Ceramic sliding member and method for manufacturing the same
The ceramic sliding member with Al and vanadium-based non-oxide additives addresses friction and wear issues by forming a self-healing lubricating layer, ensuring high mechanical strength and reduced friction at high temperatures.
Patent Information
- Application Number
- JP2023072185
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
AI Technical Summary
Ceramic sliding members face issues with increased friction and wear in high-temperature environments due to the loss of lubrication and impaired mechanical strength, particularly above 500°C, leading to reduced lifespan.
A ceramic sliding member composed of a ceramic base material containing Al and an oxidizing active non-oxide, such as vanadium-based non-oxide, is manufactured through sintering and heat-treatment in a non-oxidizing atmosphere, forming a self-healing mechanism that generates lubricating oxides to reduce friction and enhance mechanical strength.
The ceramic sliding member achieves high mechanical strength and low friction coefficients at high temperatures, with self-healing properties that restore strength and form a lubricating layer, extending its lifespan and improving sliding performance.
Smart Images

Figure 2024157687000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a ceramic sliding member and a method for producing the same. [Background technology]
[0002] Ceramic materials have excellent heat resistance, high-temperature strength, corrosion resistance, and high-temperature hardness, and are therefore used as sliding components such as bearings in high-temperature environments such as gas turbines. In addition, they are lighter than metallic bearing components and require less energy to operate, so there are high hopes that they will also reduce the environmental impact.
[0003] For example, Patent Document 1 discloses a ceramic rolling bearing material in which 0.5 volume % to 20.0 volume % of cubic ZrO2 is dispersed in an alumina-based matrix with an agglomerated particle size of 10 μm or less to improve mechanical strength.
[0004] On the other hand, the strength of ceramic-based components is very sensitive to defects in the matrix surface layer, and in order to improve the robustness of products, it is necessary to reduce surface defects that occur during the manufacturing process as much as possible. In response to this, so-called oxidation-induced self-healing ceramics have been proposed. In oxidation-induced self-healing ceramics, non-oxides that are highly active against oxidation in high-temperature air are dispersed in the ceramic matrix, and are oxidized at high temperatures by oxygen in the air present outside the matrix, triggered by cracks occurring on the matrix, and the oxides thus generated autonomously fill and bond the cracks, completely recovering the strength, i.e., they have a so-called "self-healing function." Therefore, there are high expectations for the application of oxidation-induced self-healing ceramics to next-generation high-temperature structural components that require high performance and high safety. Patent Document 2 discloses an oxidation-induced self-healing ceramic in which ceramics containing aluminum oxide as a base material are mixed with an oxidation-active non-oxide and a healing promoter, such as magnesium oxide or manganese oxide, to increase the speed required for strength recovery in the self-healing process and lower the temperature required for crack healing, thereby achieving high functionality. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2000-319064 A [Patent Document 2] Patent No. 6436513 Summary of the Invention [Problem to be solved by the invention]
[0006] Although such self-healing ceramics are said to be applicable to various applications where they are used at high temperatures, in reality, they have hardly been used as sliding components to date. Normally, sliding components require lubrication, but when used in an air atmosphere at temperatures above 500°C, polymer-based lubricants evaporate, and the lubricating function itself of solid lubricants such as graphite is lost due to oxidation, so sliding is often forced in an oil-free environment. As a result, the friction coefficient tends to become relatively large, and the increase in temperature of the components due to the increase in frictional heat generated further accelerates wear (galling and shedding) of the surface of the sliding components, resulting in a problem of a shortened lifespan.
[0007] In order to solve the above-mentioned problems, an object of the present invention is to provide a ceramic sliding member or the like that can ensure high mechanical strength and reduce the coefficient of friction at high temperatures. [Means for solving the problem]
[0008] The ceramic sliding member of the present invention comprises an Al-containing ceramic base material and an oxidation-active non-oxide dispersed in the base material, and the non-oxide has a PB ratio represented by the following (1) of 1.0 or more. P-B ratio = volume of oxide per metal ion / volume per metal atom (1) The non-oxide is preferably a V-based non-oxide.
[0009] Furthermore, the method for producing a ceramic sliding member of the present invention includes a step of sintering a mixture of an Al-containing ceramic base material powder and an oxidation-active non-oxide powder in a non-oxidizing atmosphere to obtain a sintered body, and a step of processing the sintered body into a predetermined shape to obtain a processed body. The non-oxide is preferably a V-based non-oxide. It is preferable that the method further comprises a step of heat treating the processed body at 500°C to 800°C in an air atmosphere. Effect of the Invention
[0010] According to the present invention, it is possible to provide a ceramic sliding member and the like which can ensure high mechanical strength and reduce the coefficient of friction at high temperatures. [Brief description of the drawings]
[0011] [Figure 1] Three-point bending strength of Al2O3 / 10.0vol%VC material [Diagram 2] SEM-EDX and TEM images of the healed area of Al2O3 / 10.0vol%VC material [Diagram 3] Relationship between temperature and friction coefficient in pin-on-disk tests for Al2O3 material (comparison example) and Al2O3 / 10.0 vol% VC material (Example 1) [Figure 4] High-temperature in-situ powder XRD of Al2O3 / 10.0vol%VC material (Example 1) [Diagram 5] In-situ high-temperature observation of Al2O3 / 10.0vol%VC material (Example 1) [Figure 6] Optical microscope image of the component surface after heat treatment at 700℃ for 10 minutes [Figure 7] Relationship between sliding speed and friction coefficient of Al2O3 / 10.0vol%VC material in a 500℃ environment (Stribeck curve) [Figure 8] Relationship between sliding speed and friction coefficient of Al2O3 / 10.0vol%VC material in 700℃ environment (Stribeck curve) DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described.
[0013] The ceramic sliding member of the present invention comprises a ceramic base material containing Al and an oxidation-active non-oxide dispersed in the base material, the non-oxide having a PB ratio of 1.0 or more. The non-oxide is preferably a V-based non-oxide.
[0014] Furthermore, the method for producing a ceramic sliding member of the present invention includes a step of sintering a mixture of an Al-containing ceramic base material powder and an oxidation-active non-oxide powder in a non-oxidizing atmosphere to obtain a sintered body, and a step of processing the sintered body into a predetermined shape to obtain a processed body. The non-oxide is preferably a V-based non-oxide. It is preferable that the method further comprises a step of heat treating the processed body at 500°C to 800°C in an air atmosphere.
[0015] Next, the configuration according to the present invention will be described in detail. The ceramic sliding member of the present invention is a self-healing (self-repairing) material. As a mechanism of self-healing, when a crack occurs in a ceramic base material, an oxidatively active non-oxide dispersed inside the base material reacts with oxygen in the air in a high-temperature environment to generate an oxide, which fills the crack and restores strength. For example, when the non-oxide is a vanadium (V)-based compound, the vanadium-based non-oxide oxidizes in a high-temperature environment to become a glass based on vanadium oxide as a main component, which fills the crack and restores strength. In addition, the ceramic sliding member is applied to a member in which members slide against each other in a high-temperature environment. In other words, the ceramic sliding member can be used in a high-temperature environment of 500°C or higher. For example, the sliding member can be applied to bearings used at 500°C or higher, casting cores, brake materials, etc.
[0016] [Ceramics base material] The ceramic base material is preferably one that can withstand high temperatures, and examples of such materials include alumina (Al2O3), sialon (SiAlON), zirconia (ZrO2), etc. In order to prevent unnecessary oxidation of non-oxides dispersed inside the base material, it is preferable for the base material to contain Al, which has low oxygen permeability, and alumina is particularly preferable.
[0017] [Non-oxide] An oxidatively active non-oxide has the ability to undergo an oxidation reaction with oxygen to form an oxide when it comes into contact with the oxygen. At this time, it may be combined with the ceramic base material described above to form a compound such as glass. Examples of the non-oxide include nitrides, carbides, and carbonitrides. In addition, since the formed oxide functions as a lubricant, it is desirable for the non-oxide to have a Pilling-Bedworth ratio (PB ratio) shown in the following formula (1) of 1.0 or more, and more desirably a PB ratio of more than 2.0. In particular, those having a PB ratio of 2.5 or more such as NbC (niobium carbide), NbN (niobium nitride), TaC (tantalum carbide), and TaN (tantalum nitride) in which the metal ion is Nb (PB ratio: 2.68) or Ta (PB ratio: 2.50) are more preferable, and those having a PB ratio of 3.0 or more such as VC (vanadium carbide) and VN (vanadium nitride) in which the metal ion is V (PB ratio: 3.19) (referred to as V-based non-oxides) are particularly preferable. If the PB ratio is large, the volume increase due to oxidation becomes large, so that a sliding layer made of oxides that exhibits a friction reducing effect at high temperatures can be more reliably formed. In addition, it is preferable that the material has a glass transition temperature at a lower temperature side than the operating temperature range, and it is preferable that the oxide is an oxide that takes a layered structure material that does not interfere with the lubricating state as a solid lubricant even if it crystallizes. P-B ratio = volume of oxide per metal ion / volume per metal atom (1) (=molar volume of metal oxide / molar volume of metal)
[0018] [Composition ratio] For non-oxides with a PB ratio higher than 1.0, such as VC, VN, NbC, NbN, TaC, and TaN, the amount of oxides with lubricating properties increases as the amount of added increases. Therefore, it is preferable that the ceramic base material contains 1.0 vol% or more of oxidatively active non-oxides, and particularly 3.0 vol% or more. On the other hand, if the amount added is too large, it may cause the surface roughness of the base material to deteriorate and the components to malfunction due to dimensional changes. For this reason, the amount of non-oxides added is preferably 20.0 vol% or less, and more preferably 10.0 vol% or less.
[0019] Next, a method for producing the ceramic sliding member will be described. The method for producing the ceramic sliding member includes a step of sintering a mixture of an Al-containing compound powder and an oxidation-active non-oxide powder, for example, a V-containing compound powder, in a non-oxidizing atmosphere to obtain a sintered body, and a step of processing the sintered body into a predetermined shape to obtain a target processed body.
[0020] First, a process for obtaining a sintered body by sintering a mixture of an Al-containing compound powder and an oxidatively active non-oxide powder in a non-oxidizing atmosphere will be described. In the following description, an example will be shown in which a V-containing compound powder is used as the non-oxide powder, but the same applies to other metals. The powder containing Al is a raw material that becomes the ceramic base material in the sintered body. For example, alumina can be used, and the powder properties should take into consideration dispersibility with non-oxides and densification during molding. Similarly, the compound powder containing V is a raw material that is a non-oxide. In order to achieve both the effect of reducing the friction coefficient of the sliding surface and strength, for example, it is desirable that the non-oxide powder is less than 10.0 times the average particle size of the base material particles obtained by measurement in accordance with JISZ8825:2013 "Particle size analysis - laser diffraction and scattering method". In sintering in a non-oxidizing atmosphere, for example, sintering can be performed in an atmosphere of argon or nitrogen, and an argon atmosphere is particularly preferable. In order to increase the reactivity when contacting oxygen, it is preferable to make the mixture uniformly dispersed. For this, it is preferable to use a grinding mix using media such as a ball mill. If it is mixed in a wet manner, in the subsequent drying process, a method that takes into consideration the grinding particle size and shape after drying is preferable in order to obtain a high density during sintering. In addition, in sintering, sintering with pressure such as hot pressing can be performed to obtain a high density.
[0021] Next, the sintered body is processed into a predetermined shape to obtain a processed body such as a sliding member, etc. There are no particular limitations on the processing method for processing into the predetermined shape, but high-speed processing using a grinding machine or the like is preferable.
[0022] Subsequently, a step of heat treating the processed body in an oxidizing atmosphere may be included. This heat treatment can further improve the sliding properties when used as a ceramic sliding member. The heat treatment is preferably performed under conditions in which the V-based non-oxide is oxidized to layered V2O5, and the oxygen partial pressure is 1.0×10 -4 Pa or more, and more preferably 1.0×10 4 Pa or higher is preferable. By arranging the sliding surface of the sliding member so that oxygen is in contact with it, it is preferable to prevent impurities from being mixed into the sliding surface and to facilitate the supply of oxygen to surface defects. The heat treatment temperature can be in the range of 500°C to 1300°C, and in the case of a V-based non-oxide additive system, the air atmosphere is preferably 500°C to 800°C, and particularly 700°C to 750°C. The high-temperature holding time is preferably determined depending on the level of the heat treatment temperature, and for example, when heat treatment is performed at 700°C in the air atmosphere, the high-temperature holding time can be in the range of 1 minute to 1 hour.
[0023] The mechanism of the reduction in the coefficient of friction (improvement of lubrication properties) in the ceramic sliding member of the present invention will be described. For example, when a V-based non-oxide is heated, oxides of VO2 begin to be generated at a temperature of about 500°C, and when the temperature exceeds 500°C, it becomes crystals of V2O5 having a layered structure. Such a layered structure has a friction coefficient reduction effect due to the effect of solid lubrication caused by sliding between the layered structures. When further heated, V2O5 melts at about 700°C or higher. In other words, the sliding surface can be uniformly covered with molten V2O5, so it can function as a fluid lubrication. It can be used without any problems at normal operating temperatures of 1300°C or lower, which is lower than the vaporization temperature of V2O5 (1750°C).
[0024] In this way, when a V-based non-oxide is used, theoretically, V2O5, a layered structure material, is used as a lubricant, and when the melting point is reached (approximately 700°C or higher in the air atmosphere), it is expected to behave as a fluid lubricant, and when the melting point is not reached (approximately less than 700°C in the air atmosphere), it is expected to behave as a solid lubricant as a layered structure material. This is expected to contribute to improving the lubricating properties even in an environment with severe temperature cycles. In addition, by performing a heat treatment in advance at a temperature above the layer crystallization temperature of V2O5, or even above the melting temperature of V2O5, a lubricating layer can be formed on the sliding surface in advance, so that high lubricating properties can be exhibited. In other words, it is desirable that an oxide (preferably a crystal with a layered structure) in which a non-oxide is oxidized is formed on the surface layer of the sliding member.
[0025] In this case, if the PB ratio of the non-oxide is less than 1.0, when the oxide is generated from the dispersion state of the non-oxide, the volume is reduced, so it is difficult to form a uniform lubricating layer on the sliding surface. However, if the PB ratio is 1.0 or more, a lubricating layer of oxides at least equivalent to the dispersion state of the non-oxide can be formed, and if the PB ratio is higher, it is possible to more reliably cover the entire sliding surface with the lubricating layer. For example, if the PB ratio is 2.5 or more, or even 3.0 or more, it is more effective because it is possible to cover most of the sliding surface with the lubricating layer and to increase the thickness of the lubricating layer.
[0026] In addition, non-oxides other than V-based ones can also exhibit similar effects in the temperature range in which the layered oxide forms and the melting temperature range of the oxide. For this reason, it is desirable to select a non-oxide that is suitable for the operating temperature range and has a high PB ratio. EXAMPLES
[0027] The Al2O3 material was used as a comparative example, and the Al2O3 / 10.0 vol% VC material (PB ratio of V: 3.19) was used as Example 1. The self-healing properties were confirmed by a three-point bending strength test, and the self-lubricating properties were confirmed by a high-temperature friction and wear test. However, only the Al2O3 / 10.0 vol% VC material was used to confirm the self-healing properties.
[0028] [Confirmation of self-healing properties through three-point bending strength test] First, the raw materials were weighed out so that Al2O3 was 90.0 vol% and VC was 10.0 vol%. As the raw materials, alumina (Al2O3) powder was AKP-20 manufactured by Sumitomo Chemical Co., Ltd., and vanadium carbide (VC) powder was manufactured by Nippon Shin Kinzoku Co., Ltd. After weighing, these powders were wet mixed for 24 hours using an alumina ball and a mill pod and 2-propanol as a mixed solvent. The mixed slurry was dried at 200°C for at least 2 hours in an air blowing environment, and the obtained dried powder was hot-pressed and sintered under the specified conditions (atmosphere: Ar gas, holding temperature: 1600°C, load pressure: 40MPa, holding time: 1 hour, heating rate: 10°C / min, cooling rate: 5°C / min), and a sintered body containing 10.0 vol% VC in the alumina matrix was produced, measuring approximately 40 mm x 40 mm x t5 mm. The obtained sintered body was ground and polished to obtain a bending test piece of 3 mm x 4 mm x 40 mm in accordance with JIS standard R1601 "Room temperature bending strength test of fine ceramics".
[0029] The test pieces were classified into three types [As material (base material), Damage material (pre-cracked material), and Heal material (self-healing heat-treated material)]. The Damage material and Heal material were subjected to Vickers marks (test load: 2kgf, holding time: 10sec) using a Future Tech microhardness tester, and the Heal material was subjected to self-healing heat treatment at 700℃ for 10 minutes in air using a muffle furnace with a heating rate of 10℃ / min. The SEM-EDX observation of the healed Vickers marks was performed using a JEOL FE-SEM 7001-F, and the TEM observation of the healed area was performed using a JEOL The ARM-200F was used.
[0030] Figure 1 shows the three-point bending strength of Al2O3 / 10.0vol% VC material (Example 1). In the figure, "As" is the strength of the base material, "Damage" is the strength of the pre-cracked material, and "Heal" is the strength of the self-healing heat-treated material, all of which are average values of n=4. The strength of the As material was about 700MPa, the strength of the Damage material was about 200MPa, and the strength of the Heal material was about 240MPa. The oxide formed by the V-based non-oxide also plays the role of a lubricant, and it is expected that the strength recovery by the self-healing heat treatment at 700°C for 10 minutes in an air atmosphere will recover surface defects moderately (about 40MPa) without causing the sliding surface to adhere strongly. From this, it was inferred that it is possible to use both strength recovery and self-lubrication.
[0031] FIG. 2 shows an SEM-EDX image (accelerating voltage: 15 kV) and a TEM image (accelerating voltage: 200 kV) of the healed part of the Al2O3 / 10.0 vol% VC material (Example 1). From the SEM-EDX observation, it was confirmed that the crack part 2 introduced by the Vickers mark 1 was filled with a V-based compound. In addition, from the diffraction spots of the healed part 3 and the substrate in the TEM image, a diffraction spot of Al2O3
[0012] from the substrate and a strong diffraction spot of V2O5
[0112] from the healed part 3 (including the diffraction spots of the surrounding phase) were confirmed, and it was found that the healed part 3 was crystallized. From the above, it was revealed that the healing component of the Al2O3 / 10.0 vol% VC material is V2O5 crystal.
[0032] [Confirmation of lubrication effect through high-temperature friction and wear testing] A sintered body was obtained in the same manner as the specimen for the three-point bending test (Example 1). A pin shape of φ20×11 mmt and a disk shape of φ50 mm×5 mmt were obtained from the sintered body by grinding and polishing. The surface roughness of three points on the disk was measured using a SurfCorder SE800 manufactured by Kosaka Laboratory, and it was confirmed that the arithmetic mean roughness Ra=0.20±0.01 μm was a quasi-mirror surface. The obtained pins and disks were manufactured by Bruker. A pin-on-disk test (load: 5N, sliding speed: 5.24mm / sec, temperature: 100℃-800℃) was carried out using a multi-function testing machine UMT TriboLab. The friction coefficient was calculated by averaging the friction coefficients for 30 seconds (15-45 seconds) out of a test time of 60 seconds. A similar test was also carried out on the Al2O3 material of the comparative example. For the in-situ high-temperature powder XRD of the Al2O3 / 10.0 vol% VC material, a Rigaku SmartLab was used, and continuous XRD measurements were performed under the following conditions: heating temperature: 750°C, holding time: 10 min, heating rate: 10°C / min, cooling rate: 20°C / min, 2θ: 10° to 80°. For the in-situ high-temperature observation of the Al2O3 / 10.0 vol% VC material, a Linkam high-temperature heating stage and an OLYMPUS optical microscope were used. Using SZX12, continuous optical microscope observation was performed under the following conditions: heating temperature: 1000°C, holding time: 10 min, heating rate: 10°C / min, and cooling rate: 30°C / min.
[0033] The relationship between temperature and friction coefficient in a pin-on-disk test for the Al2O3 material (comparative example) and the Al2O3 / 10.0 vol% VC material (Example 1) is shown in Figure 3. The Al2O3 material (comparative example) showed a friction coefficient of about 0.6 at all temperatures, but the Al2O3 / 10.0 vol% VC material (Example 1) showed a decrease in friction coefficient from around 500°C, and showed the lowest friction coefficient of 0.2 at around 700°C to 750°C.
[0034] Figure 4 shows the high-temperature in-situ powder XRD of Al2O3 / 10.0 vol% VC material (Example 1). Figure 4 shows the XRD results from room temperature to 750°C heating to 400°C cooling from bottom to top. At the start of the heating, the diffraction peaks of Al2O3 and VC were confirmed, but the diffraction peaks of VO2 appeared at around 480°C to 600°C, and the diffraction peaks of V2O5 appeared at around 530°C to 730°C. The peaks of V2O5 disappeared while the material was held at 750°C. From the above, it is estimated that the oxidation reaction of VC to VO2 occurred around 480°C, and the oxidation reaction of VO2 to V2O5 occurred around 530°C, and V2O5 reached its melting point at 750°C and melted. Furthermore, by comparing the results with those in Figure 3, it is clear that the precipitation of solid phase VO2 and V2O5 at around 500℃ reduces the friction coefficient from 0.6 to 0.4 or less, and the melting of V2O5 at over 700℃ reduces the friction coefficient to 0.2 or less. In other words, it is possible to demonstrate excellent self-lubricating properties at high temperatures.
[0035] Figure 5 shows the in-situ observation of Al2O3 / 10.0vol%VC material (Example 1) at high temperature. Figure 5 shows the in-situ observation results from room temperature to 750℃ heating to 610℃ cooling from bottom to top. At the start of heating, a bright spot pattern originating from the added VC was confirmed in the Al2O3 base material, but the bright spot pattern disappeared around 500℃ heating, and a low brightness spot pattern appeared around 600℃ heating. After heating passed 700℃, the behavior of liquid substances precipitating on the surface layer was confirmed, and the behavior of these liquid substances immediately solidifying around 610℃ cooling was confirmed. By comparing the above surface oxidation behavior with Figure 3, it is estimated that the initial oxidation of VC to VO2 around 500℃, the rate-limiting precipitation of solid phase V2O5 around 600℃, and V2O5 melting after 700℃. Similar to the results of in situ high-temperature powder XRD, these results, when compared with the results in Figure 4, make it clear that the precipitation of solid phase VO2 and V2O5 at around 500°C reduces the friction coefficient from 0.6 to 0.4 or less, and the melting of V2O5 at over 700°C reduces the friction coefficient to 0.2 or less. In other words, it is possible to exhibit excellent self-lubricating properties at high temperatures.
[0036] [Confirmation of the effect of heat treatment on self-lubricating properties] The Al2O3 / 10.0 vol% VC material was evaluated in the case where heat treatment at 700°C in air was performed (Example 2) and in the case where heat treatment was not performed (Example 1). Figure 6 is an optical microscope image of the surface of the member after heat treatment at 700°C for 10 minutes. After heat treatment, a speckled structure was formed on the surface layer by layered brownish precipitates (arrows in the enlarged view on the right). The brownish precipitates were presumed to be oxides formed by V-based non-oxides from SEM-EDX observation, and in combination with the results shown in Figures 4 and 5, they are considered to be V2O5. In order to reliably form V2O5 instead of VO2 even after cooling, it is desirable to set the cooling rate after heat treatment to 20°C or more.
[0037] In addition, the results of the pin-on-disk test (load: 5N, sliding speed: 0.0-52.4mm / sec, temperature: 500°C, 700°C) were compared between the case where the heat treatment at 700°C in the air atmosphere was performed (Example 2) and the case where the heat treatment was not performed (Example 1) for the Al2O3 / 10.0vol%VC material. The relationship between the sliding speed and the friction coefficient of the Al2O3 / 10.0vol%VC material in the 500°C and 700°C environments is shown in Figs. 7 and 8, respectively. A in Figs. 7 and 8 shows the result of performing the heat treatment at 700°C for 10 minutes (Example 2), and B shows the result of not performing the heat treatment (Example 1). The average friction coefficient at the test temperature of 500°C shown in Fig. 7 was 0.34 when the heat treatment was performed (Example 2) and 0.54 when the heat treatment was not performed (Example 1). The average friction coefficient at a test temperature of 700° C. shown in FIG. 8 was 0.16 when heat treatment was performed and 0.22 when no heat treatment was performed.
[0038] Thus, it was revealed that by subjecting the components to heat treatment at 700°C in an air atmosphere, the friction coefficient during use is reduced and the sliding characteristics are significantly improved. In particular, for use at 500°C to 700°C, a higher effect can be obtained by forming a layer of V2O5 on the surface by heat treatment in advance (by forming more V2O5 than VO2). This is presumably due to the precipitation of oxides formed by V-based non-oxides that are sufficient to form a lubricating film around the components during heat treatment. Note that for use at 700°C or higher, the same effect can be obtained by forming a layer of V2O5 during use even without heat treatment, but by performing heat treatment in advance, a stable friction coefficient can be obtained from the beginning of use.
[0039] From the above, it was confirmed that the Al2O3 / 10.0vol% VC material showed a strength recovery of approximately 40MPa after heat treatment at 700℃ for 10 minutes in an air atmosphere, and also that the friction coefficient was reduced (minimum 0.2) due to vanadium oxides (VO2, V2O5) that precipitated at 500℃ or higher. In other words, it was confirmed that the high-temperature oxidation of VC improved mechanical strength through strength recovery (suppression of strength deterioration) and reduced the friction coefficient (high sliding properties), and that it achieved both self-healing and self-lubricating properties when used in sliding components such as bearings. [Explanation of symbols]
[0040] 1. Vickers marks 2. Introduced crack 3. Healing Department 4. Location of Al2O3 diffraction spot acquisition 5. Location of diffraction spots of the healed area 6···VC 7. Liquid Precipitate 8. Solidified liquid precipitate
Claims
1. The present invention includes a ceramic matrix containing Al, and an oxidation-active non-oxide dispersed in the matrix, The ceramic sliding member is characterized in that the non-oxide has a PB ratio represented by the following (1) of 1.0 or more. PB ratio = oxide volume per metal ion / volume per metal atom (1)
2. 2. The ceramic sliding member according to claim 1, wherein the non-oxide is a V-based non-oxide.
3. A method for producing a ceramic sliding member according to claim 1, comprising the steps of: A step of sintering a mixture of a ceramic base material powder containing Al and a non-oxide powder having oxidation activity in a non-oxidizing atmosphere to obtain a sintered body; A step of processing the sintered body into a predetermined shape to obtain a processed body; 2. A method for producing a ceramic sliding member comprising the steps of:
4. 4. The method for producing a ceramic sliding member according to claim 3, wherein the non-oxide is a V-based non-oxide.
5. 5. The method for producing a ceramic sliding member according to claim 3, further comprising a step of heat treating the processed body at 500° C. to 800° C. in an air atmosphere.
Citation Information
Patent Citations
Shock absorber
JP1989036513A
Ceramic material, rolling bearing and cutting tool using the same and production of the ceramic material
JP2000319064A