Core-shell zeolite
The core-shell zeolite structure with a large core and small shell channel diameters addresses the low desorption temperature issue of conventional zeolites, enhancing hydrocarbon purification by increasing desorption temperatures and improving purification performance.
Patent Information
- Application Number
- JP2021149970
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-09-15
- Publication Date
- 2024-11-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional FAU zeolites adsorb a significant amount of hydrocarbons but desorb them at temperatures lower than the activation range of the three-way catalyst, limiting the reduction of hydrocarbon emissions.
Employing a core-shell zeolite structure where the core has a larger channel diameter and the shell has a smaller channel diameter, enhancing hydrocarbon desorption temperature by suppressing migration through the shell's discontinuous channels.
The core-shell zeolite design increases the desorption temperature of hydrocarbons, allowing for improved hydrocarbon purification performance by maintaining adsorption over a broader temperature range.
Smart Images

Figure 2024157067000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a core-shell zeolite. [Background technology]
[0002] In recent years, regulations on automobile exhaust gas have been strengthened. Gasoline engine vehicles are required to reduce the amount of hydrocarbon (HC) emissions that are emitted in the low temperature range immediately after the engine is started when the three-way catalyst is not yet activated. In response to this requirement, catalysts containing a hydrocarbon trap (HCT) that can adsorb hydrocarbons at low temperatures and desorb them at high temperatures are used. This makes it possible to temporarily adsorb the hydrocarbons emitted at low temperatures up to a high temperature range where they can be purified, thereby reducing the amount of hydrocarbon emissions.
[0003] Zeolite has been widely used as a hydrocarbon adsorbent in the past. For example, Patent Document 1 discloses an automobile exhaust gas purification device characterized in that the exhaust system is provided with an exhaust gas purification catalyst, and the upstream side of the catalyst is provided with an adsorbent made of a monolithic carrier coated with zeolite and carrying one or more types of catalytic metals on a part of the monolithic carrier. In addition, the document describes that, from the viewpoint of adsorption performance, H-type mordenite (MOR) or HY-type zeolite (FAU) is preferable as the zeolite. According to Patent Document 1, the automobile exhaust gas purification device can improve the purification performance of HC at a relatively low temperature at which HC starts to desorb from the adsorbent. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 2-135126 Summary of the Invention [Problem to be solved by the invention]
[0005] However, although FAU zeolite can adsorb a relatively large amount of hydrocarbons, the temperature range in which it desorbs hydrocarbons is lower than the temperature range in which a three-way catalyst is sufficiently activated, and this presents a problem in that it may not be possible to sufficiently reduce hydrocarbon emissions.
[0006] Therefore, an object of the present invention is to provide a means for increasing the desorption temperature of hydrocarbons in a hydrocarbon adsorbent made of zeolite. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved by using a core-shell zeolite having a large channel diameter as a core and a small channel diameter as a shell, thereby completing the present invention.
[0008] That is, one embodiment of the present invention is a core-shell zeolite having a core made of a first zeolite and a shell made of a second zeolite, in which the channel diameter of the first zeolite is larger than the channel diameter of the second zeolite. Effect of the Invention
[0009] According to the present invention, in a hydrocarbon adsorbent made of zeolite, the desorption temperature of hydrocarbons can be increased. [Brief description of the drawings]
[0010] [Figure 1] Figure 1 is an SEM image of powder d. [Diagram 2] Figure 2 is an SEM image of powder h. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described. In this specification, the numerical range "A to B" means "A or more and B or less". In addition, "A and / or B" means "either A or B" or "both A and B". In addition, various physical properties in this specification mean values measured by the methods described in the examples described below, unless otherwise specified.
[0012] <Core-shell type zeolite> One embodiment of the present invention is a core-shell type zeolite having a core made of a first zeolite and a shell made of a second zeolite, the channel diameter of the first zeolite being larger than the channel diameter of the second zeolite. The core-shell type zeolite according to the present invention can increase the desorption temperature of hydrocarbons in a hydrocarbon adsorbent made of zeolite.
[0013] Although it is unclear why the core-shell zeolite according to the present invention can desorb hydrocarbons at a higher temperature than conventional zeolites, the present inventors speculate as follows. Note that the present invention is not limited to the following mechanism.
[0014] Zeolites are crystalline aluminosilicates, and more than 245 types of skeletal structures are known. Zeolites have specific channel diameters due to their skeletal structures, and function as hydrocarbon adsorbents by allowing hydrocarbons to enter and exit these channels (tubular pores). It is known that there is a correlation between the channel diameter and the amount of hydrocarbon adsorbed and the desorption temperature. That is, the smaller the channel diameter, the lower the amount of hydrocarbon adsorbed and the more difficult it is for hydrocarbons to enter and exit, resulting in a higher desorption temperature. On the other hand, the larger the channel diameter, the higher the amount of hydrocarbon adsorbed and the more easily hydrocarbons can enter and exit, resulting in a lower desorption temperature.
[0015] According to the core-shell zeolite of the present invention, many hydrocarbons are adsorbed in the core having a large channel diameter, while the shell having a small channel diameter suppresses the desorption of the hydrocarbons. In addition, the presence of a crystal interface between the core and the shell may cause the channels to become discontinuous, which may be one of the reasons for the above-mentioned problem, and thus may prevent the hydrocarbons adsorbed in the core from moving to the shell. As a result, it is possible to increase the desorption temperature of the hydrocarbons. Note that, as described above, in a hydrocarbon adsorbent made only of zeolite having a small channel diameter, all of the hydrocarbons are desorbed within a short time from the start of desorption when the exhaust gas temperature rises. However, according to the core-shell zeolite of the present invention, the hydrocarbons are desorbed over a longer period of time from the start of desorption, so that it is possible to supply the hydrocarbons to the catalyst when the exhaust gas temperature is high, i.e., when the catalyst is sufficiently activated. As a result, it is possible to improve the purification performance of the hydrocarbons with the catalyst using the core-shell zeolite of the present invention.
[0016] The core-shell zeolite according to the present invention contains at least two types of zeolites (a first zeolite and a second zeolite) having different channel diameters. Hereinafter, the present invention will be described mainly by taking as an example a core-shell zeolite in which the core is composed of one type of first zeolite and the shell is composed of one type of second zeolite. However, the present invention is not limited to such an embodiment, and also includes an embodiment in which the core is composed of two or more types of first zeolites and / or the shell is composed of two or more types of second zeolites.
[0017] In this specification, the channel diameter of each zeolite is determined by identifying the type of zeolite contained in the core-shell zeolite by X-ray diffraction analysis, and the value of the maximum diameter of a sphere that can be included for the identified zeolite is adopted, as indicated by the International Zeolite Association (IZA). In this specification, the zeolite with the larger channel diameter of the two types of zeolites is defined as the first zeolite, and the zeolite with the smaller channel diameter is defined as the second zeolite. When the core is composed of two or more types of first zeolites and / or the shell is composed of two or more types of second zeolites, the smallest channel diameter of the first zeolite may be larger than the largest channel diameter of the second zeolite.
[0018] In the present invention, the specific types and combinations of the first zeolite and the second zeolite are not particularly limited, but the following types and combinations are preferred. In this specification, the type of zeolite means the skeletal structure of the zeolite. The type (skeletal structure) of the zeolite in this specification is represented by a three-letter code defined by the International Zeolite Association (IZA).
[0019] The first zeolite is preferably one that has a channel diameter larger than any hydrocarbon species contained in the exhaust gas and has a large hydrocarbon retention capacity in a low temperature range of less than 110°C, and is preferably at least one type selected from the group consisting of FAU, LEV, MWW and LTA, more preferably FAU and / or LEV, and even more preferably FAU.
[0020] The second zeolite is preferably one that has a channel diameter equal to or smaller than any hydrocarbon species contained in the exhaust gas and is capable of retaining adsorbed hydrocarbon species even in a high temperature range of 110°C or higher, and is preferably at least one type selected from the group consisting of BEA, CHA, MFI, MOR, SZR, FER and TON, more preferably at least one type selected from the group consisting of BEA, CHA, MFI, MOR and SZR, even more preferably BEA and / or MFI, and particularly preferably BEA.
[0021] Combinations of the first zeolite and the second zeolite, when written in the notation of "first zeolite (channel diameter) / second zeolite (channel diameter)", include FAU(11.24 Å) / BEA(6.68 Å), FAU(11.24 Å) / MFI(6.36 Å), FAU(11.24 Å) / MOR(6.70 Å), etc. Among them, from the viewpoint of further improving the desorption temperature of hydrocarbons, the combination is preferably FAU(11.24 Å) / BEA(6.68 Å) or FAU(11.24 Å) / MFI(6.36 Å), and more preferably FAU(11.24 Å) / BEA(6.68 Å). That is, in a preferred embodiment of the core-shell zeolite of the present invention, the first zeolite is FAU and the second zeolite is BEA.
[0022] The core-shell zeolite according to the present invention has a core-shell structure in which a first zeolite (a zeolite with a larger channel diameter) is arranged in the core and a second zeolite (a zeolite with a smaller channel diameter) is arranged in the shell. In this specification, whether or not a zeolite has a core-shell structure is determined by the following method.
[0023] First, X-ray diffraction analysis is performed on the prepared zeolite, and it is confirmed that at least two different zeolites are detected. Zeolites are identified by checking whether the 2θ of each peak seen in the XRD pattern after analysis matches the diffraction angle listed on the JCPDS card. If all the diffraction angles match, the zeolite can be identified as the zeolite in question. Also, if the 2θ of at least the three peaks with the highest intensity are at angles of 0.02° before and after the diffraction angle, the zeolite can be identified as the zeolite in question. This is because it includes error factors when the goniometer moves.
[0024] Next, the zeta potentials of the particles consisting of only the first zeolite and the particles consisting of only the second zeolite are measured at pH=3. Next, the zeta potentials of the target zeolite particles are measured at pH=3 in a similar manner. These values are then calculated using the formula: |P2-P x If the relationship | / |P2-P1|<0.10 is satisfied, it is considered to have a core-shell structure. Here, P1 represents the zeta potential (mV) of the particle made of the first zeolite. P2 represents the zeta potential (mV) of the particle made of the second zeolite. P x represents the zeta potential (mV) of the zeolite particle of interest. In this specification, the zeta potential is a value obtained by the measurement method described in the Examples below.
[0025] Since the zeta potential is a value that depends on the charge on the particle surface, the zeta potential of a particle in which the first zeolite is completely covered with the second zeolite is theoretically the same as the zeta potential of a particle consisting only of the second zeolite (|P2-P x | / |P2-P1|=0). On the other hand, when there is a portion of the first zeolite that is not covered by the second zeolite, the value of the zeta potential of the particle shifts from the value of the zeta potential of the particle consisting only of the second zeolite toward the value of the zeta potential of the particle consisting only of the first zeolite. The rate of shift (|P2-P xThe larger the ratio of |P2-P1|, the higher the proportion of the first zeolite exposed on the surface. x When | / |P2-P1|<0.10 is satisfied, the first zeolite is completely covered by the second zeolite, or even if there is an uncovered portion, the proportion is considered to be low. Therefore, in such a case, the "zeolite has a core-shell structure."
[0026] In addition, |P2-P x The value of | / |P2-P1| is essentially 0 or more and less than 0.10, preferably 0 or more and 0.09 or less, more preferably 0 or more and 0.05 or less, and further preferably 0 or more and 0.03 or less. If the value is within the above range, it is considered that the first zeolite is well covered by the second zeolite (the proportion of the first zeolite that is exposed is low), and therefore the effect of the present invention (increasing the desorption temperature of hydrocarbons) is more effectively exhibited.
[0027] In the present invention, the respective ratios of the first zeolite and the second zeolite contained in the core-shell zeolite are not particularly limited. However, in consideration of the fact that the first zeolite is well covered with the second zeolite, the mass (percentage) of the second zeolite with respect to the total mass of the core-shell zeolite is preferably more than 62 mass% and not more than 95 mass%, more preferably 71 mass% or more and 91 mass% or less, and even more preferably 71 mass% or more and 87 mass% or less. Within such a range, the second zeolite is present in a sufficient amount, so that the first zeolite can be well covered with the second zeolite. As a result, the effect of the present invention (increasing the desorption temperature of hydrocarbons) is further exerted. The mass (percentage) of the first zeolite with respect to the total mass of the core-shell zeolite is a value obtained by subtracting the mass (percentage) of the second zeolite from the total mass of 100 mass%.
[0028] In addition, as long as the effects of the present invention can be exhibited, the core of the core-shell zeolite may contain a component other than the first zeolite, and the shell may contain a component other than the second zeolite. However, from the viewpoint of further increasing the desorption temperature of hydrocarbons, the amount of the first zeolite contained in the core is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, particularly preferably 99% by mass or more, and most preferably 100% by mass, based on the total mass of the core. Similarly, the amount of the second zeolite contained in the shell is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, particularly preferably 99% by mass or more, and most preferably 100% by mass, based on the total mass of the shell.
[0029] <Method of manufacturing core-shell zeolite> The method for producing the core-shell type zeolite according to the present invention is not particularly limited, and any method for producing zeolite that can be used in the present technical field can be appropriately combined. According to a preferred example, a method for producing a core-shell type zeolite is exemplified in which particles made of a first zeolite as a core are prepared, the particles made of the first zeolite are coated with a precursor of a second zeolite, and the precursor of the second zeolite is crystallized. That is, the method for producing a core-shell type zeolite according to a preferred embodiment of the present invention includes a step of preparing particles made of a first zeolite (hereinafter also referred to as "step 1"), a step of preparing a precursor of a second zeolite (hereinafter also referred to as "step 2"), and a step of coating the particles made of the first zeolite with a precursor of the second zeolite, and then crystallizing the precursor of the second zeolite (hereinafter also referred to as "step 3"). Each step will be described in detail below.
[0030] [Process 1] In step 1, particles made of a first zeolite are prepared. A specific method for preparing particles made of a first zeolite varies depending on the type (skeletal structure) of the first zeolite, so the following will be described using an example of a method for preparing particles made of FAU zeolite (hereinafter also referred to as "FAU particles") when the first zeolite is FAU zeolite. Note that publicly known techniques can be appropriately adopted as a method for preparing particles made of zeolite other than FAU zeolite.
[0031] An example of a method for preparing FAU particles is a method in which a mixture of a silica source, an alumina source, and an alkali source (hereinafter also referred to as a "raw material mixture") is crystallized under hydrothermal conditions.
[0032] Examples of the silica source include colloidal silica (silica sol), amorphous silica, sodium silicate, tetraethyl orthosilicate, and aluminosilicate gel.
[0033] Examples of the alumina source include aluminum sulfate, sodium aluminate, aluminum hydroxide, aluminum chloride, aluminosilicate gel, and metallic aluminum.
[0034] Examples of the alkali source that can be used include various salts such as hydroxides, halides, sulfates, nitrates and carbonates of sodium, potassium and ammonium, and alkali components in aluminates, silicates and aluminosilicate gels.
[0035] The method for mixing these raw materials is not particularly limited, but a method in which the alumina source and the alkali source are dissolved in water as a solvent, and then the silica source is dropped into the aqueous solution and mixed is preferred.
[0036] As a method for crystallizing the raw material mixture under hydrothermal conditions, for example, a method using an autoclave can be mentioned. The first zeolite may be crystallized, or the crystallized zeolite may contain a part of amorphous, but preferably it is only crystallized zeolite. The crystallization conditions vary depending on the raw material, scale, etc., and can be appropriately set by those skilled in the art. The crystallization temperature is preferably 70 to 250°C, more preferably 120 to 180°C. The crystallization time varies depending on the type of the first zeolite. For example, in the case of FAU, crystallization can be performed preferably for 15 hours to 6 days, more preferably for 2 to 4 days. The crystallization can be performed either by leaving it to stand or by stirring.
[0037] After crystallization, solid-liquid separation is performed, and the excess alkaline solution is washed away with pure water, warm water, etc. Then, the water adhering to the particles is dried to obtain FAU particles.
[0038] The average particle size of the particles made of the first zeolite (e.g., FAU zeolite) is not particularly limited, but is preferably 3 to 15 μm, and more preferably 5 to 8 μm. If the average particle size is within such a range, the particles made of the first zeolite can be satisfactorily coated with a precursor of the second zeolite (e.g., a precursor of BEA zeolite) in step 2 described below. As a result, it becomes possible to obtain a core-shell zeolite having excellent hydrocarbon adsorption and desorption performance. In this specification, the average particle size of the particles is the median diameter (D50) measured by a laser diffraction / scattering type particle size distribution measuring device.
[0039] [Process 2] In step 2, a precursor of the second zeolite is prepared. In this specification, the precursor of the second zeolite means a substance in an amorphous state before crystallization to form the second zeolite. The second zeolite is amorphous, so that it can cover the surface of the first zeolite. If the second zeolite is crystallized, the surfaces of the crystals of the first and second zeolites are stable, so that it does not cover the surface of the first zeolite and tends to exist alone as the second zeolite, which is not preferable. Whether or not the substance is a precursor (amorphous state) can be determined by X-ray diffraction analysis. Since the specific preparation method of the particles made of the second zeolite varies depending on the type (skeletal structure) of the second zeolite, the following will be described by taking as an example a preparation method of a precursor of BEA zeolite (hereinafter also referred to as "BEA precursor") when the second zeolite is BEA zeolite. In addition, a method for preparing a precursor made of a zeolite other than BEA zeolite can be appropriately adopted from known techniques.
[0040] A method for preparing a BEA precursor includes, for example, hydrothermal treatment of a mixture (hereinafter also referred to as "raw material mixture") of a silica source, an alumina source, an alkali source, and an optional template molecule (also referred to as an OSDA).
[0041] Specific examples of the silica source, the alumina source and the alkali source are the same as those described in step 1, and therefore, description thereof will be omitted here.
[0042] Examples of the template molecule include tetraethylammonium hydroxide, tetraethylammonium bromide, and hexamethyleneimine.
[0043] The method for mixing these raw materials is not particularly limited, but a method in which the alumina source, the alkali source, and the template molecule used as necessary are dissolved in water as a solvent, and then the silica source is dropped into the aqueous solution and mixed is preferred.
[0044] A method of amorphizing the raw material mixture under hydrothermal conditions includes, for example, a method using an autoclave. The amorphization conditions vary depending on the raw material, scale, etc., and can be appropriately set by those skilled in the art. The amorphization temperature is preferably 70 to 250°C, more preferably 120 to 150°C. The amorphization time is preferably 2 hours to less than 6 days, more preferably 1 to 3 days. The amorphization can be carried out either by leaving it to stand or by stirring. This makes it possible to obtain a BEA precursor, which is a white gel-like product.
[0045] [Process 3] In step 3, the particles made of the first zeolite are coated with the precursor of the second zeolite, and then the precursor of the second zeolite is crystallized. Hereinafter, the method for producing the core-shell zeolite will be described by taking as an example a case where the first zeolite is FAU zeolite and the second zeolite is BEA zeolite.
[0046] A method for coating particles made of FAU zeolite with a precursor of BEA zeolite includes adding FAU particles to the BEA precursor, which is the above-mentioned white gel product, and stirring as necessary. The mixing ratio of the FAU particles and the BEA precursor is such that the mass of the first zeolite and the mass of the second zeolite in the core-shell zeolite are within the above-mentioned range.
[0047] In this case, if necessary, the FAU particles may be subjected to an ion exchange treatment in advance in order to align the cations of the FAU particles with those of the BEA precursor. In the examples described later, the proton-type FAU particles are subjected to an ion exchange treatment with tetraethylammonium ions in order to align the cations of the FAU particles with those of the BEA precursor, that is, tetraethylammonium ions.
[0048] Thereafter, the BEA precursor covering the FAU particles is crystallized under hydrothermal conditions. Examples of methods for crystallizing under hydrothermal conditions include a method using an autoclave. Crystallization conditions vary depending on the raw material, scale, etc., and can be appropriately set by those skilled in the art. The crystallization temperature is preferably 70 to 250°C, more preferably 120 to 180°C. The crystallization time is preferably 6 to 14 days, more preferably 8 to 10 days. Crystallization can be performed either by leaving it to stand or by stirring.
[0049] After the crystallization, solid-liquid separation is performed, and the excess alkaline solution is washed off with pure water, warm water, etc. Thereafter, the water adhering to the particles is dried, thereby obtaining the core-shell zeolite according to the present invention.
[0050] The average particle size of the core-shell zeolite is not particularly limited, but is preferably 4 to 20 μm, and more preferably 7 to 10 μm. If the average particle size is within this range, the zeolite can be wash-coated onto a three-dimensional structure made of cordierite without any problems.
[0051] <Exhaust gas purification catalyst> Since the core-shell type zeolite according to the present invention can increase the desorption temperature of hydrocarbons, the application of the core-shell type zeolite to an exhaust gas purification catalyst can improve the purification performance of hydrocarbons in exhaust gases. Therefore, according to another aspect of the present invention, there is provided an exhaust gas purification catalyst in which the core-shell type zeolite according to the present invention and a precious metal are supported on a three-dimensional structure.
[0052] The present embodiment will be described below. The exhaust gas purification catalyst according to the present invention (hereinafter also referred to as "catalyst") can appropriately adopt known techniques other than containing the core-shell type zeolite according to the present invention. Therefore, the present invention is not limited to the following embodiment.
[0053] [Core-shell type zeolite] The catalyst according to the present invention essentially contains a core-shell type zeolite. The content of the core-shell type zeolite is preferably 10 to 200 g, more preferably 30 to 120 g, and further preferably 55 to 85 g per 1 L of the three-dimensional structure. By containing the core-shell type zeolite in such an amount, the purification performance of hydrocarbons is further improved.
[0054] [Precious metals] The catalyst according to the present invention essentially contains a precious metal. The precious metal catalyzes an oxidation-reduction reaction for purifying exhaust gas. The type of precious metal is not particularly limited, and examples thereof include platinum (Pt), palladium (Pd), and rhodium (Rh). These precious metals may be used alone or in combination of two or more. Of these, the precious metal is preferably at least one selected from platinum, palladium, and rhodium, more preferably palladium alone; a combination of platinum and / or palladium with rhodium, and particularly preferably palladium alone or a combination of palladium with rhodium.
[0055] Considering the exhaust gas purification ability, the platinum content (metal conversion) is preferably 0.01 to 20 g, more preferably 0.05 to 10 g, and even more preferably more than 0.5 g and less than 5 g per liter of the three-dimensional structure.
[0056] Considering the exhaust gas (particularly HC) purification ability, the palladium content (metal conversion) is preferably 0.01 to 20 g, more preferably 0.05 to 5 g, and even more preferably 0.3 to 3 g per 1 L of the three-dimensional structure.
[0057] Considering the exhaust gas (particularly NOx) purification ability, the rhodium content (metal conversion) is preferably 0.01 to 20 g, more preferably 0.05 to 5 g, and even more preferably 0.1 to 3 g per 1 L of the three-dimensional structure.
[0058] [Refractory inorganic oxide] The catalyst according to the present invention may contain a refractory inorganic oxide (excluding core-shell type zeolite) as necessary. The refractory inorganic oxide functions as a support for supporting catalytic components such as precious metals, rare earth metals, and other metal elements. The refractory inorganic oxide has a high specific surface area, and by supporting a catalytic component on it, the contact area between the catalytic component and exhaust gas can be increased and reactants can be adsorbed. As a result, the reactivity of the entire catalyst can be further increased.
[0059] Examples of the refractory inorganic oxide include alumina, zeolite (excluding core-shell zeolite), titania, zirconia, and silica. These refractory inorganic oxides may be used alone or in combination of two or more. Among these, alumina and zirconia are preferred, and alumina is more preferred, from the viewpoints of high-temperature durability and high specific surface area. Here, the alumina preferably used as the refractory inorganic oxide is not particularly limited as long as it contains an oxide of aluminum, and examples thereof include activated alumina such as γ, δ, η, and θ-alumina, lanthana-containing alumina, silica-containing alumina, silica-titania-containing alumina, and silica-titania-zirconia-containing alumina. These aluminas may be used alone or in combination of two or more. Among these, γ, δ, or θ-alumina and lanthana-containing alumina are preferred from the viewpoints of high-temperature durability and high specific surface area.
[0060] The content of the refractory inorganic oxide is preferably 10 to 300 g, more preferably 40 to 200 g, per 1 L of the three-dimensional structure. When the content of the refractory inorganic oxide is 10 g / L or more, the precious metal can be sufficiently dispersed in the refractory inorganic oxide, and a catalyst having sufficient durability can be obtained. On the other hand, when the content of the refractory inorganic oxide is 300 g / L or less, the contact state between the precious metal and the exhaust gas becomes good, and the exhaust gas purification performance can be more fully exhibited.
[0061] [Ceria-zirconia composite oxide] The catalyst according to the present invention may contain ceria-zirconia composite oxide (CeO2-ZrO2) as an oxygen storage material, if necessary. Here, the oxygen storage material (also called "oxygen storage release material") has the function of stably progressing the oxidation-reduction reaction by storing oxygen in an oxidizing atmosphere (lean) and releasing oxygen in a reducing atmosphere (rich) in response to the fluctuation of the air-fuel ratio (A / F), which changes according to the driving conditions.
[0062] The ceria-zirconia composite oxide may contain at least one metal selected from the group consisting of lanthanum (La), yttrium (Y), neodymium (Nd), and praseodymium (Pr). Specific examples include ceria-zirconia-lanthana composite oxide and ceria-zirconia-lanthana-yttria composite oxide.
[0063] The content of the ceria-zirconia composite oxide (converted into oxide) is not particularly limited, but is preferably 5 to 200 g, more preferably 5 to 100 g, and further preferably 10 to 90 g per 1 L of the three-dimensional structure. By including the ceria-zirconia composite oxide in such an amount, the oxidation-reduction reaction can proceed stably.
[0064] [Other ingredients] The catalyst according to the present invention may further contain other components. Examples of the other components include Group 2 elements such as magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba). These elements may be contained in the exhaust gas purification catalyst in the form of oxides, nitrates, or carbonates. Among these, barium and / or strontium are preferred, and strontium oxide (SrO), barium sulfate (BaSO4), and / or barium oxide (BaO) are more preferred. These other components may be used alone or in combination of two or more.
[0065] When the catalyst according to the present invention contains other components, the content (in terms of oxide) of the other components (particularly, SrO, BaSO4, BaO) is preferably 0 to 50 g, more preferably 0.1 to 30 g, and further preferably 0.5 to 20 g per 1 L of the three-dimensional structure.
[0066] [Three-dimensional structure] The three-dimensional structure functions as a carrier for supporting the core-shell type zeolite, the precious metal, the refractory inorganic oxide, the ceria-zirconia composite oxide, and other components. The three-dimensional structure can be appropriately selected from refractory three-dimensional structures known in the art. As the three-dimensional structure, for example, a heat-resistant carrier such as a honeycomb carrier having a through hole (gas passage hole, cell shape) of a triangular, rectangular, or hexagonal shape can be used. A cell density (cell number / unit cross-sectional area) of 100 to 1200 cells / square inch is sufficiently usable, preferably 200 to 900 cells / square inch, and more preferably 400 to 900 cells / square inch (1 inch = 25.4 mm).
[0067] The catalyst according to the present invention can be produced by appropriately referring to known knowledge. The production method of the catalyst according to the present invention will be briefly described below.
[0068] First, the core-shell zeolite, the precious metal source, and, if necessary, the other components as described above (for example, refractory inorganic oxides, ceria-zirconia composite oxide, other components) and the aqueous medium are appropriately weighed and mixed according to the desired composition, and stirred at 5 to 95°C for 0.5 to 24 hours (if necessary, wet grinding after stirring) to prepare a slurry. Here, as the aqueous medium, water (pure water, ultrapure water, deionized water, distilled water, etc.), lower alcohols such as ethanol and 2-propanol, and organic alkaline aqueous solutions can be used. Among them, it is preferable to use water and lower alcohols, and it is more preferable to use water. The amount of the aqueous medium is not particularly limited, but it is preferable that the ratio of solids in the slurry (solids mass concentration) is 10 to 60 mass%, more preferably 30 to 50 mass%.
[0069] Next, the slurry prepared above is applied to the three-dimensional structure. A known method such as washcoat can be appropriately adopted as a method for applying the slurry to the three-dimensional structure. In addition, the amount of the slurry applied can be appropriately set by a person skilled in the art depending on the amount of solid matter in the slurry and the thickness of the catalyst layer to be formed. The amount of the slurry applied is preferably an amount such that each component has the above-mentioned content (support amount).
[0070] Next, the three-dimensional structure coated with the slurry as described above is dried in air, preferably at a temperature of 70 to 200°C, for 5 minutes to 5 hours. Next, the dried slurry coating film (catalyst precursor layer) thus obtained is fired in air at a temperature of 400°C to 900°C, for 10 minutes to 3 hours. Under these conditions, the catalyst components (core-shell type zeolite, precious metals, etc.) can be efficiently attached to the three-dimensional structure. The catalyst according to the present invention can be obtained by the above steps.
[0071] As described above, the catalyst according to the present invention may have only one catalyst layer or may have a structure in which two or more catalyst layers are laminated, so long as the catalyst has a core-shell zeolite and a precious metal. When the catalyst has a structure in which two or more catalyst layers are laminated, the core-shell zeolite and the precious metal may be contained in the same layer or in different layers. Preferably, the core-shell zeolite and the precious metal are contained in different layers, and more preferably, the core-shell zeolite is disposed in the lower layer and the precious metal is disposed in the upper layer. Such an arrangement allows the capabilities of the core-shell zeolite according to the present invention to be maximized.
[0072] <Method of purifying exhaust gas> The catalyst according to the present invention can exhibit high purification performance for exhaust gas containing hydrocarbons. Therefore, according to yet another aspect of the present invention, there is provided a method for purifying exhaust gas, which comprises contacting the exhaust gas containing hydrocarbons with the exhaust gas purification catalyst according to the present invention.
[0073] The temperature of the exhaust gas may be the same as that of the exhaust gas during the operation of a normal gasoline engine, and is preferably 0 to 1500° C., and more preferably 25 to 700° C. In this specification, the "temperature of the exhaust gas" means the temperature of the exhaust gas at the inlet of the catalyst. Here, the "inlet of the catalyst" refers to a portion 15 cm from the end face of the catalyst on the exhaust gas inlet side.
[0074] Although the catalyst according to the present invention can exhibit sufficient catalytic activity by itself, a similar or different exhaust gas purification catalyst may be arranged in the upstream (inflow side) or downstream (outflow side) of the catalyst according to the present invention. That is, it is preferable to arrange the catalyst according to the present invention alone, or to arrange the catalyst according to the present invention in both the upstream (inflow side) and downstream (outflow side), or to arrange the catalyst according to the present invention in either one of the upstream (inflow side) or downstream (outflow side) and arrange a conventionally known exhaust gas purification catalyst in the other. EXAMPLES
[0075] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples. Unless otherwise specified, each operation was performed under the conditions of room temperature (25°C) / relative humidity 40-50%RH. Furthermore, unless otherwise specified, ratios represent mass ratios.
[0076] <Preparation of Zeolite> [Comparative Example 1-1] Synthesis of Powder a (BEA Zeolite (6.68 Å)) 0.975 g of sodium hydroxide (FUJIFILM Wako Pure Chemical Industries, Ltd., special grade, the same below) was dissolved in 25 mL of purified water. 1.73 g of sodium aluminate (Al / NaOH (molar ratio) = 0.78, FUJIFILM Wako Pure Chemical Industries, Ltd., first grade) and 14.50 g of tetraethylammonium bromide (Tokyo Chemical Industry Co., Ltd., special grade, the same below) were added and dissolved. 12.86 g of ammonia water (28%, FUJIFILM Wako Pure Chemical Industries, Ltd., special grade, the same below) was added to this solution and stirred. Then, 42 mL of silica sol (LUDOX (registered trademark) HS-30, Sigma-Aldrich, the same below) was slowly added with a pipette, and the solution was stirred for 2 hours. 30 g of the resulting white gel-like product was placed in a Teflon (registered trademark) container and sealed. This Teflon (registered trademark) container was heated in a thermostatic chamber at 150° C. for 8 days to obtain powder a (average particle size: 5.35 μm).
[0077] (XRD measurement) The crystal structure of powder a was confirmed by X-ray diffraction (XRD). The measurement was performed using an X-ray diffraction measuring device (Rigaku Corporation, RINT2200VF). The measurement conditions were as follows: measurement angle range (2θ): 3° to 80°, step interval: 0.02°, measurement time: 1.2 seconds / step, radiation source: CuKα radiation, tube voltage: 40 kV, current: 20 mA.
[0078] The XRD spectrum of powder a detected BEA zeolite, but no other types of zeolite, confirming that powder a was BEA zeolite.
[0079] [Comparative Example 2-1] Synthesis of Powder h (FAU Zeolite (11.24 Å)) 5.50 g of sodium hydroxide was dissolved in 42.40 mL of purified water. 4.685 g of sodium aluminate (Al / NaOH (molar ratio) = 0.78, Fujifilm Wako Pure Chemical Industries, first grade) was added to this solution and dissolved. Then, 22 mL of silica sol (LUDOX (registered trademark) HS-40, Sigma-Aldrich) was slowly added, and the solution was stirred for 2 hours. This solution was placed in a Teflon (registered trademark) container and heated in a thermostatic bath at 150 ° C. for 2 days. The obtained white powdery product was collected by suction filtration. Then, suction filtration was performed while washing with water until the filtrate reached pH = 7. The powder after filtration was air-dried for 3 days to obtain powder h (average particle size 6.72 μm).
[0080] The crystal structure of powder h was confirmed by X-ray diffraction (XRD), and the XRD spectrum of powder h detected FAU zeolite, but no peaks derived from other types of zeolite. Therefore, powder h was confirmed to be FAU zeolite.
[0081] [Example 1-1] Synthesis of powder b (BEA / FAU=91 / 9) 47.25 g of tetraethylammonium bromide was weighed into a 500 mL beaker. 450 mL of purified water was added to the beaker to completely dissolve the tetraethylammonium bromide. 19.997 g of FAU zeolite (proton type, Si / Al (molar ratio) = 6.1) synthesized in Comparative Example 2-1 was added to this solution and stirred for 2 hours. Then, the FAU zeolite was collected by filtration. This operation was repeated three times, and then dried overnight in a thermostatic bath at 100 ° C. As a result, the FAU zeolite was ion-exchanged from the proton type to the tetraethylammonium type.
[0082] 0.992 g of sodium hydroxide was dissolved in 25 mL of purified water. 1.74 g of sodium aluminate (Al / NaOH (molar ratio) = 0.78, Fujifilm Wako Pure Chemical Industries, first grade) and 14.52 g of tetraethylammonium bromide were added and dissolved. 12.9 g of ammonia water (28%, Wako Pure Chemical Industries, special grade) was added to this solution and stirred. Then, 42 mL of silica sol (LUDOX (registered trademark) HS-30) was slowly added with a pipette, and the solution was stirred for 2 hours. 30 g of the resulting white gel-like product was placed in a Teflon (registered trademark) container and sealed. This Teflon (registered trademark) container was heated in a thermostatic bath at 150 ° C for 3 days. As a result, 9.746 g of amorphous BEA zeolite precursor was obtained. When the precursor was subjected to X-ray diffraction analysis, BEA zeolite was not detected, and an overall baseline rise was observed, confirming that the precursor was amorphous. 0.98 g of the above-mentioned ion-exchanged FAU zeolite was added to the precursor, and the mixture was heated in a thermostatic bath at 150°C for another 8 days. The resulting white powder product was collected by suction filtration. Then, suction filtration was performed while washing with water until the filtrate reached pH = 7. The filtered powder was air-dried for 3 days to obtain powder b (average particle size 5.35 μm) having a mass ratio of BEA / FAU = 91 / 9.
[0083] When the crystal structure of powder b was confirmed by X-ray diffraction (XRD), both BEA zeolite and FAU zeolite were detected in the XRD spectrum of powder b, and no other types of zeolite were detected. Therefore, it was confirmed that the powder b prepared above is composed of BEA zeolite and FAU zeolite.
[0084] [Example 2-1] Synthesis of powder c (BEA / FAU=87 / 13) Powder c (average particle size 8.25 μm) having a mass ratio of BEA / FAU=87 / 13 was obtained in the same manner as in Example 1-1, except that 1.49 g of ion-exchanged FAU zeolite was added to 9.746 g of amorphous BEA zeolite precursor.
[0085] When the crystal structure of powder c was confirmed by X-ray diffraction (XRD), both BEA zeolite and FAU zeolite were detected from the XRD spectrum of powder c, and no other types of zeolite were detected. Therefore, it was confirmed that the powder c prepared above is composed of BEA zeolite and FAU zeolite.
[0086] [Example 3-1] Synthesis of powder d (BEA / FAU=71 / 29) Powder d (average particle size 7.94 μm) having a mass ratio of BEA / FAU=71 / 29 was obtained in the same manner as in Example 1-1, except that 4 g of ion-exchanged FAU zeolite was added to 9.746 g of amorphous BEA zeolite precursor.
[0087] When the crystal structure of powder d was confirmed by X-ray diffraction (XRD), both BEA zeolite and FAU zeolite were detected from the XRD spectrum of powder d, and no other types of zeolite were detected. Therefore, it was confirmed that powder d prepared above is composed of BEA zeolite and FAU zeolite.
[0088] [Comparative Example 3-1] Synthesis of Powder e (BEA / FAU=62 / 38) Powder e (average particle size 7.32 μm) having a mass ratio of BEA / FAU=62 / 38 was obtained in the same manner as in Example 1-1, except that 5.92 g of ion-exchanged FAU zeolite was added to 9.746 g of amorphous BEA zeolite precursor.
[0089] When the crystal structure of powder e was confirmed by X-ray diffraction (XRD), both BEA zeolite and FAU zeolite were detected from the XRD spectrum of powder e, and no other types of zeolite were detected. Therefore, it was confirmed that the powder e prepared above is composed of BEA zeolite and FAU zeolite.
[0090] [Comparative Example 4-1] Preparation of powder f (mixed powder (BEA / FAU=80 / 20)) By mixing 0.801 g of powder a (BEA zeolite) obtained in Comparative Example 1-1 with 0.203 g of powder b (FAU zeolite) obtained in Comparative Example 2-1, powder f (average particle size 6.94 μm) was obtained in which BEA zeolite and FAU zeolite were mixed in a mass ratio of BEA / FAU=80 / 20.
[0091] When the crystal structure of powder f was confirmed by X-ray diffraction (XRD), both BEA zeolite and FAU zeolite were detected from the XRD spectrum of powder f, and no other types of zeolite were detected. Therefore, it was confirmed that the powder f prepared above is composed of BEA zeolite and FAU zeolite.
[0092] [Comparative Example 5-1] Preparation of Powder g (Mixed Powder (BEA / FAU=70 / 30) By mixing 0.705 g of powder a (BEA zeolite) obtained in Comparative Example 1 and 0.302 g of powder b (FAU zeolite) obtained in Comparative Example 2 in a mortar, powder g (average particle size 6.21 μm) in which BEA zeolite and FAU zeolite were mixed in a mass ratio of BEA / FAU=70 / 30 was obtained.
[0093] When the crystal structure of powder g was confirmed by X-ray diffraction (XRD), both BEA zeolite and FAU zeolite were detected from the XRD spectrum of powder g, and no other types of zeolite were detected. Therefore, it was confirmed that the powder g prepared above is composed of BEA zeolite and FAU zeolite.
[0094] (Zeta potential) The zeta potential of each powder was measured to confirm the surface condition of the particles. The measurements were performed in accordance with JIS Z8836:2017 using a zeta potential measuring device (ELSZ-2Plus, manufactured by Otsuka Electronics Co., Ltd.). The measurements were performed using the laser Doppler method at a liquid temperature of 25°C and pH = 3. The measurement solution used was a 0.5% dispersion of each powder in purified water. The pH was adjusted using 0.1 mol / L hydrochloric acid and 0.1 mol / L sodium hydroxide aqueous solution. The results are shown in Table 1 below.
[0095] [Table 1]
[0096] As shown in Table 1, powder a (BEA only) has a zeta potential of -25.75 mV, and powder h (FAU only) has a zeta potential of 32.06 mV. The "Zeta potential theoretical value (mV)" column in Table 1 lists the theoretical value calculated by the following formula from the measured zeta potential values (mV) for powder a and powder h and the respective proportions (mass%) of BEA and FAU contained in each powder. Theoretical value (mV) = -25.75 (mV) × BEA percentage (mass%) ÷ 100 + 32.06 (mV) × FAU percentage (mass%) ÷ 100.
[0097] The measured zeta potential values for powders f and g (mixed powders) were close to their theoretical values.
[0098] The measured zeta potentials for powders c and d were close to that of powder a (BEA only) (|P x (| / |P2-P1|<0.1 is satisfied). Although not shown in Table 1, similar results were obtained for powder b. Therefore, powders b to d were determined to have surfaces composed of BEA. Furthermore, taking into consideration the results of the XRD measurement, powders b to d were confirmed to be core-shell zeolites having a core composed of FAU zeolite and a shell composed of BEA zeolite.
[0099] The measured zeta potential for powder e was significantly different from that of powder a (BEA only) (|P x (| / |P2-P1|<0.1 is satisfied.) From these results, it was determined that powder e does not have a core-shell structure because it is considered that both BEA and FAU are present on the surface.
[0100] Powders f and g are mixed powders obtained by mixing particles consisting of only the first zeolite (FAU) and particles consisting of only the second zeolite (BEA) in a ratio of FAU:BEA=20:80 and 30:70, respectively. x The values of | / |P2-P1| are 0.23 and 0.30, respectively. From this result, it can be seen that the higher the ratio of particles consisting of only the first zeolite (FAU) (the larger the area of the first zeolite (FAU) on the particle surface), the lower the |P2-P x It can be seen that there is a correlation in which the value of | / |P2-P1| increases.
[0101] [HC adsorption / desorption performance] The HC adsorption and desorption performance of each powder was evaluated by toluene TPD (Temperature Programmed Desorption). The measurement was performed using a catalyst analyzer (Microtrack-Bel, BELCAT II). Helium gas containing toluene gas 3000 ppmC and water vapor (3 volume%) was used as the measurement gas. The sample amount was 0.050 g, and the measurement conditions were a temperature rise rate of 10 °C / min from 50 °C to 400 °C. The gas after the reaction was analyzed using a quadrupole mass spectrometer (BELMASS, Microtrack-Bel). At this time, the temperature at which the detected amount of toluene first coincides with the toluene concentration of 3000 ppmC that was circulated was set as the desorption start temperature, and the temperature at which the detected amount of toluene was maximized was set as the peak top temperature, and the analysis was performed. The higher the desorption start temperature and peak top temperature, the better the zeolite's hydrocarbon adsorption and desorption ability. As for powder e, it was determined that it did not have a core-shell structure as mentioned above, so this evaluation was not performed. The results are shown in Table 2 below.
[0102] [Table 2]
[0103] It is seen from Table 2 that the powders b to d according to the present invention have significantly high desorption start temperatures and peak top temperatures. This shows that the core-shell zeolite according to the present invention can increase the desorption temperature of HC.
[0104] [SEM image] The powder surfaces of the core-shell zeolite powder d and the FAU zeolite powder h were observed by FE-SEM (field emission scanning electron microscope). The observation was performed using a JEOL FE-SEM JSM-6700FS under the conditions of an emission current of 10 μA and an acceleration voltage of 12.5 kV. Figures 1 and 2 show SEM images of powders d and h, respectively. As shown in Figure 2, the surface of the FAU zeolite powder h is smooth, but since the core-shell zeolite powder d in Figure 1 has a shell of BEA zeolite, the surface has the irregularities characteristic of BEA zeolite, and it can be seen that the appearance is different from that of FAU zeolite.
[0105] <Production of exhaust gas purification catalyst> [Comparative Example 1-2] Powder a was weighed out to 70.4 parts by mass, and alumina sol was weighed out to have a solid content of 9.6 parts by mass. The alumina sol was added to distilled water and stirred, and then powder a was added and stirred for 10 minutes. Next, wet pulverization was performed to obtain slurry a1.
[0106] La-containing alumina (La2O3 content is 4 mass%, average particle size D50 is 5 μm, BET surface area is 172.4 m 2 36 parts by mass of CeO2 / g), 18.5 parts by mass of CeZrLa composite oxide (CeO2:ZrO2:La2O3 = 47:47:6 (mass ratio)), and 4.62 parts by mass of barium sulfate were weighed out. These were added to distilled water and stirred for 10 minutes, and then 2.19 parts by mass of an aqueous palladium nitrate solution (concentration 21% by mass) was added dropwise while stirring for 10 minutes. After stirring, wet pulverization was performed to obtain a slurry a2.
[0107] The slurry a1 was wash-coated onto a three-dimensional cordierite structure (diameter 25.4 mm, length 30 mm, cylindrical, 0.0157 L, 400 cells / square inch) so that the loading amount after firing was 80 g / L. Next, it was dried in air at 150°C for 5 minutes, and then fired in air at 550°C for 30 minutes.
[0108] Next, the three-dimensional structure after the wash-coating with the slurry a1 was wash-coated with the slurry a2 so that the loading amount after calcination was 59.58 g / L. Next, the structure was dried in air at 150°C for 5 minutes, and then calcined in air at 550°C for 30 minutes to obtain catalyst A.
[0109] [Comparative Example 2-2] Catalyst H was obtained in the same manner as in Comparative Example 1-2, except that powder h was used instead of powder a.
[0110] [Example 3-2] Catalyst D was obtained in the same manner as in Comparative Example 1-2, except that powder d was used instead of powder a.
[0111] [Comparative Example 5-2] Catalyst G was obtained in the same manner as in Comparative Example 1-2, except that powder g was used instead of powder a.
[0112] <Evaluation of exhaust gas purification catalysts> (HC desorption temperature) For catalysts A, D, G, and H, gas having the composition shown in Table 3 below (space velocity 50,000 h -1 While flowing a gas (linear gas velocity: 0.42 m / sec), the temperature at a position 1 cm from the gas inlet end face of the catalyst was raised from 50°C to 400°C at a heating rate of 40°C / min. The temperature at which the detected amount of toluene first coincided with the toluene concentration in the flow, 840 ppmC, was taken as the desorption start temperature, and the temperature at which the detected amount of toluene became maximum was taken as the peak top temperature, and analysis was performed. The higher the desorption start temperature and peak top temperature, the better the catalyst's ability to adsorb and desorb hydrocarbons. The results are shown in Table 4 below.
[0113] (HC purification rate) In addition, for catalysts A, D, G, and H, gas having the composition shown in Table 3 below (space velocity 50,000 h -1 Table 4 shows the HC purification rate when a gas of 0.42 m / sec (gas linear velocity) was passed through the catalyst and the temperature at a position 1 cm from the gas inlet end face of the catalyst was set to 110°C.
[0114] [Table 3]
[0115] [Table 4]
[0116] From Table 4, it can be seen that catalyst D according to the present invention has significantly high desorption start temperature and peak top temperature. With a catalyst containing the core-shell type zeolite according to the present invention, the HC desorption temperature is increased, so that HC can be desorbed in a temperature range where HC can be purified by Pd. As a result, it is possible to improve the HC purification performance of the catalyst. It can be seen that with a catalyst containing the core-shell type zeolite according to the present invention, the HC purification rate is high even at a low temperature of 110°C.
Claims
1. A core made of a first zeolite and a shell made of a second zeolite, A core-shell zeolite, wherein the channel diameter of the first zeolite is larger than the channel diameter of the second zeolite.
2. 2. The core-shell zeolite according to claim 1, wherein the first zeolite is at least one selected from the group consisting of FAU, LEV, MWW and LTA.
3. 3. The core-shell zeolite according to claim 1 or 2, wherein the second zeolite is at least one selected from the group consisting of BEA, CHA, MFI, MOR, SZR, FER and TON.
4. Formula: |P 2 -P x | / |P 2 -P 1 | < 0.1 (P 1 represents the zeta potential (mV) of the particles made of the first zeolite. 2 represents the zeta potential (mV) of the particles made of the second zeolite. x The core-shell zeolite according to any one of claims 1 to 3, wherein the zeolite particle satisfies the above formula (1).
5. The core-shell zeolite according to any one of claims 1 to 4, wherein the first zeolite is FAU and the second zeolite is BEA.
6. The core-shell zeolite according to any one of claims 1 to 5, wherein the second zeolite is contained in an amount of more than 62 mass% and not more than 95 mass% with respect to the core-shell zeolite.
7. Preparing particles of a first zeolite; Preparing a precursor of a second zeolite; A step of coating particles of the first zeolite with a precursor of the second zeolite and then crystallizing the precursor of the second zeolite; The present invention relates to a method for producing a core-shell zeolite having the above structure.
8. 7. An exhaust gas purifying catalyst comprising the core-shell zeolite according to claim 1 and a precious metal supported on a three-dimensional structure.
9. A method for purifying exhaust gas, comprising contacting the exhaust gas containing hydrocarbons with the exhaust gas purification catalyst according to claim 8.
Citation Information
Patent Citations
Cleaning device for automobile exhaust gas
JP1990135126A