproportionated rosin, acid anhydride-modified disproportionated rosin, phenol-modified rosin and α,β-unsaturated carboxylic acid modified products (acrylated rosin, maleated rosin, fumarated rosin, etc.), as well as purified products, hydrogenated products and disproportionated products of the polymerized rosins, as well as purified products, hydrogenated products and disproportionated products of the α,β-unsaturated carboxylic acid modified products, rosin alcohol, rosin amine, hydrogenated rosin alcohol, rosin ester, hydrogenated rosin ester, rosin soap, hydrogenated rosin soap, acid-modified rosin soap, etc.

[0052] <Thixotropic agents other than monoamide-based thixotropic agents> The flux of the present embodiment may contain a thixotropic agent other than the monoamide-based thixotropic agent. Examples of thixotropic agents other than the monoamide-based thixotropic agents include bisamides, other polyamides, wax-based thixotropic agents, and sorbitol-based thixotropic agents. Examples of the bisamide include methylene bisstearic acid amide, ethylene bislauric acid amide, ethylene bishydroxy fatty acid (fatty acid carbon number: C6 to C24) amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, saturated fatty acid bisamide, methylene bisoleic acid amide, unsaturated fatty acid bisamide, m-xylylene bisstearic acid amide, and aromatic bisamide. Other polyamides include saturated fatty acid polyamides, unsaturated fatty acid polyamides, aromatic polyamides, 1,2,3-propanetricarboxylic acid tris(2-methylcyclohexylamide), cyclic amide oligomers, and non-cyclic amide oligomers. Examples of the wax-based thixotropic agent include ester compounds, specifically hydrogenated castor oil. Examples of sorbitol-based thixotropic agents include dibenzylidene-D-sorbitol, bis(4-methylbenzylidene)-D-sorbitol, (D-)sorbitol, monobenzylidene (-D-) sorbitol, and mono(4-methylbenzylidene)-(D-) sorbitol.

[0053] As described above, the flux of this embodiment contains a triol solvent (S1), 0.5% by mass or more and less than 15% by mass of a monoamide-based thixotropic agent, and 50% by mass or more of at least one solvent (S2) selected from the group consisting of monovalent solvents and divalent solvents. By containing a predetermined amount of each of the monoamide-based thixotropic agent and the solvent (S2), the solder paste can be reduced in residue. In addition, by further containing the triol solvent (S1), the generation of voids during soldering can be further suppressed. In particular, when reflow is performed in a reducing gas atmosphere, the void area ratio measured in the [Example] described later can be reduced. In a normal reflow method, even a void area ratio of around 5% is a high level, but by adopting the flux of this embodiment, it is possible to further reduce voids and approach zero voids.

[0054] In addition, in the flux of this embodiment, a first triol solvent selected from the group consisting of 3-methylbutane-1,2,3-triol and 2-methylbutane-1,2,4-triol is used as the triol solvent (S1) in combination with a second triol solvent selected from the group consisting of 1,2,6-hexanetriol, glycerin and 1,2,4-butanetriol, thereby enhancing the thixotropy of the solder paste and improving the ability to suppress dripping when the solder paste is made. This allows the amount of the thixotropic agent to be reduced, further reducing the number of voids and residues in the solder paste. The flux of the present embodiment described above is particularly suitable for soldering applications in which a reflow method performed in a reducing gas atmosphere is combined with a solder paste.

[0055] (Solder paste) The solder paste according to the second embodiment contains a solder alloy powder and the flux according to the first embodiment described above.

[0056] The solder alloy powder may be composed of a powder of solder containing only Sn, or a powder of a solder alloy such as Sn-Ag, Sn-Cu, Sn-Ag-Cu, Sn-Bi, or Sn-In, or an alloy of these with the addition of Sb, Bi, In, Cu, Zn, As, Ag, Cd, Fe, Ni, Co, Au, Ge, P, or the like. The solder alloy powder may be composed of a powder of a solder alloy of Sn-Pb system or a Sn-Pb system to which Sb, Bi, In, Cu, Zn, As, Ag, Cd, Fe, Ni, Co, Au, Ge, P, etc. have been added. The solder alloy powder is preferably a Pb-free solder. The solder alloy powder that can be used has a melting temperature of, for example, 150 to 250°C.

[0057] Flux Content: The content of the flux in the solder paste is preferably 5 to 30 mass % and more preferably 5 to 15 mass % based on the total mass of the solder paste.

[0058] According to the solder paste of the present embodiment described above, since the flux according to the first aspect is used, the occurrence of voids during soldering is further suppressed. Alternatively, such a solder paste can achieve even lower voids, approaching zero voids, and when made into a solder paste, the thixotropy is enhanced and heat dripping is suppressed.

[0059] (Method of Manufacturing Joint) A method for producing a bonded body according to a third aspect includes a step of obtaining a bonded body by soldering a component and a substrate, the soldering being performed by reflowing in a reducing gas atmosphere using the solder paste according to the second aspect. Hereinafter, one embodiment of the method for producing the bonded body according to the third aspect will be described. The method for manufacturing a bonded body according to this embodiment includes a solder paste application step, a component attachment step, and a reflow step, in this order.

[0060] [Solder paste application process] In the solder paste application step, the solder paste according to the second aspect is applied to the surface of the board. Examples of the substrate include a printed wiring board and a wafer. Examples of methods for applying the solder paste include a method of printing and applying the solder paste using a mask having an opening, a method of ejecting the solder paste using a dispenser or the like, and a method of transferring the solder paste using a probe pin or the like.

[0061] [Parts installation process] In the component mounting process, components are mounted on the board on which the solder paste has been applied. Components include, for example, chips, integrated circuits, transistors, diodes, resistors, and capacitors.

[0062] [Reflow process] The reflow step includes at least an operation of performing reflow in a reducing gas atmosphere, and may include an operation in a nitrogen gas atmosphere as long as the effects of the present invention are achieved. The reducing gas atmosphere may be formed, for example, by volatilizing a reducing compound in a reflow furnace, or by supplying a reducing gas obtained by passing nitrogen through a liquid reducing compound to the reflow furnace. As the reducing compound, formic acid is preferable. When the reflow process is performed in a reducing gas atmosphere, the amount of activator in the solder paste may be reduced or the solder paste may be free of activator, which can further reduce flux residue.

[0063] In the reflow process, the board after mounting the components is heated in a reflow furnace at a temperature (i.e., peak temperature) higher than the melting point of the solder powder contained in the solder paste (this is called the main heating process). The heating temperature may be, for example, 5 to 30° C. higher than the melting point of the solder powder. The heating time may be, for example, 1 to 4 minutes.

[0064] The reflow process may include a preheating step prior to the main heating step. In the preheating step, the board after mounting the components is heated in a reflow furnace at a temperature lower than the melting point of the solder powder contained in the solder paste. The heating temperature may be, for example, 190 to 220° C. The heating time may be, for example, 1 to 5 minutes. In the preheating step, the interior of the reflow furnace may be in the above-mentioned nitrogen gas atmosphere or in a reducing gas atmosphere.

[0065] According to the manufacturing method of the bonded body of the present embodiment described above, the soldering is performed by combining the solder paste containing the flux of the present embodiment and the reflow method performed in a reducing gas atmosphere, so that the flux residue is reduced and the occurrence of voids is further suppressed, thereby extending the fatigue life of the bonded body obtained and suppressing the decrease in thermal conductivity. In addition, the risk of short circuiting in the board is reduced because the heat drip is suppressed. EXAMPLES

[0066] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples.

[0067] <Preparation of flux> (Examples 1 to 21, Comparative Examples 1 to 2) The fluxes of the examples and comparative examples having the compositions shown in Tables 1 to 4 were prepared. In the table, the content of each raw material indicates the ratio (mass %) to the total mass (100 mass %) of the flux. The raw materials used are shown below.

[0068] ·Triol Solvent (S1) As the first triol solvent, 3-methylbutane-1,2,3-triol and 2-methylbutane-1,2,4-triol were used. As the second triol solvent, 1,2,6-hexanetriol, glycerin, and 1,2,4-butanetriol were used.

[0069] Monoamide thixotropic agent p-Toluamide and stearic acid amide were used.

[0070] Solvent (S2) As monohydric solvents, isooctadecanol (5,7,7-trimethyl-2-(1,3,3-trimethylbutyl)-1-octanol), 2-hexyldecanol, and hexyldiglycol (diethylene glycol monohexyl ether) were used. As the dihydric solvent, 1,4-butanediol was used.

[0071] ·Activators Capric acid was used.

[0072] <Preparation of solder paste> Each flux was mixed with the solder alloy powder described below to prepare a solder paste. Each of the prepared solder pastes contained 9 mass % flux and 91 mass % solder alloy powder. Solder alloy powder: Powder made of a solder alloy containing 7.0 mass% Sb, 0.6 mass% Cu, and the remainder Sn. The solidus temperature of this solder alloy is 235° C., and the liquidus temperature is 242° C. The size of the solder alloy powder is a size (particle size distribution) that satisfies symbol 4 in the powder size classification (Table 2) in JIS Z 3284-1:2014.

[0073] <Evaluation> The void generation suppression ability, the thixotropy of the solder paste, and the heat drip suppression ability were evaluated as described below. The evaluation results are shown in Tables 1 to 4.

[0074] [Evaluation of void generation suppression ability] Using a metal mask (thickness 0.15 mm, opening 10 mm x 10 mm), the solder paste prepared above was printed on a Cu plate (size 50 mm x 50 mm). Next, a Cu chip (size 10 mm x 10 mm) was mounted on the Cu plate on which the solder paste was printed. Next, reflow soldering was performed under the following conditions.

[0075] Reflow conditions: The reflow profile used in this evaluation is shown in Figure 1. In FIG. 1, the operating conditions at each elapsed time (a), (b), (c), (d), and (e) are shown below. (a) Before heating, the inside of the furnace is evacuated to a vacuum and then replaced with nitrogen. (b) First temperature rise (from 30°C to 210°C, temperature rise rate 1.5°C / sec) (c) Preheat (210℃, 4 min), add formic acid during preheating. (d) The second temperature increase (from 210°C to 280°C, temperature increase rate 0.7°C / sec) is performed while drawing a vacuum. (e) Hold at 280°C for 3 minutes. After 2 minutes, return to atmospheric pressure and hold at atmospheric pressure for 1 minute.

[0076] Void evaluation method: The bonded body of the Cu plate and the Cu chip was irradiated with X-rays from the direction perpendicular to the Cu plate, and the void area was measured by analyzing the transmitted X-rays. The void area was measured using an XD7600NT Diamond X-ray inspection system (manufactured by Nordson DAGE). The void area was measured when the X-rays passed through at least one void, and voids with a diameter of 0.1 μm or more were considered to be present. Next, the ratio of the total area of ​​the voids to the total area of ​​the Cu chip underside (this was taken as 100%) was calculated to obtain the void area ratio (%). The average value of the void area ratio for the five bonded bodies was calculated. A smaller void area ratio value means a higher ability to suppress void generation.

[0077] [Evaluation of thixotropy of solder paste] The thixotropy of the solder paste prepared above was evaluated using a spiral viscometer in accordance with JIS Z3284-3:2014 4.2 "Viscosity characteristic test" 1) spiral method. The rotation speed of the viscometer was set to 3 rpm and 30 rpm, and the viscosity of the solder paste after a specified period of rotation was read to calculate the thixotropy ratio. The thixotropic ratio TI was calculated from the following formula (log is common logarithm). Thixometry ratio TI=log(η1 / η2) / log(D2 / D1) η1: Viscosity at shear rate D1 η2: Viscosity at shear rate D2 D1: shear rate 1, D1 = 1.8s -1 (3r / min) D2: shear rate 2, D2=18s -1 (30r / min) A larger value of the thixotropic ratio TI means that the solder paste has a higher thixotropic property.

[0078] [Evaluation of heat drip suppression ability] The solder paste prepared above was evaluated for heat droop in accordance with the method described in JIS Z 3284-3:2014 4.4 "Heated droop test". First, a test plate was obtained by printing solder paste using a metal mask with a pattern hole shown in I (hole size 3.0 x 0.7) in Figure 6 of JIS Z 3284-3:2014 4.3 "Printing droop test". The obtained test plate was left to stand in a thermostatic chamber at 150°C for 3 minutes. A schematic diagram of the above pattern I is shown in Fig. 2. In Fig. 2, the numerical values ​​of 0.2 to 1.2 represent the distance between pattern holes. After heating, the test plate was visually inspected for the minimum gap at which the printed solder paste did not join together, and evaluated. The smaller the value of this minimum interval, the higher the ability to suppress heat dripping.

[0079] [Table 1]

[0080] From the results shown in Table 1, it was confirmed that the solder pastes containing the fluxes of Examples 1 to 5, which contain a triol solvent, had lower void area ratios than the solder pastes containing the fluxes of Comparative Examples 1 and 2, which do not contain a triol solvent, and thus the generation of voids during soldering was further suppressed. Comparing Comparative Example 1 and Comparative Example 2, it can be seen that simply reducing the content of the monoamide thixotropic agent has little effect in suppressing the occurrence of voids; the thixotropy of the solder paste decreases, and the ability to suppress heat dripping remains low.

[0081] [Table 2]

[0082] From the results shown in Table 2, it was confirmed that when the fluxes of Examples 8 to 11, which use a combination of the first triol and the second triol, were used, good void generation suppression ability was exhibited, and the thixotropy of the solder paste and the heat drip suppression ability were also improved.

[0083] [Table 3]

[0084] Regarding triol solvent (S1) selection: From the results shown in Table 3, it can be seen that the solder pastes containing the fluxes of Examples 10 and 13 exhibited lower void area ratios than the solder pastes containing the fluxes of Examples 12, 14, and 15, and thus the generation of voids during soldering was further suppressed.

[0085] [Table 4]

[0086] Combination of triol solvent (S1) and solvent (S2): From the results shown in Table 4, it can be confirmed that in the case of Examples 18 to 21 containing a monovalent solvent, and in the case of Examples 19 and 21 in which the first triol and the second triol are used in combination, good void generation suppression ability is exhibited, and the thixotropy of the solder paste and the heat drip suppression ability are improved. In contrast, a comparison of Examples 16 and 17, which contain a divalent solvent, showed that even when the first triol and the second triol were used in combination, no improvement was observed in the thixotropy of the solder paste or the ability to suppress heat dripping.

Claims

1. A triol solvent (S1), A monoamide thixotropic agent, At least one solvent (S2) selected from the group consisting of monohydric solvents and dihydric solvents; A flux comprising: The content of the monoamide-based thixotropic agent is 0.5 mass% or more and less than 15 mass% with respect to the total mass of the flux, A flux, wherein the content of the solvent (S2) is 50 mass% or more based on the total mass of the flux.

2. The flux according to claim 1, wherein the content of the triol solvent (S1) is 1 mass% or more and 15 mass% or less with respect to the total mass of the flux.

3. 2. The flux according to claim 1, wherein the triol solvent (S1) is a triol compound in which three hydroxyl groups are bonded to a chain hydrocarbon group having 3 to 6 carbon atoms.

4. The flux according to claim 3, wherein the triol solvent (S1) is at least one selected from the group consisting of 3-methylbutane-1,2,3-triol, 2-methylbutane-1,2,4-triol, 1,2,6-hexanetriol, glycerin, and 1,2,4-butanetriol.

5. The triol solvent (S1) a first triol solvent selected from the group consisting of 3-methylbutane-1,2,3-triol and 2-methylbutane-1,2,4-triol; a second triol solvent selected from the group consisting of 1,2,6-hexanetriol, glycerin, and 1,2,4-butanetriol; The flux according to claim 4, which is a combination of

6. The mixing ratio of the first triol solvent and the second triol solvent is The flux according to claim 5, wherein the mass ratio of the first triol solvent to the second triol solvent is 1 to 10.

7. 2. The flux of claim 1, wherein the solvent (S2) comprises the monovalent solvent.

8. The flux according to claim 7, wherein the monohydric solvent is a branched aliphatic monohydric alcohol having 16 to 20 carbon atoms.

9. The mixing ratio of the solvent (S2) and the triol solvent (S1) is The flux according to claim 1, wherein the mass ratio of the solvent (S2) to the triol solvent (S1) is 7 to 31.

10. 2. The flux according to claim 1, wherein the monoamide-based thixotropic agent is a combination of an aromatic amide and a fatty acid amide.

11. Further, it contains an activator, The flux according to claim 1 , wherein the content of the activator is more than 0 mass % and not more than 5 mass % with respect to the total mass of the flux.

12. 2. The flux according to claim 1, which does not contain a rosin-based resin.

13. 10. The flux of claim 1 which does not contain an activator.

14. A solder paste comprising a solder alloy powder and the flux according to any one of claims 1 to 13.

15. The method includes a step of obtaining a bonded body by soldering a component and a substrate, A method for producing a joint body, comprising the steps of: performing reflow soldering in a reducing gas atmosphere using the solder paste according to claim 14 .

Citation Information

Patent Citations

  • Flux, solder paste and soldering product manufacturing method

    JP6706000B1