Solid carbon deposition method and solid carbon deposition system
The three-step catalytic reaction method with cementite catalysts and optimized cementite supply improves solid carbon recovery rates and simplifies reactor design for carbon dioxide fixation.
Patent Information
- Application Number
- JP2023071783
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
AI Technical Summary
Existing methods for carbon dioxide fixation and solid carbon precipitation lack sufficient study on reactor configuration, catalyst type, and catalyst supply methods, leading to suboptimal recovery rates and complex reactor configurations.
A three-step catalytic reaction method involving a methanation reaction, dry reforming reaction, and Boudoir reaction, using cementite as the catalyst for solid carbon precipitation, with continuous or intermittent supply and discharge of cementite to improve recovery rates and simplify reactor configuration.
Enhances the recovery rate of solid carbon from raw material gas and simplifies the reactor configuration by optimizing catalyst use and supply methods, achieving higher precipitation rates and reducing complexity.
Smart Images

Figure 2024157422000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and system for solid carbon deposition. [Background technology]
[0002] At present, there is an urgent need worldwide to reduce and fix carbon dioxide, which is a greenhouse gas that has a negative impact on the environment. 2 Emission reduction technology, CO 2 Separation and capture technology, CO 2 Useful resource conversion technology, CO 2 Various technologies, such as immobilization technology, are being researched and developed with the aim of practical application.
[0003] As a method for effectively utilizing carbon dioxide, for example, it is known that methane can be synthesized by a methanation reaction when a mixed gas of carbon dioxide and hydrogen is circulated in the presence of a catalyst heated to 250 to 500° C. (see Patent Document 1). In addition, a technology is also known in which solid carbon is precipitated by high-temperature pyrolysis of methane (see Patent Documents 2 to 5).
[0004] Patent Document 2 discloses a continuous carbon removal system in which a first reactor that causes a methanation reaction without using a catalyst and a second reactor that decomposes methane under temperature conditions of 1200°C or higher are connected in series.
[0005] Patent Document 3 discloses a method for fixation of carbon dioxide, which includes a first reaction step of reacting carbon dioxide and hydrogen in the presence of a catalyst to produce a mixed gas containing methane and water, and a second reaction step of producing at least one carbon product selected from the group consisting of carbon, graphite, carbon nanotubes, and diamond, using the methane gas obtained in the first reaction step as a raw material.
[0006] Patent Document 4 discloses a carbon dioxide fixation system including a methanation reactor that brings a raw material gas containing carbon dioxide and hydrogen into contact with a catalyst that activates a methanation reaction to produce methane and hydrogen from the raw material gas, and a methane pyrolysis reactor that heats the methane produced in the methanation reactor to decompose the methane into solid carbon and hydrogen.
[0007] In Patent Document 5, a mixed gas of carbon dioxide and methane in a ratio of 7:3 is treated with a catalyst of 30 wt% Ni / SiO 2 The mixture is then passed through a pre-reactor filled with 50wt%Fe / SiO2, which is heated in a heating furnace for a certain period of time at a reaction temperature of 550°C to convert it into a mixed gas of carbon dioxide, methane, hydrogen, and carbon monoxide. 2 The technology involves flowing carbon dioxide into a reactor filled with carbon dioxide and causing a catalytic reduction reaction with hydrogen at a low temperature of 400°C in a heating furnace to precipitate carbon. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2019-172595 A [Patent Document 2] Japanese Patent Application Publication No. 8-133200 [Patent Document 3] JP 2005-60137 A [Patent Document 4] JP 2015-196619 A [Patent Document 5] JP 2003-48708 A Summary of the Invention [Problem to be solved by the invention]
[0009] However, in the above Patent Documents 2 to 4, the configuration of the reactor, the type of catalyst appropriate for the reactor configuration, and the method of supplying the catalyst are not fully considered, and there is still room for improvement.
[0010] The present invention has been made in view of the above circumstances, and 2 The present invention aims to provide a method and system for precipitating solid carbon, which improves the recovery rate of solid carbon precipitated from a feed gas in a fixation system and enables a simpler reactor configuration. [Means for solving the problem]
[0011] (1) In order to achieve the above object, the method for precipitating solid carbon of the present invention includes a first step of contacting a raw material gas containing carbon dioxide and hydrogen with a catalyst that activates a methanation reaction, generating methane and water from the raw material gas, and then heating the generated methane in a state of contact with a catalyst that activates a reforming reaction, thereby converting the methane into carbon monoxide; and a second step of contacting the converted carbon monoxide with a catalyst that activates a solid carbon deposition reaction, thereby precipitating solid carbon from the carbon monoxide, wherein the catalyst that activates the solid carbon deposition reaction is cementite, and is placed on the catalyst before the gas converted in the first step is introduced into the second step.
[0012] (2) Moreover, in the solid carbon precipitation method of the present invention, the second step is characterized in that, instead of placing a catalyst for activating the solid carbon precipitation reaction in advance before the gas converted in the first step is introduced into the second step, new cementite on which solid carbon is not precipitated is continuously or intermittently supplied and the cementite on which solid carbon is precipitated is continuously or intermittently discharged.
[0013] (3) In the solid carbon deposition method of the present invention, the catalyst for activating the solid carbon deposition reaction is an iron-based catalyst at least a part of which is converted into cementite.
[0014] (4) Furthermore, the solid carbon deposition system of the present invention is characterized in that it includes a first reactor in which a raw material gas containing carbon dioxide and hydrogen is brought into contact with a catalyst that activates a methanation reaction, methane and water are generated from the raw material gas, and then the generated methane is heated in a state of being in contact with a catalyst that activates a reforming reaction, thereby carrying out a series of reactions to convert the methane into carbon monoxide; a second reactor in which the converted carbon monoxide is brought into contact with cementite to precipitate solid carbon from the carbon monoxide; and a mechanism for continuously or intermittently supplying new cementite on which solid carbon is not precipitated to the second reactor and continuously or intermittently discharging the cementite on which solid carbon has precipitated. Effect of the Invention
[0015] According to the present invention, CO 2 In the immobilization of carbon, the recovery rate of solid carbon precipitated from the feed gas can be improved and the reactor configuration can be simplified. [Brief description of the drawings]
[0016] [Figure 1] This is a conceptual diagram showing a three-stage catalytic reaction method in which the first, second and third reactions are carried out in separate reactors. [Diagram 2] FIG. 1 is a conceptual diagram showing the configuration of a reactor in a method in which the reactor configuration of a three-stage catalytic reaction method is simplified. [Diagram 3] 1 is a schematic diagram showing an example of the configuration of a solid carbon deposition device according to the present invention. [Figure 4] 1 is a schematic diagram showing an example of the configuration of a solid carbon deposition system according to the present invention. [Diagram 5] FIG. 2 is a schematic diagram showing an example of a spiral catalyst. [Figure 6] 1 is a table showing the conditions and experimental results of examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] [principle] A method for precipitating solid carbon from carbon dioxide is known that utilizes three-stage catalytic reactions consisting of a methanation reaction, a dry reforming reaction, and a Boudoir reaction (hereinafter referred to as the three-stage catalytic reaction method). The method for precipitating solid carbon using a methanation reaction, a dry reforming reaction, and a Boudoir reaction can be expressed by the following reaction formula. First reaction: CO 2 +4H 2 →CH 4 +2H 2 O ΔH=-165kJ / mol…(Formula 1) Second reaction: CO 2 +CH 4 →2CO+2H 2 ΔH=248kJ / mol…(Formula 2) Third reaction: 2CO → C + CO 2 ΔH=-172kJ / mol…(Formula 3)
[0018] As shown in formula 1, first, a methanation reaction is performed to convert carbon dioxide and hydrogen into methane. Next, as shown in formula 2, a dry reforming reaction is performed to convert carbon dioxide and methane into carbon monoxide. Then, as shown in formula 3, solid carbon is precipitated from the carbon monoxide by the Boudoir reaction, and the solid carbon is recovered. This allows solid carbon to be precipitated from carbon dioxide.
[0019] FIG. 1 is a conceptual diagram showing a three-stage catalytic reaction method in which the first to third reactions are carried out in separate reactors. Solid carbon deposition using the three-stage catalytic reaction method works, for example, as follows. The catalysts in each reactor are preheated with H 2 The reduction process is carried out in an air stream at 550°C for 1 hour. When the reduction process is completed, each reactor is changed to the set temperature. The time until the set temperature is reached is delayed by H 2 or N 2 When the temperature of each reactor is stabilized at the specified temperature, 2 / CO 2 In mole ratio, H 2 and CO 2 Over time, iron-based catalysts and H2 and reacts with CO to form cementite (Fe 3 C) is generated, and solid carbon begins to precipitate on the surface of the cementite. 2 and C.H. 4 and reacted with H 2 and CO. The CO is then heated to 400-900°C and passed through an iron-based catalyst (cementite: Fe 3 C) by contact with CO 2 It is possible to precipitate solid carbon at a precipitation rate of 24 to 30% relative to the carbon supplied as the starting material.
[0020] In the three-stage catalytic reaction method, the dry reforming reactor for the second reaction is controlled by the temperature in the center, which is the hottest. In other words, the temperatures at both ends are low. Since the methanation temperature is controlled to be lower than the dry reforming temperature, as shown in Figure 2, if a methanation catalyst is placed upstream (gas inlet) of the dry reforming reactor, the methanation reaction and the reforming reaction can be carried out in one reactor, and the methanation reactor can be omitted.
[0021] Figure 2 is a conceptual diagram showing the reactor configuration in a method that simplifies the reactor configuration of the three-stage catalytic reaction method. The difference from the three-stage catalytic reaction method in Figure 1 is that water vapor is brought into the reforming reaction process. In one example, the CO concentration of the outlet gas after the reforming reaction process is as high as 30 vol%, but the CO 2 The concentration is also high at 25 vol%, and this high CO 2 The concentration of cementite (Fe 3 It is presumed that the effect of this is to delay the formation of C) or to oxidize and decompose the formed cementite. As a result, it was discovered that the solid carbon deposition method and system thus configured have a problem in that the solid carbon deposition rate is not improved.
[0022] In response to this problem, the inventors discovered that if a catalyst that has been cementitized in advance is placed in a solid carbon precipitation reactor, solid carbon precipitates simultaneously with the start of CO flow, thereby improving the precipitation rate, and thus completed the present invention.
[0023] That is, a method for precipitating solid carbon according to one embodiment of the present invention includes a first step of contacting a feed gas containing carbon dioxide and hydrogen with a catalyst that activates a methanation reaction to generate methane and water from the feed gas, and then heating the generated methane in a state of contact with a catalyst that activates a reforming reaction to convert the methane into carbon monoxide, and a second step of contacting the converted carbon monoxide with a catalyst that activates a solid carbon deposition reaction to precipitate solid carbon from the carbon monoxide, wherein the catalyst that activates the solid carbon deposition reaction is cementite and is placed on the catalyst in advance before the mixed gas converted in the first step is introduced into the second step.
[0024] In addition, the gas discharged from the simultaneous treatment reactor (first reactor) in which the methanation reactor and the reforming reactor are connected in series is, for example, CO 2 Even if a catalyst containing 20 vol% or more of carbon dioxide and cementitized in advance is placed in a solid carbon deposition reactor (second reactor), the solid carbon that has been deposited will turn into CO over time. 2 There is a risk that the cementite will be oxidized by oxygen from the catalyst. Furthermore, if the cementite is oxidized and decomposed, it becomes difficult to continuously precipitate solid carbon. Therefore, the present inventors solved this problem by providing a means for supplying cementite to one end of the solid carbon precipitation reactor and a means for discharging the catalyst on which solid carbon has been precipitated to the other end.
[0025] That is, a method for precipitating solid carbon according to another embodiment of the present invention includes a first step of contacting a raw material gas containing carbon dioxide and hydrogen with a catalyst that activates a methanation reaction, generating methane and water from the raw material gas, and then heating the generated methane in a state of contact with a catalyst that activates a reforming reaction to convert the methane into carbon monoxide, and a second step of contacting the converted carbon monoxide with a catalyst that activates a solid carbon precipitation reaction to precipitate solid carbon from the carbon monoxide, wherein the catalyst that activates the solid carbon precipitation reaction is cementite, and the second step is characterized in that new cementite on which solid carbon is not precipitated is continuously or intermittently supplied and the cementite on which solid carbon has precipitated is continuously or intermittently discharged.
[0026] In addition, since the reactions occurring in the simultaneous treatment reactor and the solid carbon deposition reactor of the present invention do not remove the water vapor generated in the methanation reaction, it is presumed that reactions other than the above-mentioned first and second reactions also occur.
[0027] Next, a description will be given of the change in the raw material gas consisting of carbon dioxide and hydrogen when the raw material gas is reacted continuously from the first step to the second step.
[0028] In the methanation reaction, methane and water vapor are usually produced from 1 mol of carbon dioxide and 4 mol of hydrogen via a catalyst. 2 / CO 2 Even if the molar ratio of carbon dioxide and hydrogen is the theoretical value of 4, not all of the carbon dioxide and hydrogen will react to produce 1 mole of methane. In other words, the feed gas containing carbon dioxide and hydrogen will be a mixed gas containing methane synthesized in the methanation reaction, unreacted carbon dioxide, hydrogen, and water vapor. Note that the feed gas after the methanation reaction contains water vapor, but it is sent directly to the first reactor where the reforming reaction takes place.
[0029] In the reforming reaction, for example, 2 mol of carbon monoxide and 2 mol of hydrogen are produced from 1 mol of methane and 1 mol of carbon dioxide synthesized in the methanation reaction via a catalyst. In addition to this reaction, for example, 1 mol of carbon monoxide and 3 mol of hydrogen are produced from 1 mol of methane and 1 mol of water (steam) via a catalyst. Note that various reaction systems compete in the reforming reaction. Therefore, the raw gas after the reforming reaction becomes a mixed gas containing hydrogen, methane, carbon dioxide, carbon monoxide, and steam.
[0030] In the solid carbon deposition reaction, for example, 1 mol of solid carbon and 1 mol of carbon dioxide are produced from 2 mol of carbon monoxide via a catalyst. In addition to this reaction, for example, 1 mol of methane and 1 mol of water (steam) are produced from 1 mol of carbon monoxide and 3 mol of hydrogen via a catalyst. In addition, for example, 1 mol of solid carbon and 1 mol of water (steam) are produced from 1 mol of carbon monoxide and 1 mol of hydrogen via a catalyst. Since solid carbon deposits on the surface of the catalyst, the deposited solid carbon is collected together with the catalyst. Note that various reaction systems compete in the solid carbon deposition reaction. Therefore, the raw material gas that has completed the solid carbon deposition reaction becomes a mixed gas containing hydrogen, methane, carbon dioxide, carbon monoxide, and steam.
[0031] [Configuration of solid carbon deposition device] An embodiment of the present invention will be described below. Fig. 3 shows a solid carbon deposition apparatus according to the present invention. The solid carbon deposition apparatus 1 is an apparatus for depositing solid carbon from process exhaust gas containing carbon dioxide. The process exhaust gas refers to exhaust gas containing carbon dioxide emitted from a cement clinker burning process, a quicklime manufacturing process, a thermal power plant, a waste incineration treatment facility, a ceramics burning facility, an ironworks, and a chemical plant.
[0032] 3, the solid carbon deposition apparatus 1 has two reactors in which different reactions occur, and the two reactors are connected in series. When the reactor to which the raw material gas is supplied is designated as the first reactor 10, the reaction proceeds in the order of the first reactor 10 and the second reactor 20, and solid carbon is deposited in the second reactor 20.
[0033] In addition to the two reactors, the solid carbon deposition apparatus 1 includes a hydrogen supplying equipment 3, a hydrogen flowmeter 4, a gas mixer 5, a gas separator 7, water vapor removing equipment 41-42 provided at the outlets of the reactors, and a flowmeter 50. The solid carbon deposition apparatus 1 also preferably includes equipment 61 for removing sulfur oxides that cause catalyst deterioration, a carbon dioxide concentration equipment 62, and equipment 70 for recycling the mixed gas discharged from the second reactor 20. If nitrogen or oxygen is contained in the process exhaust gas, the absolute amount of the raw material gas will be large, so the apparatus may further include equipment for removing nitrogen or oxygen from the process exhaust gas in front of the first reactor.
[0034] The gas mixer 5 mixes a plurality of gases to prepare a raw material gas to be supplied to the first reactor 10. The gas mixer 5 is preferably equipped with a flow meter that measures the flow rate of each gas to be supplied to the first reactor 10.
[0035] The gas mixer 5 mixes hydrogen supplied from the hydrogen supply equipment 3 with the process exhaust gas containing carbon dioxide to generate a raw material gas to be supplied to the first reactor 10. At this time, the raw material gas is H 2 / (CO 2 +CO+CH 4 The molar ratio of H is 1.5 or more, more preferably 2.0 or more, and even more preferably 2.5 or more. 2 / (CO 2 +CO+CH 4 Since the molar ratio of H is 1.5 or more, solid carbon can be stably recovered from the raw material gas. 2 / (CO 2 +CO+CH 4The upper limit of the molar ratio of H is preferably 19 or less, more preferably 13 or less, and even more preferably 11.5 or less. If the molar ratio exceeds 19, H 2 The amount of waste gas increases, and the equipment becomes unnecessarily large. In addition, it is preferable that the process exhaust gas is supplied to the gas mixer 5 after sulfur oxides are removed by the sulfur oxide removal equipment 61 and the concentration of carbon dioxide is increased by the carbon dioxide concentration equipment 62. In addition, when the process exhaust gas is provided with the equipment 70 for circulating and utilizing the mixed gas discharged from the second reactor 20, the mixed gas discharged from the second reactor 20 may be mixed with the raw material gas.
[0036] In the first reactor 10, different reactions are carried out in the first reactor front section 10-1 and the first reactor rear section 10-2. As shown in FIG. 2, the first reactor front section 10-1 and the first reactor rear section 10-2 correspond to a low-temperature section into which the raw material gas flows and a high-temperature section located on the gas outlet side relative to the first reactor front section 10-1, respectively, inside the same gas flow reaction tube. In the first reactor front section 10-1, the raw material gas supplied from the gas mixer 5 is contacted with a catalyst that activates the methanation reaction, and methane and water are produced from the raw material gas as shown in formula 1. The raw material gas is preferably supplied to the first reactor 10 so that the space velocity is 2000 to 20000 / h. In the first reactor front section 10-1, a catalyst that activates the methanation reaction is placed at a site where the temperature is controlled to 400 to 600° C. on the side where the raw material gas flows in inside the same gas flow reaction tube.
[0037] The catalyst for activating the methanation reaction may be one capable of producing methane from carbon dioxide and hydrogen, such as Ni, Ru, Pt, or Rh. The support may be CeO 2 , ZrO 2 , Y 2 O 3 and Al 2 O 3Various oxides and aluminosilicates such as those mentioned above can be used. The catalyst may have any shape as long as it can achieve a predetermined space velocity, but a spiral shape is preferred because it requires a small catalyst volume. When the catalyst is spiral-shaped, it is produced by forming a metal plate member such as aluminum into a spiral shape and applying a paste-like catalyst to it.
[0038] The first reactor rear section 10-2 converts methane into carbon monoxide by heating the mixed gas containing methane that has passed through the first reactor front section 10-1 and partially completed the reaction in contact with a catalyst that promotes the reforming reaction. In the first reactor rear section 10-2, a catalyst that activates the reforming reaction is placed at a position where the temperature is controlled to 700 to 900°C.
[0039] It is preferable that the first reactor front section 10-1 and the first reactor rear section 10-2 have one heating furnace and are an integrated first reactor 10 as a whole. In addition, when the first reactor front section 10-1 and the first reactor rear section 10-2 are one heating furnace, it is more preferable that the heating temperature of each can be controlled independently. The first reactor front section 10-1 and the first reactor rear section 10-2 may be separate reactors each having a separate heating furnace, and the outlet of the first reactor front section 10-1 and the supply port of the first reactor rear section 10-2 may be connected in series to constitute the first reactor 10 as a whole. In that case, it is preferable to configure so that the gas temperature does not decrease at the connecting section.
[0040] The catalyst for activating the reforming reaction may be one capable of producing carbon monoxide and hydrogen from carbon dioxide and methane, such as Ni or Rh. The support may be CeO 2 , ZrO 2 , Y 2 O 3 and Al 2 O 3 Various oxides and aluminosilicates such as γ-Al can be used. 2 O 3The catalyst may have any shape as long as it can achieve a predetermined space velocity, but a spiral shape is preferred because it requires a small catalyst volume. When the catalyst is spiral-shaped, it is produced by forming a metal plate member such as stainless steel into a spiral shape and applying a paste-like catalyst thereto.
[0041] The second reactor 20 brings the mixed gas containing carbon monoxide supplied from the first reactor 10 into contact with a catalyst that activates a solid carbon deposition reaction, and precipitates solid carbon from the carbon monoxide. The mixed gas supplied to the second reactor 20 is preferably supplied so that the space velocity is a maximum of 2000 / h. The second reactor 20 includes a gas flow reaction tube filled with a catalyst that activates a solid carbon deposition reaction, and a heating furnace that can heat the gas flow reaction tube to 400 to 900°C. The catalyst that activates the solid carbon deposition reaction is cementite. The catalyst that activates the solid carbon deposition reaction is preferably placed in advance before supplying the gas containing carbon monoxide to the second reactor 20.
[0042] The second reactor 20 is preferably equipped with a mechanism capable of continuously or intermittently supplying new cementite not containing solid carbon precipitated therein into the reactor, and continuously or intermittently discharging cementite containing solid carbon precipitated therein. Such a mechanism can be, for example, an inclined rotary mechanism, a pusher mechanism, a screw feeder, or the like. The cementite supplying means and discharging means each have a means, for example, a double damper, so that outside air (oxygen) does not flow into the second reactor 20. The second reactor 20 is preferably, for example, a fluidized bed, a moving bed, or a rotary kiln.
[0043] The catalyst for activating the solid carbon deposition reaction is preferably an iron-based catalyst in which at least a part of the catalyst is cementitized. The iron-based catalyst is preferably metallic iron or iron oxide (magnetite (Fe 3 O 4 ), Hematite (Fe 2 O 3), wustite (FeO, etc.). In particular, it is preferable that at least a part of magnetite among iron oxides is cementitized. The catalyst may have any shape as long as a predetermined space velocity can be achieved, but a spiral shape is preferable because it requires a small catalyst volume. When the catalyst is spiral-shaped, it is produced by forming a metal plate member such as stainless steel into a spiral shape and applying a paste-like catalyst to it. It may be cementitized after applying the iron-based catalyst.
[0044] 3, water vapor removal equipment 41, 42 is provided at the outlet of each reactor. The water vapor removal equipment 41, 42 cools the gas discharged from the outlet of the target reactor to condense the water vapor, and discharges it as industrial wastewater.
[0045] In the methanation reaction in the first reactor front section 10-1, steam is generated, but is supplied to the first reactor rear section 10-2 as it is. This simplifies the configuration of the first reactor. In addition, a part of the steam generated in the reaction in the first reactor front section 10-1 passes through the first reactor rear section 10-2 without reacting. Furthermore, there is a risk that steam will be generated when various reaction systems compete in the first reactor 10 or when the type of catalyst or temperature conditions are changed. Therefore, it is preferable to provide a first steam removal device 41 at the outlet of the first reactor 10. In addition, although the solid carbon deposition reaction is dominant in the second reactor 20, it is considered that a reaction that generates steam will occur in some cases. Therefore, it is preferable to provide a second steam removal device 42 at the outlet of the second reactor 20.
[0046] As described above, the solid carbon deposition apparatus 1 preferably has the equipment 70 capable of recycling the mixed gas discharged from the second reactor 20. As the equipment 70 capable of recycling the mixed gas discharged from the second reactor 20, a equipment that supplies the mixed gas discharged from the second reactor 20 to the first reactor 10 is considered. Since the mixed gas discharged from the second reactor 20 contains carbon dioxide, the mixed gas is not discharged to the outside, but is used as a raw material for the raw material gas, thereby preventing the emission of carbon dioxide. It is preferable that the equipment 70 capable of recycling the mixed gas discharged from the second reactor 20 is not only the second reactor 20, but also a part of the mixed gas discharged from the first reactor 10 is separated by the gas separator 7 and circulated to the first reactor 10 again. At this time, it is preferable that the discharged mixed gas is not directly supplied to each reactor, but is supplied after controlling the flow rate of each gas supplied to the first reactor 10 and uniformly mixed in the gas mixer 5.
[0047] In order to adjust the composition ratio of the mixed gas, it is preferable to install a sensor that measures the composition ratio of the gas supplied to the gas mixer 5, a valve capable of adjusting the flow rate of each mixed gas, and the gas mixer 5. The sensor is sufficient as long as it can grasp the component ratio of at least hydrogen, methane, carbon dioxide, and carbon monoxide, and the valve capable of adjusting the flow rate of each mixed gas is preferably installed not only at the outlet where the process exhaust gas is discharged and at the hydrogen supply facility 3, but also when the mixed gas discharged from the first reactor 10 and the second reactor 20 is recycled to the gas mixer.
[0048] In addition, in the solid carbon deposition apparatus 1, the reactions in the first reactor front section 10-1 and the second reactor 20 are exothermic reactions, whereas the reaction in the first reactor rear section 10-2 is an endothermic reaction. Therefore, it is preferable to recover the sensible heat of the mixed gas discharged from the first reactor front section 10-1 and the second reactor 20 by a heat exchanger and use it as an energy source for the first reactor rear section 10-2.
[0049] [Solid carbon deposition system] Next, the solid carbon deposition system will be described. FIG. 4 is a schematic diagram showing the configuration of the solid carbon deposition system. The solid carbon deposition system 500 preferably controls the amount of catalyst (cementite) that activates the solid carbon deposition reaction, which is supplied to the second reactor 20 in the solid carbon deposition apparatus 1 or discharged from the second reactor 20, within a range designated by the user. The supply amount or discharge amount is preferably controlled based on the composition ratio of the mixed gas and the process exhaust gas discharged from each reactor. Moreover, the solid carbon deposition system 500 preferably controls the composition ratio of the mixed gas supplied to each reactor in the solid carbon deposition apparatus 1 within a range designated by the user.
[0050] The solid carbon deposition system 500 includes a solid carbon deposition apparatus 1 and a control device 100. The control device includes a memory unit 110, an operation unit 120, and a control unit 130. The memory unit 110 records values measured in the solid carbon deposition apparatus 1. The values measured in the solid carbon deposition apparatus 1 include, for example, the composition ratio of the gas supplied to the gas mixer 5, such as the composition ratio of the mixed gas and the process exhaust gas discharged from each reactor.
[0051] The operation unit 120 is a device that allows a user to input any desired information, and is, for example, a keyboard, a mouse, or a touch panel. The user can input any range for the amount of catalyst that activates the solid carbon deposition reaction supplied to the second reactor 20 or discharged from the second reactor 20 via the operation unit 120. The control unit 130 controls the amount of catalyst that activates the solid carbon deposition reaction so that the amount falls within the range specified by the user, based on the data recorded in the storage unit 110. Specifically, the control unit 130 controls mechanisms such as an inclined rotary mechanism, a pusher mechanism, and a screw feeder provided in the second reactor 20, so that the amount of catalyst that activates the solid carbon deposition reaction supplied to the second reactor 20 or discharged from the second reactor 20 falls within the range specified by the user.
[0052] Furthermore, the user can input any range for the composition ratio of the mixed gas supplied to each reactor via the operation unit 120. The control unit 130 controls the composition ratio of the mixed gas to be within the range specified by the user based on the data recorded in the storage unit 110. Specifically, the control unit 130 recognizes the gas flow rate from each facility and controls the valves of each gas supplied to the gas mixer 5, thereby controlling the composition ratio of the mixed gas in the gas mixer 5 to be within the range specified by the user.
[0053] In this embodiment, an example has been described in which both the amount of catalyst for activating the solid carbon deposition reaction, which is supplied to the second reactor 20 and discharged from the second reactor 20, can be controlled, but a configuration in which either the amount supplied or the amount discharged can be actively controlled, and as a result, the amount of the other can be controlled. In addition, in this embodiment, an example has been described in which the composition ratio of the mixed gas in all reactors can be controlled, but at least the H content in the raw material gas supplied to the first reactor 10 can be controlled. 2 / (CO 2 +CO+CH 4 It is sufficient that the molar ratio of the two components (a) and (b) can be controlled within a range designated by the user, and it is not necessary that the composition ratio of the mixed gas supplied to the second reactor 20 can be controlled.
[0054] [Solid carbon deposition method] Next, a method for precipitating solid carbon will be described. First, the raw material gas to be supplied to the first reactor 10 is adjusted. The raw material gas is a mixture of hydrogen supplied from the hydrogen supply equipment 3, process exhaust gas containing carbon dioxide, and H separated by the gas separator 7. 2 and / or CO 2 and the gas discharged from the second reactor 20 are mixed, and H 2 / (CO 2 +CO+CH 4 ) is adjusted to be 1.5 or more.
[0055] Next, the raw material gas is supplied to the first reactor 10, and the raw material gas is passed through the gas flow reaction tube in the front part 10-1 of the first reactor. The gas flow reaction tube is filled with a catalyst heated to 400 to 600°C by a heating furnace, and the raw material gas comes into contact with the catalyst that activates the methanation reaction, and methane is produced from the raw material gas. 2 / CO 2 A raw material gas having a molar ratio of 1.5 is supplied to the first reactor and methanated at a reaction temperature of 500°C. After the first reaction is completed, the mixed gas has a hydrogen concentration of 20 volume %, a methane concentration of 9 volume %, a carbon dioxide concentration of 32 volume %, a carbon monoxide concentration of 4 volume %, and a water vapor concentration of 35 volume %.
[0056] Next, the mixed gas discharged from the first reactor front part 10-1 is supplied to the first reactor rear part 10-2, and the mixed gas is passed through the gas flow reaction tube of the first reactor rear part 10-2. The gas flow reaction tube is filled with a catalyst heated to about 800°C by a heating furnace, and the mixed gas comes into contact with the catalyst that activates the reforming reaction, and methane is converted into carbon monoxide. A series of steps in which a raw material gas containing carbon dioxide and hydrogen is brought into contact with a catalyst that activates a methanation reaction, methane and water are generated from the raw material gas, and then the generated methane is heated in a state in which it is in contact with the catalyst that activates the reforming reaction, thereby converting methane into carbon monoxide, is called the first step. The mixed gas from which water vapor has been removed after the first step has, for example, a hydrogen concentration of 45 volume %, a carbon dioxide concentration of 23 volume %, and a carbon monoxide concentration of 32 volume %.
[0057] Next, the mixed gas discharged from the rear part 10-2 of the first reactor is supplied to the second reactor 20, and the mixed gas is passed through the gas flow reaction tube of the second reactor 20. The inside of the gas flow reaction tube is filled with a catalyst heated to about 450°C by a heating furnace, and the mixed gas comes into contact with the catalyst that activates the solid carbon deposition reaction, carbon monoxide becomes solid carbon, and solid carbon is deposited on the surface of the catalyst. Then, the solid carbon can be recovered by recovering the catalyst on which the solid carbon is deposited. The process of contacting the carbon monoxide converted in the first process with the catalyst that activates the solid carbon deposition reaction and precipitating solid carbon from the carbon monoxide is called the second process. The solid carbon deposited on the catalyst surface fills the free space of the second reactor 20 at a rate of, for example, 0.64 g / hr. In addition, the mixed gas from which water vapor has been removed after the second process has a hydrogen concentration of 44 volume %, a methane concentration of 3 volume %, a carbon dioxide concentration of 33 volume %, and a carbon monoxide concentration of 20 volume %.
[0058] From the above, in the method for precipitating solid carbon in the present invention, the reactions can be continuously carried out from the supply of the raw material gas to the first reactor until the solid carbon is precipitated in the second reactor. In addition, the methanation reaction and the reforming reaction can be carried out in one reactor. This simplifies the configuration of the reactor and reduces costs compared to when each reaction is independent.
[0059] [Example] Example 1 The heating furnace constituting the methanation reactor (front of the first reactor) was a one-zone electric furnace (ceramic electric tubular furnace manufactured by Asahi Rika Seisakusho, effective length 300 mm) capable of temperature control. In addition, a quartz tube with an inner diameter of 8 mm and a length of 600 mm was used as the atmospheric pressure flow reaction tube at the front of the first reactor. At the position of the thermocouple for temperature control of the heating furnace inside the atmospheric pressure flow reaction tube, 10 wt% Ni / CeO was applied to the surface of the spiral structure shown in Figure 5 as a catalyst for activating the methanation reaction. 2 Two catalysts coated with the catalyst were installed.
[0060] The catalyst that activates the methanation reaction is CeO2 (Kanto Chemical Co., Ltd.) was used as a carrier, and Ni(NO 3 ) 2 6H 2 After loading, the catalyst was fired at 500°C for 2 hours in an air atmosphere to separate the nitric acid component. After cooling the fired product, distilled water was added and it was ground in a mortar to obtain Ni / CeO 2 A paste was made.
[0061] Ni / CeO 2 Separately from the paste, a spirally twisted aluminum plate (JIS A1100 H14, width 7 mm × length 50 mm, thickness 1.5 mm) was surface-treated with a 0.8 mol NaOH aqueous solution and a 3.0 mol hydrochloric acid solution as shown in Figure 5. Then, a sufficient amount of Ni / CeO 2 The process of drying with cold air and immersion was repeated until the catalyst was supported.
[0062] The reforming reactor (rear of the first reactor) was prepared in the same manner as the front of the first reactor, except that a catalyst for activating the reforming reaction was used instead of the catalyst for activating the methanation reaction. The catalyst for activating the reforming reaction was a commercially available γ-Al 2 O 3 (C20 manufactured by Nippon Light Metal Co., Ltd.) was used as a carrier, and Ni(NO 3 ) 2 6H 2 As shown in Figure 5, a stainless steel plate (SUS304, width 7 mm × length 50 mm, thickness 0.5 mm) twisted into a spiral shape is coated with Ni / γ-Al 2 O 3 The catalyst was prepared in the same manner as the catalyst for activating the methanation reaction, except that a paste was applied.
[0063] The solid carbon deposition reactor (second reactor) was prepared in the same manner as the first reactor, except that a quartz tube with an inner diameter of 21 mm and a length of 600 mm was used as the atmospheric pressure flow-type reaction tube, and eight catalyst precursors for activating the solid carbon deposition reaction were placed inside the atmospheric pressure flow-type reaction tube (two bundles of four catalysts were placed in series) instead of a catalyst for activating the methanation reaction. The precursor for the catalyst for activating the solid carbon deposition reaction was magnetite (Fe 3 O 4 Reagents: Fujifilm Wako Pure Chemicals, 98%). Distilled water was added to magnetite to make a paste. It was prepared in the same way as the catalyst for activating the methanation reaction, except that the magnetite paste was applied to a stainless steel plate (SUS304, width 7 mm × length 50 mm, thickness 0.5 mm) twisted into a spiral shape as shown in Figure 5.
[0064] After each reactor was prepared, the catalyst and catalyst precursor were reduced by holding the temperature at 500°C for 1 hour while flowing hydrogen at 200 ml / min. Next, the following process was carried out to convert the magnetite in the solid carbon deposition reactor into cementite. First, a dry reforming reactor was prepared separately from the reforming reactor (rear of the first reactor). Next, the methanation reactor (front of the first reactor), the dry reforming reactor, and the solid carbon deposition reactor (second reactor) were connected in series, each via a moisture trap. Next, H of the raw material gas was 2 / CO 2 The molar ratio was set to 2.5, and the methanation reaction was carried out at a set temperature of 340°C. The reaction gas was introduced into a dry reforming reactor via a moisture trap, and the dry reforming reaction was carried out at a set temperature of 800°C. The reaction gas was then introduced into a second reactor set at 450°C, where cementitization was carried out for 40 minutes. In the case of the three-stage catalytic reaction method, this treatment was carried out by removing H 2 / CO 2This is because it has been found that when the ratio is 2.5, the formation of cementite is completed in about 40 minutes. By this treatment, magnetite, which is a precursor of the catalyst that activates the solid carbon deposition reaction, is reduced to metallic iron, and at least a part of it is further formed into cementite. Note that this treatment may be omitted, and cementite, which is a catalyst that activates the solid carbon deposition reaction, may be separately prepared and placed on the substrate.
[0065] After the cementitization was completed, the inside of the second reactor was filled with inert gas, the openings at both ends were closed with silicone plugs, and it was cooled. After cooling, the methanation reactor and the reforming reactor were connected without a moisture trap to form a simultaneous treatment reactor (first reactor). In addition, the entire reactor combination was made into a simultaneous treatment reactor (first reactor) and a solid carbon deposition reactor (second reactor), and the temperatures were raised to 800°C and 450°C, respectively, while passing an inert gas through them. After both reactors reached their respective predetermined temperatures, the raw material gas was supplied to the simultaneous treatment reactor (first reactor) via a mass flow controller and a gas mixer, using a standard hydrogen gas cylinder as the hydrogen supply equipment 3 instead of the inert gas, and a standard carbon dioxide gas cylinder instead of the process exhaust gas.
[0066] At this time, H in the source gas 2 / CO 2 The molar ratio of hydrogen to carbon dioxide was set to 1.5, and solid carbon was collected for 4 hours. Specifically, the flow rates of hydrogen and carbon dioxide were set to 150 ml / min and 100 ml / min, respectively, by mass flow controllers, and the total flow rate of the raw material gases was set to 250 ml / min and supplied to the first reactor.
[0067] At the outlet of each reactor, a water vapor removal device and a sampling hole were installed. Thirty minutes after the indicated temperature of each reactor reached the set temperature, samples were taken from the sampling hole using a syringe, and the hydrogen, nitrogen, oxygen, methane, carbon monoxide, and carbon dioxide were quantitatively analyzed using a gas chromatograph GC-2014 (Shimadzu Corporation).
[0068] A wet gas meter was installed at the outlet of the second reactor to measure the gas flow rate. The mixed gas discharged from the second reactor was not recycled but discharged to an outdoor abatement facility. After the second reactor was sufficiently cooled, the catalyst was removed from the atmospheric flow reaction tube, the weight of the precipitated solid carbon was measured, and the recovery rate of the solid carbon was calculated using the following formula 4. Solid carbon recovery rate (%) = (molar amount of precipitated solid carbon) / (molar amount of carbon supplied to the solid carbon precipitater) × 100 ... (Equation 4)
[0069] (Comparative Example) The same operations as in the example were carried out except that magnetite was used as the catalyst for activating the solid carbon deposition reaction and the cementitization treatment was not carried out.
[0070] (Experimental Results) The experimental results of the examples and comparative examples are shown in the table of FIG. 6. FIG. 6 is a table showing the conditions and experimental results of the examples and comparative examples. In the table of FIG. 6, H 2 / CO 2 The molar ratio of each of the reactants, the gas concentrations of hydrogen, methane, carbon dioxide and carbon monoxide in the mixed gas sampled from the sampling holes provided at the outlets of the reactors, and the solid carbon recovery rate are shown.
[0071] In the example where magnetite was converted to cementite and placed before the introduction of the raw material gas, the solid carbon recovery rate was high at 14.7%. In contrast, in the comparative example where the treatment of converting magnetite to cementite was not performed, the solid carbon recovery rate was very low at 6.5%. This is because the CO 2 It is presumed that the high concentration of niobium retards the formation of cementite, which acts as the nucleus for solid carbon precipitation, or causes the formed cementite to be oxidized and decomposed.
[0072] From the above results, in the solid carbon deposition method, device, and system having a simplified configuration of the three-stage catalytic reaction method of the present invention, a catalyst that activates the solid carbon deposition reaction is placed in advance as cementite, or new cementite on which solid carbon has not precipitated is continuously or intermittently supplied, and cementite on which solid carbon has precipitated is continuously or intermittently discharged, thereby making it possible to improve the solid carbon recovery rate. [Explanation of symbols]
[0073] 1. Solid carbon deposition device 3 Hydrogen supply equipment 4. Hydrogen flow meter 5 Gas Mixer 7 Gas separator 10 First Reactor 10-1 Front of the first reactor 10-2 Rear of the first reactor 20 Second Reactor 41 First Water Vapor Removal Facility 42 Second Water Vapor Removal Facility 50 flow meter 61 Equipment for removing sulfur oxides 62 Carbon Dioxide Concentration Equipment 70 Equipment for recycling mixed gases 100 Control device 110 Storage section 120 Operation section 130 Control section 500 Solid Carbon Deposition System
Claims
1. a first step of contacting a raw material gas containing carbon dioxide and hydrogen with a catalyst that activates a methanation reaction to generate methane and water from the raw material gas, and then heating the generated methane in a state of contact with a catalyst that activates a reforming reaction to convert the methane into carbon monoxide; a second step of contacting the converted carbon monoxide with a catalyst that activates a solid carbon deposition reaction to deposit solid carbon from the carbon monoxide; A method for precipitating solid carbon, characterized in that the catalyst for activating the solid carbon deposition reaction is cementite, and is placed on the catalyst before the gas converted in the first step is introduced into the second step.
2. 2. The method for precipitating solid carbon according to claim 1, characterized in that, in the second step, instead of placing a catalyst for activating the solid carbon precipitation reaction in advance before the gas converted in the first step is introduced into the second step, new cementite on which solid carbon has not precipitated is continuously or intermittently supplied and the cementite on which solid carbon has precipitated is continuously or intermittently discharged.
3. 2. The method for depositing solid carbon according to claim 1, wherein the catalyst for activating the solid carbon deposition reaction is an iron-based catalyst at least partly converted into cementite.
4. a first reactor in which a raw material gas containing carbon dioxide and hydrogen is contacted with a catalyst that activates a methanation reaction to generate methane and water from the raw material gas, and then the generated methane is heated in a state in which the methane is contacted with a catalyst that activates a reforming reaction, thereby carrying out a series of reactions to convert the methane into carbon monoxide; a second reactor in which the converted carbon monoxide is contacted with cementite to precipitate solid carbon from the carbon monoxide; a mechanism for continuously or intermittently supplying new cementite on which solid carbon has not precipitated to the second reactor and continuously or intermittently discharging the cementite on which solid carbon has precipitated.
Citation Information
Patent Citations
Continuous carbon removing system
JP1996133200A
Device for manufacturing carbon
JP2003048708A
Method for immobilizing carbon dioxide and its system
JP2005060137A
Carbon dioxide fixation system
JP2015196619A
Method for methanation of carbon dioxide in combustion exhaust gas and methane production facility
JP2019172595A
Cited By
Soil catalyst and method for producing solid carbon
JP2026160037A