Photocatalyst filter
The photocatalytic filter uses a porous metal carrier with titanium oxide and tungsten compounds to stabilize the particles, ensuring effective decomposition of harmful gases and prolonged catalytic activity.
Patent Information
- Application Number
- JP2024065916
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-16
- Publication Date
- 2024-11-07
AI Technical Summary
Conventional photocatalytic filters face issues with titanium oxide particles detaching from the carrier during transportation or use, reducing their effectiveness in decomposing harmful gas components.
A photocatalytic filter comprising a porous metal material as a carrier with titanium oxide and tungsten compounds supported on it, utilizing a specific mass ratio and porosity to enhance stability and photocatalytic activity.
The filter effectively decomposes harmful gas components, including volatile organic compounds, while preventing titanium oxide particles from falling off, thereby maintaining long-term catalytic activity.
Smart Images

Figure 2024157527000001 
Figure 2024157527000002 
Figure 2024157527000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a photocatalytic filter that decomposes harmful gas components such as volatile organic compounds. [Background technology]
[0002] Deodorizing devices using photocatalysts have already been put to practical use. The deodorizing devices using photocatalysts include a photocatalyst filter in which a photocatalyst is fixed to a filter substrate, and a light source that activates the photocatalyst. In the deodorizing devices using photocatalysts, the light source is turned on to activate the photocatalyst with light from the light source, and the gas is passed through the photocatalyst filter, whereby the photocatalyst of the photocatalyst filter decomposes harmful gas components (harmful gas components) such as odors contained in the gas (see, for example, Patent Document 1).
[0003] Many photocatalytic filters use titanium oxide as a photocatalyst, but various improvements are being investigated. For example, the light required to activate titanium oxide is ultraviolet light, but photocatalysts that can be used in a wide wavelength range from ultraviolet to visible light by combining it with tungsten oxide, which is activated by visible light, are being investigated (e.g., Patent Document 2). However, sufficient photocatalytic activity cannot be obtained by using both alone, so photocatalysts that further contain iron compounds have been developed (e.g., Patent Document 3). Photocatalysts that use iron compounds in combination can decompose various organic compounds even under ultraviolet light (e.g., Patent Document 4). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-050979 A [Patent Document 2] JP 2006-198464 A [Patent Document 3] JP 2006-198465 A [Patent Document 4] JP 2017-170441 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, conventional photocatalytic filters have a problem in that the titanium oxide particles fixed to the carrier, which is the filter base material, fall off during transportation or use of the photocatalytic filter, reducing the photocatalytic filter's activity in decomposing harmful gas components.
[0006] The present invention has been made in consideration of such problems, and aims to provide a photocatalytic filter that can decompose harmful gas components and in which titanium oxide particles are less likely to fall off from the carrier, which is the filter base material, during transportation or use. [Means for solving the problem]
[0007] [1] A photocatalytic filter comprising a carrier made of a porous metal body, and titanium oxide particles and a tungsten compound supported on the carrier. [2] The photocatalytic filter according to [1], wherein the tungsten compound is tungstic acid and / or tungsten oxide. [3] The photocatalytic filter according to [1], wherein the metal porous body contains iron and / or nickel as the metal constituting the metal porous body. [4] The photocatalytic filter according to [1], wherein the content ratio of the titanium oxide and the tungsten compound in the photocatalytic filter is from 99:1 to 85:15 by mass. [5] The photocatalyst filter according to [1], wherein the porosity of the metal porous body is 80% or more and 99% or less. [6] The photocatalytic filter according to [1], characterized in that the average particle diameter of the titanium oxide particles is 0.5 nm or more and 100 nm or less. [7] The amount of the titanium oxide particles supported is 100 cm of the volume of the metal porous body. 3 The photocatalytic filter according to [1], characterized in that the weight of the filter is 0.2 g or more and 10 g or less. [8] The photocatalytic filter according to [1], characterized in that the ultraviolet light transmittance is 1% or more and 10% or less. [9] A harmful gas component removal device comprising a photocatalytic filter described in any one of [1] to [8].
[10] A method for producing a photocatalytic filter, comprising the step of firing a metal porous body coated with a dispersion liquid in which titanium oxide particles and tungstic acid particles are dispersed. Effect of the Invention
[0008] According to the present invention, it is possible to provide a photocatalytic filter that is capable of decomposing harmful gas components and in which titanium oxide particles are less likely to fall off from the carrier that is the filter base material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described in detail.
[0010] The photocatalytic filter of this embodiment is a photocatalytic filter that can decompose odorous volatile substances, or volatile organic compounds that are harmful to the human body even if they do not have an odor (hereinafter, these will be collectively referred to as "harmful gas components") when irradiated with ultraviolet light or visible light.
[0011] Specific examples of harmful gas components that can be decomposed by the photocatalytic filter of this embodiment include volatile organic compounds, nitrogen compounds, and sulfur compounds. Examples of volatile organic compounds include alcohols such as methanol, ethanol, and butanol, aldehydes such as formaldehyde and acetaldehyde, fatty acids such as valeric acid, and hydrocarbons such as hexane, toluene, and xylene. Examples of nitrogen compounds include amines such as ammonia and trimethylamine, and examples of sulfur compounds include thiols such as hydrogen sulfide and methanethiol. According to the photocatalytic filter of this embodiment, even when these harmful gas components are mixed, each odor component can be decomposed. The photocatalytic filter of this embodiment is particularly effective in oxidatively decomposing organic compounds such as acetaldehyde and acetic acid among the above-mentioned harmful gas components.
[0012] The photocatalytic filter of this embodiment is a porous metal carrier carrying titanium oxide particles and a tungsten compound. The porous metal carrier has a large number of pores communicating with the outside, and the titanium oxide particles and the tungsten compound are carried on the inner surfaces of the pores and on the outer surface of the porous metal carrier excluding the inner surfaces of the pores. The titanium oxide particles and the tungsten compound may be directly carried on the porous metal carrier, or may be carried on the carrier via a binder.
[0013] First, the carrier (porous metal body) contained in the photocatalytic filter of this embodiment will be described.
[0014] The metal porous body constituting the carrier generally has a larger specific surface area than a honeycomb substrate, etc., and can support a large amount of titanium oxide particles on the surface of the internal continuous pores. For this reason, when a metal porous body is used as the carrier, it is known that the contact efficiency with the gas to be treated is increased, and the efficiency of removing harmful gas components can be increased, while at the same time the pressure loss during the permeation of the gas to be treated can be reduced.
[0015] The metal porous body in this embodiment has a so-called sponge-like shape, and has fine three-dimensional continuous pores inside, and the continuous pores are open to the outside on the outer surface of the metal porous body. Therefore, the carrier (metal porous body) used in this embodiment has air permeability, and when gas is applied from one direction to the outer surface of the metal porous body, the gas passes through the continuous pores and can pass through other outer surfaces, such as the outer surface on the opposite side of the metal porous body. In such a metal porous body having air permeability, light is directly irradiated from the openings to the inner surfaces of the continuous pores inside the metal porous body, or light reflected on the inner surfaces of the continuous pores is transmitted to the inside of the continuous pores, and light can be irradiated to the inside of the metal porous body. Therefore, if light is irradiated from the outside of the metal porous body, even titanium oxide supported on the inner surface of the continuous pores can be excited. As a result, harmful gas components in the gas to be treated come into contact with the photoexcited titanium oxide and are decomposed when the gas to be treated passes through the continuous pores.
[0016] The metal porous body is a porous body made of metal, and may be made of a single metal or an alloy of multiple metals. The type of metal constituting the metal porous body is preferably a metal element that can be stably used in the atmosphere, and examples thereof include single metals such as iron, zinc, nickel, titanium, tungsten, silver, copper, and aluminum, and alloys such as stainless steel, brass, nickel-chrome, nickel-tin, and nickel-iron. Among these, the metal porous body preferably contains iron and / or nickel as its constituent metal, and more preferably is composed only of iron and / or nickel. When the metal porous body contains iron and / or nickel as its constituent metal, it is preferable because the falling off of titanium oxide particles is more suppressed than when the metal porous body does not contain iron and / or nickel.
[0017] The pore state of a porous metal body is characterized by the porosity and the average number of cells (openings) per inch of the exterior surface of the porous metal body.
[0018] The larger the porosity, the easier the gas to be treated will pass through, and the smaller the pressure loss will be when the photocatalytic filter is incorporated into a deodorizing device. Therefore, the porosity of the metal porous body in this embodiment is preferably 80% or more and 99% or less. When the porosity of the metal porous body is 80% or more, the skeleton constituting the porous body becomes thinner than when the porosity is less than 80%, so that light can reach the inside of the porous body more easily and titanium oxide can be excited more easily. When the porosity of the metal porous body is 99% or less, it can support an amount of titanium oxide that exhibits sufficient photocatalytic activity and can exhibit sufficient mechanical properties as a carrier of a photocatalytic filter. In this embodiment, the porosity of the metal porous body can be determined by a method known to those skilled in the art, for example, in accordance with JIS Z 8807. More specifically, the porosity of the metal porous body can be determined from the following formula (1). In the following formula (1), Wp represents the weight [g] of the porous metal body, and W represents the weight [g] of a solid body having the same external dimensions and made of the same metal material as the porous metal body. Porosity (%)=(W-Wp) / W×100 (1)
[0019] The average cell number of the metal porous body is a parameter related to the pore density of the metal porous body, and the larger this value is, the larger the specific surface area of the metal porous body becomes, the larger the amount of titanium oxide particles that can be supported, and the easier it is for harmful gas components in the gas to be treated to come into contact with titanium oxide. From this perspective, the average cell number of the metal porous body in this embodiment is preferably 10 to 50 PPI (pixels per inch).
[0020] In this embodiment, the average cell number of the metal porous body can be determined, for example, by the method described in JIS-K6400-1, Appendix 1. Specifically, one test piece having a thickness of 10 mm or more and a width and length of 100 mm or more is taken. The test device is a magnifying glass with a magnification of 5 times or more, which can move left and right and is equipped with a scale that can measure the distance of movement. The measurement is performed by placing the test piece on the stand of the test device, and counting the number of cells in a straight line of 10 mm while moving the magnifying glass, and measuring three points. The number of cells is calculated by the following formula (2), and the average number of cells at the three points is rounded to a rounding width of 1 according to JIS Z 8401 to obtain the average number of cells. N = n × 2.5 (2) In the above formula (2), N represents the number of cells (PPI (cells / 25 mm)), and n represents the number of cells in the above-mentioned 10 mm interval.
[0021] The shape of the metal porous body is not particularly limited and can be various shapes such as a sphere, a rectangular prism, or a cube, and can be appropriately set depending on the shape of the device into which the photocatalytic filter of this embodiment is incorporated.
[0022] In the photocatalytic filter of this embodiment, the carrier may be composed only of a porous metal body, but may also contain a material other than the porous metal body.
[0023] Next, the components supported on the support (porous metal body) will be described.
[0024] In the photocatalytic filter of this embodiment, titanium oxide particles and a tungsten compound are supported on a carrier (porous metal body).
[0025] The titanium oxide particles supported on the carrier (metallic porous body) are particles made of titanium oxide. The titanium oxide constituting the titanium oxide particles is not particularly limited as long as it has photocatalytic activity, and for example, rutile-type titanium oxide or anatase-type titanium oxide can be used, but anatase-type titanium oxide is preferable because it has high photocatalytic activity.
[0026] The titanium oxide particles do not necessarily have to be composed only of titanium oxide, and may contain other substances such as substances other than titanium oxide (e.g., metallic titanium) that are unintentionally produced during the manufacturing process, and unavoidable impurities that are inevitably mixed in during the manufacturing process; however, it is preferable that the titanium oxide particles are composed only of titanium oxide.
[0027] The average particle diameter of the titanium oxide particles is not particularly limited, but is preferably 0.5 nm or more and 100 nm or less. By having an average particle diameter of 0.5 nm or more and 100 nm or less, harmful gas components are more easily decomposed and the titanium oxide particles are less likely to fall off, compared with the case where the average particle diameter is outside the range. In this specification, the average particle diameter of the titanium oxide particles is the particle diameter at an integrated value of 50% in the volume-based particle size distribution measured by dynamic light scattering (DLS) of the titanium oxide particles supported on the carrier (metal porous body). This average particle diameter can be measured using a commercially available particle measuring device (for example, nanoSAQLA manufactured by Otsuka Electronics Co., Ltd.).
[0028] The amount of titanium oxide particles supported is not particularly limited, but from the viewpoint of further suppressing the falling off of titanium oxide particles, it is set to 100 cm3 of the volume of the support (metal porous body). 3 For a porous metal body, the volume is preferably 0.2 g to 10 g, more preferably 0.2 g to 5 g, and particularly preferably 0.5 g to 3 g. Here, the volume of the porous metal body in this specification means its apparent volume, including the volume of the void portion. In other words, if the porous metal body is in a sheet shape, the volume is the value obtained by multiplying the area of the sheet surface by the thickness, and if it is in a cylindrical shape, the volume is the value obtained by multiplying the vertical cross-sectional area of the circle by the height perpendicular to it, and is a value obtained by arithmetic calculation of the external shape.
[0029] Examples of the tungsten compound supported on the carrier (porous metal body) include tungsten oxide, tungstic acid, sodium tungstate, potassium tungstate, ammonium tungstate parapentahydrate, tungsten carbide, and 12-tungsto(VI)phosphate n-hydrate, and one or more of these can be used.
[0030] Among the above-mentioned tungsten compounds, it is preferable to use a tungsten compound (e.g., tungsten oxide) that exhibits photocatalytic activity as the tungsten compound supported on the support (porous metal body). When a tungsten compound that exhibits photocatalytic activity is used as the tungsten compound supported on the support (porous metal body), in addition to the photocatalytic activity of titanium oxide (titanium oxide particles) supported on the support, the photocatalytic activity of the tungsten compound can be obtained, making it easier to decompose harmful gas components.
[0031] In addition, the tungsten compound supported on the carrier (porous metal body) is more preferably tungsten acid and / or tungsten oxide among the above-mentioned tungsten compounds. When tungsten acid or tungsten oxide is used as the tungsten compound supported on the carrier (porous metal body), the effect of suppressing the detachment of titanium oxide particles from the carrier (porous metal body) is higher than when other tungsten compounds are used.
[0032] Tungstic acid is a hydrate of tungsten trioxide, and is generally known to have a structure of monohydrate (WO3·H2O(H2WO4)) or dihydrate (WO3·2H2O(H4WO5)). However, the tungstic acid that can be supported on a carrier (metal porous body) can have either structure as long as it is a hydrate of tungsten trioxide. It is known that tungstic acid changes to tungsten oxide (VI) by heat treatment at 100℃ or higher.
[0033] Tungsten oxide is an oxide of tungsten, and three types are generally known: tungsten oxide (III) (W2O3), tungsten oxide (IV) (WO2), and tungsten oxide (VI) (tungsten trioxide, chemical formula WO3). Any tungsten oxide may be used as the tungsten oxide that can be supported on the support (metallic porous body) as long as it is an oxide of tungsten, but from the viewpoint of more firmly supporting the titanium oxide particles on the support (metallic porous body), tungsten oxide (VI) is preferable.
[0034] The form of the tungsten compound supported on the carrier (metallic porous body) is preferably in the form of particles, from the viewpoint of further suppressing the detachment of titanium oxide particles from the carrier. In other words, it is preferable that the carrier (metallic porous body) supports particles made of a tungsten compound (hereinafter also referred to as "tungsten compound particles") as the tungsten compound. Note that the tungsten compound particles do not necessarily have to be composed of tungsten compounds alone, and may contain other substances such as substances other than tungsten compounds that are unintentionally generated during the manufacturing process (e.g., metallic tungsten, etc.) and inevitable impurities that are inevitably mixed in during the manufacturing process, but it is preferable that they are composed of tungsten compounds alone.
[0035] The form in which the tungsten compound particles are supported on the support (porous metal body) is not particularly limited, and for example, the tungsten compound particles may be supported on the support (porous metal body) separately from the titanium oxide particles, or the tungsten compound particles may be solidified with the titanium oxide particles to form composite particles and then supported on the support.
[0036] The average particle size of the tungsten compound particles is preferably 0.5 nm or more and 100 nm or less in order to further suppress the falling off of titanium oxide particles from the carrier (metallic porous body). In this specification, the average particle size of the tungsten compound particles is the particle size at 50% of the cumulative value in the volume-based particle size distribution measured by the dynamic light scattering method (DLS method) of the tungsten compound particles supported on the carrier (metallic porous body). This average particle size can be measured using a commercially available particle measuring device (for example, nanoSAQLA manufactured by Otsuka Electronics Co., Ltd.).
[0037] The amount of the tungsten compound supported is not particularly limited, but from the viewpoint of further suppressing the falling off of titanium oxide particles, it is set to 100 cm3 of the volume of the support (metallic porous body). 3 On the other hand, the weight is preferably 0.002 g or more and 0.9 g or less, and more preferably 0.005 g or more and 0.54 g or less.
[0038] In the photocatalytic filter of this embodiment, the content ratio of titanium oxide and tungsten compound (titanium oxide: tungsten compound) constituting the titanium oxide particles is not particularly limited, but is preferably 99:1 to 85:15 by mass ratio, and more preferably 95:5 to 85:15. When the content ratio of titanium oxide and tungsten compound is within this range, the falling off of titanium oxide particles is more easily suppressed compared to when the content ratio of tungsten compound is lower than this range. In addition, although tungsten compounds generally have lower catalytic activity than titanium oxide, when the content ratio of titanium oxide and tungsten compound is within this range, the photocatalytic activity of the photocatalytic filter is higher compared to when it is outside this range or when titanium oxide is used alone in the same amount as the total amount of them.
[0039] The titanium oxide particles and the tungsten compound may be directly supported on the carrier (porous metal body), or may be supported on the carrier (porous metal body) via a binder. When the titanium oxide particles and the tungsten compound are directly supported on the carrier (porous metal body), the titanium oxide particles and the tungsten compound can be supported on the carrier (porous metal body) by, for example, chemical means (e.g., chemical bond) or physical means (e.g., van der Waals force). When the titanium oxide particles and the tungsten compound are supported on the carrier (porous metal body) via a binder, for example, a silane compound such as tetramethoxysilane or tetraethoxysilane can be used as the binder.
[0040] Next, a method for producing the photocatalytic filter of this embodiment will be described.
[0041] The photocatalytic filter of this embodiment can be manufactured by supporting titanium oxide particles and a tungsten compound on a metal porous body. The method of supporting titanium oxide particles and a tungsten compound on a metal porous body can be a conventionally known method, and is not particularly limited.
[0042] Hereinafter, an example of a method for producing a photocatalytic filter (hereinafter also referred to as "catalytic filter A") in which titanium oxide particles and tungsten compound particles are supported on a carrier (porous metal body) will be described in more detail.
[0043] The method for producing the catalytic filter A includes a firing step (hereinafter also simply referred to as the "firing step") of firing a porous metal body coated with a dispersion liquid in which titanium oxide particles and tungsten compound particles are dispersed.
[0044] The dispersion liquid used in the firing step is a liquid in which titanium oxide particles and tungsten compound particles are dispersed, and can be obtained by adding titanium oxide particles and tungsten compound particles to a dispersion medium and mixing them. The dispersion medium to which titanium oxide and tungsten compound are added can be a dispersion medium in which titanium oxide particles and tungsten compound particles do not dissolve (do not dissolve), and for example, water, methanol, ethanol, isopropyl alcohol, methyl ethyl ketone, methyl isobutyl ketone, etc. can be used. Note that the titanium oxide particles and tungsten compound particles may be added to the dispersion medium and then pulverized with a bead mill or the like to adjust their particle size.
[0045] In the dispersion liquid used in the firing step, the content of the titanium oxide particles and the tungsten compound particles can be appropriately set depending on the coating amount of the dispersion liquid on the metal porous body and the amount of the titanium oxide particles and the tungsten compound particles supported on the metal porous body, and is not particularly limited.
[0046] In addition, in the tungsten compound particles contained in the dispersion, the tungsten compound is preferably tungstic acid. That is, the tungsten compound particles contained in the dispersion are preferably tungstic acid particles made of tungstic acid. When the tungsten compound constituting the tungsten compound particles is tungstic acid, it is easier to manufacture a photocatalytic filter in which the falling off of titanium oxide particles is more suppressed compared with the case where a tungsten compound other than tungstic acid is used. Although the reason is not clear, it is considered that the hydration water of tungstic acid is lost by the firing process in the firing process, and at the same time, a stronger bond is formed with titanium oxide or metal porous body.
[0047] The dispersion liquid used in the firing step may contain a binder in addition to the titanium oxide particles and the tungsten compound particles. By containing a binder in the dispersion liquid applied to the metal porous body, the titanium oxide particles and the tungsten compound particles can be supported on the carrier (metal porous body) via the binder. When a binder is used, the binder may be added to the dispersion medium together with the titanium oxide particles and the tungsten compound particles and mixed.
[0048] When using alkoxysilane as a binder, water may be added to the dispersion medium together with the binder, and the mixture may be stirred for several hours to obtain a dispersion liquid in which titanium oxide particles and tungsten compound particles are dispersed. In addition, in order to promote the hydrolysis of alkoxysilane, a small amount of acid such as hydrochloric acid or acetic acid may be added to the dispersion medium before or after the addition of alkoxysilane. It is preferable to use a volatile acid as the acid added to the dispersion medium so that it can be removed by a process such as firing the metal porous body to which the dispersion liquid is applied.
[0049] The metal porous body coated with the dispersion liquid can be obtained by applying the above-mentioned dispersion liquid to a metal porous body that is a filter substrate. The method of applying the dispersion liquid to the metal porous body can be a method known to those skilled in the art, such as a DIp method or a spray method. The metal porous body coated with the dispersion liquid may be fired as it is, or may be fired after removing excess dispersion liquid from the metal porous body coated with the dispersion liquid by leaving it to stand or blowing air, or after drying the metal porous body coated with the dispersion liquid to remove the dispersion medium from the dispersion liquid.
[0050] In the firing process, the firing temperature of the metal porous body to which the dispersion liquid has been applied can be, for example, 100°C or higher and 800°C or lower, and is preferably 300°C or higher and 600°C or lower, as this makes it easier to produce a photocatalytic filter in which the shedding of titanium oxide particles is further suppressed.
[0051] In the firing step, the firing time for the metal porous body to which the dispersion liquid has been applied can be, for example, from 0.5 hours to 5 hours, and is preferably from 1 hour to 3 hours, since this makes it easier to produce a photocatalytic filter in which the shedding of titanium oxide particles is further suppressed.
[0052] In the firing step, the metal porous body coated with the dispersion is fired in an atmosphere such as air.
[0053] By the manufacturing method including the firing step described above, it is possible to manufacture a photocatalytic filter (catalytic filter A) in which titanium oxide particles and tungsten compound particles are supported on a carrier (porous metal body).
[0054] The photocatalytic filter of this embodiment preferably has an ultraviolet light transmittance of 1% or more, and more preferably 1% to 10%. When the ultraviolet light transmittance of the photocatalytic filter of this embodiment is 1% or more, the ultraviolet light irradiated to the photocatalytic filter is more efficiently transmitted to the inside of the carrier (metallic porous body), and the decomposition activity of harmful gas components is higher. On the other hand, when the ultraviolet light transmittance is 10% or less, the ultraviolet light is utilized by exciting titanium oxide, compared to when it exceeds 10%, so that sufficient catalytic activity is more easily obtained.
[0055] The ultraviolet light transmittance of a photocatalytic filter can be determined in accordance with the shading test of JIS L 1055. Specifically, the test can be carried out according to the following procedure. A test box is prepared with a matte black paint applied to the inside and a 100 mm diameter hole drilled at the top, and an illuminometer is placed inside the test box 100 mm from the hole. A UV lamp is placed above the test box, and the illuminance is adjusted to 100,000 ± 5,000 lx. The illuminance is measured when a test piece is placed over the 100 mm diameter hole, and the transmittance is calculated from the following formula (3). Transmittance (%) = {(Illuminance with test piece attached) / (Illuminance without test piece attached)} × 100 (3)
[0056] The ultraviolet light transmittance of the photocatalytic filter decreases when the thickness of the carrier (metallic porous body) is increased, and increases when the porosity of the carrier (metallic porous body) is increased. Therefore, taking these trends into consideration, the thickness and porosity of the carrier (metallic porous body) can be adjusted to achieve the desired ultraviolet light transmittance.
[0057] The photocatalytic filter of this embodiment can be used by circulating the gas to be treated containing harmful gas components through the photocatalytic filter while being irradiated with light including ultraviolet light, so that the gas to be treated containing harmful gas components comes into contact with the titanium oxide particles.
[0058] The gas to be treated that is passed through the photocatalytic filter may contain gas components other than harmful gas components as long as the gas contains harmful gas components. Examples of gas components other than harmful gas components include nitrogen, oxygen, carbon dioxide, water vapor, and inert gases such as argon. The concentration of harmful gas components contained in the gas to be treated is, for example, 0.01 ppm to 10,000 ppm.
[0059] The contact temperature between the gas to be treated and the titanium oxide particles is not particularly limited, but can be, for example, from -40°C to 100°C, and from the viewpoint of more efficiently decomposing harmful gas components, it is preferably from 0°C to 100°C.
[0060] The surface wind speed of the gas to be treated passing through the photocatalytic filter can be, for example, 0.0033 m / s or more and 2.0 m / s or less, and from the viewpoint of more efficiently decomposing harmful gas components, it is preferable that it be 0.0033 m / s or more and 1.0 m / s or less.
[0061] The contact time between the gas to be treated and the titanium oxide particles can be appropriately set taking into consideration the amount of titanium oxide particles supported and the decomposition rate of harmful gas components.
[0062] The photocatalytic filter of this embodiment can also be incorporated into a harmful gas component removal device. An example of a harmful gas component removal device equipped with a photocatalytic filter is a harmful gas component removal device including a flow path through which a gas to be treated containing harmful gas components flows, a photocatalytic filter of this embodiment disposed in the flow path, and a light source that irradiates the photocatalytic filter of this embodiment with light including ultraviolet light. The harmful gas component removal device may be provided with a first heater that heats the gas to be treated and a second heater that heats the photocatalytic filter, as necessary.
[0063] In the photocatalytic filter of the present embodiment described above, titanium oxide particles are supported on a carrier made of a porous metal body, so that the titanium oxide can be excited by irradiation with light including ultraviolet light, and harmful gas components in the gas to be treated flowing through the photocatalytic filter can be decomposed by the titanium oxide. Furthermore, in the photocatalytic filter of the present embodiment, a tungsten compound is supported on the carrier (porous metal body) in addition to the titanium oxide particles, so that the titanium oxide particles are less likely to fall off, and the photocatalytic activity of the titanium dioxide can be maintained for a long period of time.
[0064] In addition, the reason why the tungsten compound is supported on the carrier (porous metal body) and the titanium oxide particles supported on the carrier (porous metal body) are prevented from falling off is not clear, but it is believed that some reaction occurs between the tungsten compound and the metal of the porous metal body, and a strong adhesive layer is formed at the contact interface between the tungsten compound and the metal of the porous metal body. The strong adhesive layer is, for example, a redox reaction proceeds at the contact surface between a tungsten compound with a high oxidation number such as tungsten oxide (VI) and the metal of the porous metal body, and hexavalent tungsten is reduced to trivalent or tetravalent tungsten, while the metal of the porous metal body is oxidized to form a complex oxide layer of the metal of the porous metal body and tungsten, and this layer plays the role of an adhesive layer and firmly bonds the tungsten compound to the metal of the porous metal body. It is presumed that the titanium oxide particles are firmly held by the tungsten compound due to the strong adhesion between the tungsten compound and the porous metal body, and the falling off of the titanium oxide particles is prevented. Furthermore, when tungstic acid or ammonium tungstate is used as the raw material for the tungsten compound, the addition of a firing step is even more preferable, since it promotes the oxidation-reduction reaction between the metal of the metal porous body and tungsten and also has the effect of the aforementioned elimination of hydration water and ammonium ions. EXAMPLES
[0065] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.
[0066] Example 1 Titanium oxide powder (P25: manufactured by Nippon Aerosil) and tungstic acid (H2WO4: manufactured by Nippon Inorganic Chemical Industry Co., Ltd.) were suspended in methanol and dispersed with a bead mill to prepare a slurry (1) containing titanium oxide particles (average particle diameter 50 nm) and tungstic acid particles (average particle diameter 50 nm). The slurry (1) was sprayed and applied to a metal porous body (100 mm x 100 mm x 10 mm, average cell number 25 PPI, porosity 96%) made of Ni-Fe, an alloy of nickel and iron, using a gravity-type hand spray gun, and the metal porous body to which the slurry (1) was applied was baked at 500°C for 1 hour to obtain a photocatalytic filter of Example 1. The photocatalytic filter of this example is one in which titanium oxide particles and tungsten (VI) oxide particles (hereinafter also simply referred to as "tungsten oxide particles") are supported on a metal porous body, and the total amount of titanium oxide particles and tungsten oxide particles supported (volume of metal porous body 100 cm3) was 1000 g / cm3. 3 The amount of supported carbon relative to the amount of supported carbon is shown in Table 1.
[0067] (Examples 2 to 4) Photocatalytic filters of Examples 2 to 4 were obtained in the same manner as in Example 1, except that the amount of slurry (1) applied to the metal porous body was changed. In the photocatalytic filters of Examples 2 to 4, the total amount of titanium oxide particles and tungsten oxide particles supported (per 100 cm of the volume of the metal porous body) was 3 The amount of supported carbon relative to the amount of supported carbon is shown in Table 1.
[0068] Comparative Example 1 Slurry (2) containing titanium oxide particles was prepared in the same manner as slurry (1) prepared in Example 1, except that tungstic acid was not added to the slurry (1) prepared in Example 1, and the same amount of titanium oxide powder was further added. A photocatalytic filter of Comparative Example 1 was obtained in the same manner as Example 1, except that slurry (2) was used instead of slurry (1). In the photocatalytic filter of this comparative example, titanium oxide particles are supported on a porous metal body, and the amount of supported titanium oxide particles (volume of the porous metal body: 100 cm) was 1000 μm. 3 The amount of supported carbon relative to the amount of supported carbon is shown in Table 1.
[0069] (Comparative Examples 2 to 3) Photocatalytic filters of Comparative Examples 2 to 3 were obtained in the same manner as in Comparative Example 1, except that the amount of the slurry (2) applied to the metal porous body was changed. In the photocatalytic filters of Comparative Examples 2 to 3, the amount of titanium oxide particles supported (per 100 cm of the volume of the metal porous body) was 3 The amount of supported carbon relative to the amount of supported carbon is shown in Table 1.
[0070] <Acetaldehyde removal test 1> For Examples 1 to 4 and Comparative Examples 1 to 3, test pieces (100 mm × 50 mm × 10 mm) were taken and subjected to acetaldehyde removal test 1 in accordance with JIS R 1701-2 (acetaldehyde removal performance). The ultraviolet illuminance on the test piece was 10.0 W / m 2 The distance between the light source and the test specimen was adjusted so that the acetaldehyde concentration was 5 ppm in air, and the test gas with a temperature of 25°C and a relative humidity of 50% was passed through the test specimen at a test flow rate (1 L / min. Air velocity at passing surface: 0.0033 m / s) for 3 hours to carry out acetaldehyde removal test 1. The results are shown in Table 1.
[0071] <Peel test> For Examples 1 to 4 or Comparative Examples 1 to 3, test pieces (50 mm x 50 mm x 10 mm) were taken, completely submerged in 200 ml of water, and subjected to ultrasonic irradiation under the following conditions using an ultrasonic cleaner (ASU-10, manufactured by AS ONE). Frequency: 40kHz Irradiation time: 5 minutes
[0072] The weight of the photocatalytic filter was measured before and after ultrasonic irradiation, and the amount of particles peeled off from the photocatalytic filter per test area (mg / cm 2 The test area was the area of the upper surface of the test piece (50 mm × 50 mm). The results are shown in Table 1.
[0073] [Table 1]
[0074] As shown in the results in Table 1, the photocatalytic filters of Examples 1 to 4 had a lower amount of particles peeled off from the photocatalytic filters than the photocatalytic filters of Comparative Examples 1 to 3. It is possible that not only titanium oxide particles but also tungsten oxide particles peeled off from the catalytic filters of Examples 1 to 4, but even if it is assumed that the peeled amount in Examples 1 to 4 shown in Table 1 is the amount of only titanium oxide particles peeled off, it can be seen that the photocatalytic filters of Examples 1 to 4 are less prone to peeling of titanium oxide particles than the photocatalytic filters of Comparative Examples 1 to 3. From this result, it can be seen that the photocatalytic filters of Examples 1 to 4 make it difficult for titanium oxide particles to fall off.
[0075] Furthermore, as shown in Table 1, the photocatalytic filter of Example 1 had a higher aldehyde removal rate than Comparative Example 1, which supported only titanium oxide particles in an amount equal to the total amount of titanium oxide particles and tungsten oxide particles supported. Similarly, the photocatalytic filters of Examples 2 and 4 also had higher aldehyde removal rates than Comparative Examples 2 and 3, which supported titanium oxide particles in an amount equal to the total amount of titanium oxide particles and tungsten oxide particles supported, respectively.
[0076] (Examples 5, 6, 8 to 10) Photocatalytic filters of Examples 5, 6, 8 to 10 were obtained in the same manner as in Example 2, except that the mixing ratio of titanium oxide powder and tungstic acid in the slurry (1) was changed. In the photocatalytic filters of Examples 5, 6, 8 to 10, the total amount of titanium oxide particles and tungsten oxide particles supported (per 100 cm of the volume of the metal porous body) was 3 The amount of supported carbon relative to the amount of supported carbon is shown in Table 2.
[0077] Example 7 A photocatalytic filter was obtained in the same manner as in Example 2. This was used as the photocatalytic filter of Example 7. In the photocatalytic filter of Example 7, the total amount of titanium oxide particles and tungsten oxide particles supported (per 100 cm of the volume of the metal porous body) was 100 g / cm. 3 The amount of supported carbon relative to the amount of supported carbon is shown in Table 2.
[0078] Comparative Example 4 A photocatalytic filter was obtained in the same manner as in Comparative Example 2. This was used as the photocatalytic filter of Comparative Example 4. In the photocatalytic filter of Comparative Example 4, the amount of titanium oxide particles supported (volume of the metal porous body: 100 cm 3 ) was 1000 μm. 3 The amount of supported carbon relative to the amount of supported carbon is shown in Table 2.
[0079] <Acetaldehyde removal test 2> For Examples 5 to 10 and Comparative Example 4, test pieces (50 mm × 50 mm × 10 mm) were taken, and acetaldehyde removal test 2 was carried out in accordance with JIS R 1701-2 (acetaldehyde removal performance). The ultraviolet illuminance on the test piece was 10.0 W / m 2 The distance between the light source and the test specimen was adjusted so that the acetaldehyde concentration was 5 ppm, and the test gas with a temperature of 25°C and a relative humidity of 50% was passed through the test specimen at a test flow rate (3 L / min, passing surface wind speed: 0.02 m / s) for 3 hours to perform acetaldehyde removal test 2. The acetaldehyde removal rate (%) obtained in this test is shown in Table 2.
[0080] <Peel test> For Examples 5 to 10 and Comparative Example 4, test pieces (50 mm x 50 mm x 10 mm) were taken, immersed in 200 ml of water, and irradiated with ultrasonic waves under the following conditions using an ultrasonic cleaner (ASU-10, manufactured by AS ONE). Frequency: 40kHz Irradiation time: 5 minutes
[0081] The weight of the photocatalytic filter was measured before and after ultrasonic irradiation, and the amount of particles peeled off from the photocatalytic filter per test area (mg / cm 2 The test area was the area of the upper surface of the test piece (50 mm × 50 mm). The results are shown in Table 2.
[0082] [Table 2]
[0083] As shown in Table 2, the photocatalytic filters of Examples 5 to 10 had a lower amount of particles peeled off from the photocatalytic filters compared to the photocatalytic filter of Comparative Example 4. It is possible that not only titanium oxide particles but also tungsten oxide particles peeled off from the catalytic filters of Examples 5 to 10, but even if it is assumed that the peeled amount of Examples 5 to 10 shown in Table 2 is the amount of only titanium oxide particles peeled off, it can be seen that the photocatalytic filters of Examples 5 to 10 are less prone to peeling of titanium oxide particles than the photocatalytic filter of Comparative Example 4. From this result, it can be seen that the photocatalytic filters of Examples 5 to 10 make it difficult for titanium oxide particles to fall off.
[0084] Furthermore, as shown in Table 2, the photocatalytic filters of Examples 5 to 10 had higher aldehyde removal rates than Comparative Example 4, which supported only titanium oxide particles in an amount equal to the total amount of titanium oxide particles and tungsten oxide particles. In particular, the acetaldehyde removal rates of Examples 5 to 8 were higher than those of Comparative Example 4 and Examples 9 and 10.
[0085] (Examples 11 to 16) Photocatalytic filters of Examples 11 to 16 were obtained in the same manner as in Examples 5 to 10, except that a nickel porous metal body (100 mm x 100 mm x 10 mm, average cell number 25 PPI, porosity 96%) was used instead of the Ni-Fe porous metal body used in Examples 5 to 10. In the photocatalytic filters of Examples 11 to 16, the total amount of titanium oxide particles and tungsten oxide particles supported (volume of the porous metal body per 100 cm) was 100 g / cm. 3 The amount of supported carbon relative to the amount of supported carbon is shown in Table 3.
[0086] Comparative Example 5 A photocatalytic filter was obtained in the same manner as in Comparative Example 4, except that a nickel porous metal body (100 mm x 100 mm x 10 mm, average cell number 25 PPI, porosity 96%) was used instead of the Ni-Fe porous metal body used in Comparative Example 4. This was used as the photocatalytic filter of Comparative Example 5. In the photocatalytic filter of Comparative Example 5, the amount of titanium oxide particles supported (volume of the porous metal body per 100 cm) was 100%. 3 The amount of supported carbon relative to the amount of supported carbon is shown in Table 3.
[0087] <Acetaldehyde removal test 2> Acetaldehyde removal test 2 was carried out for Examples 11 to 16 and Comparative Example 5 in the same manner as in acetaldehyde removal test 2 carried out using Examples 5 to 10 and Comparative Example 4. The acetaldehyde removal rates (%) are shown in Table 3.
[0088] <Peel test> The peel tests were carried out for Examples 11 to 16 and Comparative Example 5 in the same manner as the peel tests carried out for Examples 5 to 10 and Comparative Example 4. The obtained results are shown in Table 3.
[0089] [Table 3]
[0090] As shown in Table 3, the photocatalytic filters of Examples 11 to 16 had a lower amount of particles peeled off from the photocatalytic filter compared to the photocatalytic filter of Comparative Example 5. It is possible that not only titanium oxide particles but also tungsten oxide particles peeled off from the photocatalytic filters of Examples 11 to 16, but even if it is assumed that the peeled amount of Examples 11 to 16 shown in Table 3 is the peeled amount of titanium oxide particles only, it can be understood that the photocatalytic filters of Examples 11 to 16 are less prone to peeling of titanium oxide particles than the photocatalytic filter of Comparative Example 5. From this result, it can be understood that the photocatalytic filters of Examples 11 to 16 make it difficult for titanium oxide particles to fall off.
[0091] Furthermore, as shown in Table 3, the photocatalytic filters of Examples 11 to 16 had higher aldehyde removal rates than Comparative Example 5, which supported only titanium oxide particles in an amount equal to the total amount of titanium oxide particles and tungsten oxide particles. In particular, the acetaldehyde removal rates of Examples 11 to 14 were higher than those of Comparative Example 5 and Examples 15 and 16.
[0092] From the above, it was understood that the present invention provides a photocatalytic filter that can decompose harmful gas components and suppress the falling off of titanium oxide particles from the metal porous body that is the filter substrate. Furthermore, from the above test results, it was also understood that the photocatalytic filter of the present invention is a photocatalytic filter that maintains catalytic activity for a long period of time.
Claims
1. A carrier made of a porous metal body; Titanium oxide particles and a tungsten compound supported on the support; A photocatalytic filter comprising:
2. 2. The photocatalytic filter according to claim 1, wherein the tungsten compound is tungstic acid and / or tungsten oxide.
3. 2. The photocatalytic filter according to claim 1, wherein the metal porous body contains iron and / or nickel as a metal constituting the metal porous body.
4. 2. The photocatalytic filter according to claim 1, wherein a content ratio of said titanium oxide and said tungsten compound in said photocatalytic filter is from 99:1 to 85:15 in terms of mass ratio.
5. 2. The photocatalytic filter according to claim 1, wherein the porosity of the metal porous body is 80% or more and 99% or less.
6. 2. The photocatalytic filter according to claim 1, wherein the average particle size of the titanium oxide particles is 0.5 nm or more and 100 nm or less.
7. The amount of the titanium oxide particles supported is 100 cm of the volume of the metal porous body. 3 2. The photocatalytic filter according to claim 1, wherein the weight of the photocatalytic filter is 0.2 g or more and 10 g or less.
8. 2. The photocatalytic filter according to claim 1, wherein the ultraviolet light transmittance is 1% or more and 10% or less.
9. A harmful gas component removing device comprising the photocatalytic filter according to any one of claims 1 to 8.
10. A method for producing a photocatalytic filter, comprising a step of firing a metal porous body coated with a dispersion liquid in which titanium oxide particles and tungstic acid particles are dispersed.
Citation Information
Patent Citations
Visible light response type photocatalyst and its production method
JP2006198464A
Photocatalyst and its production method
JP2006198465A
Deodorizing device and deodorizing method
JP2012050979A
Photocatalytic filter for degrading mixed gas efficiently and manufacturing method thereof