Method for managing electro-deposition liquid, and electro-deposition device
By controlling the organic acid concentration in the electrodeposition solution using anion exchange treatment, the method stabilizes film formation and prevents blistering, ensuring high-quality insulating films on conductive substrates.
Patent Information
- Application Number
- JP2024017168
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-02-07
- Publication Date
- 2024-11-06
AI Technical Summary
The anionic electrodeposition method risks blistering during the baking process due to the increase in organic acid concentration, leading to instability in forming insulating films on conductive substrates.
Control the concentration of organic acid in the electrodeposition solution through anion exchange treatment, maintaining it within a specific range to prevent blistering and ensure stable film formation.
Stable formation of insulating films with suppressed blistering and improved insulation properties by managing the organic acid concentration in the electrodeposition process.
Smart Images

Figure 2024156602000003 
Figure 2024156602000004 
Figure 2024156602000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for managing an electrodeposition solution used when electrodepositing an electrodeposition film on a conductive substrate by anionic electrodeposition, and to an electrodeposition apparatus. [Background technology]
[0002] 2. Description of the Related Art Insulated conductors, which are made by covering a conductive base material with an insulating coating made of insulating resin, are widely used as conductive materials and heat sink materials for various electrical devices that require insulation. Various resins are used as constituent materials for the insulating coating. For example, Patent Document 1 discloses one that uses a polyimide resin such as polyamideimide resin, and Patent Document 2 proposes one that uses a mixed resin of a polyimide resin and a fluorine-based resin.
[0003] Electrodeposition is known as a method for forming an insulating film made of such an insulating resin on the surface of a conductive substrate. The electrodeposition method is a method in which a substrate on which an insulating film is to be formed and a counter electrode are immersed in an electrodeposition solution in which the material for the insulating film is dispersed, and a voltage is applied between the substrate and the counter electrode to form an electrodeposition film by depositing the material for the insulating film on the surface of the substrate.The formed electrodeposition film is then heated to bake the electrodeposition film onto the substrate, thereby forming the insulating film.
[0004] In addition, the electrodeposition method includes an anionic electrodeposition method in which a voltage is applied to the substrate as the anode to form an insulating coating on the substrate surface, and a cationic electrodeposition method in which a voltage is applied to the substrate as the cathode to form an insulating coating on the substrate surface. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-115120 A [Patent Document 2] JP 2018-070663 A Summary of the Invention [Problem to be solved by the invention]
[0006] Incidentally, the anionic electrodeposition solution used in the anionic electrodeposition method contains solid components including the above-mentioned resin, water, an organic solvent, and a neutralizing agent. When a voltage is applied, the pH decreases near the surface of the anode (substrate), and the solid components are precipitated on the surface of the anode (substrate), forming an electrodeposition film. Here, if electrodeposition is continued by an anionic electrodeposition method, there is a risk of blistering occurring when the electrodeposited film formed on the surface of the anode is baked to form an insulating coating.
[0007] The present invention has been made in consideration of the above circumstances, and aims to provide a method for managing an electrodeposition liquid and an electrodeposition apparatus that can suppress the occurrence of blisters when baking an electrodeposition film and can stably form an insulating coating. [Means for solving the problem]
[0008] In order to solve the above problems, the present inventors conducted extensive research and found that, when electrodeposition is continued using an anionic electrodeposition method, the concentration of the organic acid contained in the electrodeposition solution increases, causing swelling when the electrodeposition film is baked. Therefore, the inventors have found that by appropriately controlling the concentration of the organic acid contained in the electrodeposition solution, it is possible to suppress the occurrence of blistering during baking.
[0009] The present invention has been made based on the above-mentioned findings, and a method for managing an electrodeposition liquid according to a first aspect of the present invention is a method for managing an electrodeposition liquid used when forming an electrodeposition film on a conductive substrate by anion electrodeposition, and is characterized in that the concentration of an organic acid contained in the electrodeposition liquid is adjusted by subjecting the electrodeposition liquid to an anion exchange treatment.
[0010] According to the method for managing the electrodeposition solution of the first aspect of the present invention, the concentration of the organic acid contained in the electrodeposition solution is controlled. Therefore, even when electrodeposition is continuously performed, the concentration of the organic acid does not become excessively high, and the occurrence of blistering during baking can be suppressed, making it possible to stably form an insulating coating.
[0011] The method for managing an electrodeposition liquid according to a second aspect of the present invention is the method for managing an electrodeposition liquid according to the first aspect of the present invention, characterized in that the electrodeposition liquid contains water, an organic solvent, a solid component, and a neutralizing agent, and the solid component contains at least a polyimide-based resin. According to the method for managing an electrodeposition solution of the second aspect of the present invention, since the solid components contain at least a polyimide resin, it becomes possible to stably form an insulating film having excellent insulating properties.
[0012] The method for managing an electrodeposition liquid according to a third aspect of the present invention is the method for managing an electrodeposition liquid according to the first or second aspect of the present invention, characterized in that the electrodeposition liquid contains at least a carboxylic acid as the organic acid. According to the method for managing an electrodeposition solution of the third aspect of the present invention, the electrodeposition solution contains at least a carboxylic acid as the organic acid. Therefore, a rapid decrease in pH on the anode (substrate) surface can be suppressed by the pH buffer effect of the carboxylic acid, which is an organic acid, and an electrodeposition film can be stably formed.
[0013] The method for managing an electrodeposition liquid according to a fourth aspect of the present invention is the method for managing an electrodeposition liquid according to the first or second aspect of the present invention, characterized in that the electrodeposition liquid contains at least a hydroxy acid as the organic acid. According to the method for managing an electrodeposition solution of the fourth aspect of the present invention, the electrodeposition solution contains at least a hydroxy acid as the organic acid. Therefore, the pH buffer effect of the hydroxy acid, which is an organic acid, can suppress a rapid decrease in pH on the surface of the anode (substrate), and an electrodeposition film can be stably formed.
[0014] The method for managing an electrodeposition solution of the fifth aspect of the present invention is characterized in that, in the method for managing an electrodeposition solution of any one of the first to fourth aspects of the present invention, the concentration of the organic acid in the electrodeposition solution is adjusted to within a range of 5 mg / L or more and 500 mg / L or less. According to the electrodeposition solution of the fifth aspect of the present invention, the concentration of the organic acid is adjusted to within the range of 5 mg / L or more and 500 mg / L or less, so that an appropriate pH buffer effect can be exerted, and the electrodeposition film can be stably formed, while the occurrence of blistering during baking can be appropriately suppressed.
[0015] The method for managing an electrodeposition liquid according to a sixth aspect of the present invention is characterized in that, in the electrodeposition liquid according to any one of the first to fifth aspects of the present invention, the solid components contain a fluororesin together with a polyimide resin. According to the method for managing an electrodeposition solution of the sixth aspect of the present invention, since the solid components contain a fluororesin as well as a polyimide resin, it is possible to form an insulating film that is particularly excellent in insulating properties and dielectric properties.
[0016] The electrodeposition apparatus of the seventh aspect of the present invention is an electrodeposition apparatus used when forming an electrodeposition film on a conductive substrate by anion electrodeposition, and is characterized by comprising an electrodeposition tank in which an electrodeposition liquid is stored and in which the substrate and a counter electrode are immersed, an anion exchange means for performing an anion exchange treatment on the electrodeposition liquid, and an electrodeposition liquid circulation means for circulating the electrodeposition liquid between the electrodeposition tank and the anion exchange means.
[0017] According to the electrodeposition apparatus of aspect 7 of the present invention, the apparatus is provided with an electrodeposition tank, an anion exchange means for performing an anion exchange treatment on the electrodeposition liquid, and an electrodeposition liquid circulation means for circulating the electrodeposition liquid between the electrodeposition tank and the anion exchange means. This makes it possible to appropriately control the concentration of the organic acid contained in the electrodeposition liquid, and even when electrodeposition is continuously performed, the concentration of the organic acid does not become excessively high, making it possible to suppress the occurrence of blistering during baking, and enabling the stable formation of an insulating coating. Effect of the Invention
[0018] According to the present invention, it is possible to provide a method for managing an electrodeposition liquid and an electrodeposition apparatus that can suppress the occurrence of blisters when baking an electrodeposition film and can stably form an insulating coating. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a flow diagram showing a method for producing an insulating coating using an electrodeposition apparatus according to an embodiment of the present invention. [Diagram 2] 1 is a schematic explanatory diagram of an electrodeposition apparatus according to one embodiment of the present invention. [Diagram 3] FIG. 4 is a schematic explanatory diagram of an electrodeposition apparatus according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] A method for managing an electrodeposition solution and an electrodeposition apparatus according to one embodiment of the present invention will be described below. The method for managing an electrodeposition liquid according to the present embodiment is for managing an electrodeposition liquid used when forming an electrodeposition film, which serves as a precursor of an insulating film, on the surface of a conductive substrate. In this embodiment, the electrodeposition solution is controlled to be used in an anionic electrodeposition method in which a voltage is applied to a substrate as an anode to form an insulating film on the surface of the substrate, which serves as the anode.
[0021] In this embodiment, the electrodeposition solution to be managed contains water, an organic solvent, a solid component, and a neutralizing agent. As described above, the electrodeposition solution of the present embodiment is used in an anionic electrodeposition method, and therefore contains an amine as a neutralizing agent. The electrodeposition solution of the present embodiment may contain an appropriate amount of organic acid in advance. When the electrodeposition film contains an appropriate amount of organic acid, it is possible to suppress the occurrence of fine cracks in the baking step S03 described below.
[0022] The organic acid may contain at least a carboxylic acid, such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, and hydroxy acids. In particular, it is preferable that the organic acid contains at least a carboxylic acid. Examples of hydroxy acids include glycolic acid, hydroxypropionic acid, hydroxybutyric acid, tartronic acid, and glyceric acid. Hydroxypropionic acid and hydroxybutyric acid are effective regardless of the position of the functional group, so that even positional isomers are effective.
[0023] In this embodiment, the solid component contains at least a polyimide resin, and preferably contains two types of resin, a polyimide resin and a fluorine-based resin. In this embodiment, examples of the polyimide resin include polyamideimide, polyetherimide, polyimide, etc. Examples of the fluorine resin include polytetrafluoroethylene, perfluoroalkoxyalkane, etc.
[0024] The average particle size of the solid component may be from 50 to 300 nm, more preferably from 50 to 250 nm, and even more preferably from 50 to 200 nm. The standard deviation of the particle size of the solid component may be 250 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less.
[0025] The polyimide resin and the fluorine resin, which are solid components, are dispersed in the water and the organic solvent. Examples of the organic solvent include N,N-dimethylacetamide, propylene carbonate, dimethylsulfoxide, N,N-dimethylformamide, 4-butyrolactone, N-methyl-2-pyrrolidone, and N-methyl-2-pyrrolidone.
[0026] The water content in the electrodeposition solution is preferably 15% by mass or more, more preferably 50% by mass or more, while the water content in the electrodeposition solution is preferably 85% by mass or less, more preferably 75% by mass or less. Furthermore, the content of the organic solvent in the electrodeposition solution is preferably 15% by mass or more, more preferably 50% by mass or more, while the content of the organic solvent in the electrodeposition solution is preferably 85% by mass or less, more preferably 75% by mass or less.
[0027] Next, a method for producing an insulating film using an electrodeposition liquid will be described with reference to FIG. As shown in FIG. 1, the method for producing an insulating coating in this embodiment includes a surface pretreatment step S01, an electrodeposition film formation step S02, and a baking step S03.
[0028] (Surface pretreatment process S01) First, a substrate on which an electrodeposited film (insulating film) is to be formed is prepared. This substrate is conductive and is made of a metal material such as copper or a copper alloy, aluminum or an aluminum alloy, etc. Then, the oil and fat and oxide film adhering to the surface of the above-mentioned base material are removed using a surface treatment liquid such as an organic solvent or a surfactant.
[0029] (Electrodeposited film formation step S02) Next, the substrate and the counter electrode are immersed in the electrodeposition solution of this embodiment, and a voltage is applied between the anode (substrate) and the cathode (counter electrode) with the substrate as the anode and the counter electrode as the cathode. This reduces the pH of the electrodeposition solution around the substrate, and a solid component (in this embodiment, a mixture of polyimide resin and fluororesin) is precipitated on the surface of the substrate. This forms an electrodeposition film on the surface of the substrate. At this time, since an organic acid is added to the electrodeposition solution in this embodiment, the organic solvent is appropriately contained in the electrodeposition film due to the pH buffer effect of the organic acid.
[0030] The temperature of the electrodeposition liquid in the electrodeposition film forming step S02 is preferably adjusted to within a range of 5° C. or higher and 35° C. or lower. By keeping the liquid temperature at 5°C or higher, it is possible to prevent water from being mixed into the electrodeposition liquid due to condensation. On the other hand, by keeping the liquid temperature at 35°C or lower, the storage stability of the electrodeposition liquid is improved, and the electrodeposition film can be stably formed.
[0031] The voltage applied between the substrate (anode) and the counter electrode (cathode) in the electrodeposition film forming step S02 is preferably within the range of 10V or more and 600V or less. By setting the applied voltage to 10 V or more, the electrodeposition speed can be ensured and productivity can be improved. On the other hand, by setting the applied voltage to 600 V or less, the generation of many bubbles on the surface of the substrate can be suppressed, and the generation of many irregularities in the insulating coating due to the bursting of the bubbles in the subsequent baking step S03 can be suppressed.
[0032] (Baking process S03) In the baking step S03, the substrate on which the electrodeposition film containing the solid components obtained in the electrodeposition film formation step S02 has been formed is dried, for example, within a temperature range of 200° C. or higher and lower than the melting point of the solid components to remove the residual electrodeposition liquid, and then the electrodeposition film is baked onto the substrate to form an insulating coating.
[0033] The baking temperature in the baking step S03 may be within a temperature range in which the electrodeposition film of the solid components is formed and an insulating coating is formed on the substrate, for example, within a range of 200° C. to 400° C. The baking time may be within a range of, for example, 0.5 minutes to 60 minutes.
[0034] Through the above-mentioned steps, an insulating coating containing solid components is formed on the conductive substrate. If electrodeposition is continued, organic acids such as carboxylic acids are generated, and the concentration of the organic acids in the electrodeposition solution increases, which may cause blistering when the electrodeposition film is baked. Therefore, in this embodiment, the electrodeposition solution is managed so as to control the concentration of the organic acid in the electrodeposition solution.
[0035] Here, the electrodeposition apparatus 10 according to this embodiment and a method for managing the electrodeposition solution using this electrodeposition apparatus 30 will be described with reference to FIG. The electrodeposition apparatus 10 shown in FIG. 2 includes an electrodeposition tank 20 in which the electrodeposition liquid is stored and in which the substrate and the counter electrode are immersed, an anion exchange means 30 that performs an anion exchange treatment on the electrodeposition liquid, and an electrodeposition liquid circulation means 40 (an outlet pipe 41 and a return pipe 42) that circulates the electrodeposition liquid between the electrodeposition tank 20 and the anion exchange means 30.
[0036] An electrodeposition solution is stored in the electrodeposition tank 20, and a substrate serving as an anode and a counter electrode serving as a cathode are immersed in the electrodeposition solution. A voltage is applied between the substrate and the counter electrode to form an electrodeposition film on the surface of the substrate.
[0037] As shown in FIG. 2, the anion exchange means 30 includes an anion exchange tank 31 in which an anion exchange resin 32 is disposed. The electrodeposition liquid is supplied from the electrodeposition tank 20 to the anion exchange tank 31 via an outlet pipe 41. By storing the electrodeposition liquid in the anion exchange tank 31, organic acids contained in the electrodeposition liquid are removed by the anion exchange resin 32. This makes it possible to control the concentration of the organic acid contained in the electrodeposition solution. The organic acid contained in the electrodeposition solution can be carboxylic acid.
[0038] The electrodeposition liquid in which the concentration of the organic acid has been controlled in the anion exchange tank 31 is then supplied to the electrodeposition tank 20 via a return pipe 42 . Here, in the electrodeposition solution stored in the electrodeposition tank 20, the concentration of the organic acid is preferably controlled within the range of 5 mg / L or more and 500 mg / L or less.
[0039] According to the method for managing the electrodeposition solution of this embodiment configured as described above, the concentration of the organic acid contained in the electrodeposition solution is controlled. Therefore, even when electrodeposition is continuously performed, the concentration of the organic acid does not become excessively high, and the occurrence of blisters during baking can be suppressed, making it possible to stably form an insulating coating.
[0040] In the present embodiment, when the electrodeposition liquid contains water, an organic solvent, a solid component, and a neutralizing agent, and the solid component contains at least a polyimide-based resin, an electrodeposition film containing at least a polyimide-based resin can be formed, and an insulating film with excellent insulating properties can be stably formed.
[0041] In this embodiment, when the electrodeposition solution contains at least a carboxylic acid as an organic acid, the pH buffer effect of the organic acid can suppress a sudden drop in pH on the anode (substrate) surface, and an electrodeposition film can be stably formed.
[0042] In this embodiment, when the electrodeposition solution contains at least a hydroxy acid as an organic acid, the pH buffer effect of the organic acid can suppress a sudden drop in pH on the anode (substrate) surface, and an electrodeposition film can be stably formed.
[0043] In this embodiment, when the concentration of the organic acid in the electrodeposition solution is adjusted to within the range of 5 mg / L or more and 500 mg / L or less, a moderate pH buffer effect can be achieved, and the electrodeposition film can be stably formed while the occurrence of blistering during baking can be appropriately suppressed.
[0044] In the present embodiment, when the electrodeposition liquid contains a fluororesin together with a polyimide resin as solid components, an electrodeposition film containing a mixed resin of a polyimide resin and a fluororesin can be formed, and an insulating coating having particularly excellent insulating properties can be stably formed.
[0045] The electrodeposition apparatus 10 of this embodiment is equipped with an electrodeposition tank in which the electrodeposition liquid is stored and in which the substrate and the counter electrode are immersed, an anion exchange means for performing anion exchange treatment on the electrodeposition liquid, and an electrodeposition liquid circulation means for circulating the electrodeposition liquid between the electrodeposition tank and the anion exchange means. This makes it possible to appropriately adjust the concentration of the organic acid contained in the electrodeposition liquid, and even when electrodeposition is performed continuously, the concentration of the organic acid does not become excessively high, making it possible to suppress the occurrence of blistering during baking, and enabling the stable formation of an insulating coating.
[0046] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. In this embodiment, the electrodeposition apparatus shown in FIG. 2 has been described as an example, but the present invention is not limited to this, and electrodeposition apparatuses of other configurations may also be used.
[0047] For example, the electrodeposition apparatus 110 shown in Fig. 3 may be used. In the electrodeposition apparatus 110 shown in Fig. 3, the anion exchange means 130 for performing anion exchange treatment on the electrodeposition solution may include an ultrafiltration device 131 and an exchange membrane tank 132 in which anion exchange membranes 133 and cation exchange membranes 134 are alternately arranged. As another method for controlling organic acids, a method using electrodialysis may be applied. EXAMPLES
[0048] The results of confirmatory experiments conducted to confirm the effectiveness of the present invention will be described below.
[0049] As shown in Tables 1 and 2, water, an organic solvent, a solid component, a neutralizing agent, and an organic acid were prepared, and mixed in the mass ratios shown in Tables 1 and 2 to obtain electrodeposition solutions. In Inventive Examples 1 to 24, the electrodeposition solution was subjected to anion exchange treatment using the electrodeposition apparatus shown in Fig. 2. The resulting changes in the organic acid concentration are shown in Tables 1 and 2.
[0050] The concentration of the organic acid contained in the electrodeposited film was evaluated as follows. The electrodeposition solution was diluted with ultrapure water, and then impurities were removed. The filtrate was passed through a membrane filter to prepare a solution for ion chromatography measurement. Next, the measurements were performed using an ion chromatograph Thermo Fisher Scientific ICS-5000+. Anion exchange columns Dionex IonPac AG15 and Dionex IonPac AS15 were used as the stationary phase of the ion chromatograph, potassium hydroxide aqueous solution was used as the eluent, Dionex ADRS 600 was used as the suppressor, and electrical conductivity was used as the detector.
[0051] In addition, the electrodeposition solutions of Inventive Examples 1 to 24, which were subjected to anion exchange treatment, and the electrodeposition solutions of Comparative Examples 1 to 3, which were not subjected to anion exchange treatment, were evaluated for stability. When the electrodeposition solution was kept at 40°C for 5 days, the solution in which precipitation or separation occurred was evaluated as "X", and the solution in which no precipitation or separation occurred was evaluated as "O". The evaluation results are shown in Tables 1 and 2.
[0052] Then, a rectangular bar of oxygen-free copper (1.47 mm x 2.94 mm x 25 cm long) was prepared as a conductive substrate, and a cylindrical copper plate was prepared as a counter electrode. The substrate and the counter electrode were immersed in the above-mentioned electrodeposition solution, and an electrodeposition film was formed by setting the temperature of the electrodeposition solution to 20° C., the applied voltage to 300 V, and the retention time to 0.5 minutes. The electrodeposited film was then baked using a three-stage heating profile, in which the work temperature during baking was kept at 140-170°C for 10 minutes, at 240-260°C for 5 minutes, and at 340-350°C for 90 seconds, followed by rapid cooling, to form an insulating coating.
[0053] The appearance of the formed insulating film was then observed and evaluated for blistering. When blistering was observed by visual inspection, the case where blistering was observed in the insulating coating was rated as "present", and when no blistering was observed, the case where blistering was observed was rated as "absent". Furthermore, the relative dielectric constant of the insulating film was measured as follows. The evaluation results are shown in Tables 1 and 2. A measurement sample was prepared by applying silver paste to the surface of the insulating film at two 10 mm points on the edges and at a 100 mm area in the center. The capacitance between the conductor and the silver paste in the center was measured using a Hioki IM3536 LCR meter, and the relative dielectric constant was calculated from the measured capacitance and the thickness of the film.
[0054] [Table 1]
[0055] [Table 2]
[0056] In Comparative Examples 1 to 3, the organic acid concentration in the electrodeposition solution was not adjusted, and therefore the stability of the electrodeposition solution was evaluated as “×.” In addition, blisters occurred in the insulating coating after baking.
[0057] In contrast, in Examples 1 to 24 of the present invention, the organic acid concentration in the electrodeposition solution was adjusted, and therefore the stability of the electrodeposition solution was evaluated as "good." In addition, no blistering occurred in the insulating coating after baking. Furthermore, in Examples 18 and 19 of the present invention, polyimide resin and fluororesin were contained as solid components, and the relative dielectric constant was sufficiently low, and the insulating properties were particularly excellent.
[0058] From the results of the above confirmation experiments, it was confirmed that the present invention can provide a method for managing an electrodeposition liquid and an electrodeposition apparatus that can suppress the occurrence of blisters when baking an electrodeposition film and can stably form an insulating coating.
Claims
1. A method for managing an electrodeposition solution used in forming an electrodeposition film on a conductive substrate by anionic electrodeposition, comprising: A method for managing an electrodeposition solution, comprising adjusting a concentration of an organic acid contained in the electrodeposition solution by subjecting the electrodeposition solution to an anion exchange treatment.
2. 2. The method for managing an electrodeposition solution according to claim 1, wherein the electrodeposition solution contains water, an organic solvent, a solid component, and a neutralizing agent, and the solid component contains at least a polyimide resin.
3. 2. The method for managing an electrodeposition solution according to claim 1, wherein the electrodeposition solution contains at least a carboxylic acid as the organic acid.
4. 2. The method for managing an electrodeposition solution according to claim 1, wherein the electrodeposition solution contains at least a hydroxy acid as the organic acid.
5. 2. The method for managing an electrodeposition solution according to claim 1, wherein the concentration of said organic acid in said electrodeposition solution is adjusted to within a range of 5 mg / L to 500 mg / L.
6. 2. The method for managing an electrodeposition solution according to claim 1, wherein the electrodeposition solution contains, as solid components, a fluororesin in addition to a polyimide resin.
7. An electrodeposition apparatus used for forming an electrodeposition film on a conductive substrate by anionic electrodeposition, comprising: An electrodeposition apparatus comprising: an electrodeposition tank in which an electrodeposition liquid is stored and in which the substrate and a counter electrode are immersed; an anion exchange means for performing an anion exchange treatment on the electrodeposition liquid; and an electrodeposition liquid circulating means for circulating the electrodeposition liquid between the electrodeposition tank and the anion exchange means.
Citation Information
Patent Citations
Electrodeposition liquid for forming water dispersion type insulation film
JP2017115120A
Cationic electrodeposition coating composition
JP2018070663A