Improved microporous separator for lithium ion secondary battery and method related thereto

The dry process for manufacturing microporous battery separators using high molecular weight resins with controlled crystalline orientation addresses the balance of strength and porosity issues, enhancing tear resistance and energy density in lithium-ion batteries.

JP2024157017APending Publication Date: 2024-11-06CELGARD LLC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024137764
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2014-11-26
Filing Date
2024-08-19
Publication Date
2024-11-06

Smart Images

  • Figure 2024157017000001_ABST
    Figure 2024157017000001_ABST
Patent Text Reader

Abstract

To provide a separator for a thin film battery, a film, or a base film which are useful for various different purposes of using a high-energy battery and present improved toughness and excellent strength performance.SOLUTION: The present invention relates to an improved multilayered separator, a film, or a base film which includes at least one microporous film manufactured according to a dry stretch method of pressing polyolefin resin or a mixture thereof into a formed material. The resin has a melt flow index (MFI) of 0.8 g / 10 min at maximum. The separator has a thickness of at least 7 μm, a porosity in the range of approximately 30% to 50%, and an electric resistance (ER) of approximately 1.5 Ω-cm2. The separator may be arbitrarily selected from a separator of a single layer, a large number of layers, two layers, or three layers or may be a base film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to and the benefit of co-pending U.S. Provisional Patent Application No. 62 / 084,628, filed November 26, 2014, which is incorporated herein by reference in its entirety.

[0002] This application relates to one or more new or improved porous membranes, base films or battery separators and / or various methods of making and / or using such membranes, films or separators. According to at least selected embodiments, aspects or objects, this application or invention relates to one or more new or improved microporous membrane battery separators, membrane base films or membrane separators for lithium batteries, such as secondary or rechargeable lithium batteries, lithium ion secondary batteries, or the like, and / or various methods of making or using such separators and / or batteries. Certain inventive battery separators described herein may exhibit a thickness of less than about 14 μm and may exhibit increased strength performance, as defined by reduced splitting tendency or splitting rate, when compared to known battery separators. Splitting failure modes are investigated, and improvements in splitting tendency or splitting rate may be quantified as Composite Splittiness Index (CSI) by novel test methods disclosed herein. The new or improved membranes, films, or separators described herein may also exhibit improved Gurley and other improvements. [Background technology]

[0003] Certain previous methods for reducing tearing in microporous battery separator membranes, and in certain tear- or puncture-resistant microporous membranes, are known and are described in U.S. Patent No. 6,602,593, which describes, among other things, a method that includes extrusion of a thin film precursor by a blown film process and using a blow-up ratio (BUR) of at least about 1.5 during blown film extrusion.

[0004] US Patent No. 8,795,565 describes, among other things, a biaxial stretching technique that involves stretching both MD and TD of a dry precursor membrane with a controlled MD relaxation process step. Biaxially stretched membranes, such as those shown in Figures 1-3 of Patent No. 8,795,565, may have some reduction in tearing or rupture. When biaxially stretched microporous membranes are strength tested using a puncture strength test method, the test sample puncture site may be a round hole as opposed to an elongated tear.

[0005] U.S. Patent No. 8,486,556 discloses, among other things, multilayer battery separator membranes with improved strength as evidenced by a mixed penetration test method, which is a measurement of the force required to create a short circuit through the separator membrane. Using a high molecular weight polypropylene resin having a melt flow index, the multilayer separators described in the '556 patent have thicknesses up to about 25 μm, porosities up to about 37%, ASTM Gurleys of 13 to 25 seconds, and resistances of about 2.5 ohms cm. 2 The ionic resistance ranges from

[0006] Also known are wet-laid microporous battery separator membranes, which are typically also biaxially stretched to have well-balanced MD and TD strength properties. Examples of microporous membranes made using wet-laid methods may be found in U.S. Patent Nos. 5,051,183; 6,096,213; 6,153,133; and 6,666,969.

[0007] Wet battery separator membranes can be manufactured using high molecular weight polymer resins that can have molecular weights greater than 500,000, and in some cases greater than 1,000,000, allowing for melt extrusion using plasticizers. Such plasticizers, for example, one or more oils, can be used to melt extrude the high molecular weight resins. The plasticizers can be extracted using one or more solvents as part of the manufacturing process. The oil / plasticizer-containing solvent from the extraction step of the manufacturing process may need to be recycled to bring the extracted solvent and oil to a usable purity quality. This is an additional energy cost that can be expensive. Thus, the various wet methods of making battery separators can have the disadvantage of being environmentally problematic processes that can require costly solvent processing and various disposal issues compared to the solvent-free, "green" or environmentally friendly dry method of making battery separators (also called the Celgard dry process).

[0008] Various known methods, such as BUR blown film methods, methods involving TD stretching of dry membranes, and wet biaxial stretching methods for porous membranes, may not fully optimize the balance of strength or performance properties for microporous or membrane separators, for thin microporous or membrane separators, etc.

[0009] Also, previous methods or products may not combine strength or performance properties with a solvent-free, environmentally friendly process to produce microporous battery separators or membrane separators with excellent cycling performance and safety in lithium batteries, particularly high energy lithium ion batteries.

[0010] In view of the above, there is a need for new or improved porous membranes, base films or battery separators and / or methods of making and / or using such membranes, films or separators for at least certain battery technologies or applications, energy applications, and / or the like, including dry microporous battery separators or membrane separators with thicknesses of less than about 14 μm, relatively low Gurley numbers, relatively high porosity, and strength performance characteristics that approach or exceed those of wet battery separators or membrane separators without the possible undesirable problems associated with various wet manufacturing methods. Summary of the Invention [Means for solving the problem]

[0011] According to at least selected embodiments, aspects or objectives, the present invention may address one or more of the above-mentioned needs and / or relate to one or more new or improved porous membranes, base films or battery separators and / or various methods of making and / or using such membranes, films or separators. According to at least selected embodiments, aspects or objectives, the present application or invention relates to one or more new or improved microporous membrane battery separators, membrane base films or membrane separators for lithium batteries, such as secondary or rechargeable lithium batteries, lithium ion secondary batteries, or the like, and / or various methods of making or using such separators and / or batteries. Certain inventive battery separators described herein may exhibit a thickness of less than about 14 μm and may exhibit increased strength performance, as defined by reduced tear tendency or tear rate, when compared to known battery separators. The tear failure mode has been investigated, and the improvement in tear or tear rate may be quantified as a Composite Tear Index (CSI) by the novel test method disclosed herein. The new or improved membranes, films, or separators described herein may also exhibit improved Gurley and other improvements.

[0012] According to at least selected embodiments, aspects, or objectives, the present invention addresses one or more of the above-mentioned needs and relates to one or more new or improved porous membranes, base films, or battery separators (or membrane separators) and / or various methods of making and / or using such membranes, films, or separators. According to at least selected embodiments, aspects, or objectives, the present invention relates to one or more new or improved microporous membrane battery separators, membrane base films, or membrane separators (or membranes that function as at least one layer in the battery separator) for lithium batteries, such as lithium ion secondary batteries, and / or various methods of making or using such separators or films. Certain inventive battery separators described herein may exhibit a thickness of less than about 14 μm and may exhibit increased strength performance as evidenced by reduced tear or tear rate when compared to known battery separators. The tear failure mode has been investigated, and the improvement in tear tendency or tear rate may be quantified as a Composite Tear Index (CSI) by the novel test method disclosed herein. The new or improved membranes, films, or separators described herein may also exhibit improved Gurley and other improvements, and may be particularly suitable for energy applications.

[0013] The present invention relates to one or more novel or improved porous membranes, base films or battery separators and / or various methods of making and / or using such membranes, films or separators. According to at least selected embodiments, aspects or objectives, the present invention relates to one or more novel or improved microporous membrane battery separators for lithium batteries, such as lithium ion secondary batteries, and / or various methods of making or using such separators. The possibly preferred battery separators described herein may exhibit a thickness of less than about 14 μm, less than about 13 μm, or less than about 8 μm, and may surprisingly exhibit increased strength performance as evidenced by reduced tearing when compared to known battery separators of the same (or greater) thickness. The improvement in tearing or tearing may be quantified as a Composite Tear Index (CSI) by the test method disclosed herein, and the novel or improved separators described herein may have a CSI between 29 and 139, and may also exhibit improved Gurley and other improvements.

[0014] The present invention, at least in selected embodiments, relates to new or improved microporous battery separators for lithium ion secondary batteries, and / or related methods of making and / or using such separators. Certain inventive dry battery separators or membrane separators exhibit thicknesses of less than about 14 μm and have increased strength performance, as evidenced by tear resistance or reduced tear, as quantified by a novel test method known as the Composite Tear Index (CSI).

[0015] The blow-up ratio method may involve radial expansion of the blown film from an annular die. Increased levels of crystal structure orientation in the transverse direction (TD) may be achieved in extruded films using blow-up ratios greater than about 1.5. Such increased crystal structure orientation in the TD achieved by radial expansion of the blown extruded precursor film may further improve the TD tensile strength and TD elongation, resulting in reduced tearing in the stretched microporous film.

[0016] Round puncture holes may indicate reduced tear tendency or tear rate of the membrane, enhanced tear resistance, balanced TD and MD strength and good TD elongation, and therefore may predict excellent strength performance when such membrane is used as at least one layer in battery separator, membrane separator, base film, or battery separator in lithium ion battery.

[0017] Various known methods, such as BUR blown film methods, methods involving TD stretching of dry membranes, and wet biaxial stretching methods for porous membranes, may not fully optimize the balance of strength or performance properties for microporous separators or membranes less than about 14 μm thick: Excellent MD and TD tensile strength; ·Excellent TD elongation; High puncture strength; · desirable gurley; and / or No cracking. Additionally, it may be desirable to combine the above identified properties with the use of a solvent-free, environmentally friendly process to produce microporous battery separator membranes with excellent cycling performance and safety in lithium batteries, such as lithium ion batteries.

[0018] A new or improved microporous battery separator has been developed for use in lithium ion secondary batteries. The separator of the present invention is preferably a dry monolayer or multilayer microporous battery separator membrane manufactured using a high molecular weight, low melt flow index polymer resin or a blend of high molecular weight, low melt flow index polymer resins that, when extruded, creates a precursor membrane with an internal microstructure that does not require the use of plasticizers and has a relatively high level of crystalline lamellar orientation. This high level of crystalline lamellar orientation can provide improved strength performance of the separator of the present invention compared to known separators. The degree of crystallinity in the lamellar structure of the non-porous precursor membrane can also affect the formation of micropores during the stretching step in the dry process manufacture of a microporous separator, base separator or base film (adapted to be coated on one or both sides or laminated to one or more other layers) or membrane (serving as at least one layer of the separator or base film).

[0019] Manufacturers of batteries for the consumer electronics industry may prefer thin microporous membrane battery separators or membrane separators, preferably with a thickness of less than about 14 μm, to optimize energy density and improve cycle life of lithium ion secondary batteries. The battery separator or membrane of the present invention is a "thin" battery separator or membrane with a thickness of less than about 14 μm and improved strength performance as evidenced by reduced tear rate or reduced rupture as a result of puncture, when compared to other separators of the same thickness made by the same process, such as conventional dry stretching.

[0020] The separator or membrane of the present invention, at least in selected embodiments, may achieve a leap frog improvement over previous battery separators or membranes, since it provides a thin dry separator or membrane having a thickness of less than about 14 μm that is characterized by reduced tear. The possibly preferred inventive separator membrane preferably uses one or more high molecular weight, low melt flow index polymer resins or blends that, when extruded using a dry process without the use of solvents and extraction steps, produce a much higher crystalline lamellar content in the precursor membrane (compared to previously known precursor membranes). When the higher crystalline lamellar content precursor membrane is stretched to create holes, the resulting microporous membrane exhibits a reduction in tear behavior, improved strength, higher porosity, lower electrical resistance and lower Gurley. The dry microporous battery separator or membrane of the present invention, manufactured using high molecular weight, low melt flow index (MFI) polymer resins, can equal or exceed the performance characteristics of known wet separators, reduce or equalize the difference between dry and wet battery separator microporous membranes, and enhance or improve battery cycle life and safety performance in lithium ion secondary batteries.

[0021] The amount of crystallinity in the lamellar structure of the precursor film can affect the formation of the porous microstructure of the dry-stretched microporous membrane. XM Zhang et al., "Oriented Structure and Anisotropy Properties of Polymer Blown Films HDPE, LLDPE and LDPE", POLYMER 45 (2004) 217-229 and S. Tabatabaei et al., "Microporous Membranes Obtained from PP / HDPE Multilayer Films by Stretching", JMS 345 (2009) 148-159, state that the structure of the crystalline phase strongly influences the mechanical properties of the film. Rupture resistance can be an important mechanical property for microporous membranes used in lithium-ion batteries. Microporous membranes may require sufficient mechanical strength to resist tearing during the rigorous winding and / or manufacturing steps of the battery, and such membranes may need to withstand the expansion and contraction forces that occur during repeated charge and discharge cycles over the life of the battery.

[0022] The split resistance of microporous membranes is often described using the term "splittiness", which can be measured in MD or TD. A standard test method for measuring the mechanical strength of membranes is known as the pin puncture strength test. Figure 1 shows a photograph of a membrane sample undergoing pin puncture strength testing with the membrane sample securely fixed in place and a test needle positioned to penetrate the test sample. The pin puncture strength test measures the "load at break", which is the compressive extension (in mm) as a function of load (in grams force).

[0023] The puncture strength test data allows for the comparison of the mechanical strength performance of various porous membranes. In addition, this test method can be used to measure the resistance of a membrane to tearing or ripping when a force is applied. When a membrane test sample is tested for puncture strength, a test needle penetrates the test sample, leaving a mark or hole at the penetration location. In the research leading to the membrane of the present invention, it has been found that the shape of the puncture hole provides a means that can be used to evaluate the resistance of a membrane to tearing. Membrane samples that exhibit good resistance to tearing have been found to have circular puncture holes, such as those shown in Figure 2A, while membranes that are prone to tearing tend to form elongated ripped holes, such as those shown in Figures 2B and 2C.

[0024] Battery separator membranes that tear during the puncture strength test may be prone to tearing or breaking during the rigorous battery winding step in the manufacture of lithium ion secondary batteries and / or during use of such batteries. The force required to tear the membrane may be substantial. Battery separator membranes that tear easily may result in possible battery failure due to direct or indirect contact between the battery's electrodes and / or electrode particles penetrating the separator, causing an internal short circuit. Furthermore, battery separator membranes that are observed to tear during the puncture strength test may possibly result in mechanical failure of the battery, allowing the anode and cathode to come into contact, causing an internal short circuit in the battery. Effect of the Invention

[0025] Tear behavior has been measured for a series of membranes used as battery separators in lithium ion batteries, and the resulting data has been used to determine the tear mode or potential "tear failure" of a separator, such as a microporous membrane separator or base film, in a given battery through application of an inventive test method known as the Composite Tear Index (CSI). [Brief description of the drawings]

[0026] [Figure 1] 1 is a photograph of a microporous membrane undergoing a puncture strength test. [Diagram 2]FIG. 2A includes three close-up optical photographs of different shaped holes resulting from puncture testing of three different microporous membrane or separator test samples, with FIG. 2A being an inventive membrane or separator and showing substantially circular shaped holes, and FIG. 2B and FIG. 2C showing slit-like holes in a comparative sample. [Diagram 3] Included are scanning electron micrographs (SEM) of the surface of an etched nonporous polypropylene membrane showing the uniform and regular structure of the crystalline domains at two magnifications. [Figure 4] 1 is a stress strain plot showing the behavior of PP and HDPE during stretching. [Diagram 5] 1 is an SEM at 20,000x magnification of the surface of a prior art microporous membrane, CE6. [Figure 6] 1 is an SEM at 20,000x magnification of the surface of a prior art microporous membrane, CE5. [Figure 7] 1 is a plot of the shear viscosity of selected resins and films in accordance with various examples and comparative examples described herein. [Figure 8] 1 is a unimodal puncture strength test plot. [Figure 9] 1 is a bimodal puncture strength test plot. [Figure 10] 1 is an SEM of the surface of an exemplary inventive membrane or separator example 5. [Figure 11] 1 is an SEM of the surface of a comparative example 1 prior art membrane. [Figure 12] 1 is a photograph of inventive Example 5 showing substantially circular puncture holes. [Figure 13] 1 is a photograph of inventive Example 1 showing substantially circular puncture holes. [Figure 14] 1 is a photograph of inventive Example 2 showing substantially circular puncture holes. [Figure 15] 1 is a photograph of inventive Example 3 showing substantially circular puncture holes. [Figure 16] 1 is a photograph of a prior art membrane, CE4, showing punctures with elongated and / or slit-shaped holes. [Figure 17]1 is a photograph of a prior art membrane, CE2, showing punctures with elongated and / or slit-shaped holes. [Figure 18] 1 is a photograph of a prior art membrane, CE1, showing punctures with elongated and / or slit-shaped holes. [Figure 19] 1 shows Composite Severity Index (CSI) plots for inventive and prior art membranes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] According to at least some embodiments, aspects, or objectives, a new or improved microporous battery separator has been developed for use in lithium batteries, such as lithium ion secondary batteries. The separator membrane of the present invention is preferably a dry monolayer or multilayer microporous battery separator or membrane, preferably manufactured using a high molecular weight, low melt flow index polymer resin or a blend of high molecular weight, low melt flow index polymer resins, which when extruded (without the need for plasticizers that need to be extracted afterwards) creates a precursor membrane with an internal microstructure with a high level of crystalline lamellar orientation. This high level of crystalline lamellar orientation can result in the excellent strength performance of the separator or membrane of the present invention. Manufacturers of batteries for the consumer electronics industry may prefer a thin microporous battery separator or membrane with a thickness of less than about 14 μm to optimize the energy density and life of various lithium ion secondary batteries, especially energy batteries or cells. The battery separator or membrane of the present invention is preferably a "thin" membrane battery separator, base film or membrane with a thickness of less than about 14 μm, for example, with improved toughness and superior strength performance as evidenced by reduced tearing or rupture as a result of puncture, when compared to other separators of the same thickness made by conventional dry stretching processes. Such microporous membranes and / or battery separators may be particularly useful in various applications where high energy batteries are used.

[0028] The amount of crystalline lamellar structure in the precursor film can affect the formation of micropores. Figure 3 shows a surface SEM of the laminated lamellar structure of an etched non-porous polypropylene film that has not been MD or TD stretched. An etching step is performed to remove the non-crystalline portion, allowing for better visualization of the crystalline lamellar structure. The mode of pore formation in commonly known membranes is well known in the art and has been published in XM Zhang et al., "Oriented Structure and Anisotropy Properties of Polymer Blown Films HDPE, LLDPE and LDPE", POLYMER 45 (2004) 217-229 and S. Tabatabaei et al., "Microporous Membranes Obtained from PP / HDPE Multilayer Films by Stretching", JMS 345 (2009) 148-159. Figure 4 shows a typical stress / strain plot showing the response of a non-porous film to an applied stress, showing the pulling apart of the laminated crystalline lamellar plates upon the initial application of stress. Following this initial separation of the lamellar plates, the polymer chains are further pulled away from the lamellae to form fibrils. Further elongation of the polymer fibrils to form the walls of the pores is shown in FIG.

[0029] 5 and 6 are SEM images showing the microscale appearance of the surface of prior art polypropylene (PP) microporous membranes CE6 and CE5, respectively, with crystalline lamella and fibril structures visible. Comparison of the crystalline lamellar regions of CE6 and CE5 membranes shows that CE6 has thicker crystalline lamellar regions. In addition, the pore size of CE6 is approximately twice that of CE5. CE6 and CE5 membranes are manufactured using different molecular weight polypropylene resins with different melt flow indices (see Table 1), which may affect the amount of crystalline lamellae that form during melt extrusion of the precursor membrane. [Table 1] The amount of crystallinity in the lamellar structure of the precursor film may be a factor in the formation of the internal porous microstructure of the dry-stretched microporous membrane. It has been stated that the structure of the crystalline phase can affect the mechanical properties of the film (XM Zhang et al., "Oriented Structure and Anisotropy Properties of Polymer Blown Films HDPE, LLDPE and LDPE", POLYMER 45 (2004) 217-229).

[0030] The separator membrane of the present invention, at least in selected embodiments, can be prepared by dry-laid or dry-stretching (also known as CELGARD® dry-laid), and the membrane of the present invention can be monolayer or multilayer. In the case of a multilayer membrane or separator, the process can include: extruding PP and / or polyethylene (PE) non-porous precursors, bonding the non-porous precursors together, for example, in a PP / PE / PP stacking configuration, to form a bonded non-porous PP / PE / PP precursor, and stretching such precursors to form a microporous multilayer membrane, where pore formation results from stretching the non-porous, semi-crystalline extruded polymer precursor in the machine direction. Additional stretching (e.g., in TD) can also occur.

[0031] An important mechanical property for microporous membranes used in lithium-ion batteries is rupture resistance: the membrane should have sufficient rupture resistance so that it does not tear or tear during winding of the battery and can withstand the expansion and contraction forces that occur during repeated charge and discharge cycles over the life of the battery.

[0032] The tear resistance of a microporous membrane is often described using the term "tear", which can be measured in MD or TD. A standard test method for measuring the mechanical strength of a membrane is known as a pin strength test. Figure 1 shows a photograph of a membrane sample secured in place in a pin strength tester set up with a test needle positioned to penetrate the test sample. The pin strength test applies a load (stress) and measures the compressive extension (displacement) in millimeters. Figure 8 shows an example of a pin strength plot where the "load at break" is determined as the maximum load at which a hole is created in the sample. In this example plot, puncture tests were performed at 15 locations on the test sample, although typically 30 locations are tested and the maximum load at break is defined as the average. In this example, the applied load was increased to about 350 grams force when the test membrane sample was displaced downwards about 6 mm and the sample was punctured. The linear relationship observed between the applied load and the resulting displacement of the test membrane produced a "unimodal" plot.

[0033] The puncture strength test data allows for the comparison of strength performance of various porous membranes. Figure 9 shows an example of a multi-layer membrane separator or membrane of the present invention where a test needle first punctures one layer of the membrane and continues to apply a downward load to further puncture the test sample completely, resulting in a bimodal plot. The first puncture is defined as the "first load apex", while the second puncture is defined as the "second load apex".

[0034] In addition to measuring the load to break, this test method can be used to apply a force to assess the resistance of a membrane to tearing or ripping. During the puncture strength test, a needle penetrates the test sample leaving a mark or hole at the penetration location. The shape of the puncture hole, as well as the load required to measure the hole, provide a means that can be used to measure the comparative resistance to tearing or ripping or to measure the tear rate of the membrane. The length of the hole (or diameter, if the puncture hole is circular in shape) was measured to the nearest millimeter using a ruler for a commercial microporous membrane and various membranes according to the present invention. Membrane samples that exhibit good resistance to tearing have been found to have circular holes as shown in FIG. 2A. In contrast, FIG. 2B shows a membrane that was punctured to a length of 3.5 cm in a straight line in one test and 9 mm in a repeated test. Films that mechanically tear and fail in this manner will likely tear during the rigorous battery winding steps during battery manufacture and / or will not be able to prevent contact between the anode and cathode electrodes during battery use, resulting in an internal short circuit in at least some batteries or applications.

[0035] The mechanical strength of a porous membrane is also commonly evaluated by measuring the tensile strength in machine direction (MD) and transverse direction (TD). Machine direction is defined as the length direction in sheet production, while transverse direction is defined as the width direction in sheet production. In addition, the distance that a membrane stretches from its original size to the point of failure is defined as elongation, and can be important in assessing the amount of strain that a membrane can undergo without failure. Elongation can be measured in MD and TD.

[0036] Mechanical strength test data has been used to investigate the tear mode or "tear failure" tendency. An inventive test method known as Composite Tear Index (CSI) has been developed where the CSI value is defined by Equation 1 (described below), where CSI is a function of the first load apex, second load apex, TD tensile strength, MD tensile strength, and TD elongation measured during the puncture strength test. CSI=(A-|BA| 1.8 )×C×(D×E) / 106 formula 1 During the ceremony: A = first load apex / thickness x (1-porosity ratio) B=second load apex / thickness C=TD extension D=MD tensile strength E = TD tensile strength where the first and second load peaks are in grams force, the thickness values ​​are in microns, the MD and TD tensile strengths are in grams force, and the TD elongation is expressed as a percentage. High CSI values ​​predict microporous membranes that may have superior strength performance in lithium ion batteries, both during the battery winding step in the manufacturing process, and during the expansion and contraction of the membrane that may occur during repeated charge and discharge cycles over the life of the battery.

[0037] example Various microporous membranes or separators were made according to the present invention. In particular, Examples 1-5 were produced as either monolayer PP membranes or trilayer (PP / PE / PP) membranes and were made using various low MFI (melt flow index) polypropylene resins. Some of the examples included blends of polypropylene resins with slightly different (low) MFI values ​​(as shown in Table 2).

[0038] Table 2 lists the resin and membrane properties of inventive membrane examples 1 to 5. In addition, comparative examples CE1 to CE6 are provided to allow comparison of the membranes of the present invention with conventional membranes. [Table 2] A = first load apex / thickness x (1-porosity ratio) B=second load apex / thickness C=TD extension D=MD tensile strength E = TD tensile strength

[0039] Examples 1-3 are single layer PP microporous membranes, while Examples 4 and 5 are three layer PP / PE / PP microporous membranes. The membranes of the present invention have thicknesses of about 13.5 μm or less, while the comparative membranes have higher thickness values ​​of about 16 μm to about 25 μm, with CE4-CE6 being more than three times thicker than Examples 1-3. Examples 1, 2 and 3 of the battery separator examples of the present invention are more than 46% thinner than the comparative prior art examples at the comparative level of porosity, and show a significant increase in mechanical strength as defined by the CSI number. The CSI number is calculated using Equation 1 and is a function of thickness, porosity, pin puncture strength, TD elongation, and MD and TD tensile strength.

[0040] The monolayer membranes of the invention, Examples 1-3, are each about 7 μm thick, making them extremely thin battery separators or membranes. For example, inventive PP monolayer membrane, Example 2, has a CSI value of 138 at a thickness of 7 μm. Comparative PP monolayer, Example CE1, at a thickness of 16 μm (more than twice the thickness of Examples 1-3), has a much lower CSI value of only 16. Furthermore, inventive trilayer membrane, Example 5, has a CSI value of 141 at a thickness of 13.5 μm. The outer PP layer in the trilayer, Example 5, is manufactured using a PP resin with an MFI value of 0.3 g / 10 min, showing the advantage that a low MFI, high molecular weight, PP resin can contribute to the CSI value of a porous separator membrane. The comparative prior art 3-ply CE2 with a thickness of 16.7 μm has a much lower CSI value of −100, and it is expected that this separator may have lower strength capabilities for some batteries compared to the separator of the present invention during the cell winding step in the manufacturing process and during the expansion and contraction of the membrane that may occur during repeated charge and discharge cycles over the life of the battery. A membrane with a low CSI value may tear for some batteries and may not be able to mechanically prevent the anode and cathode electrodes from contacting, resulting in an internal short circuit in the battery.

[0041] The membranes of the present invention may have higher levels of crystalline lamellae because they are produced using one or more low melt flow index (MFI), higher shear viscosity, high molecular weight polypropylene polymer resins. Figure 7 shows the shear viscosity of the inventive examples compared to the comparative examples. The membranes of Examples 1-5 have higher shear viscosity curves compared to CE1, CE3, CE4, CE5, and CE6. The higher shear viscosity values ​​are a direct result of the lower MFI, higher molecular weight PP resins used in the production of the inventive examples.

[0042] A comparison of the SEM of the membrane CE6 shown in FIG. 5 to the membrane example 5 of the present invention shown in FIG. 10 shows that the membrane example 5 of the present invention has more pronounced uniform thickness regions of the crystalline lamellar layers and a higher uniformity of these crystalline lamellar regions compared to CE6. It is also noted that the pore size is smaller in the membrane of the present invention. FIG. 11 is an SEM of the surface of another comparative example CE1, showing a smaller amount of crystalline lamellae and larger pores compared to the membrane of the present invention in FIG. 10. The high level of crystalline lamellar orientation in the membrane of the present invention may affect the improved strength performance of the porous membrane and / or separator of the present invention. In addition, the uniformity of the highly crystalline lamellar structure of the non-porous precursor membrane may affect the improved strength performance of the porous membrane and / or separator of the present invention. Furthermore, both the high level of crystalline lamellar orientation and the uniformity of the highly crystalline lamellar structure of the non-porous precursor membrane may affect the formation of micropores during the stretching step. When the higher and more uniform crystalline lamellar precursor membrane is stretched to create pores, the resulting microporous membrane shows a reduction in tear behavior and a higher CSI value.

[0043] During the investigation of the tear mode, the puncture strength test shows that the membrane of the present invention has a different shape of puncture hole than the comparative membrane. The membrane of the present invention has a circular puncture hole, while the comparative prior art membrane may tend to tear and have a hole with a slit shape and / or a hole with a slit shape. The shape of the hole at the puncture site during the puncture strength test provides clues to understand the tear failure mode. Figure 12 shows a circular hole at the puncture site of Example 5 after the puncture strength test. The membranes of the present invention, Examples 1, 2, and 3, shown in Figures 13, 14, and 15, also have a circular hole at the puncture site after the puncture strength test. In contrast, Comparative Examples CE4, CE2, and CE1, shown in Figures 16, 17, and 18, respectively, have a hole with a slit shape and / or a slit shape, indicating a mechanically weaker membrane that may possibly tear during the stringent winding manufacturing step of the battery and / or during use for some batteries. In addition, a membrane that shows a tendency to tear during this puncture strength test will not be able to withstand the expansion and contraction forces that occur during repeated charge and discharge cycles over the life of a lithium ion battery for a given battery. Tear or rupture resistance can be an important requirement in the mechanical performance for lithium ion secondary batteries, particularly microporous membranes in high energy batteries or cells.

[0044] 19 is a plot of the composite tear index (CSI) calculated using Equation 1 and plotted against the slit length (in millimeters) of the hole measured from the pin puncture strength test sample. The membranes of the present invention, Examples 1, 2, 3, 4, and 5, have higher CSI values ​​and smaller puncture hole size (tear) than Comparative Example CE2, which indicates the superior mechanical strength performance of the membranes of the present invention and shows that the selection of higher molecular weight and lower melt flow index PP resin provides a new route to tailor the mechanical properties of microporous membranes for lithium ion batteries.

[0045] Test Method Thickness Thickness is measured using an Emveco Microgage 210-A precision micrometer thickness gauge according to test procedure ASTM D374. Thickness values ​​are reported in units of micrometers, μm.

[0046] Puncture strength The test samples are first conditioned at 73.4°C and 50% relative humidity for a minimum of 20 minutes. The puncture strength of the test samples is measured using an Instron Model 4442. Thirty measurements are taken across the diagonal of a 1 1 / 4" x 40" continuous sample specimen and averaged. The needle radius is 0.5 mm. The drop rate is 25 mm / min. The film is securely attached to a clamping device that utilizes an O-ring to hold the test sample firmly in place. The diameter of this clamped area is 25 mm. The displacement of the film pierced by the needle (in mm) is recorded versus the force (in grams force) exerted by the tested film. The maximum force is the puncture strength in grams force (gf). A load vs. displacement plot is generated with this test method.

[0047] Cleft degree The tear size of the test sample is measured using a ruler (marked to the nearest mm) to measure the length of the hole (or slit) created as a result of the needle piercing or penetrating the test sample during the Puncture Strength Test. The tear size is expressed in millimeters (mm) and is shown in Table 2 above as "Hole Size."

[0048] Pore ​​diameter Pore ​​size is measured using an Aquapore available from Porous Materials, Inc. (PMI). Pore size is expressed in μm.

[0049] porosity The porosity of the microporous film samples was measured using ASTM method D-2873 and is defined as the percent void spaces in the microporous membrane.

[0050] TD and MD tensile strength Tensile strength along MD and TD is measured using an Instron Model 4201 according to ASTM D-882 method.

[0051] Melt Flow Index (MFI) The Melt Flow Index of polymer resins is measured using ASTM DS 1238; to measure MFI for polyethylene: use 2.16 Kg weight at temperature = 190°C; for polypropylene: use 2.16 Kg weight at temperature = 230°C. MFI is measured as grams / 10 minutes.

[0052] Electrical Resistance (ER) (also known as Ionic Resistance IR) The electrical resistance in ohms-cm of the separator filled with electrolyte 2 The unit of electrical resistance is ohm-cm. 2 The separator resistance is characterized by cutting small pieces of separator from the raw product material and then placing them between two blocking electrodes. The separator is saturated with the battery electrolyte, which is 1.0 M LiPF6 salt in EC / EMC solvent in a 3:7 ratio by volume. The resistance value R of the separator in ohms (Ω) is measured by a four-probe AC ​​impedance method. To suppress the measurement error at the electrode / separator interface, multiple measurements are required by adding more layers. The electrical (ionic) resistance R of the separator saturated with electrolyte is then measured based on the multiple layer measurements. s (Ω) into the formula R s =ρ s Calculated by l / A, where ρ s is the ionic resistivity of the separator (in Ω-cm) and A is the electrode area (cm 2 ρ is the thickness of the separator in cm. s The ratio of / A is the calculated slope of the rate of change of separator resistance (ΔR) with respect to the multilayer (Δδ), where slope=ρ s / A=ΔR / Δδ.

[0053] Gurley Gurley is defined by the Japanese Industrial Standards (JIS) and is measured using an OHKEN Permeability Tester. JIS Gurley is defined as the time (in seconds) required for 100 cc of air to pass through 1 square inch of film under a constant water pressure of 4.9 inches.

[0054] According to at least selected embodiments, aspects, or objectives, one or more new or improved porous membranes, base films, or battery separators and / or various methods of making and / or using such membranes, films, or separators are provided. According to at least some embodiments, aspects, or objectives, the present invention relates to one or more new or improved microporous membrane battery separators for lithium batteries, such as lithium ion secondary batteries, and various methods of making or using such separators. The battery separators described herein may exhibit a thickness of less than about 14 μm and may exhibit increased strength performance as evidenced by reduced tear rate compared to known battery separators. The tear failure mode has been investigated, and the improvement in tear rate may be quantified as a composite tear index (CSI) by the test method disclosed herein. The new or improved separators described herein may also exhibit improved Gurley and other improvements.

[0055] The present invention, at least in selected embodiments, relates to new or improved microporous battery separators for lithium-ion secondary batteries, and / or related methods of making and / or using such separators. Certain inventive dry battery separators or membrane separators exhibit thicknesses of less than about 14 μm and have increased strength performance as evidenced by reduced tear. The tear failure mode has been investigated, and the improvement in tear has been quantified by a novel test method known as the Composite Tear Index (CSI).

[0056] Preferred embodiments include the inventive robust Celgard® brand battery separators designed to meet the needs of battery manufacturers to provide superior energy and / or power performance, dimensional integrity, and chemical and thermal stability in lithium battery applications.

[0057] The present invention may relate to one or more novel or improved porous membranes, base films or battery separators and / or various methods of making and / or using such membranes, films or separators. According to at least selected embodiments, aspects or objectives, the present application or invention relates to one or more novel or improved microporous membrane battery separators, membrane base films or membrane separators for lithium batteries, such as secondary or rechargeable lithium batteries, lithium ion secondary batteries, or the like, and / or various methods of making or using such separators and / or batteries. Certain inventive battery separators described herein may exhibit a thickness of less than about 14 μm and may exhibit increased strength performance as evidenced by reduced tear tendency or tear rate when compared to known battery separators. The tear failure mode has been investigated, and improvements in tear tendency or tear rate may be quantified as Composite Tear Index (CSI) by novel test methods disclosed herein. The novel or improved membranes, films or separators described herein may also exhibit improved Gurley and other improvements.

[0058] The present invention, at least in selected embodiments, relates to new or improved microporous battery separators for lithium-ion secondary batteries, and / or related methods of making and / or using such separators. Certain inventive dry battery separators or membrane separators exhibit thicknesses of less than about 14 μm and have increased strength performance as evidenced by reduced tear. The tear failure mode has been investigated, and the improvement in tear has been quantified by a novel test method known as the Composite Tear Index (CSI).

[0059] At least selected embodiments may relate to improved base films or battery separators and / or methods of making and / or using such membranes, films or separators, dry microporous battery separators or membrane separators with thicknesses of less than about 14 μm, relatively low Gurley numbers, relatively high porosity, and strength performance characteristics that approach or exceed those of wet battery separators or membrane separators, at least for certain battery technologies or applications, energy applications, and / or the like, without the potentially undesirable problems associated with various wet manufacturing methods.

[0060] The present invention may be embodied in other forms without departing from its spirit or essential characteristics, and accordingly, reference should be made to the appended claims, rather than the foregoing specification, as indicating the scope of the invention. Additionally, the present invention disclosed herein may suitably be practiced in the absence of any element not specifically disclosed herein.

[0061] The present invention also includes the following aspects. (1) An improved separator, membrane or base film for lithium batteries having a CSI of at least 29. (2) The separator according to (1), wherein the separator is a single-layer separator, membrane, or base film. (3) The separator according to (1), wherein the separator is a multi-layer separator, membrane or base film. (4) The separator according to (1), wherein the separator is a three-layer separator, membrane, or base film. (5) The separator according to (1), wherein the separator is produced by a dry stretching method. (6) The separator according to (1), wherein the separator is produced by a lamination process. (7) The separator according to (1), wherein the separator has a first load peak of a pin puncture strength (PS) of at least 130 gf. (8) The separator according to (1), wherein the separator has a first load apex of a pin puncture strength (PS) of at least 130 gf and a thickness of at least 7 μm. (9) The separator according to (1), wherein the separator has a porosity of at least 25%. (10) The separator according to (1), wherein the separator has a porosity of at least 27%. (11) The separator according to (1), wherein the separator has a porosity of at least 31%. (12) The separator according to (1), wherein the separator has a porosity in the range of about 30% to 50%. (13) The separator according to (1), wherein the separator has a porosity in the range of about 31% to 40%. (14) The separator according to (1), wherein the separator is particularly well suited for energy batteries, such as those used in consumer electronics. (15) The separator has a resistance of 1.5 ohm-cm 2 2. The separator according to (1), having an ER below, a porosity of at least 25%, and suitable for high energy cells or batteries. (16) The separator has a resistance of at least 150 kgf / cm 2 The separator according to (1), having a TD tensile strength of (17) The separator according to (1), wherein the separator has a CSI of greater than 30. (18) The separator according to (1), wherein the separator has a CSI of at least 50. (19) The separator according to (1), wherein the separator has a CSI of at least 100. (20) The CSI is based on an inventive test method known as the Composite Tear Index (CSI), where the CSI value is defined by Equation 1 (described below), where CSI is a function of the first load apex, the second load apex, TD tensile strength, MD tensile strength, and TD elongation measured during a Puncture Strength Test: CSI=(A-|BA| 1.8 )×C×(D×E) / 10 6 formula 1 During the ceremony: A = first load apex / thickness x (1-porosity ratio) B=second load apex / thickness C=TD extension D=MD tensile strength E = TD tensile strength wherein the first and second load peaks are in grams-force, the caliper values ​​are in microns, the MD and TD tensile strengths are in grams-force, and the TD elongation is expressed as a percentage, and a high CSI value can predict a microporous membrane that can have excellent strength performance in a secondary lithium battery. (twenty one) The separator according to (1), comprising at least one microporous polyolefin membrane manufactured according to a dry process in which a polyolefin resin is extruded to form the membrane, the resin having a melt flow index (MFI) of about 0.8 grams / 10 minutes or less. (twenty two) The separator according to (1), comprising at least one microporous polyolefin membrane manufactured according to a dry process in which a polyolefin resin is extruded to form the membrane, the resin having a melt flow index (MFI) of about 0.5 grams / 10 minutes or less. (twenty three) At least one microporous membrane made according to a dry process in which a polyolefin resin, mixture or blend is extruded to form said membrane, said resin having a melt flow index (MFI) of about 0.8 grams / 10 minutes or less; The separator has a thickness of about 7 μm or more, a porosity in the range of about 30% to about 50%, and a resistivity of about 1.5 ohm-cm 2 and having the following electrical resistance (ER): Optionally, the separator is a monolayer, multilayer, bilayer or trilayer separator or base film, made by a dry process, made by a lamination process, has a pin puncture strength (PS) of at least 130 gf and a thickness of at least about 7 μm, has a pin puncture strength (PS) of at least 200 gf and a thickness of at least about 7 μm, has a pin puncture strength (PS) of at least 390 gf and a thickness of at least about 13 μm, has a pin puncture strength (PS) of at least 200 gf and a thickness of at least about 7 μm, has a porosity of at least 25%, has a porosity of at least 27%, has a porosity of at least 31%, has a porosity in the range of about 30%-50%, has a porosity in the range of about 31%-40%, is particularly well suited for energy batteries, such as those used in consumer electronics, and has a porosity of 1.5 ohm-cm 2 ER of less than or equal to 0.25%, has a porosity of at least 25% and is suitable for high energy cells or batteries, comprises at least two microporous polyolefin membranes made according to a dry process in which a polyolefin resin is extruded to form said membranes, said resin having a melt flow index (MFI) of about 0.8 grams / 10 minutes or less, comprises at least three microporous polyolefin membranes made according to a dry process in which a polyolefin resin is extruded to form said membranes, said resin having a melt flow index (MFI) of about 0.8 grams / 10 minutes or less, comprises at least one polyethylene or polypropylene membrane, comprises at least two polypropylene membranes, and / or has improved pin puncture strength or TD tensile strength compared to a prior art separator, multi-layer separator, or tri-layer separator of the same thickness. An improved multi-layer separator or base film comprising at least one microporous membrane.

Claims

1. 1. An improved multi-layer separator, membrane or base film comprising: at least one microporous membrane made according to a dry stretch process in which a polyolefin resin, mixture or blend is extruded to form a microporous membrane, the resin having a melt flow index (MFI) of about 0.8 grams / 10 minutes or less; The separator has a thickness of about 7 μm or greater, a porosity in the range of about 30% to about 50%, and a resistivity of about 1.5 ohm-cm 2 and an electrical resistance (ER) of: Optionally, the separator is a monolayer, multilayer, bilayer or trilayer separator or base film, made by dry stretching, made by lamination process, has a pin puncture strength (PS) of at least 130 gf and a thickness of at least about 7 μm, has a pin puncture strength (PS) of at least 200 gf and a thickness of at least about 7 μm, has a pin puncture strength (PS) of at least 390 gf and a thickness of at least about 13 μm, has a pin puncture strength (PS) of at least 200 gf and a thickness of at least about 7 μm, has a porosity of at least 25%, has a porosity of at least 27%, has a porosity of at least 31%, has a porosity in the range of about 30% to 50%, has a porosity in the range of about 31% to 40%, is particularly well suited for energy batteries, such as those used in consumer electronics, and has a porosity of 1.5 ohm-cm 2 Improved multilayer separator, membrane or base film having an ER of 0.1 to 1.0%, having a porosity of at least 25% and suitable for high energy cells or batteries, comprising at least two microporous polyolefin membranes made according to a dry process in which a polyolefin resin is extruded to form, said resin having a melt flow index (MFI) of about 0.8 grams / 10 minutes or less, comprising at least three microporous polyolefin membranes made according to a dry process in which a polyolefin resin is extruded to form, said resin having a melt flow index (MFI) of about 0.8 grams / 10 minutes or less, comprising at least one polyethylene or polypropylene membrane, comprising at least two polypropylene membranes, and / or having improved pin puncture strength or TD tensile strength compared to a prior art separator, multilayer separator, or trilayer separator of the same thickness.

2. 10. The separator of claim 1, wherein the separator has a CSI (Composite Slit Index) of at least 29.

3. 10. The separator of claim 1 which is a three-layer separator, membrane or base film.

4. 10. The separator of claim 1, wherein the separator has a first load apex of a pin puncture strength (PS) of at least 130 gf.

5. The separator of claim 1 , wherein the separator has a porosity of at least 31%.

6. The separator of claim 1 , wherein the separator has a porosity of 31% to 40%.

7. 10. The separator of claim 1, wherein the separator is particularly well suited for energy batteries, such as those used in consumer electronics.

8. The separator has a resistance of 150 kgf / cm 2 The separator of claim 1 having a TD (transverse direction) tensile strength of or greater.

9. The separator of claim 1 , wherein the separator has a CSI greater than 30.

10. The separator of claim 1 , wherein the separator has a CSI of at least 50.

11. The separator of claim 1 , wherein the separator has a CSI of at least 100.

12. The CSI is based on an inventive test method known as the Composite Tear Index (CSI), and is defined by Equation 1 (described below), where the CSI value is a function of the first load apex, the second load apex, TD tensile strength, MD tensile strength, and TD elongation measured during a Puncture Strength Test: CSI = (A - |B - A| 1.8 ) × C × (D × E) / 10 6 Equation 1 During the ceremony: A = first load apex / thickness x (1 - porosity) B = second load apex / thickness C=TD extension D = MD tensile strength E = TD tensile strength 3. The separator of claim 2, wherein the first and second load peaks are in grams force, the caliper values ​​are in microns, the MD and TD tensile strengths are in grams force, the TD elongation is expressed as a percentage, and a high CSI value can predict a microporous membrane that can have excellent strength performance in a secondary lithium battery.

13. 10. The separator of claim 1, wherein the separator comprises at least one microporous polyolefin membrane manufactured according to a dry process in which a polyolefin resin is extruded to form the membrane, the resin having a melt flow index (MFI) of about 0.5 grams / 10 minutes or less.

Citation Information

Patent Citations

  • Polyalkylene microporous diaphragm for lithiam ion battery and manufacturing method thereof

    CN101000952A

  • Battery separator

    JP1998261393A

  • Multi-layer separation film with improved strength and stability

    JP2007311332A

  • Laminated porous film and method for production thereof

    JP2012011751A

  • Laminated microporous film and method for producing the same, and cell separator

    JP2016022679A