Curable composition
A curable composition with reactive silicon groups and a non-organotin catalyst system, comprising a carboxylic acid, amine, metal, and ammonium halide, addresses the challenge of rapid curing in organic polymers, providing effective and environmentally friendly curing solutions.
Patent Information
- Application Number
- JP2023071838
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
AI Technical Summary
Conventional curable compositions containing organic polymers with reactive silicon groups face challenges in achieving rapid curing without using organotin-based curing catalysts, which are toxic and pose environmental concerns.
A curable composition comprising an organic polymer with reactive silicon groups and a curing catalyst system consisting of a carboxylic acid, an amine compound, a metal compound, and an ammonium halide, which facilitates rapid curing without using organotin compounds.
The composition exhibits excellent rapid curing properties while avoiding the use of toxic organotin catalysts, ensuring environmental safety and maintaining effective curing performance.
Smart Images

Figure 2024157454000001 
Figure 2024157454000002 
Figure 2024157454000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an organic polymer having a silicon group (hereinafter also referred to as a "reactive silicon group") that has a hydroxyl group or a hydrolyzable group bonded to a silicon atom and that can form a crosslink by forming a siloxane bond, and a curable composition containing the organic polymer. [Background technology]
[0002] Organic polymers having at least one reactive silicon group in the molecule can be crosslinked even at room temperature by the formation of siloxane bonds accompanied by hydrolysis of the silyl group due to moisture, etc. It is known that organic polymers having reactive silicon groups have the property of giving rubber-like cured products through such crosslinking reactions.
[0003] As organic polymers having these reactive silicon groups, organic polymers whose main chain structures are polyoxyalkylene, polyacrylic ester, or polyisobutylene are already being produced industrially and are widely used in applications such as sealing materials, adhesives, paints, and waterproofing materials (Patent Document 1), (Patent Document 2), (Patent Document 3), and (Patent Document 4).
[0004] When an organic polymer having a reactive silicon group is used as a curable composition such as a sealing material, adhesive, paint, or waterproofing material, the curable composition is required to have various properties such as curability, adhesiveness, workability, mechanical properties of the cured product, and waterproofness.
[0005] A curable composition containing an organic polymer having a reactive silicon group is usually cured using a silanol condensation catalyst such as an organotin compound having a carbon-tin bond, such as dibutyltin bis(acetylacetonate). The silanol condensation catalyst is also called a curing catalyst. In recent years, the toxicity of organotin compounds has been pointed out, and their use requires caution from the viewpoint of environmental safety.
[0006] For this reason, the use of tin carboxylates and other metal carboxylates, organic salts of carboxylic acids and amine compounds in combination, and metal complexes of titanium compounds and the like have been proposed as curing catalysts other than organotin compounds (Patent Document 3), (Patent Document 4), (Patent Document 5), and (Patent Document 6). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 52-73998 [Patent Document 2] Japanese Patent Application Publication No. 63-6041 [Patent Document 3] Japanese Patent Application Publication No. 55-9669 [Patent Document 4] JP 2003-206410 A [Patent Document 5] Japanese Patent Application Publication No. 5-117519 [Patent Document 6] International Publication No. 2005 / 108499 Summary of the Invention [Problem to be solved by the invention]
[0008] However, the above-mentioned conventional techniques leave room for improvement in terms of the rapid curing properties of the curable compositions.
[0009] Therefore, an object of the present invention is to provide a curable composition containing a reactive silicon group-containing organic polymer that exhibits good fast curing properties even when it contains a non-organotin curing catalyst. [Means for solving the problem]
[0010] Means for Solving the Problems The present inventors have conducted intensive research to find a solution to the above problems, and have discovered that a curable composition exhibiting rapid curing properties can be obtained by using an organic polymer having a reactive silicon group and a specific curing catalyst, thereby completing the present invention.
[0011] That is, the present invention provides: A curable composition comprising an organic polymer (A) and a curing catalyst (B), The organic polymer (A) is represented by the following formula (1): -SiR 1 3-a X a (1) (In formula (1), R 1 is a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, or R 0 It represents a triorganosiloxy group represented by 3SiO-, and has three R 0 are hydrocarbon groups having 1 to 20 carbon atoms, which may be the same or different, X represents a hydroxyl group or a hydrolyzable group; a is 1, 2, or 3; R 1 , X, when there are multiple of them, they may be the same or different.) and having a reactive silicon group represented by the formula: The curing catalyst (B) comprises a carboxylic acid (b1), an amine compound (b2), a metal compound (b3), and an ammonium halide compound (b4); two or more selected from the group consisting of the carboxylic acid (b1), the amine compound (b2), the metal compound (b3), and the ammonium halide (b4) may be reacted with each other; The amine compound (b2) is a compound that does not fall under the category of an aminosilane coupling agent, The metal compound (b3) is represented by the following formula (2): M(OR 2 ) d Y e-d (2) (In formula (2), M is a metal atom having a valence of e and selected from Ti, Al, Zr, and Hf; d is an integer between 0 and e, R 2 represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y is a chelate coordination compound. A compound represented by the formula: The ammonium halide compound (b4) is represented by the following formula (3): [ka] (In formula (3), R 3 , R 4 , R 5 , and R 6 each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, Z is Cl, Br, or I. The present invention relates to a curable composition, wherein the compound is represented by the formula: Effect of the Invention
[0012] According to the present invention, it is possible to provide a curable composition containing a reactive silicon group-containing organic polymer, which exhibits good fast curing properties even when it contains a non-organotin curing catalyst. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below.
[0014] ≪Curable composition≫ The curable composition comprises an organic polymer (A) and a curing catalyst (B). The organic polymer (A) is represented by the following formula (1): -SiR 1 3-a X a (1) (In formula (1), R 1 is a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, or R 0 It represents a triorganosiloxy group represented by 3SiO-, and has three R 0 are hydrocarbon groups having 1 to 20 carbon atoms, which may be the same or different, X represents a hydroxyl group or a hydrolyzable group; a is 1, 2, or 3; R 1 , X, when there are multiple of them, they may be the same or different.) The compound has a reactive silicon group represented by the formula: The curing catalyst (B) includes a carboxylic acid (b1), an amine compound (b2), a metal compound (b3), and an ammonium halide compound (b4).
[0015] The metal compound (b3) is represented by the following formula (2): M(OR 2 ) d Y e-d (2) (In formula (2), M is a metal atom having a valence of e and selected from Ti, Al, Zr, and Hf; d is an integer equal to or less than 0e, R 2 represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y is a chelate coordination compound. It is a compound represented by the formula: The ammonium halide compound (b4) is represented by the following formula (3): [ka] (In formula (3), R 3 , R 4 , R 5 , and R 6 each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, Z is Cl, Br, or I. It is a compound represented by the formula: The above curable composition exhibits excellent rapid curing properties.
[0016] The essential and optional components that the curable composition may contain are described below.
[0017] <Organic polymer (A)> The organic polymer has a reactive silicon group of a specific structure described below. The organic polymer (A) has a polymer backbone and a polymer chain end bonded to the polymer backbone. In the specification and claims of this application, the polymer backbone is also referred to as a "main chain structure." The polymer backbone is a structure in which a plurality of constituent units derived from monomers are bonded in succession. The monomer may be one type or multiple types.
[0018] The polymer chain end is a portion located at the end of the organic polymer (A). The number of polymer chain ends of the organic polymer (A) is 2 when the main chain structure is linear, and is 3 or more when the polymer backbone is branched. When the organic polymer (A) is a mixture of a polymer having a linear main chain structure and a polymer having a branched main chain structure, the number of polymer chain ends is a value between 2 and 3 on average.
[0019] The reactive silicon group may be present in the polymer backbone and at the polymer chain end. In addition, two or more reactive silicon groups may be present at the polymer chain end. When the curable composition is used for adhesives, sealing materials, elastic coating agents, pressure sensitive adhesives, etc., it is preferable that the reactive silicon group is present at the polymer chain end in the organic polymer (A).
[0020] The organic polymer (A) is not particularly limited as long as it is an organic polymer having a reactive silicon group represented by the following formula (1).
[0021] -SiR 1 3-a X a (1) (In formula (1), R 1 is a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, or R 0 It is a triorganosiloxy group represented by 3SiO-. 0 is a hydrocarbon group having 1 to 20 carbon atoms. 0 may be the same or different. X is a hydroxyl group or a hydrolyzable group. a is 1, 2, or 3. R 1 , or when there are multiple Xs, multiple Rs 1Or, multiple Xs may be the same or different.
[0022] R in formula (1) 1 Specific examples of include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, 2-ethylhexyl, and n-dodecyl; unsaturated hydrocarbon groups such as vinyl, isopropenyl, and allyl; alkoxymethyl groups such as methoxymethyl; halogenated methyl groups such as chloromethyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, toluyl, and 1-naphthyl; and aralkyl groups such as benzyl. Among these groups, alkyl groups and aryl groups are preferred, methyl, ethyl, and phenyl groups are more preferred, methyl and ethyl groups are even more preferred, and methyl groups are particularly preferred. In formula (1), R 1 If there are multiple R 1 may be the same group or a combination of two or more different groups.
[0023] X in formula (1) is a hydroxyl group or a hydrolyzable group. The hydrolyzable group is not particularly limited and may be a known hydrolyzable group. Specific examples of the hydrolyzable group include a hydrogen atom, a halogen atom, an alkoxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, and an alkenyloxy group. Among these, an alkoxy group, an acyloxy group, a ketoximate group, and an alkenyloxy group are preferred, and an alkoxy group such as a methoxy group and an ethoxy group is more preferred because of its mild hydrolysis and easy handling.
[0024] The reactive silicon group represented by formula (1) is not particularly limited. Specific examples of the reactive silicon group represented by formula (1) include dimethoxymethylsilyl group, diethoxymethylsilyl group, trimethoxysilyl group, triethoxysilyl group, dimethoxyphenylsilyl group, methoxymethyldimethoxysilyl group, methoxymethyldiethoxysilyl group, triisopropenyloxysilyl group, and triacetoxysilyl group. Among these, dimethoxymethylsilyl group and trimethoxysilyl group are preferred because the synthesis of organic polymer (A) is easy. Trimethoxysilyl group and methoxymethyldimethoxysilyl group are preferred because they have excellent curing properties.
[0025] (Main chain structure of organic polymer (A)) The main chain structure of the organic polymer (A) is not particularly limited, and may be any of various known main chain structures. Specific examples of the main chain structure include polyoxyalkylene polymers such as polyoxyethylene polymers, polyoxypropylene polymers, polyoxybutylene polymers, polyoxytetramethylene polymers, polyoxyethylene-polyoxypropylene copolymers, and polyoxypropylene-polyoxybutylene copolymers; hydrocarbon polymers such as ethylene-propylene copolymers, polyisobutylene, isobutylene-isoprene copolymers, polybutadiene, and hydrogenated polyolefin polymers obtained by hydrogenating these polyolefin polymers; polycondensates of dibasic acids such as adipic acid and glycols; and ring-opening polymers of lactones; (meth)acrylic acid ester-based polymers obtained by radical polymerization of (meth)acrylic acid ester-based monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and stearyl (meth)acrylate; vinyl copolymers obtained by radical polymerization of two or more monomers selected from (meth)acrylic acid ester-based monomers, vinyl acetate, acrylonitrile, and styrene; polysulfide-based polymers; and diallyl phthalate-based polymers. Note that (meth)acrylic acid ester means both acrylic acid ester and methacrylic acid ester.
[0026] As the main chain structure, polyoxyalkylene polymers and (meth)acrylic acid ester polymers are particularly preferred, since they have excellent deep curing properties as a one-component composition due to their high moisture permeability, and also have excellent adhesive properties. As the main chain structure, polyoxyalkylene polymers are more preferred, and polyoxypropylene is even more preferred.
[0027] By varying the composition of the monomers constituting the polymer, it is possible to obtain effects such as improving adhesiveness and reducing the heat resistance, weather resistance, and water absorption of the cured product, and therefore (meth)acrylic acid ester-based polymers are also useful as main chain structures. The main chain structure of the organic polymer (A) may be one of the above or a combination of a plurality of them. For example, an organic polymer (A) whose main chain structure is a polyoxypropylene-based polymer and an organic polymer (A) whose main chain structure is a (meth)acrylic acid ester-based polymer are uniformly compatible with each other, and give the obtained cured product a good balance of elasticity, mechanical strength, adhesive strength, etc. In this respect, it is also preferable to use a combination of an organic polymer (A) whose main chain structure is a polyoxypropylene-based polymer and an organic polymer (A) whose main chain structure is a (meth)acrylic acid ester-based polymer.
[0028] The polyoxyalkylene polymer is -R 7 It is a polymer having a repeating unit represented by -O-. 7 R is a linear or branched alkylene group having 1 to 14 carbon atoms. 7 is preferably a linear or branched alkylene group having 2 to 4 carbon atoms. 7Specific examples of the repeating unit represented by -O- include -CHO-, -CHCHO-, -CHCH(CH)O-, -CHCH(CH)O-, -CHC(CH)(CH)O-, and -CHCHCHCHO-. The main chain structure of the polyoxyalkylene polymer may be composed of only one type of repeating unit, or may be composed of two or more types of repeating units. In particular, when the curable composition is used as a sealant, adhesive, or the like, a polyoxypropylene polymer having oxypropylene repeating units in an amount of 50% by weight or more, preferably 80% by weight or more of the polymer main chain structure is preferred as the polyoxyalkylene polymer. This is because such a polyoxyalkylene polymer is amorphous and has a relatively low viscosity.
[0029] The main chain structure of the polyoxyalkylene polymer may be either linear or branched.
[0030] The polyoxyalkylene polymer is preferably a polymer obtained by ring-opening polymerization reaction of a cyclic ether compound in the presence of an initiator using a polymerization catalyst.
[0031] Examples of the cyclic ether compound include ethylene oxide, propylene oxide, butylene oxide, tetramethylene oxide, tetrahydrofuran, etc. These cyclic ether compounds may be used alone or in combination of two or more. Among these cyclic ether compounds, propylene oxide is particularly preferred since it is possible to obtain an amorphous polyether polymer having a relatively low viscosity.
[0032] Specific examples of the initiator include alcohols such as butanol, ethylene glycol, propylene glycol, propylene glycol monoalkyl ether, butanediol, hexamethylene glycol, neopentyl glycol, diethylene glycol, dipropylene glycol, triethylene glycol, glycerin, trimethylolmethane, trimethylolpropane, pentaerythritol, and sorbitol; and polyoxyalkylene polymers such as polyoxypropylene diol, polyoxypropylene triol, polyoxyethylene diol, and polyoxyethylene triol.
[0033] The method for synthesizing the polyoxyalkylene polymer is not particularly limited. Examples of methods for synthesizing polyoxyalkylene polymers include a polymerization method using an alkali catalyst such as KOH, a polymerization method using a transition metal compound-porphyrin complex catalyst such as a complex obtained by reacting an organoaluminum compound with porphyrin as disclosed in JP-A-61-215623, a polymerization method using a composite metal cyanide complex catalyst as disclosed in JP-B-46-27250, JP-B-59-15336, U.S. Pat. No. 3,278,457, U.S. Pat. No. 3,278,458, U.S. Pat. No. 3,278,459, U.S. Pat. No. 3,427,256, U.S. Pat. No. 3,427,334, and U.S. Pat. No. 3,427,335, and the like, a polymerization method using a catalyst made of a polyphosphazene salt as exemplified in JP-A-10-273512, and a polymerization method using a catalyst made of a phosphazene compound as exemplified in JP-A-11-060722. A polymerization method using a double metal cyanide complex catalyst is more preferred because of its low production cost and the fact that it can produce a polymer with a narrow molecular weight distribution.
[0034] The main chain structure of the organic polymer (A) may be a polyoxyalkylene polymer containing bonds other than ether bonds such as urethane bonds and urea bonds, within the range that does not significantly impair the desired effects. Specific examples of polymers having such a main chain structure include polyurethane prepolymers and polyurea prepolymers.
[0035] The polyurethane prepolymer can be obtained by a known method such as a method of reacting a polyol compound with a polyisocyanate compound, and the polyurea prepolymer can be obtained by a known method such as a method of reacting a polyamine compound with a polyisocyanate compound. The main chain structure may be a prepolymer having a combination of urethane bonds and urea bonds, which is obtained by reacting a polyol compound and a polyamine compound with a polyisocyanate compound.
[0036] Specific examples of the polyol compound include polyether polyol, polyester polyol, polycarbonate polyol, and polyether polyester polyol.
[0037] Specific examples of the polyisocyanate compound include diphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, methylene-bis(cyclohexyl isocyanate), isophorone diisocyanate, and hexamethylene diisocyanate.
[0038] The polyurethane prepolymer may have a terminal group of either a hydroxyl group or an isocyanate group, and the polyurea prepolymer may have a terminal group of either an amino group or an isocyanate group.
[0039] In a cured product of a curable composition containing, as the organic polymer (A), a polymer having one or more bonds selected from a urethane bond, a urea bond, and an ester bond in the main chain structure, the strength of the cured product may decrease due to cleavage of the urethane bond, the urea bond, or the ester bond in the main chain structure due to heat or the like.
[0040] When a polymer containing an amide bond in the main chain structure is used as the organic polymer, the curability of the curable composition may be improved. 8 It is represented by -C(=O)-. 8is a hydrogen atom or an organic group which may have a substituent. When the amount of amide bonds in the main chain structure is within an appropriate range, the viscosity of the polymer is low, and a decrease in strength of the cured product due to cleavage of the amide bonds caused by heat or the like and an increase in viscosity of the curable composition due to storage are unlikely to occur, and the workability of the curable composition is good.
[0041] When the organic polymer (A) contains an amide bond in the main chain structure, the average number of amide bonds per molecule is preferably 1 to 10, more preferably 1.5 to 5, and even more preferably 2 to 3. When the average number of amide bonds per molecule is within this range, the curable composition has good curability, the organic polymer (A) has a low viscosity, and the organic polymer (A) and the curable composition are easy to handle.
[0042] As the organic polymer (A) described above, from the viewpoint of obtaining a curable composition excellent in storage stability and workability, a polyoxyalkylene polymer that does not contain a urethane bond, a urea bond, an ester bond, or an amide bond in the main chain structure is most preferable.
[0043] The organic polymer (A) is preferably a polymer obtained by introducing a reactive silicon group into a polymer by any one of the following methods (a) to (d). (a) After converting the terminal hydroxyl groups of a hydroxyl-terminated organic polymer into carbon-carbon unsaturated groups, the carbon-carbon unsaturated groups are converted into HSiR 1 3-a X a A method of hydrosilylation using a hydrosilane represented by the formula: R 1 , X, and a are the same as those in general formula (1). (b) OCN-W-SiR 1 3-a X a A method of reacting an isocyanate alkylsilane compound represented by the formula: W is a divalent organic group. 1 , X, and a are the same as those in general formula (1). (c) After converting the terminal hydroxyl groups of the hydroxyl-terminated organic polymer to carbon-carbon unsaturated groups, the carbon-carbon unsaturated groups and the HS-W-SiR 1 3-a X a A method of carrying out an ene-thiol reaction with a mercaptoalkylsilane compound represented by the formula: W is a divalent organic group. 1 , X, and a are the same as those in general formula (1). (d) A hydroxyl-terminated organic polymer is reacted with a polyisocyanate compound to synthesize an NCO-terminated organic polymer, and then the terminal NCO groups are converted to an NCO-terminated organic polymer by the reaction of HNR 9 -W-SiR 1 3-a X a , or HS-W-SiR 1 3-a X a A method of reacting with a silane compound represented by the formula: W is a divalent organic group. 9 is a hydrogen atom or an alkyl group. 1 , X, and a are the same as those in general formula (1).
[0044] In the above methods (a) and (c), examples of the terminal carbon-carbon unsaturated group include a vinyl group, an allyl group, a methallyl group, an allenyl group, and a propargyl group.
[0045] In any of the above methods (b) to (d), the organic polymer (A) obtained by using a silane compound in which W is methylene exhibits extremely high curability.
[0046] The method (a) is preferred because it is easy to obtain an organic polymer (A) having good storage stability, whereas the methods (b), (c), and (d) are preferred because they can obtain a high conversion rate in a relatively short reaction time.
[0047] Methods for introducing reactive silicon groups by method (a) have been proposed in JP-B-45-36319, JP-B-46-12154, JP-A-50-156599, JP-A-54-6096, JP-A-55-13767, JP-A-55-13468, JP-A-57-164123, JP-B-3-2450, U.S. Pat. No. 3,632,557, U.S. Pat. No. 4,345,053, U.S. Pat. No. 4,366,307, and U.S. Pat. No. 4,960,844, etc. Examples of such methods include the method proposed in JP-A-61-197631, JP-A-61-215622, JP-A-61-215623, and JP-A-61-218632, in which reactive silicon groups are introduced by hydrosilylation or the like into a polyoxypropylene polymer having a high molecular weight and narrow molecular weight distribution, that is, a number average molecular weight of 6,000 or more and a Mw / Mn ratio of 1.6 or less, and the method proposed in JP-A-3-72527.
[0048] The number average molecular weight of the organic polymer (A) is not particularly limited. The number average molecular weight of the organic polymer (A) is preferably 3,000 to 100,000, more preferably 3,000 to 50,000, and particularly preferably 3,000 to 30,000, as a polystyrene-equivalent molecular weight in GPC. When the number average molecular weight is within the above range, the amount of hydrolyzable silyl group introduced is appropriate, and thus it is easy to obtain a polymer (A) that has a viscosity that is easy to handle and is excellent in workability while keeping the production cost within an appropriate range.
[0049] The molecular weight of the organic polymer (A) can also be shown as the end group-converted molecular weight calculated by directly measuring the end group concentration of the polymer precursor before the introduction of hydrolyzable silyl groups by titration analysis based on the principles of the hydroxyl value measurement method of JIS K 1557 and the iodine value measurement method specified in JIS K 0070, and taking into consideration the structure of the polymer (the degree of branching determined by the polymerization initiator used). The end group-converted molecular weight of the organic polymer (A) can also be calculated by preparing a calibration curve of the number average molecular weight measured by general GPC measurement of the polymer precursor and the above end group-converted molecular weight, and converting the number average molecular weight measured by GPC of the organic polymer (A) into the end group-converted molecular weight.
[0050] The molecular weight distribution (Mw / Mn) of the organic polymer (A) is not particularly limited. It is preferable that the molecular weight distribution of the organic polymer (A) is narrow. Specifically, the molecular weight distribution is preferably 1.6 or less, more preferably 1.4 or less, even more preferably 1.3 or less, and particularly preferably 1.2 or less. The molecular weight distribution of the organic polymer (A) can be determined from the number average molecular weight and weight average molecular weight obtained by GPC measurement.
[0051] In order to obtain a good rubber-like cured product, the reactive silicon group of the organic polymer (A) is preferably present at the polymer chain end. The number of reactive silicon groups is preferably 0.5 or more on average per polymer chain end, more preferably 0.6 or more, even more preferably 0.7 or more, and particularly preferably 0.8 or more. When the number of reactive silicon groups is 0.5 or more, the curability of the organic polymer (A) and the curable composition is good, and the cured product of the curable composition has good rubber elasticity.
[0052] The number of reactive silicon groups in one molecule is preferably 1 to 7 on average, more preferably 1 to 4, and particularly preferably 1 to 3.
[0053] In addition, as described in WO2013 / 180203, an organic polymer having two or more reactive silicon groups at the polymer chain terminals can also be used as the organic polymer (A). Such an organic polymer (A) exhibits high curability, and the resulting cured product is expected to have high strength and high recovery.
[0054] Specific examples of commercially available organic polymers (A) include various reactive silicon group-containing polyoxypropylene products such as Kaneka MS Polymer (registered trademark) and Kaneka Silyl (registered trademark), reactive silicon group-containing poly(meth)acrylic acid ester products such as Kaneka TA Polymer (registered trademark) and KANEKA XMAP (registered trademark), reactive silicon group-containing polyisobutylene products such as EPION (registered trademark), etc. All of these commercially available organic polymers (A) are products of Kaneka Corporation.
[0055] <Curing catalyst (B)> The curable composition contains a curing catalyst (B) that cures the organic polymer (A) by hydrolysis and condensation. The curing catalyst (B) includes a carboxylic acid (b1), an amine compound (b2), a metal compound (b3), and an ammonium halide compound (b4). The curing catalyst (B) is preferably a mixture of a carboxylic acid (b1), an amine compound (b2), a metal compound (b3), and an ammonium halide compound (b4). The amine compound (b2) is not an aminosilane coupling agent. Although the reason is unclear, as shown in the comparative example described later, the aminosilane coupling agent (b2) does not function as an amine compound (b2). The metal compound (b3) is represented by the following formula (2): M(OR 2 ) d Y e-d (2) (In formula (2), M is a metal atom having a valence of e and selected from Ti, Al, Zr, and Hf; d is an integer between 0 and e, R 2 represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y is a chelate coordination compound. It is a compound represented by the formula: Two or more compounds selected from the carboxylic acid (b1), the amine compound (b2), the metal compound (b3), and the ammonium halide compound (b4) may be reacted with each other. The ammonium halide compound (b4) is represented by the following formula (3): [ka] (In formula (3), R 3 , R 4 , R 5 , and R 6 each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, Z is Cl, Br, or I. It is a compound represented by the formula:
[0056] An amine compound having a carboxy group can be used as either the carboxylic acid (b1) or the amine compound (b2), provided that the amine compound having a carboxy group is used in combination with a carboxylic acid (b1) that is not an amine compound or an amine compound (b2) that does not have a carboxy group. In other words, the carboxylic acid (b1) and the amine compound (b2) are not both amine compounds having a carboxy group.
[0057] The carboxylic acid (b1) is not particularly limited as long as it is an organic compound having a carboxy group. The carboxylic acid (b1) may form a salt in the curable composition as long as the desired effect is not impaired. The salt of the carboxylic acid (b1) may be a metal salt or a non-metal salt. The carboxylic acid may be a monocarboxylic acid compound having one carboxy group, or a polycarboxylic acid compound having two or more carboxy groups. Examples of the carboxylic acid include aliphatic monocarboxylic acids, aliphatic dicarboxylic acids, trivalent or higher aliphatic polycarboxylic acids, and aromatic carboxylic acids.
[0058] Specific examples of aliphatic monocarboxylic acids include linear saturated fatty acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, undecanoic acid, lauric acid, tridecylic acid, myristic acid, pentadecylic acid, palmitic acid, heptadecylic acid, stearic acid, nonadecanoic acid, arachic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, and lacteric acid; undecylenic acid, linderic acid, tsuzuic acid, physeteric acid, myristoleic acid, and 2-hexadecenoic acid. Monoenoic unsaturated fatty acids such as 6-hexadecenoic acid, 7-hexadecenoic acid, palmitoleic acid, petroselinic acid, oleic acid, elaidic acid, asclepinic acid, vaccenic acid, gadoleic acid, gondoic acid, cetoleic acid, erucic acid, brassidic acid, selacholeic acid, xymenic acid, lumecic acid, acrylic acid, methacrylic acid, angelic acid, crotonic acid, isocrotonic acid, and 10-undecenoic acid; linoelaidic acid, linoleic acid, 10,12-octadecadienoic acid, hiragonic acid, α-eleostearic acid, β-eleostearic ... Polyenoic unsaturated fatty acids such as stearic acid, punicic acid, linoleic acid, 8,11,14-eicosatrienoic acid, 7,10,13-docosatrienoic acid, 4,8,11,14-hexadecatetraenoic acid, moroctic acid, stearidonic acid, arachidonic acid, 8,12,16,19-docosatetraenoic acid, 4,8,12,15,18-eicosapentaenoic acid, sardine acid, herring acid, and docosahexaenoic acid; 2-methylbutyric acid, isobutyric acid, 2-ethylbutyric acid, pivalic acid, 2,2-dimethylbutyric acid, 2-ethyl-2-methylbutyric acid, 2,2-diaminobutyric acid, 2-methylbutyric acid, 2-ethyl-2-methylbutyric acid, ... Branched fatty acids such as ethylbutyric acid, 2-phenylbutyric acid, isovaleric acid, 2,2-dimethylvaleric acid, 2-ethyl-2-methylvaleric acid, 2,2-diethylvaleric acid, 2-ethylhexanoic acid, 2,2-dimethylhexanoic acid, 2,2-diethylhexanoic acid, 2,2-dimethyloctanoic acid, 2-ethyl-2,5-dimethylhexanoic acid, versatic acid, neodecanoic acid, and tuberculostearic acid; fatty acids with triple bonds such as propiolic acid, talic acid, stearic acid, crepenic acid, ximenynic acid, and 7-hexadecynoic acid;Alicyclic carboxylic acids such as naphthenic acid, malvalic acid, sterculic acid, hydnocarpic acid, schormugic acid, golric acid, 1-methylcyclopentanecarboxylic acid, 1-methylcyclohexanecarboxylic acid, 1-adamantanecarboxylic acid, bicyclo[2.2.2]octane-1-carboxylic acid, and bicyclo[2.2.1]heptane-1-carboxylic acid; acetoacetic acid, ethoxyacetic acid, glyoxylic acid, glycolic acid, gluconic acid, savinic acid, 2-hydroxytetradecanoic acid, iprolic acid, 2-hydroxyhexadecanoic acid, yarapinolic acid, uniperinic acid, ambracic acid, and the like. Examples of the fatty acids include oxygen-containing fatty acids such as tallic acid, aleurite acid, 3-hydroxyisoacetic acid, 2-hydroxyoctadecanoic acid, 12-hydroxyoctadecanoic acid, 18-hydroxyoctadecanoic acid, 9,10-dihydroxyoctadecanoic acid, 2,2-dimethyl-3-hydroxypropionic acid, ricinoleic acid, camulolenic acid, licanic acid, ferronic acid, and cerebronic acid; halogen-substituted monocarboxylic acids such as chloroacetic acid and 2-chloroacrylic acid; piperidine carboxylic acids such as piperidine-2-carboxylic acid, piperidine-3-carboxylic acid, and piperidine-4-carboxylic acid. The aliphatic monocarboxylic acids are not limited to the above compounds; Among the above compounds, piperidine carboxylic acid can also be used as the amine compound (b2).
[0059] Examples of the aliphatic dicarboxylic acid include adipic acid, azelaic acid, pimelic acid, suberic acid, sebacic acid, glutaric acid, oxalic acid, malonic acid, ethyl malonic acid, dimethyl malonic acid, ethyl methyl malonic acid, diethyl malonic acid, succinic acid, 2,2-dimethyl succinic acid, 2,2-diethyl succinic acid, 2,2-dimethyl glutaric acid, and other chain dicarboxylic acids, 1,2,2-trimethyl-1,3-cyclopentane dicarboxylic acid, oxydiacetic acid, and other saturated dicarboxylic acids, and maleic acid, fumaric acid, acetylenedicarboxylic acid, and itaconic acid, and other unsaturated dicarboxylic acids. The aliphatic dicarboxylic acid is not limited to the above compounds.
[0060] Examples of the trivalent or higher aliphatic polycarboxylic acid include linear tricarboxylic acids such as aconitic acid, citric acid, isocitric acid, 3-methylisocitric acid, and 4,4-dimethylaconitic acid. The trivalent or higher aliphatic polycarboxylic acid is not limited to the above compounds.
[0061] Examples of aromatic carboxylic acids include aromatic monocarboxylic acids such as benzoic acid, chlorobenzoic acid, 9-anthracene carboxylic acid, atrolactic acid, anisic acid, isopropyl benzoic acid, salicylic acid, and toluic acid, and aromatic polycarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, carboxyphenylacetic acid, and pyromellitic acid. The aromatic dicarboxylic acid is not limited to the above compounds.
[0062] Further, carboxylic acid derivatives which generate a carboxylic acid upon hydrolysis, such as carboxylic acid anhydrides, esters, amides, nitriles, and acyl chlorides, can also be used as the carboxylic acid.
[0063] In terms of rapid curing properties, the carboxylic acid (b1) is preferably a carboxylic acid having a carboxy group bonded to a tertiary carbon atom or a secondary carbon atom, or a metal salt of a carboxylic acid having a carboxy group bonded to a tertiary carbon atom or a secondary carbon atom. As the carboxylic acid (b1), a carboxylic acid having a carboxy group bonded to a tertiary carbon atom and a metal salt of a carboxylic acid having a carboxy group bonded to a tertiary carbon atom are more preferred. Suitable examples of carboxylic acids having a carboxy group bonded to a tertiary or secondary carbon atom include 2-methylbutyric acid, isobutyric acid, 2-ethylbutyric acid, pivalic acid, 2,2-dimethylbutyric acid, 2-ethyl-2-methylbutyric acid, 2,2-diethylbutyric acid, 2,2-dimethylvaleric acid, 2-ethyl-2-methylvaleric acid, 2,2-diethylvaleric acid, 2-ethylhexanoic acid, 2,2-dimethylhexanoic acid, 2,2-diethylhexanoic acid, 2,2-dimethyloctanoic acid, 2-ethyl-2,5-dimethylhexanoic acid, and neodecanoic acid. Among these, pivalic acid, 2,2-dimethylbutyric acid, 2-ethyl-2-methylbutyric acid, 2,2-diethylbutyric acid, 2,2-dimethylvaleric acid, 2-ethyl-2-methylvaleric acid, 2,2-diethylvaleric acid, 2,2-dimethylhexanoic acid, 2,2-diethylhexanoic acid, 2,2-dimethyloctanoic acid, 2-ethyl-2,5-dimethylhexanoic acid, and neodecanoic acid are preferred, and neodecanoic acid is more preferred.
[0064] Specific examples of metal carboxylates include salts of alkali metals such as lithium, sodium, and potassium, salts of alkaline earth metals such as calcium, strontium, barium, and magnesium, etc. Metal salts of carboxylates may also be of metals such as aluminum, titanium, zirconium, hafnium, and vanadium.
[0065] Of these, 2-ethylhexanoic acid, octanoic acid, neodecanoic acid, oleic acid, and naphthenic acid are preferred because they are easily available, inexpensive, and have good compatibility with the reactive silicon group-containing organic polymer (A). Neodecanoic acid is particularly preferred because it is easy to obtain high catalytic activity. The carboxylic acid or metal salt thereof (b1) may be used alone or in combination.
[0066] In terms of rapid curing property, the amount of the carboxylic acid (b1) used is preferably 0.5 parts by weight or more and 10.0 parts by weight or less, more preferably 1.0 parts by weight or more and 8.0 parts by weight or less, and even more preferably 2.0 parts by weight or more and 6.0 parts by weight or less, relative to 100 parts by weight of the organic polymer (A).
[0067] Specific examples of the amine compound (b2) include aliphatic primary monoamines such as methylamine, ethylamine, propylamine, isopropylamine, butylamine, amylamine, hexylamine, octylamine, 2-ethylhexylamine, nonylamine, decylamine, laurylamine, pentadecylamine, cetylamine, stearylamine, cyclohexylamine, monoethanolamine, 3-hydroxypropylamine, 3-methoxypropylamine, and 3-lauryloxypropylamine; dimethylamine, diethylamine, dimethylamine, diethyl ... ethylamine, dipropylamine, diisopropylamine, dibutylamine, diamylamine, dihexylamine, dioctylamine, di(2-ethylhexyl)amine, didecylamine, dilaurylamine, dicetylamine, distearylamine, methylstearylamine, ethylstearylamine, butylstearylamine, pyrrolidine, piperidine, 2-methylpiperidine, 4-methylpiperidine, 3,5-dimethylpiperidine, 1,3-bis(4-piperidyl)propane, piperidine 2-carboxylic acid, piperidine 3-carboxamide, Aliphatic secondary monoamines such as carboxylic acid, piperidine 4-carboxylic acid, hexamethyleneimine, and diethanolamine; aliphatic tertiary monoamines such as triamylamine, trihexylamine, trioctylamine, and triethanolamine; aliphatic unsaturated amines such as triallylamine and oleylamine; aromatic amines such as aniline, laurylaniline, stearylaniline, and triphenylamine; ethylenediamine, propylenediamine, hexamethylenediamine, N-methyl-1,3-propanediamine, N,N aliphatic diamines such as '-dimethyl-1,3-propanediamine, 2-(2-aminoethylamino)ethanol, 3-dimethylaminopropylamine, 3-diethylaminopropylamine, 3-dibutylaminopropylamine, and 3-morpholinopropylamine; trivalent or higher polyvalent amines such as diethylenetriamine, triethylenetetramine, and 2-(1-piperazinyl)ethylamine; and other amines such as benzylamine, xylylenediamine, and 2,4,6-tris(dimethylaminomethyl)phenol. Among the above compounds, piperidine carboxylic acids such as piperidine 2-carboxylic acid, piperidine 3-carboxylic acid, and piperidine 4-carboxylic acid can also be used as the carboxylic acid (b1).
[0068] Among these, laurylamine, 3-dimethylaminopropylamine, 3-diethylaminopropylamine, 3-dibutylaminopropylamine, hexamethyleneimine, 3,5-dimethylpiperidine, and 4-methylpiperidine are preferred from the viewpoints of availability, compatibility with the organic polymer (A), and curability. The amine compound (b2) may be used alone or in combination of two or more components.
[0069] The amine compound (b2) may form a salt with the above-mentioned carboxylic acid or the metal salt thereof (b1) in the curable composition.
[0070] In terms of rapid curing property, the amount of the amine compound (b2) used is preferably 0.1 parts by weight or more and 3.0 parts by weight or less, more preferably 0.3 parts by weight or more and 2.5 parts by weight or less, and even more preferably 0.3 parts by weight or more and 2.0 parts by weight or less, based on 100 parts by weight of the organic polymer (A).
[0071] The metal compound (b3) is represented by the following formula (2): M(OR 2 ) d Y e-d (2) (In formula (2), M is a metal atom having a valence of e and selected from Ti, Al, Zr, and Hf; d is an integer between 0 and e, R 2 represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y is a chelate coordination compound. It is a compound represented by the formula: In formula (2), it is preferable that M is Ti or Al, and d is the valence number e of the metal atom represented by M.
[0072] R 2The hydrocarbon group as R may be an aliphatic hydrocarbon group, an aromatic hydrocarbon group, or a group in which an aliphatic hydrocarbon group and an aromatic hydrocarbon group are combined. 2 When the hydrocarbon group represented by R is an aliphatic hydrocarbon group, the aliphatic hydrocarbon group may have one or more unsaturated bonds. 2 When the hydrocarbon group as the alkyl group is an aliphatic hydrocarbon group, the structure of the aliphatic hydrocarbon group may be linear, branched, or cyclic, or may be a combination of these structures.
[0073] The chelating coordination compound Y is preferably a bidentate organic ligand. Examples of the chelating coordination compound include β-diketones and β-ketoesters. Specific examples of β-diketones include acetylacetone (ACAC), trifluoroacetylacetone, hexafluoroacetylacetone, benzoylacetone, thenoyltrifluoroacetone, dipivaloylmethane, dibenzoylmethane, and ascorbic acid.Specific examples of β-ketoesters include methyl acetoacetate, ethyl acetoacetate, allyl acetoacetate, benzyl acetoacetate, n-propyl acetoacetate, isopropyl acetoacetate, n-butyl acetoacetate, isobutyl acetoacetate, tert-butyl acetoacetate, 2-methoxyethyl acetoacetate, and methyl 3-oxopentanoate.
[0074] Specific examples of the metal compound (b3) include tetramethoxytitanium, trimethoxyethoxytitanium, trimethoxyisopropoxytitanium, trimethoxybutoxytitanium, dimethoxydiethoxytitanium, dimethoxydiisopropoxytitanium, dimethoxydibutoxytitanium, methoxytriethoxytitanium, methoxytriisopropoxytitanium, methoxytributoxytitanium, tetraethoxytitanium, triethoxyisopropoxytitanium, triethoxybutoxytitanium, diethoxydiisopropoxytitanium, diethoxydibutoxytitanium, ethoxytriisopropoxytitanium, ethoxytributoxytitanium, tetraisopropoxytitanium, triisopropoxybutoxytitanium, diisopropoxydibutoxytitanium, tetrabutoxytitanium, and tetraisopropoxytitanium. Examples of the titanium compounds include titanium compounds such as la-tert-butoxytitanium, bis(acetylacetonato)diisopropoxytitanium, bis(ethylacetoacetate)diisopropoxytitanium, and bis(ethylacetoacetate)diisobutoxytitanium; aluminum compounds such as triisopropoxyaluminum, tri-tert-butoxyaluminum, tri-sec-butoxyaluminum, tri-n-butoxyaluminum, aluminum tris(acetylacetonate), aluminum tris(ethylacetoacetate), and diisopropoxyaluminum ethylacetoacetate; zirconium compounds such as tetrapropoxyzirconium and zirconium tetrakis(acetylacetonate); and hafnium compounds such as tetrabutoxyhafnium.
[0075] From the viewpoints of availability, compatibility with the organic polymer (A), and curability, tetraisopropoxytitanium, tetrabutoxytitanium, tetratert-butoxytitanium, bis(acetylacetonato)diisopropoxytitanium, bis(ethylacetoacetate)diisopropoxytitanium, triisopropoxyaluminum, trisec-butoxyaluminum, and tetrapropoxyzirconium are more preferred, and tetraisopropoxytitanium, tetratert-butoxytitanium, and bis(ethylacetoacetate)diisopropoxytitanium are particularly preferred. Triisopropoxyaluminum and trisec-butoxyaluminum are particularly preferred in terms of activity and non-coloration. The metal compound (b3) may be a single component or a combination of multiple components.
[0076] In terms of rapid curing property, the amount of the metal compound (b3) used is preferably 0.1 part by weight or more and 5.0 parts by weight or less, more preferably 0.5 parts by weight or more and 4.5 parts by weight or less, and even more preferably 1.0 part by weight or more and 4.0 parts by weight or less, based on 100 parts by weight of the organic polymer (A).
[0077] The ammonium halide compound (b4) is represented by the following formula (3): [ka] (In formula (3), R 3 , R 4 , R 5 , and R 6 each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, Z is Cl, Br, or I. It is a compound represented by the formula: The ammonium halide compound (b4) may be used alone or in combination of two or more kinds.
[0078] R 3 , R 4 , R 5 , and R 6The hydrocarbon group as R may be an aliphatic hydrocarbon group, an aromatic hydrocarbon group, or a group in which an aliphatic hydrocarbon group and an aromatic hydrocarbon group are combined. 3 , R 4 , R 5 , and R 6 When the hydrocarbon group represented by R is an aliphatic hydrocarbon group, the aliphatic hydrocarbon group may have one or more unsaturated bonds. 3 , R 4 , R 5 , and R 6 When the hydrocarbon group as the alkyl group is an aliphatic hydrocarbon group, the structure of the aliphatic hydrocarbon group may be linear, branched, or cyclic, or may be a combination of these structures.
[0079] Specific examples of ammonium chloride among the ammonium halides (b4) include tetraalkylammonium chlorides such as tetramethylammonium chloride, tetraethylammonium chloride, tetrapropylammonium chloride, and tetrabutylammonium chloride, trimethylbenzylammonium chloride, benzyltriethylammonium chloride, trimethylphenylammonium chloride, and tris(2-hydroxyethyl)methylammonium chloride.
[0080] Furthermore, compounds in which the chloride ion in the above compounds listed as specific examples of ammonium chloride is replaced with a bromide ion or an iodide ion can also be used as the ammonium halide (b4).
[0081] As the ammonium halide (b4), tetraalkylammonium halide is preferable, and tetrabutylammonium halide is more preferable, because they are easily available. As the ammonium halide (b4), one kind may be used alone, or two or more kinds may be used in combination.
[0082] In terms of rapid curing property, the amount of the ammonium halide compound (b4) used is preferably 0.1 parts by weight or more and 5.0 parts by weight or less, more preferably 0.2 parts by weight or more and 3.0 parts by weight or less, and even more preferably 0.3 parts by weight or more and 1.0 parts by weight or less, based on 100 parts by weight of the organic polymer (A).
[0083] <Other additives> The curable composition may contain additives other than the organic polymer (A) and the curing catalyst (B) to the extent that the desired effect is not impaired. Examples of the additives include silanol condensation catalysts other than the curing catalyst (B), fillers, adhesion promoters, plasticizers, solvents, diluents, antisagging agents, antioxidants, light stabilizers, ultraviolet absorbers, physical property adjusters, tackifier resins, compounds containing epoxy groups, photocurable substances, oxygen curable substances, epoxy resins, other resins, surface improvers, foaming agents, curability adjusters, flame retardants, silicates, radical inhibitors, metal deactivators, phosphorus-based peroxide decomposers, lubricants, pigments, and fungicides.
[0084] (Silanol condensation catalyst) The curable composition may contain a silanol condensation catalyst other than the curing catalyst (B) for the purpose of promoting the hydrolysis condensation reaction between reactive silicon groups of the organic polymer (A) and chain-extending or crosslinking the polymer. Examples of such condensation catalysts include organotin compounds, metal alkoxides, inorganic acids, etc. The silanol condensation catalyst may be used in combination of two or more different catalysts. The amount of the silanol condensation catalyst used is preferably from 0.001 to 20 parts by weight, more preferably from 0.01 to 15 parts by weight, and particularly preferably from 0.01 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A).
[0085] (Filler) The curable composition may contain various fillers. Examples of the fillers include reinforcing fillers such as fumed silica, precipitated silica, crystalline silica, fused silica, dolomite, anhydrous silicic acid, hydrous silicic acid, and carbon black; heavy calcium carbonate, colloidal calcium carbonate, magnesium carbonate, diatomaceous earth, calcined clay, clay, talc, titanium oxide, bentonite, organic bentonite, ferric oxide, aluminum fine powder, flint powder, zinc oxide, activated zinc oxide, and resin powder; and fibrous fillers such as asbestos, glass fiber, and filaments. Examples of the resin powder include PVC powder and PMMA powder. When a filler is used, the amount of the filler used is preferably from 1 to 300 parts by weight, more preferably from 10 to 200 parts by weight, per 100 parts by weight of the organic polymer (A).
[0086] When it is desired to obtain a cured product having high strength by using these fillers, fillers selected from the group consisting of fumed silica, precipitated silica, crystalline silica, fused silica, dolomite, silicic anhydride, hydrated silicic acid, carbon black, surface-treated fine calcium carbonate, calcined clay, clay, and active zinc oxide can be preferably used. The amount of these fillers used, which is preferable in terms of the strength of the cured product, is preferably 1 to 200 parts by weight per 100 parts by weight of the organic polymer (A). When it is desired to obtain a cured product with low strength and high breaking elongation, fillers mainly selected from titanium oxide, calcium carbonate, magnesium carbonate, talc, ferric oxide, zinc oxide, and shirasu balloons can be preferably used. The amount of these fillers used, which is preferable in terms of the breaking elongation of the cured product, is preferably 5 to 200 parts by weight per 100 parts by weight of the organic polymer (A).
[0087] The curable composition may contain spherical hollow bodies such as balloons for the purpose of reducing the weight (specific gravity) of the cured product. A balloon is a spherical filler with a hollow interior. Examples of materials for the balloon include inorganic materials such as glass, silase, and silica, and organic materials such as phenolic resin, urea resin, polystyrene, saran, and acrylonitrile. The materials for the balloon are not limited to these materials. The materials for the balloon may be composite materials made of inorganic materials and organic materials. In addition, the materials for the balloon may be laminated with multiple layers. In addition, the balloon may be used alone or in combination with two or more types. The surface of the balloon may be surface-treated, coated, or treated with various surface treatment agents. For example, organic balloons coated with calcium carbonate, talc, titanium oxide, etc., and inorganic balloons surface-treated with a silane coupling agent can be used.
[0088] Specific examples of balloons are described in JP-A-2-129262, JP-A-4-8788, JP-A-4-173867, JP-A-5-1225, JP-A-7-113073, JP-A-9-53063, JP-A-10-251618, JP-A-2000-154368, JP-A-2001-164237, WO97 / 05201, and the like.
[0089] The amount of the spherical hollow bodies (balloons) used is preferably 0.01 to 30 parts by weight based on 100 parts by weight of the organic polymer (A). The lower limit is more preferably 0.1 parts by weight, and the upper limit is more preferably 20 parts by weight. When the amount of the spherical hollow bodies is within the above range, the curable composition has good properties, and a cured product excellent in elongation and breaking strength is easily formed.
[0090] (Adhesion promoter) The curable composition may contain an adhesion promoter. Examples of the adhesion promoter include a silane coupling agent. Silane coupling agent is a compound having a hydrolyzable silicon group and a functional group other than the hydrolyzable silicon group in the molecule. By using silane coupling agent, the effect of improving adhesion to various adherends is particularly remarkable. In addition to the above functions, silane coupling agent can also function as a dehydrating agent, a physical property adjuster, and an agent for improving the dispersion of inorganic fillers.
[0091] The hydrolyzable group in the hydrolyzable silicon group of the silane coupling agent is not particularly limited. Examples of the hydrolyzable group include hydrogen atoms, halogen atoms, alkoxy groups, aryloxy groups, alkenyloxy groups, acyloxy groups, ketoximate groups, amino groups, amide groups, acid amide groups, aminooxy groups, and mercapto groups. Among these, alkoxy groups such as methoxy groups and ethoxy groups are more preferred because they are mildly hydrolyzable and easy to handle, and methoxy groups and ethoxy groups are particularly preferred. The number of hydrolyzable groups bonded to silicon atoms in the silane coupling agent may be 3 in order to ensure good adhesion. In addition, 2 may be better in order to ensure the storage stability of the curable composition.
[0092] When using a silane coupling agent as an adhesion promoter, an aminosilane coupling agent having a hydrolyzable silicon group and a substituted or unsubstituted amino group is preferred because it has a large adhesion improving effect. The substituent in the substituted amino group is not particularly limited. Examples of the substituent include an alkyl group, an aralkyl group, and an aryl group.
[0093] Specific examples of aminosilane coupling agents include γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2-(2-aminoethyl)aminoethyl)aminopropyltrimethoxysilane, γ-(6-aminohexyl)aminopropyltrimethoxysilane, 3-(N-ethylamino)-2-methylpropyltrimethoxysilane, γ-ureidopropyltrimethoxysilane, γ-ureidopropyltriethoxysilane, N- Examples of the silanes include amino group-containing silanes such as phenyl-γ-aminopropyltrimethoxysilane, N-benzyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, N-cyclohexylaminomethyltriethoxysilane, N-cyclohexylaminomethyldiethoxymethylsilane, N-phenylaminomethyltrimethoxysilane, N-butylaminopropyltrimethoxysilane, (2-aminoethyl)aminomethyltrimethoxysilane, N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine, and bis(trimethoxysilylpropyl)amine; and ketimine type silanes such as N-(1,3-dimethylbutylidene)-3-(triethoxysilyl)-1-propanamine.
[0094] Among these, γ-aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, and γ-(2-aminoethyl)aminopropylmethyldimethoxysilane are preferred in terms of good adhesiveness of the cured product. Only one type of aminosilane coupling agent may be used, or two or more types may be used in combination. Silane coupling agents obtained by partially condensing a water-decomposable silicon group to form an oligomer can be used preferably in terms of safety and stability. The silane coupling agents to be condensed may be one or more types. Examples of oligomerized silane coupling agents include Dynasylan 1146 from Evonik. In terms of good storage stability of the curable composition, γ-aminopropyltrimethoxysilane and γ-(2-aminoethyl)aminopropylmethyldimethoxysilane are preferred.
[0095] Specific examples of silane coupling agents other than aminosilane coupling agents include epoxy group-containing silane coupling agents such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltriethoxysilane; isocyanate group-containing silane coupling agents such as γ-isocyanatepropyltrimethoxysilane, γ-isocyanatepropyltriethoxysilane, γ-isocyanatepropylmethyldiethoxysilane, γ-isocyanatepropylmethyldimethoxysilane, (isocyanatemethyl)trimethoxysilane, and (isocyanatemethyl)dimethoxymethylsilane; and γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane. mercapto group-containing silane coupling agents such as γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, and mercaptomethyltriethoxysilane; carboxy silane coupling agents such as β-carboxyethyltriethoxysilane, β-carboxyethylphenylbis(2-methoxyethoxy)silane, and N-β-(carboxymethyl)aminoethyl-γ-aminopropyltrimethoxysilane; vinyl type unsaturated group-containing silane coupling agents such as vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloyloxypropylmethyldimethoxysilane, and γ-acryloyloxypropylmethyltriethoxysilane; halogen-containing silane coupling agents such as γ-chloropropyltrimethoxysilane; isocyanurate silane coupling agents such as tris(trimethoxysilyl)isocyanurate, etc. can also be used. In addition, condensates obtained by partially condensing the above silane coupling agents can also be used. Examples of such condensates include Dynasylan 6490 and Dynasylan 6498 manufactured by Evonik.
[0096] Of these, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and γ-glycidoxypropylmethyldimethoxysilane are preferred from the viewpoint of good adhesiveness of the cured product.
[0097] The above silane coupling agents may be used alone or in combination of two or more. The amount of the silane coupling agent used is preferably from 0.1 to 20 parts by weight, more preferably from 0.5 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A).
[0098] (Plasticizer) The curable composition may contain a plasticizer. The addition of a plasticizer makes it possible to adjust the viscosity and slump of the curable composition, and the mechanical properties, such as the tensile strength and elongation, of the cured product.
[0099] Specific examples of plasticizers include phthalate compounds such as dibutyl phthalate, diisononyl phthalate (DINP), diheptyl phthalate, di(2-ethylhexyl) phthalate, diisodecyl phthalate (DIDP), and butyl benzyl phthalate; terephthalate compounds such as bis(2-ethylhexyl)-1,4-benzenedicarboxylate; non-phthalate compounds such as 1,2-cyclohexanedicarboxylic acid diisononyl ester; dioctyl adipate, dioctyl sebacate, dibutyl sebacate, diisodecyl succinate, and the like. Examples of suitable oils include aliphatic polycarboxylic acid ester compounds such as sodecyl and tributyl acetyl citrate; unsaturated fatty acid ester compounds such as butyl oleate and methyl acetylricinoleate; alkylsulfonic acid phenyl esters; phosphate compounds such as tricresyl phosphate and tributyl phosphate; trimellitic acid ester compounds; chlorinated paraffins; hydrocarbon oils such as alkyl diphenyls and partially hydrogenated terphenyls; process oils; epoxidized soybean oil, and epoxy plasticizers such as epoxy benzyl stearate. A specific example of the terephthalic acid ester compound is EASTMAN168 (trade name, manufactured by EASTMAN CHEMICAL). A specific example of the non-phthalic acid ester compound is Hexamoll DINCH (trade name, manufactured by BASF). A specific example of the alkylsulfonic acid phenyl ester is Mesamoll (trade name, manufactured by LANXESS).
[0100] Polymeric plasticizers can also be used. The use of polymeric plasticizers allows the initial physical properties of the cured product to be maintained for a long period of time compared to the use of low molecular weight plasticizers. Furthermore, the drying properties (paintability) of the cured product when coated with an alkyd paint are improved.
[0101] Specific examples of polymer plasticizers include vinyl polymers, which are polymers of vinyl monomers; esters of polyalkylene glycols and polyols, such as diethylene glycol dibenzoate, triethylene glycol dibenzoate, and pentaerythritol ester; polyester plasticizers obtained from dibasic acids, such as sebacic acid, adipic acid, azelaic acid, and phthalic acid, and dihydric alcohols, such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, and dipropylene glycol; polyether polyols, such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, having a number average molecular weight of 500 or more, or even 1,000 or more; derivatives of these polyether polyols in which the hydroxyl groups are converted to ester groups, ether groups, and the like; polystyrenes, such as polystyrene and poly-α-methylstyrene; polybutadiene, polybutene, polyisobutylene, butadiene-acrylonitrile, and polychloroprene. Polymer plasticizers are not limited to these.
[0102] The polymer plasticizer is preferably compatible with the organic polymer (A). From this point of view, polyethers and vinyl polymers are preferred. When polyethers are used as plasticizers, the surface curability and deep curability are improved, and curing delay after storage does not occur. Among polyethers, polypropylene glycol is more preferred. Also, vinyl polymers are preferred from the viewpoint of compatibility with the organic polymer (A) and the viewpoint of weather resistance and heat resistance of the cured product. Among vinyl polymers, acrylic polymers and / or methacrylic polymers are preferred, and acrylic polymers such as polyacrylic acid alkyl esters are more preferred. As a method for synthesizing vinyl polymers, living radical polymerization is preferred, and atom transfer radical polymerization is more preferred, since it provides a polymer with a narrow molecular weight distribution and low viscosity. Also, the so-called SGO process described in JP-A-2001-207157, in which acrylic acid alkyl ester monomers are continuously bulk polymerized at high temperature and high pressure, is also preferred as a method for producing vinyl polymers.
[0103] The number average molecular weight of the polymer plasticizer is preferably from 500 to 15,000, more preferably from 800 to 10,000, further preferably from 1,000 to 8,000, particularly preferably from 1,000 to 5,000, and most preferably from 1,000 to 3,000. When the number average molecular weight of the polymer plasticizer is within the above range, the outflow of the plasticizer from the cured product over time due to heat, rainfall, etc. can be suppressed, while the initial physical properties of the cured product can be maintained for a long period of time, the curable composition has an appropriate viscosity, and the workability of the curable composition is good. The molecular weight distribution of the polymer plasticizer is not particularly limited, but is preferably narrow. Specifically, the molecular weight distribution is preferably less than 1.80, more preferably 1.70 or less, even more preferably 1.60 or less, even more preferably 1.50 or less, particularly preferably 1.40 or less, and most preferably 1.30 or less.
[0104] The number average molecular weight of vinyl polymers is measured by the GPC method. The number average molecular weight of polyether polymers is measured by the end group analysis method. The molecular weight distribution (Mw / Mn) is measured by the GPC method (polystyrene equivalent).
[0105] The polymer plasticizer may or may not have a reactive silicon group. When the polymer plasticizer has a reactive silicon group, the polymer plasticizer acts as a reactive plasticizer and can prevent the plasticizer from migrating from the cured product. When the polymer plasticizer has a reactive silicon group, the number of reactive silicon groups is preferably 1 or less on average per molecule, more preferably 0.8 or less. When using a plasticizer having a reactive silicon group, particularly a polyether polymer having a reactive silicon group, it is necessary that the number average molecular weight is lower than that of the organic polymer (A).
[0106] The amount of the plasticizer used is preferably 5 to 150 parts by weight, more preferably 10 to 120 parts by weight, and even more preferably 20 to 100 parts by weight, based on 100 parts by weight of the organic polymer (A). When the amount of the plasticizer used is within the above range, a cured product excellent in mechanical strength can be formed while fully obtaining the desired effect of using the plasticizer. The plasticizer may be used alone or in combination of two or more kinds. A low molecular weight plasticizer and a polymeric plasticizer may be used in combination. These plasticizers may be blended with the organic polymer (A) when producing the organic polymer (A).
[0107] (Solvent, diluent) The curable composition may contain a solvent or a diluent. The solvent and the diluent are not particularly limited. As the solvent and the diluent, aliphatic hydrocarbons, aromatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, alcohols, esters, ketones, ethers, etc. can be used. When using a solvent or a diluent, the boiling point of the solvent is preferably 150°C or higher, more preferably 200°C or higher, and particularly preferably 250°C or higher, in view of the problem of air pollution when the curable composition is used indoors. The above-mentioned solvents or diluents may be used alone or in combination of two or more kinds.
[0108] (Anti-sagging agent) The curable composition may contain an anti-sagging agent as necessary to prevent sagging and improve workability. The anti-sagging agent is not particularly limited. Examples of the anti-sagging agent include polyamide waxes; hydrogenated castor oil derivatives; and metal soaps such as calcium stearate, aluminum stearate, and barium stearate. These anti-sagging agents may be used alone or in combination of two or more. The amount of the sagging prevention agent used is preferably 0.1 to 20 parts by weight based on 100 parts by weight of the organic polymer (A).
[0109] (Antioxidants) The curable composition may contain an antioxidant (antiaging agent). The use of an antioxidant can improve the weather resistance of the cured product. Examples of the antioxidant include hindered phenol compounds, monophenol compounds, bisphenol compounds, and polyphenol compounds, and hindered phenol compounds are particularly preferred. Examples of the antioxidant include Irganox 245, Irganox 1010, Irganox 1035, Irganox 1076, Irganox 1135, Irganox 1330, Irganox 1520 (all manufactured by BASF); SONGNOX 1076 (manufactured by SONGWON), and BHT. Hindered amine light stabilizers such as TINUVIN 622LD, TINUVIN 144, TINUVIN 292, CHIMASSORB944LD, CHIMASSORB119FL (all manufactured by BASF); ADK STAB LA-57, ADK STAB LA-62, ADK STAB LA-67, ADK STAB LA-63, ADK STAB LA-68 (all manufactured by ADEKA Corporation); SANOL LS-2626, SANOL LS-1114, SANOL LS-744 (all manufactured by Sankyo Lifetech Co., Ltd.); and NOCRAC CD (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) can also be used. Other antioxidants that can be used include SONGNOX4120, Naugard 445, and OKABEST CLX050. Specific examples of antioxidants are also described in JP-A-4-283259 and JP-A-9-194731. The amount of the antioxidant used is preferably from 0.1 to 10 parts by weight, more preferably from 0.2 to 5 parts by weight, based on 100 parts by weight of the organic polymer (A).
[0110] (Light stabilizer) The curable composition may contain a light stabilizer. The use of a light stabilizer can prevent photo-oxidative deterioration of the cured product. Examples of the light stabilizer include benzotriazole-based compounds, hindered amine-based compounds, and benzoate-based compounds. As the light stabilizer, a hindered amine-based compound is particularly preferred. The amount of the light stabilizer used is preferably from 0.1 to 10 parts by weight, and more preferably from 0.2 to 5 parts by weight, based on 100 parts by weight of the organic polymer (A). Specific examples of light stabilizers are described in, for example, JP-A-9-194731.
[0111] When a photocurable substance is blended in the curable composition, particularly when an unsaturated acrylic compound is used, it is preferable to use a tertiary amine-containing hindered amine light stabilizer as the hindered amine light stabilizer in order to improve the storage stability of the curable composition, as described in JP-A-5-70531. Examples of tertiary amine-containing hindered amine light stabilizers include TINUVIN 123, TINUVIN 144, TINUVIN 249, TINUVIN 292, TINUVIN 312, TINUVIN 622LD, TINUVIN 765, TINUVIN 770, TINUVIN 880, TINUVIN 5866, TINUVIN B97, CHIMASSORB119FL, and CHIMASSORB944LD (all manufactured by BASF); ADK STAB LA-57, LA-62, LA-63, LA-67, and LA-68 (all manufactured by ADEKA Corporation); SANOL LS-292, LS-2626, LS-765, LS-744, and LS-1114 (all manufactured by Sankyo Lifetech Co., Ltd.), SABOSTAB UV91, SABOSTAB UV119, SONGSORB CS5100, SONGSORB CS622, and SONGSORB Examples include CS944 (all manufactured by SONGWON), Nocrac CD (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), etc.
[0112] (UV absorber) The curable composition may contain an ultraviolet absorber. Use of an ultraviolet absorber can improve the surface weather resistance of the cured product. Examples of ultraviolet absorbers include benzophenone compounds, benzotriazole compounds, salicylate compounds, triazine compounds, substituted tolyl compounds, and metal chelate compounds. Among these, benzotriazole compounds are particularly preferred. Specific examples of benzotriazole compounds include Tinuvin 234, Tinuvin 326, Tinuvin 327, Tinuvin 328, Tinuvin 329, Tinuvin 350, Tinuvin 571, Tinuvin 900, Tinuvin 928, Tinuvin 1130, and Tinuvin 1600 (all manufactured by BASF); and SONGSORB 3290 (manufactured by SONGWON). Specific examples of triazine compounds include TINUVIN 400, TINUVIN 405, TINUVIN 477, and TINUVIN 1577ED (all manufactured by BASF); SONGSORB CS400 and SONGSORB 1577 (manufactured by SONGWON). Specific examples of benzophenone compounds include SONGSORB 8100 (manufactured by SONGWON). The amount of the ultraviolet absorber used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the organic polymer (A). It is preferable to use a phenol-based antioxidant or a hindered phenol-based antioxidant in combination with a hindered amine-based light stabilizer and a benzotriazole-based ultraviolet absorber. Addworks IBC760 (Clariant) can be used as a product containing a mixture of antioxidants, light stabilizers, and UV absorbers.
[0113] (Physical property adjuster) The curable composition may contain a physical property adjuster to adjust the tensile properties of the cured product as necessary. The physical property adjuster is not particularly limited. Examples of the physical property adjuster include alkyl alkoxysilanes such as methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, and n-propyltrimethoxysilane; alkyl isopropenoxysilanes such as dimethyldiisopropenoxysilane, methyltriisopropenoxysilane, and γ-glycidoxypropylmethyldiisopropenoxysilane; alkoxysilanes having functional groups such as γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyldimethylmethoxysilane, γ-aminopropyltrimethoxysilane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, γ-mercaptopropyltrimethoxysilane, and γ-mercaptopropylmethyldimethoxysilane; silicone varnishes; and polysiloxanes. The physical property modifier can be used to increase the hardness of the cured product, or conversely, to decrease the hardness of the cured product and provide breaking elongation. The physical property modifiers may be used alone or in combination of two or more kinds.
[0114] In particular, compounds that generate a compound having a monovalent silanol group in the molecule by hydrolysis have the effect of reducing the modulus of the cured product without worsening the stickiness of the surface of the cured product. Compounds that generate a compound having a monovalent silanol group in the molecule by hydrolysis are particularly preferred, and compounds that generate trimethylsilanol are particularly preferred. Compounds that generate a compound having a monovalent silanol group in the molecule by hydrolysis include compounds described in JP-A-5-117521. In addition, derivatives of alkyl alcohols such as hexanol, octanol, and decanol that generate trialkylsilanols such as trimethylsilanol by hydrolysis, and derivatives of polyhydric alcohols having three or more hydroxyl groups such as trimethylolpropane, glycerin, pentaerythritol, or sorbitol that generate trialkylsilanols such as trimethylsilanol by hydrolysis, as described in JP-A-11-241029, can be mentioned. Examples of the derivatives include those of oxyalkylene polymers that produce silicon compounds that produce trialkylsilanols such as trimethylsilanol by hydrolysis, as described in JP-A-7-258534.Furthermore, polymers having crosslinkable hydrolyzable silicon-containing groups and silicon-containing groups that can become monosilanol-containing compounds by hydrolysis, as described in JP-A-6-279693, can also be used. The physical property adjusting agent is used in an amount of 0.1 to 20 parts by weight, preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A).
[0115] (tackifier resin) The curable composition may contain a tackifier resin for the purpose of increasing the adhesiveness or adhesion of the cured product to a substrate, etc. The tackifier resin is not particularly limited, and any tackifier resin that is commonly used in various curable compositions can be used. Specific examples of tackifier resins include terpene resins, aromatic modified terpene resins, hydrogenated terpene resins, terpene-phenol resins, phenol resins, modified phenol resins, xylene-phenol resins, cyclopentadiene-phenol resins, coumarone-indene resins, rosin resins, rosin ester resins, hydrogenated rosin ester resins, xylene resins, low molecular weight polystyrene resins, styrene copolymer resins, styrene block copolymers, hydrogenated styrene block copolymers, petroleum resins, hydrogenated petroleum resins, and DCPD resins. Examples of petroleum resins include C5 hydrocarbon resins, C9 hydrocarbon resins, and C5C9 hydrocarbon copolymer resins. These may be used alone or in combination of two or more. The amount of the tackifier resin used is preferably 2 to 100 parts by weight, more preferably 5 to 50 parts by weight, and even more preferably 5 to 30 parts by weight, based on 100 parts by weight of the organic polymer (A). By using the tackifier resin in an amount within this range, a cured product having good adhesion and adhesion to the substrate can be formed. The curable composition has an appropriate viscosity, and the handleability of the curable composition is good.
[0116] (Compounds containing epoxy groups) The curable composition may contain a compound containing an epoxy group. The use of a compound having an epoxy group can improve the restorability of the cured product. Examples of the compound having an epoxy group include epoxidized unsaturated fats and oils, epoxidized unsaturated fatty acid esters, alicyclic epoxy compounds, epichlorohydrin derivatives, and mixtures thereof. Specific examples of the compound having an epoxy group include epoxidized soybean oil, epoxidized linseed oil, bis(2-ethylhexyl)-4,5-epoxycyclohexane-1,2-dicarboxylate (E-PS), epoxy octyl stearate, and epoxy butyl stearate. The amount of the compound containing an epoxy group used is preferably 0.5 to 50 parts by weight based on 100 parts by weight of the organic polymer (A).
[0117] (Epoxy resin) The curable composition may contain an epoxy resin. The curable composition containing an epoxy resin is preferably used as an adhesive, particularly as an adhesive for exterior wall tiles. Examples of the epoxy resin include bisphenol A type epoxy resins and novolac type epoxy resins. The weight ratio of the organic polymer (A) to the epoxy resin is preferably in the range of 100 / 1 to 1 / 100, expressed as (weight of organic polymer (A)) / (weight of epoxy resin). When the organic polymer (A) and the epoxy resin are used in the above ratio, a high-strength cured product having excellent impact strength and toughness is easily formed. When an epoxy resin is used, the curable composition may contain a curing agent together with the epoxy resin. The type of the curing agent is not particularly limited, and a commonly used curing agent may be used. The amount of the curing agent used is preferably 0.1 to 300 parts by weight based on 100 parts by weight of the epoxy resin.
[0118] (light curing substance) The curable composition may contain a photocurable substance. When a photocurable substance is used, a film of the photocurable substance is formed on the surface of the cured product, which improves the stickiness and weather resistance of the cured product. As photocurable substances, various compounds such as organic monomers, oligomers, and resins are known. In addition, many compositions containing photocurable substances are known. Representative photocurable substances include unsaturated acrylic compounds, polyvinyl cinnamates, and azido resins. As unsaturated acrylic compounds, monomers, oligomers, or mixtures thereof having one or more acrylic unsaturated groups or methacrylic unsaturated groups can be mentioned. The amount of the photocurable substance used is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A). When the amount of the photocurable substance used falls within this range, it is easy to form a flexible cured product that has excellent weather resistance and is less susceptible to cracking.
[0119] (oxygen curing substance) The curable composition may contain an oxygen curing substance. Examples of the oxygen curing substance include unsaturated compounds that can react with oxygen in the air. When the curable substance contains an oxygen curing substance, the oxygen curing substance reacts with oxygen in the air to form a cured film near the surface of the cured product. By forming a cured film on the surface of the cured product, stickiness and adhesion of dirt and dust to the surface of the cured product can be prevented. Specific examples of the oxygen curing substance include drying oils such as tung oil and linseed oil; various alkyd resins obtained by modifying drying oils; acrylic polymers, epoxy resins, and silicone resins modified with drying oils; liquid polymers such as 1,2-polybutadiene, 1,4-polybutadiene, or C5-C8 diene polymers obtained by polymerizing or copolymerizing diene compounds such as butadiene, chloroprene, isoprene, or 1,3-pentadiene. These may be used alone or in combination of two or more. The amount of the oxygen curing substance used is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A). When the oxygen curing substance is used in an amount within this range, the surface is less likely to be contaminated by dirt or dust, and a cured product having excellent mechanical properties such as tensile properties is easily formed. As described in JP-A-3-160053, the oxygen curing substance is preferably used in combination with a photocuring substance.
[0120] <Preparation of Curable Composition> The curable composition can be prepared as a one-component type in which all ingredients are mixed in advance, sealed, and stored, and then cured by moisture in the air after application. The curing agent composition can also be prepared as a two-component type in which a compounding material as a curing agent containing a curing catalyst (B), a filler, a plasticizer, water, and other ingredients, and a composition containing a separately prepared organic polymer (A) are mixed before use. From the viewpoint of workability, the one-component type is preferred. When the curable composition is a one-component type, all the ingredients are mixed in advance, so that the ingredients containing water are preferably dehydrated and dried before use, or dehydrated by reducing pressure during mixing and kneading. In addition to the dehydration and drying method, the storage stability can be further improved by adding an alkoxysilane compound such as methyltrimethoxysilane, phenyltrimethoxysilane, n-propyltrimethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, and γ-glycidoxypropyltrimethoxysilane. As the dehydrating agent, a partially condensed silane compound such as Dynasylan 6490 from Evonik can also be used preferably from the viewpoint of safety and stability. The amount of the dehydrating agent, particularly the silicon compound capable of reacting with water such as vinyltrimethoxysilane, is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A).
[0121] The order of adding the carboxylic acid (b1), the amine compound (b2), the metal compound (b3), and the ammonium halide compound (b4) to the compounding ingredients constituting the one-component type curable composition or the two-component type curable composition is not particularly limited as long as the desired effect is not impaired. It is preferable to add the ammonium halide compound (b4), the metal compound (b3), the amine compound (b2), and the carboxylic acid (b1) in this order, since this makes it easier to obtain a curable composition having excellent rapid curing properties.
[0122] The curable composition can be used as a building sealant, industrial adhesive, waterproof coating film forming composition, adhesive raw material, etc. The curable composition can also be used as a sealant for buildings, ships, automobiles, roads, etc. Furthermore, the curable composition can adhere to a wide range of substrates such as glass, porcelain, wood, metal, and resin moldings, either alone or with the aid of a primer. Therefore, the curable composition can also be used as various types of sealing compositions and adhesive compositions. The curable composition can also be used as a contact adhesive in addition to ordinary adhesives. Furthermore, the curable composition is also useful as a food packaging material, a cast rubber material, a material for molding, and a paint. The cured product of the above curable composition exhibits low water absorption. Therefore, the above curable composition and its cured product are particularly suitable for use as waterproof materials such as sealing materials, waterproof adhesives, and waterproof coating films.
[0123] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
[0124] That is, one aspect of the present invention includes the following.
[0125] <1> A curable composition comprising an organic polymer (A) and a curing catalyst (B), The organic polymer (A) is represented by the following formula (1): -SiR 1 3-a Xa (1) (In formula (1), R 1 is a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, or R 0 It represents a triorganosiloxy group represented by 3SiO-, and has three R 0 are hydrocarbon groups having 1 to 20 carbon atoms, which may be the same or different, X represents a hydroxyl group or a hydrolyzable group; a is 1, 2, or 3; R 1 , X, when there are multiple of them, they may be the same or different.) and having a reactive silicon group represented by the formula: The curing catalyst (B) comprises a carboxylic acid (b1), an amine compound (b2), a metal compound (b3), and an ammonium halide compound (b4); two or more selected from the group consisting of the carboxylic acid (b1), the amine compound (b2), the metal compound (b3), and the ammonium halide compound (b4) may be reacted with each other; The amine compound (b2) is a compound that does not fall under the category of an aminosilane coupling agent, The metal compound (b3) is represented by the following formula (2): M(OR 2 ) d Y e-d (2) (In formula (2), M is a metal atom having a valence of e and selected from Ti, Al, Zr, and Hf; d is an integer between 0 and e, R 2 represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y is a chelate coordination compound. A compound represented by the formula: The ammonium halide compound (b4) is represented by the following formula (3): [ka] (In formula (3), R 3 , R 4 , R 5 , and R6 each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, Z is Cl, Br, or I. The curable composition is a compound represented by the formula: <2> The main chain structure of the organic polymer (A) is one or more selected from the group consisting of polyoxyalkylene polymers, saturated hydrocarbon polymers, and (meth)acrylic acid ester polymers. <1> The curable composition according to claim 1. <3> The main chain structure of the organic polymer (A) is a polyoxyalkylene polymer. <2> The curable composition according to claim 1. <4> The curing catalyst (B) is a mixture of a carboxylic acid (b1), an amine compound (b2), a metal compound (b3), and an ammonium halide compound (b4); <1> ~ <3> 13. The curable composition according to claim 12, <5> In the formula (2), M is Ti or Al, and d is the valence e of the metal atom represented by M. <1> The curable composition according to claim 1. <6> <1> ~ <5> 2. A cured product of the curable composition according to claim 1. EXAMPLES
[0126] The present invention will be described in more detail below with reference to specific examples, but the present invention is not limited to the following examples.
[0127] <Synthesis Example of Organic Polymer (A)> Hereinafter, the number average molecular weight is a GPC molecular weight measured under the following conditions. Liquid delivery system: Tosoh HLC-8120GPC Column: Tosoh TSKgel SuperH series Solvent: THF (tetrahydrofuran) Molecular weight: Polystyrene equivalent Measurement temperature: 40℃
[0128] The end group calculated molecular weight in the examples is a molecular weight calculated by taking into consideration the structure of the organic polymer, determining the hydroxyl value according to the measurement method of JIS K 1557 and the iodine value according to the measurement method of JIS K 0070. The organic polymer structure taken into consideration is the branching degree determined by the polymerization initiator used.
[0129] The average number of silyl groups per terminal or per molecule of the polymer shown in the examples is 1 Calculation was performed by H-NMR (measured in CDCl3 solvent using AVANCE III HD-500 manufactured by Bruker).
[0130] [Preparation Example 1: Synthesis of Organic Polymer (A-1)] Propylene oxide was polymerized using a polyoxypropylene diol having a molecular weight of about 2,000 as an initiator and a zinc hexacyanocobaltate glyme complex catalyst to obtain a hydroxyl-terminated polypropylene oxide having a number average molecular weight of 28,500. Subsequently, a methanol solution of 1.2 molar equivalents of NaOMe was added to the hydroxyl groups of this hydroxyl-terminated polypropylene oxide. After distilling off methanol from the reaction solution, allyl chloride was added to the reaction solution to convert the terminal hydroxyl groups to allyl groups. Unreacted allyl chloride was removed by devolatilization under reduced pressure. 300 parts by weight of n-hexane and 300 parts by weight of water were mixed with 100 parts by weight of the obtained unpurified allyl-terminated polypropylene oxide, and then stirred. Next, the mixture was separated into an aqueous phase and a hexane phase by centrifugation, and then the aqueous phase was removed. 300 parts by weight of water was mixed with the obtained hexane phase, and then stirred. Again, the mixture was separated into an aqueous phase and a hexane phase by centrifugation, and then the aqueous phase was removed. Then, hexane was removed from the hexane phase by volatilization under reduced pressure. As a result, a bifunctional polypropylene oxide with an allyl group at the end and a number average molecular weight of about 28,500 was obtained. 150 ppm of a 2-propanol solution of a platinum vinylsiloxane complex with a platinum content of 3 wt% was added as a catalyst to 100 parts by weight of the obtained allyl-terminated polypropylene oxide. Next, 0.8 molar equivalents of trimethoxysilane relative to the allyl groups of the allyl-terminated polypropylene oxide were added to the allyl-terminated polypropylene oxide, and the allyl terminal groups and trimethoxysilane were reacted at 90°C for 5 hours to obtain a trimethoxysilyl-terminated polyoxypropylene polymer (A-1). The number of trimethoxysilyl groups was about 0.8 per polymer chain end.
[0131] Hereinafter, a curable composition was prepared using the organic polymer and catalyst obtained by the above method, and the curability of the curable composition was confirmed. Details of the components (b1) to (b4) shown in Table 1 below are as follows. ((b1) component) Neodecanoic acid: Hexion ((b2) component) 4-Methylpiperidine: Tokyo Chemical Industry Co., Ltd. (Component (b3)) Ti(O i Pr) 4: Titanium tetraisopropoxide, manufactured by Tokyo Chemical Industry Co., Ltd. Tyzor 9000: Titanium tetrabutoxide, manufactured by Dorf Ketal Ti(O n Bu)4: Titanium tetraoxide, manufactured by Tokyo Chemical Industry Co., Ltd. Al(O s Bu)3: Trisec-butoxyaluminum, manufactured by Tokyo Chemical Industry Co., Ltd. ((b4) component) TBAC: Tetrabutylammonium chloride, manufactured by Tokyo Chemical Industry Co., Ltd. TBAB: Tetrabutylammonium bromide, manufactured by Tokyo Chemical Industry Co., Ltd. TBAI: Tetrabutylammonium iodide, manufactured by Tokyo Chemical Industry Co., Ltd. TBAF: Tetrabutylammonium fluoride-tetrahydrofuran solution (approximately 1 mol / L), Fujifilm Wako Pure Chemical Industries, Ltd.
[0132] [Examples 1 to 8 and Comparative Examples 1 to 5] 100 parts by weight of organic polymer (A-1), 160 parts by weight of gelatinous calcium carbonate (Shiraishi Industrial Co., Ltd., product name: Hakuenka CCR), 54 parts by weight of heavy calcium carbonate (Shiraishi Calcium Co., Ltd., product name: Whiten SB), 90 parts by weight of plasticizer (BASF, product name: Hexamoll DINCH), 5 parts by weight of pigment (Ishihara Sangyo Kaisha, Ltd., product name: Typek R820), 1 part by weight of thixotropic agent (ARKEMA, product name: Crayvallac SLT), 1 part by weight of antioxidant (BASF, product name: Irganox1010), 1 part by weight of ultraviolet absorber (BASF, product name: Tinuvin326), and 1 part by weight of light stabilizer (BASF, product name: Tinuvin770) were mixed using a spatula. The mixture obtained was dispersed by passing it through a three-roll mill three times. Thereafter, the mixture was dehydrated under reduced pressure using a planetary mixer to obtain a dehydrated mixture, which was then filled as the base material into a moisture-proof cartridge.
[0133] Under an atmosphere of 23°C and 50% relative humidity, the base material was extruded from the cartridge and weighed into a plastic container, and the dehydrating agent Dynasylan VTMO (vinyl trimethoxysilane, manufactured by Evonik), the ammonium halide compound (b4) (component (b4) of the curing catalyst (B)), and the adhesion promoter Dynasylan AMMO (γ-aminopropyl trimethoxysilane, manufactured by Evonik) were added and mixed. Next, the metal compound (b3) (component (b3) of the curing catalyst (B)) was added and mixed, and then the amine compound (b2) (component (b2) of the curing catalyst (B)) was added and mixed. Finally, the carboxylic acid (b1) (component (b1) of the curing catalyst (B)) was added and mixed to obtain a curable composition. However, in Comparative Example 2, the (b4) component was not used, in Comparative Example 3, the (b3) component was not used, in Comparative Example 4, the (b2) component was not used, and in Comparative Example 5, the (b1) component was not used. The numerical values for each component listed in Table 1 indicate the amount (parts by weight) of each component used.
[0134] (Skinning time (hardening evaluation)) The obtained curable composition was filled into a mold of approximately 5 mm thickness in an atmosphere of 23°C and relative humidity of 50%, and the curable composition in the mold was then touched with a spatula. The time when the mixture no longer adhered to the spatula was taken as the skinning time, and the curing time (curability) was measured.
[0135] [Table 1]
[0136] A comparison between Examples 1 to 8 and Comparative Examples 1 to 5 shows that when the curable composition containing the organic polymer (A) having a reactive silicon group is mixed with the curing catalyst (B) of the predetermined components (b1), (b2), (b3), and (b4), the curable composition cures rapidly. The curable composition of Comparative Example 4 contains an aminosilane coupling agent (Dynasylan AMMO) in addition to the components (b1), (b3), and (b4). However, the curable composition of Comparative Example 4 took a long time to cure. This shows that the aminosilane coupling agent does not function as the amine compound (b2).
Claims
1. A curable composition comprising an organic polymer (A) and a curing catalyst (B), The organic polymer (A) is represented by the following formula (1): -SiR 1 3-a X a (1) (In formula (1), R 1 is a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, or R 0 3 A triorganosiloxy group represented by SiO-, 0 are hydrocarbon groups having 1 to 20 carbon atoms, which may be the same or different, X represents a hydroxyl group or a hydrolyzable group; a is 1, 2, or 3; R 1 , X, when there are a plurality of them, they may be the same or different. and having a reactive silicon group represented by the formula: the curing catalyst (B) comprises a carboxylic acid (b1), an amine compound (b2), a metal compound (b3), and an ammonium halide compound (b4); two or more selected from the group consisting of the carboxylic acid (b1), the amine compound (b2), the metal compound (b3), and the ammonium halide compound (b4) may be reacted with each other; The amine compound (b2) is a compound that does not fall under the category of an aminosilane coupling agent, The metal compound (b3) is represented by the following formula (2): M(OR 2 ) d Y e-d (2) In formula (2), M is a metal atom having a valence of e and selected from Ti, Al, Zr, and Hf; d is an integer from 0 to e, R 2 represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y is a chelate coordination compound. A compound represented by the formula: The ammonium halide compound (b4) is represented by the following formula (3): 【Chemistry 1】 (In formula (3), R 3 , R 4 , R 5 , and R 6 each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, Z is Cl, Br, or I. The curable composition is a compound represented by the formula:
2. The curable composition according to claim 1, wherein the main chain structure of the organic polymer (A) is at least one selected from the group consisting of polyoxyalkylene polymers, saturated hydrocarbon polymers, and (meth)acrylic acid ester polymers.
3. The curable composition according to claim 2 , wherein the main chain structure of the organic polymer (A) is the polyoxyalkylene polymer.
4. The curable composition according to claim 1, wherein the curing catalyst (B) is a mixture of the carboxylic acid (b1), the amine compound (b2), the metal compound (b3), and the ammonium halide compound (b4).
5. The curable composition according to claim 1, wherein, in the formula (2), M is Ti or Al, and d is the valence number e of the metal atom represented by M.
6. A cured product of the curable composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
Room temperature curing compositions
JP1977073998A
Curable composition
JP1980009669A
Curable composition