Method for evaluating water-based pigment dispersion liquid and method for producing water-based pigment dispersion liquid
The method uses pulse NMR to evaluate and produce aqueous pigment dispersions with optimal polymer dispersants and solvents, addressing inefficiencies in existing methods by achieving enhanced dispersibility, storage stability, and redispersibility.
Patent Information
- Application Number
- JP2023071095
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2043-04-24
AI Technical Summary
Existing methods for evaluating polymer dispersants in aqueous pigment dispersions are time-consuming and inefficient, making it difficult to predict and achieve excellent dispersibility, storage stability, and redispersibility of organic pigments.
A method using pulse NMR to measure T2 relaxation times and calculate Rsp values to evaluate and produce aqueous pigment dispersions with optimal polymer dispersants and solvents, ensuring good dispersibility, storage stability, and redispersibility.
Enables rapid evaluation and production of aqueous pigment dispersions with improved dispersibility, storage stability, and redispersibility by identifying suitable polymer dispersant and solvent combinations.
Smart Images

Figure 2024156542000004 
Figure 2024156542000005 
Figure 2024156542000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for evaluating an aqueous pigment dispersion and a method for producing an aqueous pigment dispersion. [Background technology]
[0002] Due to the increasing functionality of inkjet printing methods, they are widely used for personal, office, and commercial purposes. In recent years, the scope of application of inkjet printing methods has expanded from consumer inkjet printers and wide-format inkjet printers for large-format printing to inkjet printers for industrial use. The printing speed of inkjet printing methods has improved in line with productivity. In addition, recording devices are also required to be suitable for high-speed printing, such as maintenance-free print heads. Furthermore, inkjet printing methods using aqueous inks are mainly adopted due to environmental considerations.
[0003] Unlike aqueous inks containing dyes (aqueous dye inks), aqueous inks containing pigments (aqueous pigment inks) tend to have particulate pigments that tend to aggregate and settle over time. For this reason, when discharging aqueous pigment inks using an inkjet method, it is important to prevent clogging of the discharge nozzles in order to ensure discharge stability. As dispersions with good pigment dispersibility, for example, various inkjet dispersions using amphiphilic polymers having hydrophobic and hydrophilic segments as polymer dispersants for dispersing pigments have been proposed (Patent Documents 1 to 7). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-053628 A [Patent Document 2] Patent No. 4157868 [Patent Document 3] Patent No. 6979142 [Patent Document 4] Patent No. 6967168 [Patent Document 5] International Publication No. 2011 / 136000 [Patent Document 6] JP 2017-214469 A [Patent Document 7] JP 2012-021120 A Summary of the Invention [Problem to be solved by the invention]
[0005] The polymer dispersants used in the dispersions proposed in Patent Documents 1 to 7, etc., suppress the aggregation and precipitation of the pigment by adsorbing the hydrophobic segment to the surface of the pigment and dissolving the hydrophilic segment in the aqueous medium. Therefore, the dispersion effect of the pigment in the aqueous medium varies depending on the monomer composition of the polymer dispersant and the ratio of the hydrophilic segment to the hydrophobic segment. In addition, the hydrophobic segment of the polymer dispersant may shrink or form micelles in the aqueous medium and not be exposed. Therefore, depending on the composition of the aqueous medium, etc., the hydrophobic segment may not be easily adsorbed to the surface of the pigment, making it difficult to increase the dispersibility of the pigment.
[0006] Prior to producing an aqueous pigment dispersion in which pigment aggregation and sedimentation are suppressed and which has excellent dispersibility, it is difficult to directly observe and quantify the behavior of a polymer dispersant in an aqueous medium. Therefore, in order to evaluate the performance of a polymer dispersant, a series of test verifications from pigment dispersion to printing evaluation is required. However, it takes a lot of time to carry out a series of test verifications for all of the many polymer dispersants produced experimentally, which has been a factor in reducing development efficiency.
[0007] The present invention has been made in consideration of the problems of the conventional techniques, and an object of the present invention is to provide a method for evaluating an aqueous pigment dispersion that is useful for producing an aqueous pigment dispersion excellent in dispersibility, storage stability, and redispersibility of an organic pigment, by which a suitable combination of a polymer dispersant and a water-soluble organic solvent that provides good dispersibility of the organic pigment can be predicted and evaluated.Another object of the present invention is to provide a method for producing an aqueous pigment dispersion that is capable of producing an aqueous pigment dispersion excellent in dispersibility, storage stability, and redispersibility of an organic pigment. [Means for solving the problem]
[0008] That is, according to the present invention, there is provided a method for evaluating an aqueous pigment dispersion as described below. [1] A method for evaluating an aqueous pigment dispersion liquid containing an organic pigment, a polymer dispersant, a water-soluble organic solvent, and water, comprising the steps of obtaining a mixture a that contains the polymer dispersant, the water-soluble organic solvent, and the water but does not contain the organic pigment, obtaining a mixture b that contains the water-soluble organic solvent and the water but does not contain the organic pigment and the polymer dispersant, and measuring the T2 relaxation time (T2 a ) and the T2 relaxation time of the mixture b (T2 b ) and obtain the Rsp value by the following formula (1); obtaining a mixture o containing the polymer dispersant and the water, the concentration of the polymer dispersant being the same as the concentration of the polymer dispersant in the mixture a; and measuring the T2 relaxation time (T2 o ) and the T2 relaxation time of the water (T2 w ) and calculate Rsp using the following formula (2) o obtaining a value of Rsp o calculating a rate of decrease (%) of the Rsp value based on the Rsp value, and evaluating the dispersibility of the organic pigment in the aqueous pigment dispersion based on the magnitude of the calculated rate of decrease. Rsp = (R a / R b )-1 (1) (In the above formula (1), Ra is T2 a represents the reciprocal of R b is T2 b (represents the reciprocal of Rsp o =(R o / R w )-1 (2) (In the above formula (2), R o is T2 o represents the reciprocal of R w is T2 w (represents the reciprocal of [2] The method for evaluating an aqueous pigment dispersion according to [1] above, wherein the composition of the mixture a is equivalent to a raw material mixture used in the dispersion treatment of the organic pigment, except that the mixture a does not contain the organic pigment, and the composition of the mixture b is equivalent to the raw material mixture, except that the mixture b does not contain the organic pigment component and the polymer dispersant. [3] The method for evaluating an aqueous pigment dispersion according to [1] or [2] above, wherein the acid-precipitated polymer dispersant, the water, and a neutralizing agent are mixed to dissolve the polymer dispersant, and then the mixture o is obtained by diluting with the water. [4] The method for evaluating an aqueous pigment dispersion according to any one of [1] to [3], wherein the polymer dispersant is a block copolymer having a hydrophobic segment and a hydrophilic segment derived from a methacrylate monomer containing methacrylic acid. [5] The method for evaluating an aqueous pigment dispersion according to any one of [1] to [3], wherein the content of the polymer dispersant in the aqueous pigment dispersion is 5 to 50 parts by mass per 100 parts by mass of the organic pigment. [6] The method for evaluating an aqueous pigment dispersion according to [4], wherein the content of the polymer dispersant in the aqueous pigment dispersion is 5 to 50 parts by mass per 100 parts by mass of the organic pigment.
[0009] According to the present invention, there is also provided a method for producing an aqueous pigment dispersion liquid as described below. [7] A method for producing an aqueous pigment dispersion liquid containing an organic pigment, a polymer dispersant, a water-soluble organic solvent, and water, the method comprising the steps of: obtaining a plurality of mixtures a containing the polymer dispersant, the water-soluble organic solvent, and the water, but not containing the organic pigment, the mixtures a being different in the type of at least one of the polymer dispersant and the water-soluble organic solvent; obtaining a plurality of mixtures b being different in the type of the water-soluble organic solvent, the mixtures b being different in the type of the water-soluble organic solvent, but not containing the organic pigment or the polymer dispersant; and measuring the T2 relaxation times (T2 a ) and the T2 relaxation times (T2 b ) and obtain an Rsp value by the following formula (1); obtaining a plurality of mixtures o containing the polymer dispersant and the water, the concentration of the polymer dispersant being the same as the concentration of the polymer dispersant in the plurality of mixtures a, and different types of the polymer dispersant; and measuring the T2 relaxation time (T2 o ) and the T2 relaxation time of the water (T2 w ) and calculate Rsp using the following formula (2) o obtaining a value of Rsp o a step of calculating a rate of decrease (%) of the Rsp value based on a standard value, and selecting the mixture a for which the calculated rate of decrease is 20% or more; and a step of mixing the polymer dispersant and the water-soluble organic solvent contained in the selected mixture a, as well as the organic pigment and water, to obtain a raw material mixture, and dispersing the organic pigment in the raw material mixture. Rsp = (R a / R b )-1 (1) (In the above formula (1), R a is T2 a represents the reciprocal of R b is T2 b (represents the reciprocal of Rsp o =(R o / R w )-1 (2) (In the above formula (2), R o is T2 o represents the reciprocal of R w is T2w (represents the reciprocal of [8] The method for producing an aqueous pigment dispersion according to [7] above, wherein the composition of the mixture a is the same as that of the raw material mixture except that it does not contain the organic pigment, and the composition of the mixture b is the same as that of the raw material mixture except that it does not contain the organic pigment component and the polymer dispersant. [9] The method for producing an aqueous pigment dispersion liquid according to [7] or [8] above, comprising mixing the acid-precipitated polymer dispersant, the water, and a neutralizing agent to dissolve the polymer dispersant, and then diluting the mixture with water to obtain the mixture o.
[10] The method for producing an aqueous pigment dispersion liquid according to any one of [7] to [9], wherein the polymer dispersant is a block copolymer having a hydrophobic segment and a hydrophilic segment derived from a methacrylate monomer containing methacrylic acid.
[11] The method for producing an aqueous pigment dispersion according to any one of [7] to [9], wherein the content of the polymer dispersant in the aqueous pigment dispersion is 5 to 50 parts by mass per 100 parts by mass of the organic pigment.
[12] The method for producing an aqueous pigment dispersion according to
[10] , wherein the content of the polymer dispersant in the aqueous pigment dispersion is 5 to 50 parts by mass per 100 parts by mass of the organic pigment. Effect of the Invention
[0010] According to the present invention, it is possible to provide a method for evaluating an aqueous pigment dispersion that is useful for producing an aqueous pigment dispersion excellent in dispersibility, storage stability, and redispersibility of an organic pigment, by which a suitable combination of a polymer dispersant and a water-soluble organic solvent that provides good dispersibility of the organic pigment can be predicted and evaluated. Also, according to the present invention, it is possible to provide a method for producing an aqueous pigment dispersion that is excellent in dispersibility, storage stability, and redispersibility of an organic pigment. [Brief description of the drawings]
[0011] [Figure 1] 1 is a graph in which "average particle size (nm)" is plotted against "decrease rate (%) of Rsp value" for the aqueous pigment dispersions prepared in Examples 1 and 2, and Comparative Examples 1 to 3. [Diagram 2] 1 is a graph in which "average particle size (nm)" is plotted against "decrease rate (%) of Rsp value" for the aqueous pigment dispersions prepared in Examples 3 to 7 and Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <Evaluation method and production method of aqueous pigment dispersion> Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited to the following embodiment. One embodiment of the method for evaluating an aqueous pigment dispersion of the present invention is a method for evaluating an aqueous pigment dispersion containing an organic pigment, a polymer dispersant, a water-soluble organic solvent, and water. The evaluation method of this embodiment includes the steps of obtaining a mixture a that contains a polymer dispersant, a water-soluble organic solvent, and water but does not contain an organic pigment, obtaining a mixture b that contains a water-soluble organic solvent and water but does not contain an organic pigment and a polymer dispersant, and measuring the T2 relaxation time (T2 a ) and the T2 relaxation time of mixture b (T2 b ) and obtain the Rsp value by the following formula (1); obtaining a mixture o containing a polymer dispersant and water, the concentration of the polymer dispersant being the same as the concentration of the polymer dispersant in the mixture a; and measuring the T2 relaxation time (T2 o ) and the T2 relaxation time of water (T2 w ) and calculate Rsp using the following formula (2) o A step of obtaining the value of Rsp o and calculating a rate of decrease (%) of the Rsp value based on the value, and evaluating the dispersibility of the organic pigment in the aqueous pigment dispersion liquid based on the magnitude of the calculated rate of decrease.
[0013] Rsp = (R a / R b )-1 (1) (In the above formula (1), R a is T2 a represents the reciprocal of R b is T2 b (represents the reciprocal of Rsp o =(Ro / R w )-1 (2) (In the above formula (2), R o is T2 o represents the reciprocal of R w is T2 w (represents the reciprocal of
[0014] Moreover, one embodiment of the method for producing an aqueous pigment dispersion of the present invention is a method for producing an aqueous pigment dispersion containing an organic pigment, a polymer dispersant, a water-soluble organic solvent, and water. The production method of this embodiment includes the steps of obtaining a plurality of mixtures a, which contain a polymer dispersant, a water-soluble organic solvent, and water, but do not contain an organic pigment, and in which at least one of the polymer dispersant and the water-soluble organic solvent is different; obtaining a plurality of mixtures b, which contain a water-soluble organic solvent and water, but do not contain an organic pigment and a polymer dispersant, and in which the type of the water-soluble organic solvent is different; and measuring the T2 relaxation times (T2 a ) and the T2 relaxation times (T2 b ) and obtain the Rsp value by the following formula (1); obtaining a plurality of mixtures o containing a polymer dispersant and water, the concentration of the polymer dispersant being the same as the concentration of the polymer dispersant in the plurality of mixtures a, and different types of polymer dispersants; and measuring the T2 relaxation time (T2 o ) and the T2 relaxation time of water (T2 w ) and calculate Rsp using the following formula (2) o A step of obtaining the value of Rsp o the step of calculating the rate of decrease (%) of the Rsp value based on the value as a reference, and selecting mixture a for which the calculated rate of decrease is 20% or more; and the step of dispersing the organic pigment in a raw material mixture obtained by mixing the polymer dispersant and the water-soluble organic solvent contained in the selected mixture a, as well as the organic pigment and water.
[0015] Rsp = (R a / R b )-1 (1) (In the above formula (1), R a is T2 a represents the reciprocal of R b is T2 b(represents the reciprocal of Rsp o =(R o / R w )-1 (2) (In the above formula (2), R o is T2 o represents the reciprocal of R w is T2 w (represents the reciprocal of
[0016] According to the pulse NMR (Pulse Nuclear Magnetic Resonance) measurement method, the mobility of molecules can be evaluated by measuring the relaxation time of nuclear magnetic resonance. In an aqueous pigment dispersion containing a polymer dispersant and an aqueous medium (a mixed solvent of a water-soluble organic solvent and water), the relaxation time of protons bound to the polymer dispersant is shorter than the relaxation time of protons freely present in the aqueous medium. This is thought to be because the molecules of the aqueous medium are bound to the hydrophilic segments constituting the polymer dispersant, reducing the mobility of the protons. On the other hand, the hydrophobic segments constituting the polymer dispersant have a weaker force for binding protons than the hydrophilic segments. In other words, the amount of protons bound to the polymer dispersant differs depending on the monomer composition of the polymer dispersant, the ratio of the hydrophilic segments to the hydrophobic segments, and the dissolution state in the aqueous medium.
[0017] In the evaluation method and production method of this embodiment, the degree (level) of water affinity of a polymer dispersant in an aqueous medium, which is a mixed solvent of water and a water-soluble organic solvent, is quantified by the T2 relaxation time measured by pulse NMR, and properties such as the solubility and molecular mobility of the polymer dispersant in the aqueous medium are grasped. This makes it possible to predict and evaluate a suitable combination of a polymer dispersant and a water-soluble organic solvent that provides good dispersibility of an organic pigment, and to produce an aqueous pigment dispersion that is excellent in dispersibility, storage stability, and redispersibility of the organic pigment.
[0018] In this embodiment, a mixture a containing a polymer dispersant, a water-soluble organic solvent, and water but not containing an organic pigment, and a mixture b containing a water-soluble organic solvent and water but not containing an organic pigment and a polymer dispersant are prepared. Then, the T2 relaxation time (T2 a ) and the T2 relaxation time of mixture b (T2 b ) is measured and the Rsp value is calculated using the following formula (1).
[0019] Rsp = (R a / R b )-1 (1) (In the above formula (1), R a is T2 a represents the reciprocal of R b is T2 b (represents the reciprocal of
[0020] The Rsp value calculated by formula (1) is a physical property value that is an index of the degree of water affinity of the polymer dispersant. It is preferable to prepare a plurality of mixtures a, each of which contains different types of polymer dispersants and / or water-soluble organic solvents, and a plurality of mixtures b, each of which contains different types of water-soluble organic solvents, and obtain the Rsp value for each of the combinations of mixtures a and b.
[0021] In this embodiment, a mixture o is prepared, which contains a polymer dispersant and water and in which the concentration of the polymer dispersant is substantially the same as the concentration of the polymer dispersant in the mixture a. Then, the T2 relaxation time (T2 o ) and the T2 relaxation time of water (T2 w ) and calculate Rsp using the following formula (2) o The mixture o is preferably prepared by mixing the acid-precipitated polymer dispersant, water, and a neutralizing agent to dissolve the polymer dispersant, and then diluting the mixture with water.
[0022] Rsp o =(R o / R w )-1 (2) (In the above formula (2), R o is T2 orepresents the reciprocal of R w is T2 w (represents the reciprocal of
[0023] Rsp calculated using formula (2) o The Rsp value is a physical property that is an index of the degree of water affinity of the polymer dispersant, similar to the Rsp value calculated by formula (1). In addition, multiple mixtures o with different types of polymer dispersants were prepared, and the Rsp o It is preferable to obtain a value.
[0024] Examples of pulse sequences for measuring pulse NMR include the Hahn echo method, the solid echo method, the CPMG method, and the saturation recovery method. Since the measurement target is an aqueous sample containing multiple components, it is preferable to apply the CPMG method. An example of the measurement conditions for pulse NMR is shown below. Measurement equipment: Product name "TD-NMR Spectrometer Spin Track", manufactured by Resonance Systems, Observation nuclei: 1 H Pulse sequence: CPMG (Carr-Purcell-Meiboom-Gill) method ·Measurement temperature: 30℃ Sample volume: ≦2.0mL
[0025] Obtained Rsp value and Rsp o From value, Rsp oThe Rsp value reduction rate (%) is calculated based on the value. Based on the magnitude of the Rsp value reduction rate (%) calculated in this way, the dispersibility of the organic pigment in the aqueous pigment dispersion can be evaluated. In the manufacturing method of this embodiment, a mixture a is selected in which the Rsp value reduction rate (%) is 20% or more, preferably 30% or more, and more preferably 40% or more. Then, the polymer dispersant and water-soluble organic solvent contained in the selected mixture a, as well as the organic pigment and water, are mixed to prepare a raw material mixture such as a mill base. The prepared raw material mixture such as a mill base is dispersed, and the organic pigment is dispersed in the raw material mixture, thereby obtaining the desired aqueous pigment dispersion. The raw material mixture after the dispersion treatment may be used as the aqueous pigment dispersion as it is, or may be diluted with a liquid medium such as water as necessary, or may be filtered through a filter to remove coarse particles, to obtain the aqueous pigment dispersion.
[0026] The composition of mixture a is preferably the same as the raw material mixture such as a mill base, except that it does not contain an organic pigment, and more preferably it is substantially the same. The composition of mixture b is preferably the same as the raw material mixture such as a mill base, except that it does not contain an organic pigment component and a polymer dispersant, and more preferably it is substantially the same. The composition of mixture a being "same as" the raw material mixture except that it does not contain an organic pigment means that the composition of mixture a is the same as the raw material mixture in which the organic pigment in the raw material mixture is replaced with the same amount of water. Similarly, the composition of mixture b being "same as" the raw material mixture except that it does not contain an organic pigment and a polymer dispersant means that the composition of mixture b is the same as the raw material mixture in which the organic pigment and the polymer dispersant in the raw material mixture are replaced with the same amount of water.
[0027] Each of the mixture a, the mixture b, and the mixture o may further contain other additives. Examples of the other additives include alkalis used for neutralizing the polymer dispersant or adjusting the pH. Examples of the alkalis include ammonia, dimethylaminoethanol, sodium hydroxide, lithium hydroxide, and potassium hydroxide. The content of the alkali in the mixture is preferably 0.5 to 5 mass%.
[0028] As the organic pigment, organic pigments used in ordinary inkjet inks such as CI Pigment Blue 15:3, 15:4, 15:6; CI Pigment Red 122, 176, 254, 269, 291; CI Pigment Violet 19, 23; CI Pigment Yellow 74, 155, 180; CI Pigment Green 36, 58; CI Pigment Orange 43, 71; CI Pigment Black 7; and CI Pigment White 6 can be used.
[0029] The average particle size (primary particle size) of the organic pigment is preferably 250 nm or less, and more preferably 150 nm or less. By using an organic pigment having an average particle size within the above range, the optical density, saturation, and color development properties of the recorded image are improved, the ink ejection stability and print quality can be improved, and sedimentation of the organic pigment in the ink can be appropriately suppressed. The average particle size of the organic pigment is determined by the median diameter (D) measured using an electron microscope or a particle size distribution meter using a dynamic light scattering method. 50 ).
[0030] The content of the pigment in the aqueous pigment dispersion is preferably 5 to 30% by mass, and more preferably 10 to 20% by mass. If the content of the pigment is less than 5% by mass, it may be difficult to add additives when preparing the ink. On the other hand, if the content of the pigment is more than 30% by mass, the free movement of the pigment particles may be hindered, and the pigment may be more likely to aggregate.
[0031] As the polymer molecular dispersant, it is preferable to use a block copolymer having a hydrophobic segment and a hydrophilic segment derived from a methacrylate monomer containing methacrylic acid. The hydrophobic segment is a polymer block that is insoluble in an aqueous medium. Examples of components (monomers) that constitute the hydrophobic segment include vinyl monomers; aliphatic, alicyclic, and aromatic alkyl (meth)acrylates; and monomers having a hydroxyl group or an amino group.
[0032] The hydrophilic segment is a hydrophilic polymer block containing a constituent unit derived from a monomer having an acid group. As the monomer having an acid group, a monomer having a carboxy group, a sulfonic acid group, a phosphoric acid group, or the like can be used. As the monomer having a carboxy group, acrylic acid, an acrylic acid dimer, methacrylic acid, maleic acid, itaconic acid, fumaric acid, crotonic acid, or the like can be mentioned. Furthermore, there can be mentioned a monomer in which a hydroxyalkyl (meth)acrylate such as 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate is reacted with maleic anhydride, succinic anhydride, phthalic anhydride, or the like.
[0033] Examples of monomers having a sulfonic acid group include styrene sulfonic acid, dimethylpropylsulfonic acid (meth)acrylamide, sulfonic acid ether (meth)acrylate, sulfonic acid ether (meth)acrylamide, vinyl sulfonic acid, etc. Examples of monomers having a phosphoric acid group include methacryloxyethyl phosphoric acid ester, etc.
[0034] If the amount of the polymer dispersant is too small, the organic pigment cannot be covered and encapsulated, and it may be difficult to improve the dispersibility. On the other hand, if the amount of the polymer dispersant is too large, the viscosity of the raw material mixture to be dispersed may become too high, and the efficiency of the dispersion treatment may be easily reduced. For this reason, the content of the polymer dispersant in the aqueous pigment dispersion is preferably 5 to 50 parts by mass, more preferably 10 to 30 parts by mass, relative to 100 parts by mass of the organic pigment.
[0035] Examples of the water-soluble organic solvent include alcohol solvents such as methanol, ethanol, isopropanol, propyl alcohol, butanol, and isobutanol; glycol solvents such as ethylene glycol, propylene glycol, and glycerin; diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, tetraethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monopropyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monopropyl ether, propylene glycol monopropyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monopropyl ether, propylene glycol monopropyl ether, dipropylene glycol monopropyl ether, tri ... Examples of suitable solvents include glycol ethers such as ethylene glycol monomethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol butyl methyl ether, dipropylene glycol dimethyl ether, and 3-methoxy-3-methyl-1-butanol; amide solvents such as dimethylformamide, dimethylacetamide, pyrrolidone, N-methylpyrrolidone, 3-methoxy-N,N-dimethylpropanamide, and 3-butoxy-N,N-dimethylpropanamide; carbonate solvents such as ethylene carbonate, propylene carbonate, and dimethyl carbonate; dimethyl sulfoxide; tetramethylurea; and dimethylimidazolidinone.
[0036] The water-soluble organic solvent has the role of wetting the surface of the organic pigment in a dry state, replacing the air layer on the surface with the aqueous medium, and dissolving the polymer dispersant, thereby facilitating the progress of the dispersion treatment. However, if the amount of the water-soluble organic solvent is too large, the viscosity of the aqueous pigment dispersion becomes excessively high, and the drying property of the resulting ink may be easily deteriorated. For this reason, the content of the water-soluble organic solvent in the aqueous pigment dispersion is preferably 5 to 80 parts by mass, more preferably 10 to 50 parts by mass, relative to 100 parts by mass of the organic pigment.
[0037] A method for dispersing a raw material mixture such as a mill base can employ a conventionally known method. For example, an organic pigment can be dispersed by treating the raw material mixture using a dispersing machine. Examples of dispersing machines include kneaders such as kneader, two-roll mill, three-roll mill, SS5 (trade name, manufactured by M Technique Co., Ltd.), and Miracle KCK (trade name, manufactured by Asada Iron Works Co., Ltd.); high-speed mixers; ultrasonic dispersers; and high-pressure homogenizers. Examples of high-speed mixers include, under the trade names below, TK Homomixer, TK Robomix, and TK Filmix (all manufactured by Primix Co., Ltd.); Clearmix (manufactured by M Technique Co., Ltd.); and Ultra Disper (manufactured by Asada Iron Works Co., Ltd.). Examples of high-pressure homogenizers include, under the trade names below, Microfluidizer (manufactured by Mizuho Kogyo Co., Ltd.), Nanomizer (manufactured by Yoshida Kikai Kogyo Co., Ltd.), Starburst (manufactured by Sugino Machine Co., Ltd.), and G-Smasher (manufactured by Ricks Co., Ltd.). Also usable are ball mills, sand mills, horizontal media mill dispersers, colloid mills, etc., using bead media such as glass or zircon. As the media used in the bead mill, bead media having a diameter of 1 mm or less is preferable, and bead media having a diameter of 0.5 mm or less is more preferable.
[0038] The mixture of raw materials such as a mill base may be dispersed to obtain an aqueous pigment dispersion as it is, or coarse particles may be removed as necessary. To remove coarse particles, a centrifuge, an ultracentrifuge, a filter, or the like may be used.
[0039] The aqueous pigment dispersion may further contain additives such as an organic solvent other than the water-soluble organic solvent described above, a leveling agent, a surface tension adjuster, a pH adjuster, an ultraviolet absorber, a light stabilizer, an antioxidant, a dye, a filler, a wax, a thickener, an antifoaming agent, an antifungal agent, a preservative, and an antistatic agent, as necessary.
[0040] Examples of the preservative include sodium benzoate, benzimidazole, thiabendazole, potassium sorbitanate, sodium sorbitanate, sodium dehydroacetate, thiazosulfamide, pyridinethiol oxide, etc. The content of the preservative in the aqueous pigment dispersant is preferably 0.05 to 2.0% by mass, and more preferably 0.1 to 1.0% by mass. EXAMPLES
[0041] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are by mass unless otherwise specified.
[0042] <Synthesis of polymer dispersant> (Polymer Dispersant D-1) 300 parts of diethylene glycol monobutyl ether (DEGMBE), 3 parts of 2-iodo-2-cyanopropane (CP-1), 52 parts of benzyl methacrylate (BzMA), 60 parts of methacrylic acid (MAA), 2.5 parts of azobisisobutyronitrile (AIBN), and 0.1 parts of iodosuccinimide (NIS) were placed in a reaction vessel and stirred while flowing nitrogen. The temperature was raised to 40°C and polymerization was carried out for 3 hours to form a BzMA / MAA polymer block, which is a hydrophilic segment. A part of the polymerization solution was sampled and measured by gel permeation chromatography (GPC) to find that the number average molecular weight (Mn) was 3,500, and the polymerization rate was about 100%.
[0043] A mixture of 35 parts of cyclohexyl methacrylate (CHMA), 70 parts of BzMA, 20 parts of methyl methacrylate (MMA), and 0.2 parts of AIBN was added to the polymerization solution. Polymerization was carried out at 40°C for 3 hours to form a hydrophobic segment, a CHMA / BzMA / MMA polymer block, and a polymer dispersant D-1, an AB block copolymer, was obtained. The Mn of the obtained polymer dispersant D-1 was 7,500, and the acid value was 146 mg KOH / g. After adding an amount of lithium hydroxide aqueous solution to neutralize the carboxyl group, acetic acid was added dropwise while stirring. The precipitate was washed with pure water, and then pure water and a lithium hydroxide aqueous solution were added to obtain a light brown transparent aqueous solution of polymer dispersant D-1. The solid content of the obtained aqueous solution was 40%, and the pH was 9.3.
[0044] (Polymer Dispersant D-2~5) Aqueous solutions of polymer dispersants D-2 to D-5 were obtained in the same manner as for the above-mentioned polymer dispersant D-1, except that the materials (monomers) of the types and amounts shown in Table 1 were used. The solid content of each of the obtained aqueous solutions was 40%.
[0045] TIFF2024156542000001.tif70170
[0046] <Pulsed NMR measurement method> The T2 relaxation times (T2 a , T2 b , T2 o , and T2 w The T2 relaxation time was measured three times and the average value was used. The Rsp value was calculated using the following formula (1) and the Rsp o The values are calculated and Rsp o The rate of decrease in Rsp value based on the value (%) (= {(Rsp o -Rsp) / Rsp o} × 100) was calculated. [Pulse NMR measurement conditions] Measurement equipment: Product name "TD-NMR Spectrometer Spin Track", manufactured by Resonance Systems, Observation nuclei: 1 H Pulse sequence: CPMG (Carr-Purcell-Meiboom-Gill) method ·Measurement temperature: 30℃ Sample volume: ≦2.0mL
[0047] Rsp = (R a / R b )-1 (1) (In the above formula (1), R a is T2 a represents the reciprocal of R b is T2 b (represents the reciprocal of Rsp o =(R o / R w )-1 (2) (In the above formula (2), R o is T2 o represents the reciprocal of R w is T2 w (represents the reciprocal of
[0048] <Production of aqueous pigment dispersion (1)> Example 1 212.5 parts of the aqueous solution of polymer dispersant D-1, 52.5 parts of triethylene glycol monobutyl ether (TEGMBE), and 140 parts of pure water were mixed. 150 parts of pure water were added and mixed to obtain mixture a. 2 mL of the obtained mixture a was sampled and measured by pulse NMR to determine the T2 relaxation time (T2 a ) value was obtained. Mixture b was obtained by mixing 52.5 parts of TEGMBE and 502.5 parts of pure water. 2 mL of the obtained mixture b was sampled and pulse NMR was measured to obtain the T2 relaxation time (T2 b ) value was obtained. The Rsp value was calculated from formula (1). Furthermore, 212.5 parts of the aqueous solution of polymer dispersant D-1 and 342.5 parts of pure water were mixed to obtain mixture o. 2 mL of the obtained mixture o and 2 mL of pure water were sampled and pulse NMR was measured to obtain the T2 relaxation time (T2 o and Tw ) was obtained. Then, from equation (2), Rsp o The calculated Rsp value and Rsp o The "Rsp value reduction rate (%)" was calculated from the values. The results are shown in Table 2.
[0049] 212.5 parts of an aqueous solution of polymer dispersant D-1, 52.5 parts of TEGMBE, and 140 parts of pure water were mixed. 150 parts of copper phthalocyanine pigment (PB-15:3, product name "Cyanine Blue A220JC", manufactured by Dainichi Seika Chemicals Co., Ltd.) were added, and the mixture was stirred for 30 minutes using a disperser to prepare a mill base. The pigment was thoroughly dispersed in the mill base using a horizontal media disperser (product name "Dyno Mill 0.6 liter ECM type", manufactured by Shinmaru Enterprises Co., Ltd., zirconia bead diameter: 0.3 mm). The pigment was diluted with pure water until the pigment concentration reached 14%, and then filtered through a membrane filter with a pore size of 5 μm to obtain an aqueous pigment dispersion S1 (cyan color) for inkjet. The average particle diameter (median diameter; D 50 (nm) are shown in Table 2.
[0050] (Example 2, Comparative Examples 1 to 3) Aqueous pigment dispersions S2 to S5 (cyan) for inkjet printing were obtained in the same manner as in Example 1, except that the types of polymer dispersants (aqueous solutions thereof) shown in Table 2 were used. o The rate of decrease in Rsp value (%) and the average particle size (nm) of the pigment in the dispersion are shown in Table 2. Figure 1 shows a graph plotting the "average particle size (nm)" against the "rate of decrease in Rsp value (%)."
[0051] <Evaluation (1)> (Storage stability) The prepared aqueous pigment dispersion was stored at 70° C. for one week. The average particle size, pH value, and viscosity of the pigment in the aqueous pigment dispersion were measured before and after storage, and the rate of change (%) of each was calculated. The storage stability of the aqueous pigment dispersion was evaluated according to the following evaluation criteria. The results are shown in Table 2. ◯: The rate of change in average particle size, pH value, and viscosity was all 5.0% or less. ×: The rate of change in at least one of the average particle size, pH value, and viscosity was 5.0% or more.
[0052] (Redispersibility) The aqueous pigment dispersion was diluted with pure water to prepare a sample with a pigment concentration of 3.5%. A drop of the prepared sample was placed on a concave slide glass using a pipette. The concave slide glass on which the sample was placed was placed in a thermohygrostat (product name "Low Temperature and Humidity Regulator PL-3J", manufactured by ESPEC Co., Ltd.) and heated at 60°C for 10 hours to dry the sample. Pure water was then dropped onto the dried residue on the concave slide glass, and the dispersion state was observed under a microscope, and the redispersibility of the aqueous pigment dispersion was evaluated according to the following evaluation criteria. The results are shown in Table 2. ○: Completely redispersed when visually observed. △: Partially redispersed, but visually visible residues were present. When there was little residue and the mixture was almost completely dispersed, it was rated as "○△". On the other hand, when there was a lot of residue and the mixture was more like a disintegrated state than a dispersed state, it was rated as "△×". ×: Not redispersed.
[0053] TIFF2024156542000002.tif61170
[0054] <Production of aqueous pigment dispersion (2)> Example 3 212.5 parts of an aqueous solution of polymer dispersant D-4, 52.5 parts of DEGMBE, and 140 parts of pure water were mixed. 150 parts of pure water were added and mixed to obtain mixture a. 2 mL of the obtained mixture a was sampled and measured by pulse NMR to determine the T2 relaxation time (T2 a ) value was obtained. In addition, 52.5 parts of DEGMBE and 502.5 parts of pure water were mixed to obtain mixture b. 2 mL of the obtained mixture b was sampled and pulse NMR was measured to obtain the T2 relaxation time (T2 b) value was obtained. The Rsp value was calculated from formula (1). Furthermore, 212.5 parts of the aqueous solution of polymer dispersant D-4 and 342.5 parts of pure water were mixed to obtain mixture o. 2 mL of the obtained mixture o and 2 mL of pure water were sampled and pulse NMR was measured to obtain the T2 relaxation time (T2 o and T w ) was obtained. Then, from equation (2), Rsp o The calculated Rsp value and Rsp o The "Rsp value reduction rate (%)" was calculated from the values. The results are shown in Table 3.
[0055] 212.5 parts of an aqueous solution of polymer dispersant D-4, 52.5 parts of DEGMBE, and 140 parts of pure water were mixed. 150 parts of copper phthalocyanine pigment (PB-15:3, product name "Cyanine Blue A220JC", manufactured by Dainichi Seika Chemicals Co., Ltd.) were added, and the mixture was stirred for 30 minutes using a disperser to prepare a mill base. The pigment was thoroughly dispersed in the mill base using a horizontal media disperser (product name "Dyno Mill 0.6 liter ECM type", manufactured by Shinmaru Enterprises, zirconia bead diameter: 0.3 mm). The pigment was diluted with pure water until the pigment concentration reached 14%, and then filtered through a membrane filter with a pore size of 5 μm to obtain an aqueous pigment dispersion S6 (cyan color) for inkjet. The average particle diameter (median diameter; D 50 (nm) are shown in Table 3.
[0056] (Examples 4 to 7) Aqueous pigment dispersions S7 to 10 (cyan color) for inkjet were obtained in the same manner as in Example 3 described above, except that the types and amounts of water-soluble organic solvents shown in Table 3 were used. The reduction rate (%) of the Rsp value and the average particle size (nm) of the pigment in the dispersion are shown in Table 3. FIG. 2 shows a graph in which "average particle size (nm)" is plotted against "reduction rate (%) of the Rsp value." The meanings of the abbreviations in Table 3 are as follows: BEG: Ethylene glycol monobutyl ether PFG: Propylene glycol monopropyl ether ·BDM: Diethylene glycol butyl methyl ether IPA: Isopropylene glycol ·MFG: Propylene glycol monomethyl ether
[0057] (Comparative Examples 4 and 5) An attempt was made to prepare aqueous pigment dispersions S11 and S12 for inkjet use in the same manner as in Example 3, except that the types and amounts of water-soluble organic solvents shown in Table 3 were used. However, due to poor dispersion, the desired dispersions could not be obtained.
[0058] Comparative Example 6 Except for not using a water-soluble organic solvent, an attempt was made to prepare an aqueous pigment dispersion S13 for inkjet use in the same manner as in Example 3. However, due to poor dispersion, the desired dispersion could not be obtained.
[0059] <Evaluation (2)> The storage stability and redispersibility of the prepared aqueous pigment dispersion were evaluated by the same method as in the above "Evaluation (1)". The results are shown in Table 3.
[0060] TIFF2024156542000003.tif86170 [Industrial Applicability]
[0061] The evaluation method of the present invention is useful as a method for predicting and evaluating a suitable combination of a polymer dispersant and a water-soluble organic solvent that will provide good dispersibility of an organic pigment when producing an aqueous pigment dispersion that has excellent dispersibility, storage stability, and redispersibility of the organic pigment.
Claims
1. A method for evaluating an aqueous pigment dispersion containing an organic pigment, a polymer dispersant, a water-soluble organic solvent, and water, comprising the steps of: obtaining a mixture a containing the polymer dispersant, the water-soluble organic solvent, and the water, but not containing the organic pigment; obtaining a mixture b containing the water-soluble organic solvent and the water, but not containing the organic pigment or the polymer dispersant; The T2 relaxation time (T2 a ) and the T2 relaxation time of the mixture b (T2 b ) and obtain the Rsp value by the following formula (1); obtaining a mixture o containing the polymer dispersant and the water, the mixture o having a concentration of the polymer dispersant equal to a concentration of the polymer dispersant in the mixture a; The T2 relaxation time (T2 o ) and the T2 relaxation time of the water (T2 w ) was measured, and Rsp was calculated by the following formula (2). o obtaining a value; The Rsp o calculating a rate of decrease (%) of the Rsp value based on the Rsp value, and evaluating the dispersibility of the organic pigment in the aqueous pigment dispersion liquid based on the magnitude of the calculated rate of decrease; A method for evaluating an aqueous pigment dispersion having the following properties: Rsp = (R a / R b ) −1 ... (1) (In the above formula (1), R a is T2 a represents the reciprocal of R b is T2 b (represents the reciprocal of Rsp o = (R o / R w ) −1 ... (2) (In the above formula (2), R o is T2 o represents the reciprocal of R w is T2 w (represents the reciprocal of
2. The composition of the mixture a is the same as that of the raw material mixture used in the dispersion treatment of the organic pigment, except that the mixture a does not contain the organic pigment, The method for evaluating an aqueous pigment dispersion according to claim 1 , wherein the composition of the mixture b is the same as that of the raw material mixture except that the mixture b does not contain the organic pigment component and the polymer dispersant.
3. The method for evaluating an aqueous pigment dispersion according to claim 1 , further comprising the steps of: mixing the acid-precipitated polymer dispersant, the water, and a neutralizing agent to dissolve the polymer dispersant; and then diluting the mixture with the water to obtain the mixture o.
4. The method for evaluating an aqueous pigment dispersion according to any one of claims 1 to 3, wherein the polymer dispersant is a block copolymer having a hydrophobic segment and a hydrophilic segment derived from a methacrylate monomer containing methacrylic acid.
5. The method for evaluating an aqueous pigment dispersion according to any one of claims 1 to 3, wherein a content of the polymer dispersant in the aqueous pigment dispersion is 5 to 50 parts by mass with respect to 100 parts by mass of the organic pigment.
6. The method for evaluating an aqueous pigment dispersion according to claim 4, wherein a content of the polymer dispersant in the aqueous pigment dispersion is 5 to 50 parts by mass with respect to 100 parts by mass of the organic pigment.
7. A method for producing an aqueous pigment dispersion liquid containing an organic pigment, a polymer dispersant, a water-soluble organic solvent, and water, comprising the steps of: obtaining a plurality of mixtures a containing the polymer dispersant, the water-soluble organic solvent, and the water, but not containing the organic pigment, the mixtures a having different types of at least the polymer dispersant and the water-soluble organic solvent; obtaining a plurality of mixtures b containing the water-soluble organic solvent and the water, but not containing the organic pigment or the polymer dispersant, the mixtures b containing different kinds of the water-soluble organic solvent; The T2 relaxation times (T2 a ) and the T2 relaxation times (T2 b) and obtain the Rsp value by the following formula (1); obtaining a plurality of mixtures o containing the polymer dispersant and the water, the concentration of the polymer dispersant being the same as the concentration of the polymer dispersant in the plurality of mixtures a, and the mixtures o containing different types of polymer dispersants; The T2 relaxation times (T2 o ) and the T2 relaxation time of the water (T2 w ) was measured, and Rsp was calculated by the following formula (2). o obtaining a value; The Rsp o calculating a rate of decrease (%) of the Rsp value based on the value, and selecting the mixture a for which the calculated rate of decrease is 20% or more; a step of dispersing the organic pigment in a raw material mixture obtained by mixing the polymer dispersant and the water-soluble organic solvent contained in the selected mixture a, the organic pigment, and the water; A method for producing an aqueous pigment dispersion comprising the steps of: Rsp = (R a / R b ) −1 ... (1) (In the above formula (1), R a is T2 a represents the reciprocal of R b is T2 b (represents the reciprocal of Rsp o = (R o / R w ) −1 ... (2) (In the above formula (2), R o is T2 o represents the reciprocal of R w is T2 w (represents the reciprocal of
8. The composition of the mixture a is the same as that of the raw material mixture except that the mixture a does not contain the organic pigment, 8. The method for producing an aqueous pigment dispersion according to claim 7, wherein the composition of the mixture b is the same as that of the raw material mixture except that the mixture b does not contain the organic pigment component and the polymer dispersant.
9. The method for producing an aqueous pigment dispersion liquid according to claim 7, further comprising mixing the acid-precipitated polymer dispersant, the water, and a neutralizing agent to dissolve the polymer dispersant, and then diluting the mixture with the water to obtain the mixture o.
10. The method for producing an aqueous pigment dispersion liquid according to any one of claims 7 to 9, wherein the polymer dispersant is a block copolymer having a hydrophobic segment and a hydrophilic segment derived from a methacrylate monomer containing methacrylic acid.
11. 10. The method for producing an aqueous pigment dispersion according to claim 7, wherein a content of the polymer dispersant in the aqueous pigment dispersion is 5 to 50 parts by mass with respect to 100 parts by mass of the organic pigment.
12. The method for producing an aqueous pigment dispersion according to claim 10, wherein a content of the polymer dispersant in the aqueous pigment dispersion is 5 to 50 parts by mass with respect to 100 parts by mass of the organic pigment.
Citation Information
Patent Citations
Aqueous pigment dispersion and manufacturing method of aqueous ink, as well as design method of aqueous pigment dispersion and aqueous ink
JP2021172755A
Method for producing pigment dispersion resin and aqueous pigment dispersing element containing the resin
JP2002053628A
Aqueous pigment dispersion for inkjet ink, and aqueous pigment ink for inkjet printer
JP2012021120A
Aqueous ink-jet ink and ink-jet printing method using the ink
JP2017214469A
PIGMENT DISPERSION AND INK COMPOSITION FOR INKJET
JP4157868B2
Cited By
Method and apparatus for determining optical density of a solution
US12366528B2