Conductive member, electrochemical cell device, module, and module housing device

The conductive member's layered structure with chromium base material and conductive oxide layers enhances bonding strength, addressing durability issues in fuel cell stack devices and improving the overall durability of the cell stack and module housing devices.

JP2024157036APending Publication Date: 2024-11-06KYOCERA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024139893
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-29
Filing Date
2024-08-21
Publication Date
2024-11-06

Smart Images

  • Figure 2024157036000001_ABST
    Figure 2024157036000001_ABST
Patent Text Reader

Abstract

To provide a highly durable conductive member, electrochemical cell device, module, and module housing device.SOLUTION: A conductive member includes a base material containing chromium, a first layer including first particles of a conductive oxide, and a second layer including second particles of a conductive oxide. The first layer is located on the base material. The second layer is located on the first layer. The first layer has open pores that open to an interface with the second layer. The second particles include particles having a diameter smaller than the diameter of the open pores.SELECTED DRAWING: Figure 3B
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an electrically conductive member, an electrochemical cell device, a module, and a module housing device. [Background technology]

[0002] In recent years, various fuel cell stack devices having a plurality of fuel cells have been proposed as next-generation energy sources. A fuel cell is a type of electrochemical cell that can obtain electric power using a fuel gas such as a hydrogen-containing gas and an oxygen-containing gas such as air. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2009 / 131180 Summary of the Invention

[0004] A conductive member according to one aspect of the embodiment includes a base material containing chromium, a first layer including first particles of a conductive oxide, and a second layer including second particles of a conductive oxide. The first layer is located on the base material. The second layer is located on the first layer. The first layer has open pores that open to an interface with the second layer. The second particles include particles having a diameter smaller than the diameter of the open pores.

[0005] The present disclosure also provides an electrochemical cell device comprising the conductive member described above and an electrochemical cell having a first electrode joined to a third layer located on the second layer, the third layer including third particles having an average particle size larger than that of the second particles.

[0006] The module of the present disclosure includes the electrochemical cell device described above and a container for housing the electrochemical cell device.

[0007] The module housing device of the present disclosure includes the above-described module, an auxiliary device for operating the module, and an exterior case for housing the module and the auxiliary device. [Brief description of the drawings]

[0008] [Figure 1A] FIG. 1A is a cross-sectional view illustrating an example of an electrochemical cell according to a first embodiment. [Figure 1B] FIG. 1B is a side view of an example of the electrochemical cell according to the first embodiment, as viewed from the air electrode side. [Figure 1C] FIG. 1C is a side view of an example of an electrochemical cell according to the first embodiment, viewed from the interconnector side. [Figure 2A] FIG. 2A is a perspective view showing an example of an electrochemical cell device according to the first embodiment. [Figure 2B] FIG. 2B is a cross-sectional view taken along line XX shown in FIG. 2A. [Figure 2C] FIG. 2C is a top view illustrating an example of the electrochemical cell device according to the first embodiment. [Figure 3A] FIG. 3A is a cross-sectional view showing an example of an electrochemical cell device according to the first embodiment. [Figure 3B] FIG. 3B is a cross-sectional view taken along line AA shown in FIG. 3A. [Figure 4A] FIG. 4A is an enlarged view of region B shown in FIG. 3B. [Figure 4B] FIG. 4B is an enlarged view of area C shown in FIG. 4A. [Diagram 5] FIG. 5 is an external perspective view illustrating an example of the module according to the first embodiment. [Figure 6] FIG. 6 is an exploded perspective view illustrating an example of a module housing device according to the first embodiment. [Figure 7A] FIG. 7A is a cross-sectional view showing an example of an electrochemical cell device according to the second embodiment. [Figure 7B] FIG. 7B is a cross-sectional view showing another example of the electrochemical cell device according to the second embodiment. [Figure 8A]FIG. 8A is an enlarged view of a cross section taken along line DD shown in FIG. 7A. [Figure 8B] FIG. 8B is an enlarged view of the cross section taken along line DD shown in FIG. 7A. [Figure 8C] FIG. 8C is an enlarged cross-sectional view showing another example of the conductive member according to the second embodiment. [Figure 9] FIG. 9 is a cross-sectional view showing an example of an electrochemical cell device according to the third embodiment. [Figure 10] FIG. 10 is an enlarged view of region E shown in FIG. [Figure 11A] FIG. 11A is a perspective view illustrating an example of an electrochemical cell according to a fourth embodiment. [Figure 11B] FIG. 11B is a partial cross-sectional view of the electrochemical cell shown in FIG. 11A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In the above-mentioned fuel cell stack device, there is room for improvement in the durability of the conductive members joined to the fuel cells.

[0010] Therefore, it is desirable to provide a highly durable conductive member, electrochemical cell device, module, and module housing device.

[0011] Hereinafter, embodiments of the conductive member, electrochemical cell device, module, and module housing device disclosed in the present application will be described in detail with reference to the accompanying drawings. Note that the disclosure is not limited to the embodiments described below.

[0012] In addition, it should be noted that the drawings are schematic, and that the dimensional relationships, ratios, etc. of each element may differ from the reality. Furthermore, there may be cases where the dimensional relationships, ratios, etc. of each element differ from those of the drawings.

[0013] [First embodiment] <Electrochemical cell configuration> First, with reference to Figures 1A to 1C, an electrochemical cell according to a first embodiment will be described using an example of a solid oxide fuel cell. The electrochemical cell device may include a cell stack having a plurality of electrochemical cells. An electrochemical cell device having a plurality of electrochemical cells will be simply referred to as a cell stack device.

[0014] FIG. 1A is a cross-sectional view showing an example of an electrochemical cell according to the first embodiment. FIG. 1B is a side view of the example of the electrochemical cell according to the first embodiment, seen from the air electrode side. FIG. 1C is a side view of the example of the electrochemical cell according to the first embodiment, seen from the interconnector side. Note that FIGS. 1A to 1C show enlarged views of parts of each component of the electrochemical cell. Hereinafter, the electrochemical cell may simply be referred to as a cell.

[0015] 1A to 1C, the cell 1 is a hollow flat plate-like elongated plate. As shown in Fig. 1B, the shape of the entire cell 1 seen from the side is, for example, a rectangle with a side length in a length direction L of 5 cm to 50 cm and a length in a width direction W perpendicular to the length direction L of 1 cm to 10 cm. The thickness of the entire cell 1 in a thickness direction T is, for example, 1 mm to 5 mm.

[0016] 1A, the cell 1 includes a conductive support substrate 2, an element portion 3, and an interconnector 4. The support substrate 2 is columnar having a pair of opposing first and second surfaces n1 and n2, and a pair of arc-shaped side surfaces m connecting the first and second surfaces n1 and n2.

[0017] The element unit 3 is located on a first surface n1 of the support substrate 2. The element unit 3 has a fuel electrode 5, a solid electrolyte layer 6, and an air electrode 8. In the example shown in FIG. 1A, an interconnector 4 is located on a second surface n2 of the cell 1. The cell 1 may include an intermediate layer 7 between the solid electrolyte layer 6 and the air electrode 8.

[0018] As shown in FIG. 1B, the air electrode 8 does not extend to the lower end of the cell 1. At the lower end of the cell 1, only the solid electrolyte layer 6 is exposed on the surface of the first face n1. As shown in FIG. 1C, the interconnector 4 may extend to the lower end of the cell 1. At the lower end of the cell 1, the interconnector 4 and the solid electrolyte layer 6 are exposed on the surface. As shown in FIG. 1A, the solid electrolyte layer 6 is exposed on the surface of a pair of arc-shaped side faces m of the cell 1. The interconnector 4 does not have to extend to the lower end of the cell 1.

[0019] Each of the components constituting the cell 1 will be described below.

[0020] The support substrate 2 has therein gas flow channels 2a through which gas flows. The example of the support substrate 2 shown in FIG. 1A has six gas flow channels 2a. The support substrate 2 has gas permeability and allows the gas flowing through the gas flow channels 2a to permeate to the anode 5. The support substrate 2 may be conductive. The conductive support substrate 2 collects electricity generated in the element section 3 to the interconnector 4.

[0021] The material of the support substrate 2 includes, for example, an iron group metal component and an inorganic oxide. The iron group metal component may be, for example, Ni (nickel) and / or NiO. The inorganic oxide may be, for example, a specific rare earth element oxide. The rare earth element oxide may include, for example, one or more rare earth elements selected from Sc, Y, La, Nd, Sm, Gd, Dy, and Yb.

[0022] The material of the fuel electrode 5 may be a generally known material. The fuel electrode 5 may be a porous conductive ceramic containing a material having electronic conductivity and a material having ion conductivity. The conductive ceramic may be, for example, a ceramic containing calcium oxide, magnesium oxide, or ZrO2 in which a rare earth element oxide is solid-dissolved, and Ni and / or NiO. The rare earth element oxide may contain, for example, a plurality of rare earth elements selected from Sc, Y, La, Nd, Sm, Gd, Dy, and Yb. Calcium oxide, magnesium oxide, or ZrO2 in which a rare earth element oxide is solid-dissolved may be referred to as stabilized zirconia. The stabilized zirconia may also include partially stabilized zirconia.

[0023] The solid electrolyte layer 6 is an electrolyte and transfers ions between the fuel electrode 5 and the air electrode 8. At the same time, the solid electrolyte layer 6 has gas barrier properties and makes it difficult for leakage of the fuel gas and oxygen-containing gas to occur.

[0024] The material of the solid electrolyte layer 6 may be, for example, ZrO2 in which 3 mol % to 15 mol % of a rare earth element oxide is dissolved. The rare earth element oxide may include, for example, one or more rare earth elements selected from Sc, Y, La, Nd, Sm, Gd, Dy, and Yb. The solid electrolyte layer 6 may include, for example, ZrO2 in which Yb, Sc, or Gd is dissolved, CeO2 in which La, Nd, or Yb is dissolved, BaZrO3 in which Sc or Yb is dissolved, or BaCeO3 in which Sc or Yb is dissolved.

[0025] The air electrode 8 has gas permeability. The open porosity of the air electrode 8 may be, for example, in the range of 20% to 50%, particularly 30% to 50%. The open porosity of the air electrode 8 may also be referred to as the void ratio of the air electrode 8.

[0026] There are no particular limitations on the material of the air electrode 8 as long as it is a material generally used for air electrodes. The material of the air electrode 8 may be, for example, a conductive ceramic such as a so-called ABO3 type perovskite oxide.

[0027] The material of the air electrode 8 may be, for example, a composite oxide in which Sr (strontium) and La (lanthanum) coexist at the A site. x Sr 1-x Co y Fe 1-y O3, La x Sr 1-x MnO3, La x Sr 1-x FeO3, La x Sr 1-x CoO3, etc. Note that x is 0 <x<1、yは0<y<1である。

[0028] Furthermore, when the element unit 3 has the intermediate layer 7, the intermediate layer 7 functions as a diffusion suppression layer. When Sr (strontium) contained in the air electrode 8 diffuses into the solid electrolyte layer 6, a resistance layer of SrZrO3 is formed in the solid electrolyte layer 6. The intermediate layer 7 makes it difficult for Sr to diffuse, thereby making it difficult for SrZrO3 to be formed.

[0029] The material of the intermediate layer 7 is not particularly limited as long as it generally prevents diffusion of elements between the air electrode 8 and the solid electrolyte layer 6. The material of the intermediate layer 7 may include, for example, cerium oxide (CeO2) in which a rare earth element other than Ce (cerium) is dissolved. As such a rare earth element, for example, Gd (gadolinium), Sm (samarium), etc. may be used.

[0030] Moreover, the interconnector 4 is dense and prevents leakage of the fuel gas flowing through the gas flow passage 2a located inside the support substrate 2 and the oxygen-containing gas flowing outside the support substrate 2. The interconnector 4 may have a relative density of 93% or more, particularly 95% or more.

[0031] Lanthanum chromite-based perovskite oxides (LaCrO3-based oxides), lanthanum strontium titanium-based perovskite oxides (LaSrTiO3-based oxides), etc. may be used as the material for the interconnector 4. These materials are conductive and are not easily reduced or oxidized even when in contact with a fuel gas such as a hydrogen-containing gas and an oxygen-containing gas such as air.

[0032] <Configuration of electrochemical cell device> Next, an electrochemical cell device according to the present embodiment using the above-mentioned cell 1 will be described with reference to Figs. 2A to 2C. Fig. 2A is a perspective view showing an example of the electrochemical cell device according to the first embodiment. Fig. 2B is a cross-sectional view taken along line XX shown in Fig. 2A. Fig. 2C is a top view showing an example of the electrochemical cell device according to the first embodiment.

[0033] As shown in FIG. 2A, the cell stack device 10 includes a cell stack 11 having a plurality of cells 1 arranged (stacked) in a thickness direction T of the cells 1 (see FIG. 1A), and a fixing member 12.

[0034] The fixing member 12 has a fixing material 13 and a support member 14. The support member 14 supports the cell 1. The fixing material 13 fixes the cell 1 to the support member 14. The support member 14 also has a support body 15 and a gas tank 16. The support body 15 and the gas tank 16, which are the support member 14, are made of metal and are conductive.

[0035] 2B, the support 15 has insertion holes 15a into which the lower ends of the multiple cells 1 are inserted. The lower ends of the multiple cells 1 and the inner wall of the insertion holes 15a are joined with a fixing material 13.

[0036] The gas tank 16 has an opening for supplying a reaction gas to the cells 1 through the insertion holes 15a, and a groove 16a located around the opening. The outer peripheral edge of the support 15 is joined to the gas tank 16 by a joining material 21 filled in the groove 16a of the gas tank 16.

[0037] In the example shown in Fig. 2A, fuel gas is stored in an internal space 22 formed by a support body 15, which is the support member 14, and a gas tank 16. A gas circulation pipe 20 is connected to the gas tank 16. The fuel gas is supplied to the gas tank 16 through this gas circulation pipe 20, and is supplied from the gas tank 16 to a gas flow path 2a (see Fig. 1A) inside the cell 1. The fuel gas supplied to the gas tank 16 is generated in a reformer 102 (see Fig. 5), which will be described later.

[0038] The hydrogen-rich fuel gas can be produced by steam reforming of the raw fuel, etc. When the fuel gas is produced by steam reforming, the fuel gas contains water vapor.

[0039] The example shown in FIG. 2A includes two rows of cell stacks 11, two supports 15, and a gas tank 16. Each of the two rows of cell stacks 11 has a plurality of cells 1. Each cell stack 11 is fixed to each of the supports 15. The gas tank 16 has two through holes on the upper surface. Each of the supports 15 is disposed in each of the through holes. An internal space 22 is formed by one gas tank 16 and two supports 15.

[0040] The shape of the insertion hole 15a is, for example, an oval shape when viewed from above. For example, the length of the insertion hole 15a in the arrangement direction of the cells 1, i.e., the thickness direction T, is greater than the distance between the two end current collecting members 17 located at both ends of the cell stack 11. The width of the insertion hole 15a is, for example, greater than the length of the cell 1 in the width direction W (see FIG. 1A).

[0041] 2B, the joints between the inner walls of the insertion holes 15a and the lower ends of the cells 1 are filled with a fixing material 13 and solidified. This bonds and fixes the inner walls of the insertion holes 15a to the lower ends of the cells 1, respectively, and also bonds and fixes the lower ends of the cells 1 to each other. The gas flow paths 2a of each cell 1 communicate with the internal space 22 of the support member 14 at their lower ends.

[0042] A material having low electrical conductivity, such as glass, can be used for the fixing material 13 and the bonding material 21. Specific materials for the fixing material 13 and the bonding material 21 include amorphous glass, and in particular, crystallized glass.

[0043] As the crystallized glass, for example, any of materials such as SiO2-CaO, MgO-B2O3, La2O3-B2O3-MgO, La2O3-B2O3-ZnO, and SiO2-CaO-ZnO may be used, and in particular, SiO2-MgO-based materials may be used.

[0044] 2B, a conductive member 18 is interposed between adjacent cells 1 among the multiple cells 1. The conductive member 18 electrically connects the fuel electrode 5 of one adjacent cell 1 to the air electrode 8 of the other cell 1 in series. More specifically, it connects the interconnector 4 electrically connected to the fuel electrode 5 of one adjacent cell 1 to the air electrode 8 of the other cell 1. The connection between the adjacent cells 1 and the conductive member 18 will be described in detail later.

[0045] As shown in Fig. 2B, an end current collecting member 17 is electrically connected to the cell 1 located at the outermost position in the arrangement direction of the multiple cells 1. The end current collecting member 17 is connected to a conductive part 19 protruding to the outside of the cell stack 11. The conductive part 19 collects electricity generated by power generation in the cells 1 and draws it out to the outside. Note that the end current collecting member 17 is not shown in Fig. 2A.

[0046] 2C, the cell stack device 10 has two cell stacks 11A and 11B connected in series to function as one battery. Therefore, the conductive portion 19 of the cell stack device 10 is divided into a positive terminal 19A, a negative terminal 19B, and a connection terminal 19C.

[0047] The positive electrode terminal 19A is a positive electrode when the electric power generated by the cell stack 11 is output to the outside, and is electrically connected to the end current collecting member 17 on the positive electrode side of the cell stack 11A. The negative electrode terminal 19B is a negative electrode when the electric power generated by the cell stack 11 is output to the outside, and is electrically connected to the end current collecting member 17 on the negative electrode side of the cell stack 11B.

[0048] The connection terminal 19C electrically connects the end current collecting member 17 on the negative electrode side in the cell stack 11A and the end current collecting member 17 on the positive electrode side in the cell stack 11B.

[0049] <Details of electrochemical cell device> Next, details of the electrochemical cell device according to the first embodiment will be described with reference to Figures 3A to 4B. Figure 3A is a cross-sectional view showing an example of the electrochemical cell device according to the first embodiment.

[0050] As shown in FIG. 3A, the cell stack device 10 has cells 1a and 1b adjacent to each other in the thickness direction T, and a conductive member 18 located between the cells 1a and 1b.

[0051] The conductive member 18 has a connection portion 18a connected to cell 1a, which is one of the adjacent cells 1, and a connection portion 18b connected to cell 1b, which is the other cell 1. The conductive member 18 also has linking portions 18c at both ends in the width direction W, which connect the connection portions 18a and 18b. This allows the conductive member 18 to electrically connect the cells 1 adjacent to each other in the thickness direction T. Note that the shape of the cell 1 is simplified in FIG. 3A.

[0052] Fig. 3B is a cross-sectional view taken along line AA shown in Fig. 3A. The conductive member 18 extends in the longitudinal direction L of the cell 1. As shown in Fig. 3B, a plurality of connection portions 18a and 18b of the conductive member 18 are alternately positioned along the longitudinal direction L of the cell 1. The conductive member 18 is in contact with the cells 1a and 1b at the connection portions 18a and 18b, respectively.

[0053] Fig. 4A is an enlarged view of region B shown in Fig. 3B. As shown in Fig. 4A, the conductive member 18 has a base material 40, a first layer 41, and a second layer .

[0054] The substrate 40 has electrical conductivity and heat resistance. The substrate 40 contains chromium. The substrate 40 is, for example, stainless steel. The substrate 40 may contain, for example, a metal oxide.

[0055] The substrate 40 may have a laminated structure. In the example shown in FIG. 4A, the substrate 40 has a first substrate portion 40a and a second substrate portion 40b. The second substrate portion 40b may have a higher chromium content than the first substrate portion 40a. The second substrate portion 40b may contain chromium oxide (Cr2O3), for example. The substrate 40 has the second substrate portion 40b in this manner, which enhances the durability of the conductive member 18. The substrate 40 may have the second substrate portion 40b so as to cover the entire first substrate portion 40a, or may have the second substrate portion 40b partially. The substrate 40 may not have the second substrate portion 40b. The substrate 40 may have a further laminated structure.

[0056] The first layer 41 is located on the substrate 40. The first layer 41 is located between the substrate 40 and the second layer 42. The first layer 41 has a conductive oxide. Such an oxide may contain, for example, Mn (manganese) and Co (cobalt). The oxide may also contain elements other than Mn and Co, for example, Zn (zinc) and Al (aluminum). Such an oxide may be a composite oxide having a spinel structure. An example of a composite oxide having such a structure is a Zn(Co)MnCoO4 such as ZnMnCoO4. x Mn 1-x )2O4(0 <x<1)、Mn 1.5 Co 1.5 O4, MnCo2O4, CoMn2O4, etc. may also be used. The first layer 41 may contain, for example, CeO2.

[0057] The first layer 41 may have a plurality of first particles containing a conductive oxide. The first layer 41 may be a coating that covers the base material 40. The first layer 41 may be a single coating that covers the entire base material 40. The first layer 41 may contain a component other than the conductive oxide.

[0058] The first layer 41 may be a sintered body or a green compact. The first layer 41 may be crystalline or amorphous. The first layer 41 may contain a mixture of a crystalline phase and an amorphous phase.

[0059] The second layer 42 is located on the first layer 41. The second layer 42 has a first surface 181 and a second surface 182 that face each other with the base material 40 in between. In addition, the conductive member 18 has third surfaces 183, 184 that connect the first surface 181 and the second surface 182.

[0060] The second layer 42 includes a plurality of second particles containing a conductive oxide. The material of the second layer 42 may be, for example, a conductive ceramic such as a so-called ABO3 type perovskite oxide.

[0061] The material of the second layer 42 may be, for example, a composite oxide in which Sr (strontium) and La (lanthanum) coexist at the A site. x Sr 1-x Co y Fe 1-y O3, La x Sr 1-x MnO3, La x Sr 1-x FeO3, La x Sr 1-x CoO3, etc. Note that x is 0 <x<1、yは0<y<1である。

[0062] The second layer 42 can be positioned on the surface of the first layer 41 by a film forming method such as a DIP method.

[0063] The conductive member 18 (connection portion 18a) may further include a third layer 43. The third layer 43 is located on the second layer 42. In the example shown in FIG. 4A, the third layer 43 is located only on the first surface 181 of the second layer 42, but the third layer 43 may be located on the third surfaces 183, 184, for example. The third layer 43 is located between the air electrode 8 of the cell 1a and the second layer 42, and bonds the air electrode 8 of the cell 1a to the conductive member 18. The air electrode 8 is a first electrode bonded to the conductive member 18.

[0064] The material of the third layer 43 may be, for example, a conductive ceramic such as a so-called ABO3 type perovskite oxide.

[0065] The material of the third layer 43 may be, for example, a composite oxide in which Sr (strontium) and La (lanthanum) coexist at the A site. x Sr 1-x Co y Fe 1-y O3, La x Sr 1-x MnO3, La x Sr 1-x FeO3, La x Sr 1-x CoO3, etc. Note that x is 0 <x<1、yは0<y<1である。

[0066] The third layer 43 may be gas permeable. The porosity of the third layer 43 may be, for example, 50% or less. The porosity of the third layer 43 may be, for example, greater than the porosity of the second layer 42.

[0067] Fig. 4B is an enlarged view of region C shown in Fig. 4A. As shown in Fig. 4B, the first layer 41 of the conductive member 18 may have a plurality of first particles 411 and first pores 412 located between the plurality of first particles 411. The first pores 412 include open pores that open to an interface 410 with the second layer 42. The first layer 41 may include closed pores located inside the plurality of first particles 411 or between the plurality of first particles 411.

[0068] The plurality of first particles 411 may have an average particle size of, for example, 0.3 μm or more and 0.6 μm or less. The average pore size of first pores 412 may be, for example, 0.3 μm or more and 1.0 μm or less.

[0069] The second layer 42 may have a plurality of second particles 421. The second particles 421 may include second particles 421 having a particle size smaller than the diameter of the first pores 412 opening to the interface 410. This makes it easier for some of the second particles 421 to enter the first pores 412 opening to the interface 410, increasing the bonding strength between the first layer 41 and the second layer 42. This makes it harder for the first layer 41 and the second layer 42 to peel off, improving the durability of the conductive member 18 and the cell stack device 10.

[0070] Furthermore, the average particle size of the second particles 421 may be smaller than the average pore size of the first pores 412 contained in the first layer 41. This makes it easier for some of the second particles 421 to enter the first pores 412 opening at the interface 410, thereby increasing the bonding strength between the first layer 41 and the second layer 42. As a result, the first layer 41 and the second layer 42 are less likely to peel off, improving the durability of the conductive member 18 and the cell stack device 10.

[0071] The average pore diameter of the second pores contained in the second layer 42 may be smaller than the average pore diameter of the first pores 412 contained in the first layer 41. This increases the strength of the second layer 42 and makes it less likely for cracks to occur inside the second layer 42, thereby improving the durability of the conductive member 18 and the cell stack device 10.

[0072] The average particle size of the second particles 421 may be, for example, not less than 0.2 μm and not more than 0.6 μm. The average pore size of the second pores contained in the second layer 42 may be, for example, not less than 0.06 μm and not more than 0.3 μm. The second layer 42 may have a porosity of, for example, not less than 10% and not more than 16%.

[0073] Furthermore, the first layer 41 may have a first region 41a facing the substrate 40, and a second region 41b facing the second layer 42 and having a larger porosity than the first region 41a. This increases the adhesion of the first region 41a to the substrate 40, thereby increasing the bonding strength, and increases the bonding strength of the second region 41b to the second layer 42. This makes it difficult for the first region 41a and the substrate 40, and the second region 41b and the second layer 42 to peel off from each other, thereby improving the durability of the conductive member 18 and the cell stack device 10.

[0074] The porosity of the first region 41a may be, for example, 5% or less. The porosity of the second region 41b may be, for example, 10% or more and 30% or less. The first layer 41 may be formed, for example, by sequentially stacking a plurality of first particles 411 having different average particle sizes, or by varying the time required for heat treatment. However, there is no limitation on the method of producing the first region 41a and the second region 41b, and they may be produced by any method.

[0075] The third layer 43 may also include third particles 431 having a larger average particle size than the second particles 421. This allows a portion of the second particles 421 to enter the gaps between the third particles 431, increasing the bonding strength between the second layer 42 and the third layer 43. This makes it difficult for the second layer 42 and the third layer 43 to peel off, improving durability. The third particles 431 may further include particles having a particle size approximately equal to the average particle size of the second particles 421, or may include particles having a particle size smaller than the average particle size of the second particles 421.

[0076] The average pore diameter of the third pores contained in the third layer 43 may be larger than the average particle diameter of the second particles 421. This allows the second particles 421 to easily enter the gaps between the third particles 431, increasing the bonding strength between the second layer 42 and the third layer 43. As a result, the second layer 42 and the third layer 43 are less likely to peel off, improving the durability of the conductive member 18 and the cell stack device 10.

[0077] Furthermore, the third layer 43 may contain at least one of the metal elements contained in the second layer 42. This increases the affinity between the second layer 42 and the third layer 43, and increases the bonding strength between the second layer 42 and the third layer 43. This makes it difficult for the second layer 42 and the third layer 43 to peel off, improving durability. The metal elements contained in the third layer 43 and the second layer 42 can be identified by, for example, performing point analysis, line analysis, mapping, or the like of each element on a cross section of the conductive member 18 using a HAADF-STEM (high-angle annular dark-field scanning transmission electron microscope), a FIB-SEM (focused ion beam scanning electron microscope), or an EPMA (electron probe microanalyzer).

[0078] The material of the third layer 43 may have the same crystal structure as the material of the second layer 42. The material of the third layer 43 may have the same composition as the material of the second layer 42. When the material of the third layer 43 has the same crystal structure or composition as the material of the second layer 42, the affinity between the second layer 42 and the third layer 43 is further increased, and the bonding strength between the second layer 42 and the third layer 43 is further increased.

[0079] The average particle size of the third particles 431 contained in the third layer 43 may be, for example, not less than 0.25 μm and not more than 6.5 μm. The average pore size of the third pores may be, for example, not less than 0.1 μm and not more than 0.9 μm. The third layer 43 may have third particles 431 having a particle size smaller than the average particle size of the second particles 421.

[0080] In this way, the conductive member 18 has the first layer 41, the second layer 42, and the third layer 43, so that the bonding strength within the conductive member 18 is increased and durability is improved. Furthermore, by bonding the conductive member 18 and the air electrode 8 using the third layer 43 of the conductive member 18, the bonding strength between the conductive member 18 and the air electrode 8 is improved. This makes it possible to improve the durability of the cell stack device 10.

[0081] The average particle size of each particle in the first layer 41, the second layer 42, and the third layer 43, the porosity of the first layer 41, the second layer 42, and the third layer 43, and the average pore size of each pore in the first layer 41, the second layer 42, and the third layer 43 can be measured based on the results of observing a cross section of the conductive member 18 with a SEM (Scanning Electron Microscope).

[0082] <module> Next, a module according to an embodiment of the present disclosure using the above-mentioned cell stack device 10 will be described with reference to Fig. 5. Fig. 5 is an external perspective view showing a module according to a first embodiment. Fig. 5 shows a state in which the front and rear surfaces, which are part of the storage container 101, have been removed and the cell stack device 10 of the fuel cell stored inside has been removed to the rear.

[0083] 5, the module 100 includes a storage container 101 and a cell stack device 10 housed in the storage container 101. In addition, above the cell stack device 10, a reformer 102 is disposed.

[0084] The reformer 102 reforms raw fuel such as natural gas or kerosene to generate fuel gas and supplies it to the cell 1. The raw fuel is supplied to the reformer 102 through a raw fuel supply pipe 103. The reformer 102 may include a vaporizer 102a that vaporizes water, and a reformer 102b. The reformer 102b includes a reforming catalyst (not shown) and reforms the raw fuel into fuel gas. Such a reformer 102 can perform steam reforming, which is a highly efficient reforming reaction.

[0085] The fuel gas generated in the reformer 102 is supplied to the gas flow channel 2a of the cell 1 (see FIG. 1A) through the gas distribution pipe 20, the gas tank 16, and the support member 14.

[0086] Furthermore, in the module 100 having the above-mentioned configuration, the temperature inside the module 100 during normal power generation becomes approximately 500°C to 1000°C as the gas is combusted and the cells 1 generate power.

[0087] In such a module 100, as described above, by being configured to house a cell stack device 10 that can improve durability, it is possible to make the module 100 have improved durability.

[0088] <Module storage device> Fig. 6 is an exploded perspective view showing an example of a module housing device according to the first embodiment. A module housing device 110 according to this embodiment includes an outer case 111, the module 100 shown in Fig. 5, and auxiliary equipment (not shown). The auxiliary equipment operates the module 100. The module 100 and the auxiliary equipment are housed in the outer case 111. Note that some components are omitted in Fig. 6.

[0089] An exterior case 111 of a module accommodating device 110 shown in Fig. 6 has support columns 112 and an exterior plate 113. A partition plate 114 divides the interior of the exterior case 111 into upper and lower sections. The space above the partition plate 114 in the exterior case 111 is a module accommodating chamber 115 that accommodates the module 100, and the space below the partition plate 114 in the exterior case 111 is an auxiliary equipment accommodating chamber 116 that accommodates auxiliary equipment that operates the module 100. Note that in Fig. 6, the auxiliary equipment accommodated in the auxiliary equipment accommodating chamber 116 is omitted.

[0090] In addition, the partition plate 114 has an air flow port 117 for allowing air from the auxiliary equipment housing chamber 116 to flow toward the module housing chamber 115. The exterior plate 113 constituting the module housing chamber 115 has an exhaust port 118 for exhausting air from within the module housing chamber 115.

[0091] In such a module housing device 110, as described above, by providing the module 100, which can improve durability, in the module housing chamber 115, it is possible to make the module housing device 110 have improved durability.

[0092] In the above embodiment, a case where a hollow flat support substrate is used is exemplified, but the present invention can also be applied to a cell stack device that uses a cylindrical support substrate.

[0093] [Second embodiment] Fig. 7A is a cross-sectional view showing an example of an electrochemical cell according to the second embodiment, and Fig. 7B is a cross-sectional view showing another example of an electrochemical cell according to the second embodiment.

[0094] As shown in FIG. 7A and FIG. 7B, the cell 1A has an element section 3A in which an anode 5, a solid electrolyte layer 6, and an air electrode 8 are laminated, and a support substrate 2. The support substrate 2 has a through hole or a fine hole at a portion of the element section 3A in contact with the anode 5, and has a member 120 located outside the gas flow path 2a. The support substrate 2 can distribute gas between the gas flow path 2a and the element section 3A. The support substrate 2 may be composed of, for example, one or more metal plates. The material of the metal plate may contain chromium. The metal plate may have a conductive coating layer.

[0095] The conductive member 18 electrically connects adjacent cells 1A to each other. The conductive member 18 has a connection portion 18a connected to cell 1a, which is one of the adjacent cells 1, and a connection portion 18b connected to cell 1b, which is the other adjacent cell 1.

[0096] Figures 8A and 8B are enlarged views of a cross section taken along line DD shown in Figure 7A. It should be noted that Figures 8A and 8B can also be applied to the example of Figure 7B.

[0097] As shown in FIG. 8A, the connection portion 18a of the conductive member 18 includes a base material 40 containing chromium, a first layer 41 including first particles of a conductive oxide located on the base material 40, and a second layer 42 including second particles of a conductive oxide located on the first layer 41. The first layer 41 has open pores that open at the interface with the second layer 42. The second particles include particles having a diameter smaller than the diameter of the open pores of the first layer 41. This makes it easier for some of the second particles to enter the open pores that open at the interface between the first layer 41 and the second layer 42, and the bonding strength between the first layer 41 and the second layer 42 is increased. Therefore, the first layer 41 and the second layer 42 are less likely to peel off, improving the durability of the conductive member 18 and the cell stack device 10A.

[0098] The conductive member 18 may also include a third layer 43 located on the second layer 42. The third layer 43 includes, for example, third particles having an average particle size larger than that of the second particles. The air electrode 8 of the cell 1a is bonded to the third layer 43. This makes it difficult for the conductive member 18 and the cell 1a to peel off, improving the durability of the cell stack device 10A.

[0099] As shown in FIG. 8B, the connection portion 18b of the conductive member 18 includes a base material 40 containing chromium, a first layer 41 including first particles of a conductive oxide located on the base material 40, and a second layer 42 including second particles of a conductive oxide located on the first layer 41. The first layer 41 has open pores that open at the interface with the second layer 42. The second particles include particles having a diameter smaller than the diameter of the open pores of the first layer 41. This makes it easier for some of the second particles to enter the open pores that open at the interface between the first layer 41 and the second layer 42, and the bonding strength between the first layer 41 and the second layer 42 is increased. Therefore, the first layer 41 and the second layer 42 are less likely to peel off, improving the durability of the conductive member 18 and the cell stack device 10A.

[0100] The conductive member 18 may also include a third layer 43a located on the second layer 42. The third layer 43a includes, for example, third particles having an average particle size larger than that of the second particles. The member 120 of the cell 1b is bonded to the third layer 43a. This makes it difficult for the conductive member 18 and the cell 1a to peel off, improving the durability of the cell stack device 10A. The material of the third layer 43a may be the same as or different from the material of the third layer 43.

[0101] In the example shown in Fig. 7A, the side surface of the anode 5 is covered with a solid electrolyte layer 6, which airtightly seals a gas flow channel 2a through which the fuel gas flows. As shown in Fig. 7B, the side surface of the anode 5 may be covered and sealed with a dense sealant 9. The sealant 9 covering the side surface of the anode 5 may have electrical insulation properties. The material of the sealant 9 may be, for example, glass or ceramics.

[0102] FIG. 8C is an enlarged cross-sectional view showing another example of the conductive member according to the second embodiment. As shown in FIG. 8C, the member 120 of the support substrate 2 may include a base material 50 containing chromium, a first layer 51 containing first particles of a conductive oxide located on the base material 50, and a second layer 52 containing second particles of a conductive oxide located on the first layer 51. The base material 50 may include a first base material portion 50a and a second base material portion 50b having a chromium content higher than that of the first base material portion 50a. The first layer 51 may have open pores opening at the interface with the second layer 52. The second particles may include particles having a particle size smaller than the diameter of the open pores of the first layer 51. This makes it easier for a part of the second particles to enter the open pores opening at the interface between the first layer 51 and the second layer 52, thereby increasing the bonding strength between the first layer 51 and the second layer 52. This makes it difficult for the first layer 51 and the second layer 52 to peel off, improving the durability of the member 120 and the cell stack device 10A. The materials of the base material 50, the first layer 51, and the second layer 52 may be the same as or different from the materials of the base material 40, the first layer 41, and the second layer 42.

[0103] [Third embodiment] Fig. 9 is a cross-sectional view showing an example of an electrochemical cell device according to the third embodiment. As shown in Fig. 9, the gas flow path 2a of the support substrate 2 may be formed of a member 120 having projections and recesses instead of the conductive member 18 shown in Fig. 7A. The member 120 is an example of the conductive member 18 that electrically connects adjacent cells 1B to each other.

[0104] FIG. 10 is an enlarged view of region E shown in FIG. 9. As shown in FIG. 10, the member 120 as the conductive member 18 includes a base material 40 containing chromium, a first layer 41 including first particles of a conductive oxide located on the base material 40, and a second layer 42 including second particles of a conductive oxide located on the first layer 41. The first layer 41 has open pores that open at the interface with the second layer 42. The second particles include particles having a particle size smaller than the diameter of the open pores of the first layer 41. This makes it easier for a part of the second particles to enter the open pores that open at the interface between the first layer 41 and the second layer 42, and the bonding strength between the first layer 41 and the second layer 42 is increased. Therefore, the first layer 41 and the second layer 42 are less likely to peel off, and the durability of the member 120 and the cell stack device 10B is improved.

[0105] The member 120 may also include a third layer 43 located on the second layer 42. The third layer 43 includes, for example, third particles having an average particle size larger than that of the second particles. The air electrode 8 of the cell 1a is bonded to the third layer 43. This makes it difficult for the conductive member 18 and the cell 1a to peel off, improving the durability of the cell stack device 10B.

[0106] The third layer 43 may be located on the entire surface 121 facing the cell 1 a , or may be located only on the joint portion with the air electrode 8 .

[0107] [Fourth embodiment] Fig. 11A is a perspective view showing an electrochemical cell according to a fourth embodiment, and Fig. 11B is a partial cross-sectional view of the electrochemical cell shown in Fig. 11A.

[0108] 11A, cell 1C, which is a flat plate type electrochemical cell, has an element portion 3C in which a fuel electrode 5, a solid electrolyte layer 6, and an air electrode 8 are stacked. In a cell stack device in which a plurality of flat plate type cells are stacked, for example, the plurality of cells 1C are electrically connected by conductive members 91, 92 which are adjacent metal layers. The conductive members 91, 92 electrically connect adjacent cells 1C to each other, and have gas flow paths that supply gas to the fuel electrode 5 or the air electrode 8.

[0109] As shown in FIG. 11B, in this embodiment, the conductive member 92 as the conductive member 18 has a gas flow path 93 that supplies gas to the air electrode 8. The conductive member 92 includes a base material 40 containing chromium, a first layer 41 including first particles of a conductive oxide located on the base material 40, and a second layer 42 including second particles of a conductive oxide located on the first layer 41. The first layer 41 has open pores that open at the interface with the second layer 42. The second particles include particles with a diameter smaller than the diameter of the open pores of the first layer 41. This makes it easier for a part of the second particles to enter the open pores that open at the interface between the first layer 41 and the second layer 42, and the bonding strength between the first layer 41 and the second layer 42 is increased. Therefore, the first layer 41 and the second layer 42 are less likely to peel off, and the durability of the conductive member 92 and the cell 1C is improved.

[0110] Furthermore, the conductive member 92 may include a third layer 43 located on the second layer 42. The third layer 43 includes, for example, third particles having an average particle size larger than that of the second particles. The air electrode 8 of the cell 1C is joined to the third layer 43. This makes it difficult for the conductive member 92 and the element portion 3C to peel off, improving the durability of the cell stack device.

[0111] The conductive member 92 may be in contact with the element portion 3C without the third layer 43. In other words, in this embodiment, the second layer 42 may be directly connected to the element portion 3C without using the third layer 43.

[0112] [Other embodiments] Next, electrochemical cell devices according to other embodiments will be described.

[0113] In the above-mentioned embodiments, a fuel cell, a fuel cell stack device, a fuel cell module, and a fuel cell device are shown as examples of an "electrochemical cell", "electrochemical cell device", "module", and "module housing device", but other examples may be an electrolysis cell, an electrolysis cell stack device, an electrolysis module, and an electrolysis device, respectively. The electrolysis cell has an anode (oxygen electrode) as a first electrode and a cathode as a second electrode, and decomposes water vapor into hydrogen and oxygen, or decomposes carbon dioxide into carbon monoxide and oxygen, when supplied with electric power. In the above-mentioned embodiments, an oxide ion conductor or a hydrogen ion conductor is shown as an example of an electrolyte material for the electrochemical cell, but a hydroxide ion conductor may also be used.

[0114] Although the present disclosure has been described in detail above, the present disclosure is not limited to the above-described embodiments, and various modifications, improvements, etc. are possible without departing from the gist of the present disclosure.

[0115] In one embodiment, (1) the conductive member comprises a substrate containing chromium; a first layer located on the substrate and including first particles of a conductive oxide; a second layer comprising second particles of a conductive oxide disposed on the first layer; Equipped with the first layer has open pores that open to an interface with the second layer, The second particles include particles having a diameter smaller than the diameter of the open pores.

[0116] (2) In the conductive member of (1) above, the second particles may have an average particle size smaller than an average pore size of the first pores contained in the first layer.

[0117] (3) In the conductive member of (1) or (2) above, the second pores contained in the second layer may have an average pore diameter smaller than the average pore diameter of the first pores contained in the first layer.

[0118] (4) In the conductive member of any one of (1) to (3) above, the first layer may have a first region facing the substrate and a second region facing the second layer and having a higher porosity than the first region.

[0119] (5) The conductive member according to any one of (1) to (4) above may further include a third layer located on the second layer and including third particles having an average particle size larger than that of the second particles.

[0120] (6) In the conductive member according to (5) above, the third pores contained in the third layer may have an average pore size larger than an average particle size of the second particles.

[0121] (7) In the conductive member according to (5) or (6) above, the third layer may contain at least one element selected from the metal elements contained in the second layer.

[0122] In one embodiment, (8) an electrochemical cell device includes: an electrochemical cell having a first electrode; Equipped with The first electrode is in contact with the third layer.

[0123] (9) The module comprises the electrochemical cell device according to (8), and a container for housing the electrochemical cell device.

[0124] (10) The module housing device includes the module (9) and Auxiliary equipment for operating the module; and an exterior case that houses the module and the auxiliary equipment.

[0125] The disclosed embodiments should be considered to be illustrative and not restrictive in all respects. Indeed, the above-described embodiments may be embodied in various forms. Furthermore, the above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. [Explanation of symbols]

[0126] 1,1A,1B,1C Cell 2 Support substrate 3,3A,3B,3C element part 4 Interconnector 5 Fuel electrode 6 Solid electrolyte layer 7. Middle Tier 8 Air electrode 10, 10A, 10B Cell stack device 11 Cell stack 12 Fixing member 13 Fixing material 14 Support member 15 Support 16 Gas Tank 17 End current collecting member 18 Conductive materials 40 Base material 41 1st layer 42 2nd layer 43 3rd layer 100 Modules 110 Module storage device

Claims

1. A substrate containing chromium; a first layer located on the substrate and including first particles of a conductive oxide; a second layer disposed on the first layer and including second particles of a conductive oxide; Equipped with the first layer has open pores that open to an interface with the second layer, The second particles include particles having a diameter smaller than the diameter of the open pores. Conductive material.

2. The average particle size of the second particles is smaller than the average pore size of the first pores contained in the first layer. The conductive member according to claim 1 .

3. The second layer has a smaller average pore size than the first layer has a smaller average pore size. The conductive member according to claim 1 .

4. The first layer has a first region facing the substrate and a second region facing the second layer and having a larger porosity than the first region. The conductive member according to claim 1 .

5. a third layer located on the second layer and including third particles having an average particle size larger than that of the second particles; The conductive member according to claim 1 .

6. The average pore diameter of the third pores contained in the third layer is larger than the average particle diameter of the second particles. The conductive member according to claim 5 .

7. The third layer contains at least one element selected from the metal elements contained in the second layer. The conductive member according to claim 5 .

8. A conductive member according to any one of claims 5 to 7, an electrochemical cell having a first electrode; Equipped with The first electrode is joined to the third layer. Electrochemical cell setup.

9. The electrochemical cell device according to claim 8 ; A container for housing the electrochemical cell device; A module comprising:

10. A module according to claim 9; Auxiliary equipment for operating the module; an exterior case that houses the module and the auxiliary equipment; A module housing device comprising: