Solid carbon deposition system and solid carbon deposition method
The system controls gas ratios and concentrations in a multi-reactor process to reduce greenhouse gas emissions and stabilize solid carbon recovery, addressing the inefficiencies of existing methods.
Patent Information
- Application Number
- JP2023071663
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
AI Technical Summary
Existing methods for precipitating solid carbon from carbon dioxide emit greenhouse gases and lack stability in carbon recovery.
A system and method that controls the molar ratios and concentrations of gases in a multi-reactor process, including methanation, dry reforming, and solid carbon precipitation reactions, to recycle gases and stabilize solid carbon recovery.
Reduces greenhouse gas emissions and stabilizes solid carbon recovery by controlling gas flow rates and compositions, enhancing the precipitation rate of solid carbon.
Smart Images

Figure 2024157349000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a solid carbon deposition system and method for depositing solid carbon. [Background technology]
[0002] At present, there is an urgent need worldwide to reduce and fix carbon dioxide, which is a greenhouse gas that has a negative impact on the environment. In response to this, various technologies, such as CO2 emission reduction technology, CO2 separation and capture technology, CO2 useful resource conversion technology, and CO2 fixation technology, are being researched and developed for practical use in various places.
[0003] As a method for effectively utilizing carbon dioxide, for example, it is known that methane can be synthesized by a methanation reaction when a mixed gas of carbon dioxide and hydrogen is circulated in the presence of a catalyst heated to 250 to 500° C. (see Patent Document 1). In addition, a technology is also known in which solid carbon is precipitated by high-temperature pyrolysis of methane (see Patent Documents 2 to 5).
[0004] Patent Document 2 discloses a continuous carbon removal system in which a first reactor that causes a methanation reaction without using a catalyst and a second reactor that decomposes methane under temperature conditions of 1200°C or higher are connected in series.
[0005] Patent Document 3 discloses a method for fixation of carbon dioxide, which includes a first reaction step of reacting carbon dioxide and hydrogen in the presence of a catalyst to produce a mixed gas containing methane and water, and a second reaction step of producing at least one carbon product selected from the group consisting of carbon, graphite, carbon nanotubes, and diamond, using the methane gas obtained in the first reaction step as a raw material.
[0006] Patent Document 4 discloses a carbon dioxide fixation system including a methanation reactor that brings a raw material gas containing carbon dioxide and hydrogen into contact with a catalyst that activates a methanation reaction to produce methane and hydrogen from the raw material gas, and a methane pyrolysis reactor that heats the methane produced in the methanation reactor to decompose the methane into solid carbon and hydrogen.
[0007] Patent Document 5 discloses a technology in which a mixed gas of carbon dioxide and methane in a ratio of 7:3 is passed through a pre-reaction tank filled with a 30 wt% Ni / SiO2 catalyst, and reacted for a fixed period of time in a heating furnace at a reaction temperature of 550°C, thereby converting it into a mixed gas of carbon dioxide, methane, hydrogen, and carbon monoxide, and then the gas is passed through a main reaction tank filled with a 50 wt% Fe / SiO2 catalyst whose main component is iron, and the carbon dioxide is subjected to a catalytic reduction reaction with hydrogen at a low temperature of 400°C in a heating furnace, thereby precipitating carbon. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2019-172595 A [Patent Document 2] Japanese Patent Application Publication No. 8-133200 [Patent Document 3] JP 2005-60137 A [Patent Document 4] JP 2015-196619 A [Patent Document 5] JP 2003-48708 A Summary of the Invention [Problem to be solved by the invention]
[0009] Meanwhile, a method for precipitating solid carbon using the Boudoir reaction, which precipitates solid carbon from carbon monoxide, is known. However, in the Boudoir reaction, carbon dioxide is generated as well as the precipitation of solid carbon. Therefore, there is still room for improvement in terms of reducing greenhouse gas emissions.
[0010] The present invention has been made in consideration of the above circumstances, and aims to provide a solid carbon deposition system and a solid carbon deposition method that enable a further reduction in greenhouse gas emissions in the fixation of CO2 and a stable recovery of solid carbon. [Means for solving the problem]
[0011] (1) In order to achieve the above object, the solid carbon deposition system of the present invention is a solid carbon deposition system that deposits solid carbon from a raw material gas containing carbon dioxide and hydrogen, comprising: a first reactor that brings the raw material gas into contact with a catalyst that activates a methanation reaction to produce methane and water from the raw material gas; a second reactor that converts the produced methane into carbon monoxide by heating the produced methane in a state of contact with a catalyst that activates a dry reforming reaction; a third reactor that brings the converted carbon monoxide into contact with a catalyst that activates a solid carbon deposition reaction to deposit the solid carbon from the converted carbon monoxide; an off-gas circulation path that circulates off-gas discharged from the third reactor to the first reactor; and a control unit that controls the flow rate of each gas circulating within the solid carbon deposition system, wherein the control unit controls the flow rate of each gas, including the gas flow rate of the off-gas circulation path, so that the H2 / C molar ratio in the mixed gas supplied to the first reactor is within a specified range.
[0012] The off-gas discharged from the third reactor is circulated, which reduces the amount of greenhouse gases emitted from the entire solid carbon deposition system. In addition, by controlling the H2 / C molar ratio in the mixed gas supplied to the first reactor within a specified range, solid carbon can be stably recovered.
[0013] (2) Furthermore, the solid carbon deposition system described in (1) above is characterized in that it further includes a hydrogen separation flow path that separates hydrogen from the gas discharged from the second reactor, and the control unit controls each gas flow rate, including the gas flow rate of the hydrogen separation flow path, so that the H2 / CO molar ratio in the mixed gas supplied to the third reactor is within a specified range.
[0014] Since the reactor has a hydrogen separation passage for separating hydrogen from the gas discharged from the second reactor, it is easy to control the H2 / CO molar ratio in the mixed gas supplied to the third reactor. In addition, by controlling the H2 / CO molar ratio in the mixed gas supplied to the third reactor within a specified range, the deposition rate of solid carbon in the third reactor can be improved.
[0015] (3) Furthermore, in the solid carbon deposition system described in (2) above, the control unit is characterized in that it controls each gas flow rate, including the gas flow rate of the hydrogen separation channel, so that the carbon monoxide concentration in the mixed gas supplied to the third reactor is within a specified range.
[0016] By controlling the carbon monoxide concentration in the mixed gas supplied to the third reactor so as to be within a specified range, the deposition rate of solid carbon in the third reactor can be improved.
[0017] (4) Moreover, the solid carbon deposition system according to any one of (1) to (3) above is characterized in that it further includes a methane separation flow path that separates methane from the gas discharged from the first reactor, and the control unit controls each gas flow rate, including the gas flow rate of the methane separation flow path, so that the CO2 / CH4 molar ratio in the gas supplied to the second reactor is within a specified range.
[0018] Since the gas supplied to the second reactor is separated from methane by a methane separation passage, the CO2 / CH4 molar ratio in the gas supplied to the second reactor can be easily controlled, thereby suppressing the deposition of solid carbon that accompanies the dry reforming reaction.
[0019] (5) Moreover, the solid carbon deposition system according to any one of (1) to (4) above is characterized in that it further includes a carbon dioxide supply flow path that supplies carbon dioxide to the second reactor, and the control unit controls each gas flow rate, including the gas flow rate of the carbon dioxide supply flow path, so that a CO2 / CH4 molar ratio in the gas supplied to the second reactor is within a specified range.
[0020] Since the second reactor is provided with a carbon dioxide supply passage, it is easy to control the CO2 / CH4 molar ratio in the gas supplied to the second reactor, which makes it possible to suppress the deposition of solid carbon accompanying the dry reforming reaction.
[0021] (6) Furthermore, the method for precipitating solid carbon of the present invention includes a first step of contacting a raw material gas containing carbon dioxide and hydrogen with a catalyst that activates a methanation reaction to produce methane and water from the raw material gas; a second step of converting the produced methane-containing gas into carbon monoxide by heating the produced methane-containing gas in contact with a catalyst that activates a dry reforming reaction; a third step of contacting the converted carbon monoxide-containing gas with a catalyst that activates a solid carbon deposition reaction to precipitate solid carbon from the converted carbon monoxide; and a step of circulating the gas produced in the third step for reuse in the first step, wherein the raw material gas has an H2 / C molar ratio of 2.5 or more.
[0022] The gas generated in the third step is recycled to the first step for reuse in the methanation reaction, which reduces the amount of greenhouse gases emitted during the deposition of solid carbon. In addition, the H2 / C molar ratio of the raw gas is 2.5 or more, so solid carbon can be stably recovered.
[0023] (7) Moreover, the solid carbon deposition method according to (6) above further comprises a step of separating hydrogen from the gas generated in the second step, and as a result of adjusting the amount of separated hydrogen, the converted gas containing carbon monoxide has an H / CO molar ratio of 1.0 or more and 2.0 or less and a carbon monoxide concentration of 30 vol% or more.
[0024] Since the process includes a step of separating hydrogen from the gas after the dry reforming reaction, it becomes easier to control the H2 / CO molar ratio and carbon monoxide concentration in the mixed gas supplied to the third reactor. In addition, the converted carbon monoxide-containing gas has an H2 / CO molar ratio of 1.0 to 2.0 and a carbon monoxide concentration of 30 vol% or more, so that the deposition rate of solid carbon can be improved.
[0025] (8) In the solid carbon deposition method according to (6) or (7) above, the methane-containing gas produced has a CO2 / CH4 molar ratio of 1.0 or more. Since the methane-containing gas produced has a CO2 / CH4 molar ratio of 1.0 or more, deposition of solid carbon accompanying the dry reforming reaction can be suppressed. Effect of the Invention
[0026] According to the present invention, it is possible to further reduce greenhouse gas emissions in the fixation of CO2 and to stably recover solid carbon. [Brief description of the drawings]
[0027] [Figure 1] 1 is a schematic diagram showing a configuration of a solid carbon deposition apparatus according to a first embodiment of the present invention. FIG. [Diagram 2] 1 is a schematic diagram showing a configuration of a solid carbon deposition system according to a first embodiment of the present invention. FIG. [Diagram 3] FIG. 4 is a schematic diagram showing a configuration of a solid carbon deposition apparatus according to a second embodiment of the present invention. [Figure 4]FIG. 4 is a schematic diagram showing a configuration of a solid carbon deposition apparatus according to a third embodiment of the present invention. [Diagram 5] FIG. 11 is a schematic diagram showing the configuration of a solid carbon deposition device according to a fourth embodiment of the present invention. [Figure 6] FIG. 13 is a schematic diagram showing the configuration of a solid carbon deposition device according to a fifth embodiment of the present invention. [Figure 7] FIG. 1 is a schematic diagram showing an experimental system used in Verification Example 1. [Figure 8] FIG. 2 is a schematic diagram showing a spiral catalyst. [Figure 9] 1 is a table showing various conditions and measurement results in each test example. [Figure 10] 1 is a graph showing the solid carbon deposition rate when the horizontal axis represents the H2 / CO molar ratio in the mixed gas supplied to the third reactor. [Figure 11] 1 is a graph showing the solid carbon deposition rate when the horizontal axis represents the carbon monoxide concentration in the mixed gas supplied to the third reactor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] [principle] As a method for precipitating solid carbon from carbon dioxide, a method using a solid carbon precipitating reaction including a methanation reaction, a dry reforming reaction, and a Boudoir reaction is known. The method for precipitating solid carbon using a methanation reaction, a dry reforming reaction, and a solid carbon precipitating reaction can be represented by the following reaction formula. First reaction: CO2 + 4H2 → CH4 + 2H2O ΔH = -165 kJ / mol… (Equation 1) Second reaction: CO2+CH4→2CO+2H2ΔH=248kJ / mol…(Formula 2) Third reaction: 2CO→C+CO2ΔH=-172kJ / mol…(Eq. 3)
[0029] As shown in formula 1, first, a methanation reaction is caused to convert carbon dioxide and hydrogen into methane. Next, as shown in formula 2, a dry reforming reaction is caused to convert carbon dioxide and methane into carbon monoxide. Then, as shown in formula 3, solid carbon is precipitated from the carbon monoxide by a solid carbon precipitation reaction, and the solid carbon is recovered. In this way, solid carbon can be precipitated from carbon dioxide.
[0030] The present inventors have focused on the fact that carbon dioxide is generated along with the precipitation of solid carbon in the solid carbon precipitation reaction, and have found that the gas generated by the solid carbon precipitation reaction can be reused in the methanation reaction. The present inventors have also found that since the gas generated by the solid carbon precipitation reaction contains methane and carbon dioxide in addition to carbon dioxide and hydrogen, the precipitation of solid carbon in the methanation reaction can be suppressed by controlling the H2 / C molar ratio in the feed gas to be 3.0 or more. As a result, the present inventors have been able to further reduce greenhouse gas emissions in the fixation of CO2 and efficiently precipitate solid carbon.
[0031] [First embodiment] A first embodiment of the present invention will be described below.
[0032] [Configuration of solid carbon deposition device] FIG. 1 shows a solid carbon deposition apparatus according to a first embodiment of the present invention. The solid carbon deposition apparatus 1 is an apparatus for depositing solid carbon from process exhaust gas containing carbon dioxide. The process exhaust gas refers to exhaust gas containing carbon dioxide discharged from a cement clinker burning process, a quicklime manufacturing process, a thermal power plant, a waste incineration treatment facility, a firing facility for ceramics or the like, an ironworks, and a chemical plant. In this embodiment, as an example, a case will be described in which solid carbon is deposited from process exhaust gas discharged from a kiln 200 that performs cement clinker burning. The kiln 200 is supplied with limestone and oxygen, performs clinker burning, and discharges exhaust gas containing water and carbon dioxide.
[0033] As shown in Fig. 1, the solid carbon deposition apparatus 1 has three reactors in which different reactions occur, and the three reactors are connected in series. When the reactor to which the raw material gas is supplied is the first reactor 10, the reactions proceed in the order of the first reactor 10, the second reactor 20, and the third reactor 30, and solid carbon is deposited in the third reactor 30. The solid carbon deposition apparatus 1 further includes a gas circulation facility.
[0034] The gas circulation equipment is an equipment for circulating a part of the mixed gas discharged from each reactor to the solid carbon deposition device 1, and has at least a first off-gas circulation path 71 for supplying the off-gas discharged from the third reactor 30 to the first reactor 10. In addition to the first off-gas circulation path 71, the gas circulation equipment has a second off-gas circulation path 72, a methane circulation path 73, a carbon monoxide circulation path 74, a carbon dioxide circulation path 75, and a hydrogen circulation path 76. Since the off-gas contains a large amount of carbon dioxide, it is possible to reduce the emission of greenhouse gases by using the off-gas as a raw material for the raw material gas without discharging it to the outside. In addition, since the off-gas also contains a large amount of methane and carbon monoxide, it can be used as a fuel. Therefore, it may be supplied not only to the first reactor 10 but also to a calcination facility, a steelworks, or a chemical plant, and in this embodiment, it is supplied to the kiln 200 through the second off-gas circulation path 72. The first off-gas circulation path 71 and the second off-gas circulation path 72 may have a facility for separating at least one of carbon monoxide, carbon dioxide, hydrogen, and methane from the off-gas, and may be configured to be capable of supplying the gas separated from the off-gas. The gas circulation facility may have a tank for storing gas in each circulation path. The carbon monoxide circulation path 74, the carbon dioxide circulation path 75, and the hydrogen circulation path 76 may be discharge paths for discharging gas to the outside of the solid carbon deposition apparatus 1, instead of circulation paths.
[0035] In addition to the three reactors and the gas circulation equipment, the solid carbon deposition apparatus 1 includes a hydrogen supply equipment 7, a hydrogen flowmeter 9, a first gas mixer 15, a carbon monoxide separator 21, a methane separator 23, a second gas mixer 25, a carbon dioxide separator 31, a hydrogen separator 33, a first water vapor removal equipment 51 provided at the outlet of the first reactor, a third water vapor removal equipment 53 provided at the outlet of the third reactor, a flowmeter 50, and a carbon dioxide concentration equipment 60. The carbon dioxide concentration equipment 60 includes a first carbon dioxide supply passage 61 for supplying carbon dioxide to the first reactor 10, and a second carbon dioxide supply passage 62 for supplying carbon dioxide to the second reactor 20. In addition, the solid carbon deposition apparatus 1 is preferably provided with equipment for removing sulfur oxides that cause catalyst deterioration. In addition, if nitrogen or oxygen is contained in the process exhaust gas, the absolute amount of the raw material gas becomes large, so an equipment for removing nitrogen or oxygen from the process exhaust gas may be further provided in the upstream of the first reactor.
[0036] The first gas mixer 15 mixes hydrogen supplied from the hydrogen supply equipment 7, the process exhaust gas containing carbon dioxide, the off-gas discharged from the third reactor 30, and the hydrogen separated by the hydrogen separator 33 to generate a raw material gas to be supplied to the first reactor 10. At this time, the raw material gas is mixed so that the molar ratio of H2 / C is 2.5 or more. The H2 / C molar ratio is a molar ratio calculated from (H2+2CH4) / (CO2+CO+CH4). The molar ratio of H2 / C in the raw material gas is more preferably 3.0 or more, and further preferably 3.5 or more. Since the molar ratio of H2 / C in the raw material gas is 2.5 or more, the deposition of solid carbon in the first reactor 10 is suppressed, and solid carbon can be stably recovered. In addition, the process exhaust gas is preferably supplied to the first gas mixer 15 after the concentration of carbon dioxide is increased by the carbon dioxide concentration equipment 60. The first gas mixer 15 is preferably equipped with a flowmeter that measures the flow rate of the raw material gas.
[0037] The first reactor 10 contacts the raw material gas supplied from the first gas mixer 15 with a catalyst that activates the methanation reaction, and produces methane and water from the raw material gas as shown in formula 1. The raw material gas is preferably supplied to the first reactor 10 so that the space velocity is 2000 to 20000 / h. The first reactor 10 includes a gas flow reaction tube filled with a catalyst that activates the methanation reaction, and a heating furnace that can heat the gas flow reaction tube to 300 to 550°C. For the first reactor 10, a normal pressure flow reactor that is a fixed gas flow tube is used, for example, because the gas flow path is not blocked by solid products.
[0038] Examples of catalysts that activate the methanation reaction include Ni, Ru, Pt, and Rh. As the carrier, various oxides such as CeO2, ZrO2, Y2O3, and Al2O3, and aluminosilicates can be used. The shape of the catalyst may be any shape as long as a predetermined space velocity can be achieved, but a spiral shape is preferred because it requires a small catalyst volume. When making the catalyst into a spiral shape, it is produced by forming a metal plate member such as aluminum into a spiral shape and applying a paste-like catalyst to it.
[0039] The carbon monoxide separator 21 separates carbon monoxide from the gas discharged from the first reactor 10. The carbon monoxide separator 21 may be one that utilizes, for example, a PSA method, a membrane separation method, or a cryogenic separation method. The separated carbon monoxide can be supplied to a calcination facility including a kiln 200, a steel mill, or a chemical plant through a carbon monoxide circulation line 74, and can be used as fuel. In FIG. 1, the carbon monoxide circulation line 74 is connected to the second off-gas circulation line 72, and is mixed with the off-gas and then supplied to the kiln 200, but it may also be directly supplied to the kiln 200. The carbon monoxide separator 21 is not essential to the solid carbon deposition device 1, but is preferably provided because the dry reforming reaction is a reversible reaction and the reverse reaction can be suppressed by separating carbon monoxide.
[0040] The methane separator 23 separates methane from the gas discharged from the first reactor 10. Examples of the methane separator 23 include those using the PSA method, the membrane separation method, and the high-pressure water absorption method. The separated methane can be used as fuel by supplying it to a firing facility including a kiln 200, a steelworks, or a chemical plant through the methane discharge path 24 or the methane circulation path 73, which is a methane separation flow path. In FIG. 1, the methane circulation path 73 is connected to the second off-gas circulation path 72, and is mixed with the off-gas and then supplied to the kiln 200, but it may also be directly supplied to the kiln 200. When an amount of methane that cannot be used as fuel is separated in the kiln 200, it is discharged to the outside of the solid carbon deposition device 1 through the methane discharge path 24.
[0041] The second gas mixer 25 mixes the carbon dioxide supplied from the carbon dioxide concentration equipment 60 with the mixed gas discharged from the first reactor 10 to generate a mixed gas to be supplied to the second reactor 20. At this time, the mixed gas to be supplied to the second reactor 20 is preferably mixed so that the CO2 / CH4 molar ratio is 1.0 or more. The CO2 / CH4 molar ratio in the mixed gas to be supplied to the second reactor 20 is more preferably 1.2 or more. Since the CO2 / CH4 molar ratio in the mixed gas to be supplied to the second reactor 20 is 1.0 or more, the reaction rate of the dry reforming reaction can be improved. This is based on "C. Guerra, A. Lanzini, P. Leone, M. Santarelli, NP Brandon, "Optimization of dry reforming of methane over Ni / YSZ anodes for solid oxide fuel cells", Journal of Power Sources, 245, 154-163, (2014)" and "Kawasaki Wataru, Research on structural catalytic reaction systems for utilizing C1 resources, Shizuoka University Graduate School Doctoral thesis, December 2017."
[0042] The second reactor 20 converts methane into carbon monoxide as shown in formula 2 by heating the mixed gas containing methane supplied from the first reactor 10 in contact with a catalyst that promotes the dry reforming reaction. The mixed gas supplied to the second reactor 20 is preferably supplied so that the space velocity is 1300 to 15000 / h. The second reactor 20 includes a gas flow reaction tube filled with a catalyst that activates the dry reforming reaction, and a heating furnace that can heat the gas flow reaction tube to 700 to 900°C. Since there is little concern that the gas flow path in the reactor will be blocked by solid products, for example, a normal pressure flow reactor that is a fixed gas flow side tube is used as the second reactor 20.
[0043] Examples of catalysts that activate the dry reforming reaction include Ni and Rh. As the carrier, various oxides and aluminosilicates such as CeO2, ZrO2, Y2O3, and Al2O3 can be used, but γ-Al2O3 is preferred. The catalyst may have any shape as long as it can achieve a predetermined space velocity, but a spiral shape is preferred because it requires a small catalyst volume. When making the catalyst into a spiral shape, it is produced by forming a metal plate member such as stainless steel into a spiral shape and applying a paste-like catalyst to it.
[0044] The carbon dioxide separator 31 separates carbon dioxide from the mixed gas discharged from the second reactor 20 and supplies carbon dioxide to the carbon dioxide concentration equipment 60 through the carbon dioxide circulation line 75. The carbon dioxide separator 31 utilizes, for example, a PSA method, a chemical absorption method, or a membrane separation method. The carbon dioxide separator 31 can improve the carbon monoxide concentration and reduce the carbon dioxide concentration in the mixed gas supplied to the third reactor by separating carbon dioxide from the gas discharged from the second reactor to reduce the total amount of gas. The carbon dioxide separator 31 is not essential to the solid carbon deposition device 1, but is preferably provided in order to improve the recovery rate of solid carbon. Note that, when the amount of carbon dioxide is excessive in the solid carbon deposition device, the carbon dioxide separated by the carbon dioxide separator 31 may be returned to the carbon dioxide concentration equipment 60.
[0045] The hydrogen separator 33 separates hydrogen from the gas discharged from the second reactor 20 and supplies the hydrogen to the first gas mixer 15 through a hydrogen circulation path 76. The hydrogen separator 33 may be, for example, one that utilizes a PSA method, a membrane separation method, or a chemical adsorption method.
[0046] The third reactor 30 brings the mixed gas containing carbon monoxide supplied from the second reactor 20 into contact with a catalyst that activates the solid carbon deposition reaction, and deposits solid carbon from the carbon monoxide as shown in formula 3. The mixed gas supplied to the third reactor 30 is preferably supplied so that the space velocity is a maximum of 2000 / h. The third reactor 30 includes a gas flow reaction tube filled with a catalyst that activates the solid carbon deposition reaction, and a heating furnace that can heat the gas flow reaction tube to 400 to 900°C. The third reactor 30 is preferably one that can continuously discharge the catalyst on which solid carbon has been deposited, and can continuously supply new catalyst into the reactor, and is preferably, for example, a fluidized bed, a moving bed, or a rotary kiln.
[0047] The mixed gas supplied to the third reactor 30 is preferably supplied so that the H2 / CO molar ratio is 1.0 or more and 2.0 or less, the carbon monoxide concentration is 30 vol% or more, and the carbon dioxide concentration is 15% or less. This can improve the deposition rate of solid carbon. The H2 / CO molar ratio in the mixed gas supplied to the third reactor is more preferably 1.1 or more and 2.0 or less. The carbon monoxide concentration in the mixed gas supplied to the third reactor is preferably 40 vol% or more, more preferably 43 vol% or more, and even more preferably 45 vol% or more. The carbon dioxide concentration in the mixed gas supplied to the third reactor is preferably 10% or less, and more preferably 5% or less.
[0048] Catalysts that activate the solid carbon deposition reaction include Ni, Fe, Mn, Co, Cu, and Zn, but iron-based catalysts are preferred from an environmental perspective. Various oxides and aluminosilicates, such as CeO2, ZrO2, Y2O3, and Al2O3, can be used as supports. The catalyst may have any shape as long as it can achieve a certain space velocity, but a spiral shape is preferred because it requires a small catalyst volume. When making a spiral catalyst, it is produced by forming a metal plate member, such as stainless steel, into a spiral shape and applying a paste-like catalyst to it.
[0049] 1, water vapor removal equipment 51, 53 are provided at the outlets of the first and third reactors. The water vapor removal equipment 51, 53 cools the gas discharged from the outlet of the target reactor to condense the water vapor, and discharges it as industrial wastewater.
[0050] In the methanation reaction in the first reactor 10, water vapor is generated, but if the mixed gas moves to the second reactor 20 while still containing water vapor, the conversion rate of methane may decrease. Therefore, it is preferable to provide a first water vapor removal device 51 at the outlet of the first reactor 10 to actively remove water vapor. In the third reactor 30, the solid carbon deposition reaction is dominant, but it is possible that some reactions that generate water vapor may occur. Therefore, it is preferable to provide a third water vapor removal device 53 at the outlet of the third reactor 30. On the other hand, the dry reforming reaction in the second reactor 20 does not basically generate water vapor. Therefore, it is not necessary to provide a water vapor removal device at the outlet of the second reactor 20, but it may be provided in consideration of the fact that various reaction systems compete in the second reactor 20 and the possibility that water vapor may be generated when the type of catalyst, temperature conditions, etc. are changed.
[0051] In order to adjust the composition ratio of the mixed gas, it is preferable to install a sensor that measures the composition ratio of the gas supplied to the gas mixers 15 and 25, a valve capable of adjusting the flow rate of each mixed gas, and the gas mixers 15 and 25. The sensor may be one that can grasp at least the component ratios of hydrogen, methane, carbon dioxide, and carbon monoxide, and it is preferable that the valve capable of adjusting the flow rate of each mixed gas is installed not only at the outlet where the process exhaust gas is discharged and at the hydrogen supply facility 7, but also when the gas separated from the mixed gas and the off-gas discharged from the third reactor 30 are recycled to each gas mixer.
[0052] In addition, in the solid carbon deposition apparatus 1, the reactions in the first reactor 10 and the third reactor 30 are exothermic reactions, whereas the reaction in the second reactor 20 is an endothermic reaction. Therefore, it is preferable to recover the sensible heat of the mixed gas discharged from the first reactor 10 and the third reactor 30 by a heat exchanger and use it as an energy source for the second reactor 20.
[0053] [Solid carbon deposition system] Next, the solid carbon deposition system will be described. Fig. 2 is a schematic diagram showing the configuration of the solid carbon deposition system. The solid carbon deposition system 500 controls the composition ratio of the mixed gas supplied to each reactor in the solid carbon deposition device 1 to be within a specified range. The specification may be made by a user, but may also be made by a previous setting, a setting by automatic calculation, or an instruction via a network.
[0054] The solid carbon deposition system 500 includes a solid carbon deposition apparatus 1 and a gas composition ratio control device 100. The gas composition ratio control device includes a memory unit 110, an operation unit 120, and a control unit 130. The memory unit 110 records values measured in the solid carbon deposition apparatus 1. The values measured in the solid carbon deposition apparatus 1 include, for example, the composition ratios of the gases supplied to the gas mixers 15 and 25, such as the composition ratios of the mixed gas and process exhaust gas discharged from each reactor.
[0055] The operation unit 120 is a device that allows a user to input data arbitrarily, such as a keyboard, a mouse, or a touch panel. The user can input an arbitrary range for the composition ratio of the mixed gas supplied to each reactor via the operation unit 120. The control unit 130 controls the composition ratio of the mixed gas to be within a specified range based on the data recorded in the storage unit 110. Specifically, the control unit 130 recognizes the gas flow rate from each facility and controls the valves of the gas supplied to each gas mixer 15, 25 and each separator 21, 23, 31, 33, thereby controlling the composition ratio of the mixed gas supplied to each reactor 10, 20, 30 to be within a range specified by the user.
[0056] In this embodiment, an example has been described in which the composition ratio of the mixed gas in all reactors is controllable, but it is sufficient that the H2 / C molar ratio in the raw material gas supplied to at least the first reactor 10 is controllable within a specified range, and it is not necessary that the composition ratio of the mixed gas supplied to at least one of the second reactor 20 and the third reactor 30 is controllable.
[0057] [Solid carbon deposition method] Next, a method for precipitating solid carbon will be described.
[0058] The method of depositing solid carbon varies depending on the methanation rate in the first reactor 10, the type of gas supplied to the kiln from the solid carbon depositor, and whether or not methane is discharged. The methanation rate refers to the rate at which carbon monoxide and carbon dioxide are converted to methane in the first reactor 10. The methods of depositing solid carbon are described below in order.
[0059] (First Method) A case will be described where the methanation rate in the first reactor 10 is low or within an appropriate range, off-gas is supplied to the kiln, and no methane is emitted. First, the raw material gas to be supplied to the first reactor 10 is adjusted. The raw material gas is prepared by mixing hydrogen supplied from the hydrogen supply equipment 7, process exhaust gas containing carbon dioxide, and off-gas, and is adjusted so that the H2 / C molar ratio is 2.5 or more.
[0060] Next, the raw material gas is supplied to the first reactor 10, and the raw material gas is caused to flow through the gas flow reaction tube of the first reactor 10. The gas flow reaction tube is filled with a catalyst heated to 300 to 500°C by a heating furnace, and the raw material gas comes into contact with the catalyst that activates the methanation reaction, producing methane and water from the raw material gas. The produced water is removed by the first water vapor removal equipment 51.
[0061] Next, carbon dioxide is added from the carbon dioxide concentration equipment 60 to the mixed gas discharged from the first reactor 10, and the mixed gas to which carbon dioxide has been added is supplied to the second reactor 20. The mixed gas to which carbon dioxide has been added is caused to flow through the gas flow reaction tube of the second reactor 20. The gas flow reaction tube is filled with a catalyst heated to about 800°C by a heating furnace, and the mixed gas comes into contact with the catalyst that activates the dry reforming reaction, converting methane into carbon monoxide.
[0062] Next, hydrogen is separated from the mixed gas discharged from the second reactor 20, and the mixed gas from which hydrogen has been separated is supplied to the third reactor 30. The separated hydrogen is preferably mixed with off-gas and supplied to the first reactor 10. Then, the mixed gas from which hydrogen has been separated is caused to flow through the gas flow reaction tube of the third reactor 30. The gas flow reaction tube is filled with a catalyst heated to about 450°C by a heating furnace, and the mixed gas comes into contact with the catalyst that activates the solid carbon deposition reaction, carbon monoxide becomes solid carbon, and solid carbon deposits on the surface of the catalyst. Then, the solid carbon can be recovered by recovering the catalyst on which the solid carbon has been deposited.
[0063] Next, the off-gas discharged from the third reactor 30 is circulated by removing water vapor from the off-gas and supplying the removed gas to the first reactor 10 and the kiln 200. At this time, the hydrogen separated from the second reactor 20 is merged with the off-gas flowing through the first off-gas circulation passage 71 and then supplied to the first gas mixer 15.
[0064] In addition, when solid carbon is precipitated by recycling off-gas, it is preferable that the reaction rate in each reactor is relatively high and the separation or addition of gas is small. An example of operation of the solid carbon precipitation device when the methanation rate in the first reactor 10 is 0.57 will be described. In addition, for the example of operation, air is usually used as the combustion supporting gas of the fuel used to heat the kiln 200, but oxygen was used as the combustion supporting gas for calculation. First, 256 mol of limestone of CO2, 193 mol of O2, and 400 mol of off-gas from the off-gas circulation equipment 70 are supplied to the kiln 200. 262 mol of H2O is discharged from the kiln 200, and 265 mol of CO2 is supplied to the first reactor 10 via the carbon dioxide concentration equipment 60. In addition to CO2 from the carbon dioxide concentration equipment 60, 900 mol of H2 from the hydrogen supply equipment 7, a part of the off-gas, and hydrogen separated by the hydrogen separator 33 are supplied to the first reactor 10. Then, the first water vapor removal equipment 51 removes water vapor equivalent to 548 mol of H2O, the carbon dioxide concentration equipment 60 supplies 192 mol of CO2 to the second reactor 20, and the hydrogen separator 33 separates 1065 mol of H2 from the mixed gas discharged from the second reactor 20. This allows 256 mol of solid carbon to be recovered. In addition, the third water vapor removal equipment 53 removes water vapor equivalent to 79 mol of H2O from the off-gas. The amount of off-gas after the water vapor removal is 1339 mol, of which 939 mol is supplied to the first reactor 10 and the remaining off-gas is supplied to the kiln 200 as fuel for burning cement clinker. This suppresses the deposition of solid carbon in each reactor, allowing the stable reaction to continue.
[0065] Next, an example of operation of the solid carbon deposition apparatus when the methanation rate in the first reactor 10 drops to 0.46 will be described. First, 256 mol of limestone, 194 mol of O2, and 400 mol of off-gas from the off-gas circulation equipment 70 are supplied to the kiln 200. 263 mol of H2O is discharged from the kiln 200, and 440 mol of CO2 is supplied to the first reactor 10 via the carbon dioxide concentration equipment 60. In addition to CO2 from the carbon dioxide concentration equipment 60, 900 mol of H2, a part of the off-gas, and hydrogen separated by the hydrogen separator 33 are supplied to the first reactor 10 from the hydrogen supply equipment 7. Then, 557 mol of water vapor of H2O is removed by the first water vapor removal equipment 51, 17 mol of CO2 is supplied to the second reactor 20 from the carbon dioxide concentration equipment 60, and 1670 mol of H2 is separated from the mixed gas discharged from the second reactor 20 by the hydrogen separator 33. As a result, 256 mol of solid carbon can be recovered. In addition, water vapor equivalent to 79 mol of H2O is removed from the off-gas by the third water vapor removal equipment 53. The amount of off-gas after the water vapor removal is 1338 mol, of which 938 mol is supplied to the first reactor 10, and the remaining off-gas is supplied to the kiln 200 for use as fuel. This suppresses the deposition of solid carbon in each reactor, allowing the stable reaction to continue.
[0066] From the above, in the solid carbon deposition method of the present invention, since the H2 / C molar ratio in the raw material gas is adjusted to 2.5 or more, even if the off-gas is supplied to the first reactor and recycled, deposition of solid carbon on the surface of the methanation catalyst in the first reactor can be suppressed and solid carbon can be stably recovered. This makes it possible to reduce the amount of greenhouse gases emitted from the solid carbon deposition device compared to the case where the off-gas is not recycled.
[0067] (Second Method) Next, a case will be described in which the carbon dioxide reaction rate in the first reactor 10 is within an appropriate range, methane is supplied to the kiln, and no methane is discharged. The second method differs from the first method in that methane is supplied to the kiln from a solid carbon deposition device. Therefore, only the adjustment of the mixed gas discharged from the first reactor and the circulation of the off-gas will be described, and other explanations will be omitted.
[0068] The mixed gas supplied to the second reactor 20 is adjusted by adding carbon dioxide from the carbon dioxide concentration equipment 60 to the mixed gas discharged from the first reactor 10, and by separating methane by the methane separator 23. At this time, it is preferable to control the amount of methane separated so that the CO2 / CH4 molar ratio in the mixed gas supplied to the second reactor is 1.0 or more and 2.0 or less. The separated methane is supplied to the kiln 200 and used as fuel. In addition, it is preferable that the off-gas discharged from the third reactor is not supplied to the kiln 200, but is supplied only to the first reactor 10.
[0069] An example of operation of the solid carbon deposition apparatus when the methanation rate in the first reactor 10 is 0.62 will be described. First, limestone of 256 mol of CO2, 183 mol of O2, and methane separated by the methane separator 23 are supplied to the kiln 200. 184 mol of H2O is discharged from the kiln 200, and 157 mol of CO2 is supplied to the first reactor 10 via the carbon dioxide concentration equipment 60. In addition to CO2 from the carbon dioxide concentration equipment 60, the first reactor 10 is supplied with 882 mol of H2 from the hydrogen supply equipment 7, off-gas, and hydrogen separated by the hydrogen separator 33. Then, the first water vapor removal equipment 51 removes water vapor equivalent to 617 mol of H2O, the methane separator 23 separates 92 mol of CH4 from the mixed gas discharged from the first reactor 10, the carbon dioxide concentration equipment 60 supplies 191 mol of CO2 to the second reactor 20, and the hydrogen separator 33 separates 1141 mol of H2 from the mixed gas discharged from the second reactor 20. This allows 256 mol of solid carbon to be recovered. In addition, the third water vapor removal equipment 53 removes water vapor equivalent to 79 mol of H2O from the off-gas, and supplies the entire amount of 1339 mol of the off-gas after the water vapor removal to the first reactor 10. This suppresses the deposition of solid carbon in each reactor, allowing the stable reaction to continue.
[0070] An example of operation of the solid carbon deposition apparatus when the methanation rate in the first reactor 10 is 0.71 will be described. First, limestone of 256 mol of CO2, 184 mol of O2, and methane separated by the methane separator 23 are supplied to the kiln 200. 184 mol of H2O is discharged from the kiln 200, and 52 mol of CO2 is supplied to the first reactor 10 via the carbon dioxide concentration equipment 60. In addition to CO2 from the carbon dioxide concentration equipment 60, the first reactor 10 is supplied with 881 mol of H2 from the hydrogen supply equipment 7, off-gas, and hydrogen separated by the hydrogen separator 33. Then, in the first water vapor removal equipment 51, water vapor equivalent to 617 mol of H2O is removed, 92 mol of CH4 is separated from the mixed gas discharged from the first reactor 10 by the methane separator 23, 296 mol of CO2 is supplied to the second reactor 20 from the carbon dioxide concentration equipment 60, and 775 mol of H2 is separated from the mixed gas discharged from the second reactor 20 by the hydrogen separator 33. As a result, 256 mol of solid carbon can be recovered. In addition, water vapor equivalent to 79 mol of H2O is removed from the off-gas by the third water vapor removal equipment 53, and the total amount of 1339 mol of the off-gas after the water vapor removal is supplied to the first reactor 10. As a result, the deposition of solid carbon in each reactor is suppressed, and a stable reaction can be continued.
[0071] Since methane is supplied to the kiln, it is easier to control the kiln compared to off-gas, which is a mixed gas. Also, when the methanation rate is high, methane cannot be consumed completely in the second reactor 20, so it is necessary to discharge the methane. In contrast, in the present invention, the dry reforming reaction is promoted by separating methane while supplying carbon dioxide. This allows solid carbon to be stably precipitated even if the off-gas is circulated to the first reactor.
[0072] (Third Method) Next, a case will be described in which the carbon dioxide reaction rate in the first reactor 10 is high, methane is supplied to the kiln, and no methane is discharged. The third method differs from the second method in that carbon dioxide is not supplied from the carbon dioxide concentration equipment to the first reactor. Therefore, only the adjustment of the raw material gas supplied to the first reactor will be described, and other explanations will be omitted.
[0073] The raw material gas supplied to the first reactor 10 is prepared by mixing hydrogen and off-gas, and the H2 / C molar ratio is adjusted to be 3.0 or more. It is preferable to recycle not only hydrogen supplied from the hydrogen supply facility 7, but also hydrogen separated from the mixed gas discharged from the second reactor.
[0074] An example of the operation of the solid carbon deposition apparatus when the methanation rate in the first reactor 10 is 0.76 will be described. First, limestone of 256 mol of CO2, 184 mol of O2, and methane separated by the methane separator 23 are supplied to the kiln 200. 184 mol of H2O is discharged from the kiln 200. The first reactor 10 is supplied with 882 mol of H2, off-gas, and hydrogen separated by the hydrogen separator 33 from the hydrogen supply equipment 7. Then, the first water vapor removal equipment 51 removes water vapor of 618 mol of H2O, the methane separator 23 separates 92 mol of CH4 from the mixed gas discharged from the first reactor 10, the carbon dioxide concentration equipment 60 supplies 348 mol of CO2 to the second reactor 20, and the hydrogen separator 33 separates 625 mol of H2 from the mixed gas discharged from the second reactor 20. As a result, 256 mol of solid carbon can be recovered. Furthermore, the third water vapor removal equipment 53 removes water vapor equivalent to 79 mol of H2O from the off-gas, and the total amount of 1339 mol of the off-gas after the water vapor removal is supplied to the first reactor 10. This suppresses the deposition of solid carbon in the reactor, allowing the reaction to continue stably.
[0075] Methane is separated from the mixed gas discharged from the first reactor 10. The separated methane is supplied to a calcination facility including a kiln 200, a steel mill, or a chemical plant, or is discharged to the outside of the solid carbon deposition device 1. Then, carbon dioxide is mixed with the mixed gas from which methane has been separated. Carbon dioxide is supplied from a carbon dioxide concentration facility 60. At this time, it is preferable to control the amount of methane to be separated and the amount of carbon dioxide to be supplied so that the CO2 / CH4 molar ratio in the mixed gas supplied to the second reactor is 1.0 or more and 2.0 or less, and the carbon dioxide concentration in the mixed gas supplied to the third reactor is 15% or less. In this way, the mixed gas from which methane has been separated and carbon dioxide has been mixed is supplied to the second reactor 20.
[0076] When the methanation rate is high, the CO2 / CH4 ratio of the gas flowing into the second reactor falls below 1.0, and solid carbon is likely to precipitate on the catalyst surface of the second reactor. Therefore, the ratio of carbon dioxide supplied from the carbon dioxide enrichment equipment to the second reactor is increased so that the CO2 / CH4 ratio is 1.0 or more. This suppresses the precipitation of solid carbon on the catalyst surface of the second reactor, and allows solid carbon to be stably precipitated in the third reactor.
[0077] In the above, a case has been described in which methane is separated from the mixed gas discharged from the first reactor 10 and then carbon dioxide is mixed therewith. However, carbon dioxide may be mixed in first and then methane may be separated therefrom.
[0078] (Fourth Method) Next, a case will be described in which the carbon dioxide reaction rate in the first reactor 10 is higher than that in the fifth method, off-gas is supplied to the kiln, and methane is discharged. The fourth method differs from the third method in that methane is discharged outside the solid carbon deposition system. Therefore, only the adjustment of the mixed gas discharged from the second reactor will be described, and other explanations will be omitted.
[0079] The mixed gas supplied to the second reactor 20 is adjusted by adding carbon dioxide from the carbon dioxide enrichment equipment 60 to the mixed gas discharged from the first reactor 10 and separating methane by the methane separator 23. The separated methane is supplied to the kiln 200 as fuel, and the excess methane is discharged outside the solid carbon deposition device 1.
[0080] An example of operation of the solid carbon deposition apparatus when the methanation rate in the first reactor 10 is 0.76 will be described. First, limestone of 256 mol of CO2, 184 mol of O2, and methane separated by the methane separator 23 are supplied to the kiln 200. 184 mol of H2O is discharged from the kiln 200. The first reactor 10 is supplied with 896 mol of H2 from the hydrogen supply equipment 7, off-gas, and hydrogen separated by the hydrogen separator 33. Then, the first water vapor removal equipment 51 removes water vapor of 620 mol of H2O, and the methane separator 23 separates methane from the mixed gas discharged from the first reactor 10. Of the separated methane, 92 mol of CH4 is supplied to the kiln 200, and 8 mol of CH4 is discharged outside the solid carbon deposition system. 348 mol of CO2 is supplied from the carbon dioxide concentration equipment 60 to the second reactor 20, and 613 mol of H2 is separated from the mixed gas discharged from the second reactor 20 by the hydrogen separator 33. This allows 248 mol of solid carbon to be recovered. In addition, the third water vapor removal equipment 53 removes water vapor equivalent to 76 mol of H2O from the off-gas, and the total amount of 1219 mol of the off-gas after the water vapor removal is supplied to the first reactor 10. This suppresses the deposition of solid carbon in the reactor, allowing the reaction to continue stably.
[0081] As described above, by changing the control of the solid carbon deposition device 1 depending on the methanation rate, the type of gas supplied from the solid carbon deposition device to the kiln, and whether or not methane is emitted, solid carbon can be stably recovered even if the off-gas is circulated to the first reactor.
[0082] [Second embodiment] Next, a second embodiment of the present invention will be described. In the first embodiment, among the solid carbon deposition methods that differ depending on the methanation rate in the first reactor 10, the type of gas supplied from the solid carbon deposition device to the kiln, and the presence or absence of methane emission, all of the first to fourth methods can be supported, but the second embodiment may be configured to be compatible with only one of them. The second embodiment differs from the first embodiment in that, among the above-mentioned solid carbon deposition methods, only the first method can be supported.
[0083] 3 shows a solid carbon deposition apparatus according to a second embodiment. Compared with the solid carbon deposition apparatus 1, the solid carbon deposition apparatus 2 does not include a carbon monoxide separator 21, a methane separator 23, or a carbon dioxide separator 31. When the carbon monoxide concentration in the reaction gas of the first reactor is low, the carbon monoxide separator 21 is not necessary. Also, when the methane concentration and the carbon dioxide concentration in the reaction gas of the second reactor are low, it is possible to stably deposit solid carbon even without the methane separator 23 and the carbon dioxide separator 31. The absence of the carbon monoxide separator 21, the methane separator 23, and the carbon dioxide separator 31 allows the cost associated with the equipment of the solid carbon deposition apparatus to be reduced.
[0084] [Third embodiment] Next, a third embodiment of the present invention will be described. The third embodiment differs from the first embodiment in that the third embodiment is applicable only to the second method among the solid carbon deposition methods.
[0085] 4 shows a solid carbon deposition apparatus according to a third embodiment. Compared to the solid carbon deposition apparatus 1, the solid carbon deposition apparatus 3 does not include the carbon monoxide separator 21, the carbon dioxide separator 31, the methane discharge passage 24, and the second off-gas circulation passage 72. Therefore, the methane separator 23 directly supplies methane to the kiln 200 through the methane circulation passage 73.
[0086] [Fourth embodiment] Next, a fourth embodiment of the present invention will be described. The fourth embodiment differs from the first embodiment in that the fourth embodiment is applicable only to the third method among the solid carbon deposition methods.
[0087] 5 shows a solid carbon deposition apparatus according to a fourth embodiment. The solid carbon deposition apparatus 4 does not include a first carbon dioxide supply passage 61, as compared with the solid carbon deposition apparatus 3. This makes it possible to reduce the cost of installing the solid carbon deposition apparatus.
[0088] [Fifth embodiment] Next, a fifth embodiment of the present invention will be described. The fifth embodiment differs from the first embodiment in that the fifth embodiment is applicable only to the fourth method among the solid carbon deposition methods.
[0089] 6 shows a solid carbon deposition apparatus according to a fifth embodiment. The solid carbon deposition apparatus 5 is different from the solid carbon deposition apparatus 4 in that it includes a methane discharge passage 24, through which methane can be discharged from the methane separator 23 to the outside of the solid carbon deposition apparatus.
[0090] In the above second to fifth embodiments, the embodiments are described as being applicable to any one of the first to fourth methods of precipitating solid carbon. However, the second to fifth embodiments may be combined to be applicable to two or more methods.
[0091] [Verification example 1] First, the inventors used the gas that had completed the methanation reaction, dry reforming reaction, and solid carbon deposition reaction in the methanation reaction, and measured the gas composition ratio in each reaction. As shown in Figure 7, a gas with a H2 / CO2 molar ratio controlled to 2.5 was supplied as a raw material gas to four reactors connected in series in the order of a first reactor 10, a second reactor 20, a third reactor 30, and a fourth reactor 40, and the methanation reaction, dry reforming reaction, and solid carbon deposition reaction were carried out in that order, and then the methanation reaction was carried out again to verify the results.
[0092] The heating furnaces constituting the first and fourth reactors were one-zone electric furnaces capable of controlling temperature (ceramic electric tubular furnace manufactured by Asahi Rika Seisakusho, effective length 300 mm), and the atmospheric pressure flow-type reaction tube was a quartz tube with an inner diameter of 8 mm and a length of 600 mm. Two catalysts with 10 wt% Ni / CeO2 coated on the surface of a spiral structure as shown in Figure 8 were installed at the position of the temperature control thermocouple of the heating furnace inside the atmospheric pressure flow-type reaction tube as a catalyst to activate the methanation reaction.
[0093] The catalyst to activate the methanation reaction was made by using CeO2 (a reagent manufactured by Kanto Chemical Co., Ltd.) as a carrier and supporting 10 wt% Ni(NO3)2·6H2O (98% manufactured by Wako Pure Chemical Industries, Ltd.) by evaporation to dryness. After supporting, the material was fired at 500℃ for 2 hours in an air atmosphere to separate the nitric acid component. After cooling the fired material, distilled water was added and it was ground in a mortar to produce a Ni / CeO2 paste.
[0094] Separate from the Ni / CeO2 paste, a spirally twisted aluminum plate (JIS A1100 H14, width 7 mm × length 50 mm, thickness 1.5 mm) was surface treated with a 0.8 mol NaOH aqueous solution and a 3.0 mol hydrochloric acid solution as shown in Figure 8. The spirally twisted aluminum plate was then dried with cold air and repeatedly immersed until a sufficient amount of Ni / CeO2 catalyst was supported on it to achieve the desired methanation.
[0095] The second reactor was prepared in the same manner as the first reactor, except that a catalyst for activating the dry reforming reaction was used instead of a catalyst for activating the methanation reaction. The catalyst for activating the dry reforming reaction was a commercially available γ-Al2O3 (C20 manufactured by Nippon Light Metal Co., Ltd.) carrier, on which 10 wt% Ni(NO3)2·6H2O (98% manufactured by Wako Pure Chemical Industries, Ltd.) was supported by the evaporation-to-dry method. The catalyst was prepared in the same manner as the catalyst for activating the methanation reaction, except that the Ni / γ-Al2O3 paste was applied to a stainless steel plate (SUS304, width 7 mm × length 50 mm, thickness 0.5 mm) twisted into a spiral shape as shown in Figure 8.
[0096] The third reactor was prepared in the same manner as the first reactor, except that a quartz tube with an inner diameter of 21 mm and a length of 600 mm was used as the atmospheric pressure flow-type reaction tube, and eight catalysts for activating the solid carbon deposition reaction were placed inside the atmospheric pressure flow-type reaction tube (four catalysts were bundled together, and two bundles were arranged in series) instead of the catalyst for activating the methanation reaction. The catalyst for activating the solid carbon deposition reaction was magnetite (Fe3O4 reagent: Wako Pure Chemical Industries, 98%), which was made into a paste by adding distilled water to the magnetite. It was prepared in the same manner as the catalyst for activating the methanation reaction, except that the magnetite paste was applied to a spirally twisted stainless steel plate (SUS304, width 7 mm x length 50 mm, thickness 0.5 mm) as shown in Figure 8.
[0097] After preparing each reactor, in order to reduce each catalyst, the temperature was kept at 500°C for 1 hour while flowing hydrogen at 200ml / min. Next, the control temperature of the first reactor was set to 340°C, the control temperature of the second reactor to 800°C, the control temperature of the third reactor to 450°C, and the control temperature of the fourth reactor to 340°C. After all the reactors reached the designated temperatures, a standard hydrogen gas cylinder was used as the hydrogen supply equipment, and a standard carbon dioxide gas cylinder was used instead of the process exhaust gas, and the raw material gas was supplied to the first reactor via the mass flow controller and the first gas mixer.
[0098] At this time, the flow rate of hydrogen was set to 179 ml / min and the flow rate of carbon dioxide was set to 71 ml / min using mass flow controllers so that the H2 / CO2 molar ratio in the raw material gas was 2.5, and the total flow rate of the raw material gas was set to 250 ml / min and supplied to the first reactor.
[0099] At the outlet of each reactor, a water vapor removal device and a sampling hole were installed. Thirty minutes after the indicated temperature of each reactor reached the set temperature, samples were taken from the sampling hole using a syringe, and the hydrogen, methane, carbon dioxide, and carbon monoxide were quantitatively analyzed using a gas chromatograph GC-2014 (Shimadzu Corporation).
[0100] Table 1 shows the conditions for each reaction, the composition ratio of the outlet gas in each reactor, the H2 / C molar ratio, and the reaction rate of the main reaction in each reactor. The H2 / C molar ratio was calculated from (H2+2CH4) / (CO2+CO+CH4) in the outlet gas of each reactor. For example, the reaction rate of the first reactor indicates the conversion rate of carbon dioxide supplied to the first reactor to methane. Also, the reaction rate of the second reactor indicates the decomposition rate of methane flowing into the second reactor. [Table 1]
[0101] As shown in Table 1, while sufficient methanation was achieved in the first reactor, solid carbon was precipitated on the catalyst surface in the fourth reactor, and sufficient methanation did not occur. This is believed to be because the low H2 / C molar ratio in the fourth reactor caused solid carbon to precipitate, causing the catalyst to lose activity. When using recycled feed gas, a mixed gas containing methane and carbon dioxide is used for the methanation reaction. Therefore, it is believed that the H2 / C molar ratio needs to be even higher than when a feed gas consisting of hydrogen and oxygen is supplied. As a result of examining the numerical range of H2 / C molar ratios in which solid carbon does not precipitate in the methanation reaction, it was found that solid carbon precipitation is significantly suppressed when the H2 / C molar ratio is 2.5 or higher, and is even more significantly suppressed when the H2 / C molar ratio is 3.0 or higher.
[0102] [Verification example 2] Next, the inventors investigated the conditions for precipitating solid carbon in order to improve the reaction efficiency in the third reactor. Hydrogen and carbon monoxide produced by the dry reforming reaction flow into the third reactor. Therefore, the inventors investigated the carbon dioxide concentration, carbon monoxide concentration, and H2 / CO molar ratio in the mixed gas supplied to the third reactor as conditions for precipitating solid carbon.
[0103] (Test Example 2) The total flow rate of the mixed gas supplied to the first reactor was 125 ml / min (hydrogen 90 ml / min, carbon dioxide 35 ml / min), and the carbon dioxide concentration in the mixed gas flowing into the third reactor was 0 vol%, the carbon monoxide concentration was 23.3 vol%, and the H2 / CO molar ratio was 2.43.
[0104] (Test Example 3) The same procedure as in Test Example 2 was repeated, except that the flow rate of the entire mixed gas supplied to the first reactor was 250 ml / min (hydrogen 179 ml / min, carbon dioxide 71 ml / min), the carbon dioxide concentration in the mixed gas flowing into the third reactor was 0 vol%, the carbon monoxide concentration was 30.2 vol%, and the H2 / CO molar ratio was 2.04.
[0105] (Test Example 4) The same procedure as in Test Example 2 was repeated, except that the flow rate of the total mixed gas supplied to the first reactor was 250 ml / min (hydrogen 179 ml / min, carbon dioxide 71 ml / min), the carbon dioxide concentration in the mixed gas flowing into the third reactor was 1.9 vol%, the carbon monoxide concentration was 33.5 vol%, and the H2 / CO molar ratio was 1.81.
[0106] (Test Example 5) The same procedure as in Test Example 2 was repeated, except that the flow rate of the total mixed gas supplied to the first reactor was 500 ml / min (hydrogen 358 ml / min, carbon dioxide 142 ml / min), the carbon dioxide concentration in the mixed gas flowing into the third reactor was 3.3 vol%, the carbon monoxide concentration was 30.7 vol%, and the H2 / CO molar ratio was 1.75.
[0107] (Test Example 6) In the third reactor, two atmospheric flow-type reaction tubes (quartz tubes with an inner diameter of 21 mm and a length of 600 mm) containing a catalyst for activating the solid carbon deposition reaction were placed, and a solid carbon recovery experiment was conducted. The same procedure as in Test Example 2 was carried out, except that the flow rate of the entire mixed gas supplied to the first reactor was 250 ml / min (hydrogen 179 ml / min, carbon dioxide 71 ml / min), the carbon dioxide concentration in the mixed gas flowing into the third reactor was 3.7 vol%, the carbon monoxide concentration was 32.8 vol%, and the H2 / CO molar ratio was 1.70, and two solid carbon precipitation reaction tubes were installed.
[0108] (Test Example 7) The same procedure as in Test Example 2 was repeated, except that the flow rate of the total mixed gas supplied to the first reactor was 250 ml / min (hydrogen 179 ml / min, carbon dioxide 71 ml / min), the carbon dioxide concentration in the mixed gas flowing into the third reactor was 1.8 vol%, the carbon monoxide concentration was 36.9 vol%, and the H2 / CO molar ratio was 1.61.
[0109] (Test Example 8) The same procedure as in Test Example 2 was repeated, except that the flow rate of the total mixed gas supplied to the first reactor was 250 ml / min (hydrogen 180 ml / min, carbon dioxide 70 ml / min), the carbon dioxide concentration in the mixed gas flowing into the third reactor was 1.2 vol%, the carbon monoxide concentration was 37.7 vol%, and the H2 / CO molar ratio was 1.60.
[0110] (Test Example 9) The same procedure as in Test Example 2 was repeated, except that the flow rate of the total mixed gas supplied to the first reactor was 250 ml / min (hydrogen 170 ml / min, carbon dioxide 80 ml / min), the carbon dioxide concentration in the mixed gas flowing into the third reactor was 5 vol%, the carbon monoxide concentration was 46.3 vol%, and the H2 / CO molar ratio was 1.04.
[0111] (Test Example 12) The same procedure as in Test Example 2 was repeated, except that the flow rate of the total mixed gas supplied to the first reactor was 250 ml / min (hydrogen 150 ml / min, carbon dioxide 100 ml / min), the carbon dioxide concentration in the mixed gas flowing into the third reactor was 15.8 vol%, the carbon monoxide concentration was 46.5 vol%, and the H2 / CO molar ratio was 0.80.
[0112] (Test Example 1) In Test Example 1, a solid carbon recovery experiment was carried out by connecting a fourth reactor for solid carbon deposition in series to the rear stage of the third reactor in Verification Example 1 for an atmospheric pressure flow-type reaction tube and a catalyst for activating a solid carbon deposition reaction. The total flow rate of the mixed gas supplied to the first reactor was 250 ml / min (hydrogen 179 ml / min, carbon dioxide 71 ml / min), and the carbon dioxide concentration in the mixed gas flowing into the fourth reactor was 15.4 vol%, the carbon monoxide concentration was 13.8 vol%, and the H2 / CO molar ratio was 4.51.
[0113] (Test Example 10) The methanation catalyst in the first reactor was removed, and a methanation catalyst was placed in the low-temperature section at the inlet of the second reactor. A dry reforming catalyst was placed in the high-temperature section (temperature control section) in the center of the second reactor, and a solid carbon recovery experiment was conducted.
[0114] The total flow rate of the mixed gas supplied to the first reactor was 250 ml / min (hydrogen 125 ml / min, carbon dioxide 125 ml / min), and the carbon dioxide concentration in the mixed gas flowing into the fourth reactor was 30.8 vol%, the carbon monoxide concentration was 30.8 vol%, and the H2 / CO molar ratio was 1.05.
[0115] (Test Example 11) The methanation catalyst in the first reactor was removed, and a catalyst to activate the reverse shift reaction was used in the second reactor, which was made by mixing alumina with ordinary cement paste made by a known method and then solidifying it. The total flow rate of the mixed gas supplied to the first reactor was 202 ml / min (hydrogen 86 ml / min, carbon dioxide 116 ml / min), and the carbon dioxide concentration in the mixed gas flowing into the fourth reactor was 33.5 vol%, the carbon monoxide concentration was 32.6 vol%, and the H2 / CO molar ratio was 0.93. The blend ratio of ordinary cement paste was cement:water:alumina = 58:29:13 by mass.
[0116] FIG. 9 is a table summarizing the experimental conditions and experimental results of Test Examples 1 to 12. FIG. 10 is a graph showing the solid carbon deposition rate when the H2 / CO molar ratio in the mixed gas supplied to the third reactor is taken on the horizontal axis. From the graph in FIG. 10, it was confirmed that the solid carbon deposition rate is good when the H2 / CO molar ratio in the mixed gas supplied to the third reactor is 1.0 or more and 2.0 or less. The solid carbon deposition reaction is a reaction that produces solid carbon and carbon dioxide from carbon monoxide, but since the solid carbon deposition rate changes depending on the H2 / CO molar ratio in FIG. 10, it is considered that hydrogen may be necessary to separate solid carbon from carbon monoxide.
[0117] Moreover, in Test Examples 2 to 9, the solid carbon deposition rate was good, being 10% or more. In contrast, in Test Examples 1 and 10 to 12, in which the carbon dioxide concentration in the mixed gas supplied to the third reactor was 15% or less, the solid carbon deposition rate was less than 15%. From this, it was confirmed that the solid carbon deposition rate is good when the carbon dioxide concentration in the mixed gas supplied to the third reactor is 15% or less.
[0118] [Verification example 3] Next, the inventors of the present invention examined the carbon monoxide concentration as a condition for precipitating solid carbon. Figure 11 is a graph summarizing the results of Test Examples 1 to 9, and shows the deposition rate of solid carbon when the carbon monoxide concentration supplied to the third reactor is taken on the horizontal axis.
[0119] As shown in Fig. 11, the deposition rate of solid carbon tends to be proportional to the carbon monoxide concentration in the mixed gas supplied to the third reactor. It was confirmed that the deposition rate of solid carbon becomes good when the carbon monoxide concentration in the mixed gas supplied to the third reactor is 30 vol% or more. [Explanation of symbols]
[0120] 1, 2, 3, 4, 5 Solid carbon deposition device 7 Hydrogen supply equipment 9. Hydrogen flow meter 10 First Reactor 15 First gas mixer 20 Second Reactor 21 Carbon monoxide separator 23 Methane separator 24 Methane Exhaust Pipe 25 Second gas mixer 30 Third Reactor 31 Carbon dioxide separator 33 Hydrogen separator 40 Fourth Reactor 50 flow meter 51 First Water Vapor Removal Facility 53 Third Water Vapor Removal Facility 60 Carbon Dioxide Concentration Equipment 61 First carbon dioxide supply line 62 Second carbon dioxide supply line 71 First off-gas circulation line 72 Second off-gas circulation line 73 Methane Circulation 74 Carbon monoxide circuit 75 Carbon dioxide circulation path 76 Hydrogen Circulation 100 Gas composition ratio control device 110 Storage section 120 Operation section 130 Control section 200 Kiln 500 Solid Carbon Deposition System
Claims
1. A solid carbon deposition system for depositing solid carbon from a feed gas containing carbon dioxide and hydrogen, comprising: a first reactor for contacting the raw material gas with a catalyst for activating a methanation reaction to produce methane and water from the raw material gas; a second reactor for converting the produced methane into carbon monoxide by heating the produced methane in contact with a catalyst that activates a dry reforming reaction; a third reactor in which the converted carbon monoxide is contacted with a catalyst that activates a solid carbon deposition reaction to deposit solid carbon from the converted carbon monoxide; an off-gas circulation path for circulating the off-gas discharged from the third reactor to the first reactor; a control unit for controlling a flow rate of each gas flowing through the solid carbon deposition system; The control unit is configured to adjust the H 2 A solid carbon deposition system comprising: a gas flow rate control section for controlling the flow rate of each gas, including the gas flow rate of the off-gas circulation passage, so that the / C molar ratio falls within a specified range.
2. A hydrogen separation flow path is further provided to separate hydrogen from the gas discharged from the second reactor, The control unit is configured to adjust the H 2 2. The solid carbon deposition system according to claim 1, wherein the flow rates of each gas, including the gas flow rate in the hydrogen separation channel, are controlled so that the H2O / CO molar ratio falls within a specified range.
3. 3. The solid carbon deposition system according to claim 2, wherein the control unit controls each gas flow rate, including the gas flow rate in the hydrogen separation channel, so that a carbon monoxide concentration in the mixed gas supplied to the third reactor is within a specified range.
4. A methane separation passage for separating methane from the gas discharged from the first reactor is further provided. The control unit is configured to detect CO in the gas supplied to the second reactor. 2 / CH 4 4. The solid carbon deposition system according to claim 2, wherein the flow rates of each gas, including the gas flow rate in the methane separation channel, are controlled so that the molar ratio falls within a specified range.
5. A carbon dioxide supply flow path is further provided for supplying carbon dioxide to the second reactor, The control unit is configured to detect CO in the gas supplied to the second reactor. 2 / CH 4 4. The solid carbon deposition system according to claim 2, wherein the flow rates of each gas, including the gas flow rate of the carbon dioxide supply passage, are controlled so that the molar ratio falls within a specified range.
6. A first step of contacting a raw material gas containing carbon dioxide and hydrogen with a catalyst that activates a methanation reaction to produce methane and water from the raw material gas; a second step of converting the generated methane into carbon monoxide by heating the generated methane-containing gas in contact with a catalyst that activates a dry reforming reaction; a third step of contacting the converted carbon monoxide-containing gas with a catalyst that activates a solid carbon deposition reaction to deposit solid carbon from the converted carbon monoxide; and circulating the gas produced by the third step for reuse in the first step. The source gas H 2 A method for depositing solid carbon, characterized in that the / C molar ratio is 2.5 or more.
7. The method further comprises the step of separating hydrogen from the gas produced in the second step; As a result of adjusting the amount of hydrogen separated, the converted carbon monoxide-containing gas is 2 7. The method for depositing solid carbon according to claim 6, wherein the / CO molar ratio is 1.0 or more and 2.0 or less, and the carbon monoxide concentration is 30 vol % or more.
8. The methane-containing gas produced is 2 / CH 4 8. The method for depositing solid carbon according to claim 6 or 7, wherein the molar ratio is 1.0 or more.
Citation Information
Patent Citations
Continuous carbon removing system
JP1996133200A
Device for manufacturing carbon
JP2003048708A
Method for immobilizing carbon dioxide and its system
JP2005060137A
Carbon dioxide fixation system
JP2015196619A
Method for methanation of carbon dioxide in combustion exhaust gas and methane production facility
JP2019172595A
Cited By
Soil catalyst and method for producing solid carbon
JP2026160037A