Additive granulated material and method for producing plastic composition

Additive granules with a specific crystal structure of phenolic antioxidants, combined with phosphorus and sulfur antioxidants, address the issue of fluidity loss in phenolic antioxidant granules, ensuring stable and uniform blending with plastics.

JP2024157693AInactive Publication Date: 2024-11-08SUMITOMO CHEM CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023072195
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The fluidity of granules containing 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5·5]undecane, a phenolic antioxidant, deteriorates over time, especially during transportation and storage, making it difficult to handle and blend effectively in plastics.

Method used

The development of additive granules comprising a specific crystal structure of the phenolic antioxidant with sharp X-ray diffraction peaks at 2θ=4.2° and 2θ=10.6°, optimized with a ratio of phenolic antioxidant (1-1-1) to maintain fluidity, and optionally combined with phosphorus and sulfur antioxidants, along with other additives, to enhance stability and processing.

Benefits of technology

The additive granules maintain excellent fluidity even after storage, facilitating uniform dispersion and blending with plastics, thereby improving the handling and processing stability of phenolic antioxidants in plastic compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157693000001_ABST
    Figure 2024157693000001_ABST
Patent Text Reader

Abstract

To provide a granulated material containing 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, the granulated material exhibiting excellent flowability.SOLUTION: An additive granulated material is formed from a composition (A) containing an antioxidant (a) containing a phenolic antioxidant (1), and contains 40-100 mass% of a phenolic antioxidant (1-1-1) with respect to the total amount of the phenolic antioxidant (1). The phenolic antioxidant (1-1-1) is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystal structure exhibiting sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6°, as measured by powder X-ray diffraction using X-rays having a Cu-Kα wavelength.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an additive granule and a plastic composition. [Background technology]

[0002] 3,9-Bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5·5]undecane is a hydroxyphenylpropionic acid ester known as a phenolic antioxidant, and is known to have an ε, δ, αβ, or γ crystal structure (Patent Document 1).

[0003] Among these, the ε crystal has a crystal structure that shows a sharp X-ray diffraction peak at a diffraction angle 2θ=7.9° in X-ray diffraction measurement, and a powder of the ε crystal hydroxyphenylpropionic acid ester is also known (Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-87860 [Patent Document 2] JP 2015-157853 A Summary of the Invention [Problem to be solved by the invention]

[0005] 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5·5]undecane has an excellent antioxidant effect, but when the phenolic antioxidant is added to plastics and used as a granule, the fluidity of the granule may be deteriorated. In particular, such granules are often used after a certain period of time has passed since production, such as when they are transported or stored in a warehouse, and it has been found that the fluidity of the granules may be deteriorated during such storage periods. Therefore, the present invention aims to provide a granule containing 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5·5]undecane, which has good fluidity. [Means for solving the problem]

[0006] The present inventors conducted a detailed study on factors affecting the fluidity of a granulated product and found that the crystal structure of the phenolic antioxidant affects the fluidity of a granulated product, thereby completing the present invention.

[0007] That is, the present invention includes the following preferred embodiments. [1] An additive granule formed from a composition (A) containing an antioxidant (a) containing a phenolic antioxidant (1), the additive granule containing 40 to 100 mass% of the phenolic antioxidant (1-1-1) which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystal structure which shows sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6° in X-ray diffraction measurement using X-rays of Cu-Kα wavelength. [2] The additive granule according to [1], wherein the content of the phenolic antioxidant (1-1-1) is 40 to 100 mass% based on the total amount of the phenolic antioxidant (1-1), which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, contained in the phenolic antioxidant (1). [3] The additive granule according to [1] or [2], wherein in the phenolic antioxidant (1), the ratio of the amount of the phenolic antioxidant (1-1-1) to the amount of the phenolic antioxidant (1-1-2) which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystal structure showing a sharp X-ray diffraction peak at a diffraction angle 2θ=7.9° in X-ray diffraction measurement using X-rays of Cu-Kα wavelength is (1-1-1):(1-1-2)=100:0 to 40:60. [4] The additive granule according to any one of [1] to [3], wherein the amount of the phenol-based antioxidant (1) contained in the composition (A) is 2 to 30 mass% based on the total amount of the composition (A). [5] The additive granule according to any one of [1] to [4], wherein the amount of the antioxidant (a) contained in the composition (A) is 25 to 100 mass% based on the total amount of the composition (A). [6] The additive granule according to any one of [1] to [5], wherein the antioxidant (a) further contains a phosphorus-based antioxidant (2) and / or a sulfur-based antioxidant (3). [7] The additive granule according to [6], wherein the total amount of the phenol-based antioxidant (1), and the phosphorus-based antioxidant (2) and / or the sulfur-based antioxidant (3) contained in the composition (A) is 25 to 100 mass% based on the total amount of the composition (A). [8] The additive granule according to [6] or [7], wherein the amount of the phenol-based antioxidant (1) is 5 to 30 mass% and the total amount of the phosphorus-based antioxidant (2) and / or the sulfur-based antioxidant (3) is 70 to 95 mass% based on the total amount of the antioxidant (a). [9] The additive granule according to any one of [6] to [8], wherein the amount of the phenol-based antioxidant (1) is 10 to 15 mass%, the amount of the phosphorus-based antioxidant (2) is 48 to 53 mass%, and the amount of the sulfur-based antioxidant (3) is 35 to 40 mass%, relative to the total amount of the antioxidant (a).

[10] The additive granule according to any one of [1] to [9], wherein the composition (A) further contains at least one additive selected from the group consisting of a neutralizing agent, a lubricant, a hindered amine light stabilizer, an ultraviolet absorber, a metal soap, an antistatic agent, an antiblocking agent, a pigment, a flame retardant, a filler, a nucleating agent, a plasticizer, a processing aid, a foaming agent, and an emulsifier.

[11] The additive granule according to any one of [1] to

[10] , wherein the additive granule has a median diameter (by mass) of 0.1 to 7 mm.

[12] A method for producing a plastic composition, comprising a step of blending 0.005 to 10 parts by mass of the additive granule according to any one of [1] to

[11] with respect to 100 parts by mass of plastic.

[13] The method for producing a plastic composition according to

[12] , wherein the plastic is a thermoplastic resin.

[14] A method for producing a plastic composition according to claim

[12] , wherein the plastic is a polyolefin resin. Effect of the Invention

[0008] According to the present invention, it is possible to provide a granulated product containing 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5·5]undecane, which has good fluidity. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a diagram showing the results of X-ray diffraction measurement of compound (1-1-1) used in the examples using X-rays with a Cu-Kα wavelength. [Diagram 2] FIG. 2 is a diagram showing the results of X-ray diffraction measurement of compound (1-1-2) used in the examples using X-rays with a Cu-Kα wavelength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention. In addition, when multiple upper and lower limit values ​​are described for a specific feature, any upper and lower limit values ​​can be combined to form a suitable numerical range.

[0011] The additive granule of the present invention is a granule formed from a composition (A), and the composition (A) contains at least one or more phenolic antioxidants (1) as an antioxidant (a). The phenolic antioxidant (1) contains 40 to 100 mass% of the total amount of the phenolic antioxidant (1-1-1), which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5·5]undecane having a crystal structure that shows sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6° in X-ray diffraction measurement using X-rays of Cu-Kα wavelength. In addition, 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, which has a crystal structure that shows sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6°, has a δ crystal structure, and this compound in the δ crystal form is referred to as a phenolic antioxidant (1-1-1) in this specification.

[0012] It has been surprisingly found that the fluidity of the additive granules is improved by containing a specific amount of the phenolic antioxidant (1-1-1) in the phenolic antioxidant (1) in the composition (A) forming the additive granules. It has also been found that the fluidity of the additive granules can be maintained even after a certain period of time has passed since the production of the granules.

[0013] [Antioxidants (a)] (Phenol-based antioxidants (1)) In the present invention, the composition (A) contains an antioxidant (a) containing at least a phenol-based antioxidant (1). The phenol-based antioxidant (1) is, for example, a phenol-based antioxidant represented by the formula (I): [ka] The phenolic antioxidant (1-1) is represented by the formula: 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5·5]undecane (1-1). As described in JP-A-6-87860, the phenolic antioxidant (1-1) is known to have crystal structures such as δ crystals that show sharp X-ray diffraction peaks at diffraction angles of 2θ=4.2° and 2θ=10.6°, ε crystals that show sharp X-ray diffraction peaks at diffraction angles of 2θ=7.9°, αβ crystals that show sharp X-ray diffraction peaks at diffraction angles of 2θ=2.8°, 2θ=8.7°, and 2θ=11.7°, and γ crystals that do not show any specific X-ray diffraction peaks, in X-ray diffraction measurements using X-rays of Cu-Kα wavelength. In this specification, among the phenolic antioxidants (1-1) represented by formula (I), a δ-crystalline compound having a crystal structure showing sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6° is also referred to as a phenolic antioxidant (1-1-1), an ε-crystalline compound having a crystal structure showing sharp X-ray diffraction peaks at diffraction angles 2θ=7.9° is also referred to as a phenolic antioxidant (1-1-2), an αβ-crystalline compound having a crystal structure showing sharp X-ray diffraction peaks at diffraction angles 2θ=2.8°, 2θ=8.7°, and 2θ=11.7° is also referred to as a phenolic antioxidant (1-1-3), and a γ-crystalline compound having a crystal structure showing no specific X-ray diffraction peak is also referred to as a phenolic antioxidant (1-1-4). Note that the phenolic antioxidants having the crystal structures showing the specific X-ray diffraction peaks are each a single crystal system and usually have a specific melting point. Specifically, the melting point of the δ-crystalline phenolic antioxidant (1-1-1) having a crystal structure showing sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6° is usually about 124 to 127° C. Similarly, the melting point of the phenolic antioxidant (1-1-2) is usually about 116 to 119° C., the melting point of the phenolic antioxidant (1-1-3) is usually about 104 to 109° C., and the melting point of the phenolic antioxidant (1-1-4) is usually about 45 to 55° C.

[0014] The composition (A) may contain, as the antioxidant (a), one type of phenol-based antioxidant, two or more types of phenol-based antioxidants, or an antioxidant other than a phenol-based antioxidant, but it at least contains a compound represented by formula (I) in a δ crystal form having a crystal structure showing sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6°, i.e., a phenol-based antioxidant (1-1-1).

[0015] The amount of the phenolic antioxidant (1-1-1) relative to the total amount of the phenolic antioxidant (1) contained in the composition (A) is 40 to 100% by mass. If the amount is less than 40% by mass, it becomes difficult to obtain the effect of improving the fluidity of the granulated material by the phenolic antioxidant (1-1-1). The amount of the phenolic antioxidant (1-1-1) is 40% by mass or more, but from the viewpoint of improving the fluidity, it is preferably 50% by mass or more, more preferably 75% by mass or more, even more preferably 90% by mass or more, and even more preferably 99% by mass or more. There is no particular upper limit to the amount, and it may be 100% by mass or less.

[0016] In one embodiment of the present invention, the content of the phenolic antioxidant (1-1-1) is preferably 40 to 100 mass%, more preferably 50 to 100 mass%, even more preferably 75 to 100 mass%, even more preferably 90 to 100 mass%, and even more preferably 99 to 100 mass%, based on the total amount of the phenolic antioxidant (1-1), which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, contained in the phenolic antioxidant (1), from the viewpoint of fluidity of the granules.

[0017] The phenolic antioxidant (1) contained in the composition (A) may be, in addition to the above-mentioned phenolic antioxidant (1-1-1), an antioxidant having a crystal system other than a δ crystal represented by formula (I) (e.g., the above-mentioned phenolic antioxidants (1-1-2), (1-1-3), or (1-1-4)), a phenolic antioxidant represented by formula (II): [ka] [In formula (II), R 1 represents an alkyl group having 1 to 9 carbon atoms, X represents an n-valent alcohol residue having 1 to 18 carbon atoms which may contain a heteroatom and / or a cyclic group, and n represents an integer of 2 or 4. (excluding phenol-based antioxidants represented by formula (I)), 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid, 4,4'-thiobis(2-t-butyl-5-methylphenol), 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propanamide], and 4,4'-butylidenebis(6-t-butyl-m-cresol).

[0018] R in formula (II) 1 Examples of R include linear alkyl groups having 1 to 8 carbon atoms, such as methyl, t-butyl, t-pentyl, and t-octyl groups, and branched alkyl groups having 3 to 8 carbon atoms. 1 is preferably a methyl group or a t-butyl group.

[0019] In formula (II), n is 2 or 4.

[0020] X in formula (II) is an n-valent alcohol residue, and X contains 1 to 18 carbon atoms. Here, the alcohol residue means a substituent obtained by removing a hydroxyl group from an alcohol. X may contain a heteroatom such as an oxygen atom, a sulfur atom, or a nitrogen atom, or may contain a cyclic group such as an alicyclic group such as a cyclopentane structure or a cyclohexane structure, or an aromatic group such as a benzene structure. A carbon atom of the cyclic group may be substituted with a heteroatom.

[0021] Examples of alcohols that provide alcohol residues include stearyl alcohol, decyl alcohol, octyl alcohol, triethylene glycol, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5·5]undecane, and pentaerythritol. Of these, stearyl alcohol, triethylene glycol, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5·5]undecane, and pentaerythritol are preferred.

[0022] Examples of the phenolic compound (II) include bis{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionic acid}triethylene glycolyl ester, tetrakis{3-(3,5-di-t-butyl-4-hydroxyphenyl)propionic acid}pentaerythrityl ester, etc. However, the phenolic antioxidant represented by formula (I) is not included in the phenolic antioxidant represented by formula (II).

[0023] The composition (A) forming the additive granules contains a phenolic antioxidant (1). From the viewpoint of heat discoloration resistance (the property of suppressing discoloration even when kneaded and molded at high temperatures), the total amount of the phenolic compound represented by formula (I) and the compound represented by formula (II) contained in the phenolic antioxidant (1) is preferably 90 parts by mass or more, more preferably 95 parts by mass or more, and even more preferably 99 parts by mass or more, per 100 parts by mass of the phenolic antioxidant (1) contained in the composition (A).

[0024] The amount of the phenolic antioxidant (1) contained in the composition (A) forming the additive granules is, from the viewpoint of improving processing stability, preferably 2 mass % or more, more preferably 2.5 mass % or more, and even more preferably 3 mass % or more, based on the total amount of the composition (A); from the viewpoint of cost reduction, it is preferably 30 mass % or less, more preferably 20 mass % or less, and even more preferably 15 mass % or less, based on the total amount of the composition (A).

[0025] The amount of antioxidant (a) contained in the composition (A) forming the additive granule is preferably 25% by mass or more, more preferably 26% by mass or more, and even more preferably 27% by mass or more, based on the total amount of the composition (A), from the viewpoint of improving processing stability. The upper limit of the amount is not particularly limited, and may be 100% by mass or less based on the total amount of the composition (A), but from the viewpoint of cost reduction, it is preferably 99% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less.

[0026] In the composition (A) forming the additive granules, the ratio (1-1-1):(1-1-2) of the amount of the phenolic antioxidant (1-1-1) contained as the phenolic antioxidant (1) to the amount of the phenolic antioxidant (1-1-2) is preferably 100:0 to 40:60, more preferably 100:0 to 45:55, and even more preferably 100:0 to 50:50. In this embodiment, the additive granules may contain the above components as a whole granules. Therefore, the additive granules may be, for example, an additive granules made of a composition (A) containing a phenolic antioxidant (1-1-1), an additive granules made of a composition (A) containing a phenolic antioxidant (1-1-1) and a phenolic antioxidant (1-1-2), or a mixture obtained by mixing an additive granule (a1) made of a composition (A) containing a phenolic antioxidant (1-1-1) with an additive granule (b1) made of a composition (B) containing a phenolic antioxidant (1-1-2) in such a ratio that the ratio (1-1-1):(1-1-2) of the amount of the phenolic antioxidant (1-1-1) to the amount of the phenolic antioxidant (1-1-2) is preferably 100:0 to 40:60, more preferably 100:0 to 45:55, and even more preferably 100:0 to 50:50.

[0027] The composition (A) forming the additive granules may contain only the phenol-based antioxidant (1) as the antioxidant (a), or may further contain an antioxidant other than the phenol-based antioxidant (1). Examples of the antioxidant other than the phenol-based antioxidant (1) include a phosphorus-based antioxidant (2), a sulfur-based antioxidant (3), and a hindered amine-based antioxidant. The composition (A) may further contain, for example, a phosphorus-based antioxidant (2) and / or a sulfur-based antioxidant (3) as the antioxidant (a).

[0028] (Phosphorus-based antioxidants (2)) Examples of the phosphorus-based antioxidant (2) include 2,2'-methylenebis(4,6-di-t-butylphenyl)2-ethylhexyl phosphite and triisodecyl phosphite. The composition (A) may contain one type of phosphorus-based antioxidant as the phosphorus-based antioxidant (2), or may contain two or more types of phosphorus-based antioxidants. From the viewpoint of improving heat coloration resistance and antioxidant properties, the phosphorus-based antioxidant is preferably a phosphorus-based antioxidant represented by the formula (III): [ka] [In formula (III), R 3 , R 4 , and R 5 each independently represents a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, or a hydrogen atom. a phosphorus-based antioxidant represented by formula (IV): [ka] [In formula (IV), R 6 , R 7 , and R 8 each independently represents a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, or a hydrogen atom. and / or a phosphorus-based antioxidant represented by formula (V): [ka] [In formula (V), R 9 , R10 , and R 11 each independently represents a hydrogen atom, a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, an alkylcycloalkyl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or a phenyl group. It is preferable that the antioxidant is a phosphorus-based antioxidant represented by the formula:

[0029] In formula (III), R 3 , R 4 , and R 5 R each independently represents a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, or a hydrogen atom. Examples of linear alkyl groups and branched alkyl groups include a methyl group, a t-butyl group, a t-pentyl group, and a t-octyl group. 3 , R 4 , R 5 is preferably a hydrogen atom, a methyl group, or a t-butyl group. Examples of the phosphorus-based antioxidant represented by formula (III) include tris(nonylphenyl)phosphite, tris(2,4-di-t-butylphenyl)phosphite, and the like.

[0030] In formula (IV), R 6 , R 7 , and R 8 Each independently represents a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, or a hydrogen atom. As the linear alkyl group and the branched alkyl group, R 3 Examples of the groups include the same groups as those exemplified for R 6 , R 7 , R 8 is preferably a hydrogen atom, a methyl group, or a t-butyl group. Examples of the phosphorus-based antioxidant represented by formula (IV) include bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, and the like.

[0031] In formula (V), R 9 , R10 , and R 11 each independently represents a hydrogen atom, a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, an alkylcycloalkyl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or a phenyl group. As the linear alkyl group and the branched alkyl group, R 3 Examples of the cycloalkyl group having 5 to 8 carbon atoms include a cyclopentyl group, a cyclohexyl group, and a cyclopentyl group, examples of the alkylcycloalkyl group having 6 to 12 carbon atoms include a methylcyclopentyl group, a methylcyclohexyl group, and a dimethylcyclohexyl group, and examples of the aralkyl group having 7 to 12 carbon atoms include a benzyl group.

[0032] In formula (V), R 9 preferably represents a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, or an alkylcycloalkyl group having 6 to 12 carbon atoms, and more preferably represents a t-alkyl group, a cyclohexyl group, or a 1-methylcyclohexyl group.

[0033] In formula (V), R 10 preferably represents a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, or an alkylcycloalkyl group having 6 to 12 carbon atoms, and more preferably represents a methyl group, a t-butyl group, or a t-pentyl group.

[0034] In formula (V), R 11 preferably represents a hydrogen atom, a linear alkyl group having 1 to 8 carbon atoms, or a branched alkyl group having 3 to 8 carbon atoms, and more preferably represents a hydrogen atom or a methyl group.

[0035] In formula (V), B is a single bond, a sulfur atom or -CHR 12 - group, R 12represents a hydrogen atom, a linear alkyl group having 1 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, or a cycloalkyl group having 5 to 8 carbon atoms. The linear alkyl group having 1 to 8 carbon atoms, the branched alkyl group having 3 to 8 carbon atoms, and the cycloalkyl group having 5 to 8 carbon atoms are as described above for R 9 Examples include the same groups as those shown in the above. 12 Examples of the - group include a methylene group, an ethylidene group, a propylidene group, a 1-cyclohexylmethyl group, etc. B preferably represents a single bond, a methylene group or an ethylidene group.

[0036] In formula (V), A is an alkylene group having 2 to 8 carbon atoms or *-C(=O)-R 13 - group, R 13 represents a single bond or an alkylene group having 1 to 8 carbon atoms, and the * symbol represents a bond to the oxygen atom side of the >PO- portion. Examples of the alkylene group having 1 to 8 carbon atoms include a methylene group, an ethylene group, a trimethylene group, and a tetramethylene group. A represents an alkylene group having 2 to 4 carbon atoms or the above-mentioned *-C(=O)-R 13 - group is preferred. The carbon-carbon bond of the alkylene group having 2 to 4 carbon atoms may be interrupted by a group containing a heteroatom. In this case, examples of the group containing a heteroatom include -OC(=O)- or -C(=O)-O- group. R 13 is preferably an alkylene group having 1 to 4 carbon atoms.

[0037] Either Y or Z represents a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, or an aralkyloxy group having 7 to 12 carbon atoms, and the other represents a hydrogen atom, a linear alkyl group having 1 to 8 carbon atoms, or a branched alkyl group having 3 to 8 carbon atoms. When Y is a hydroxyl group, R 12 and R 13It is preferable that either one of them is a linear alkyl group having 3 to 8 carbon atoms, a branched alkyl group having 3 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, an alkylcycloalkyl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or a phenyl group. Examples of the alkoxy group having 1 to 8 carbon atoms include a methoxy group, an ethoxy group, and a t-butoxy group, and examples of the aralkyloxy group having 7 to 12 carbon atoms include a benzyloxy group.

[0038] When Y in formula (V) is a hydroxyl group, it is more preferable that Z is a hydrogen atom or a methyl group, and R 12 and R 13 More preferably, one of them is a t-butyl group.

[0039] When Z in formula (V) is a hydroxyl group, R 13 is a methyl group, Y is a hydrogen atom, and R 12 is preferably a t-butyl group.

[0040] In addition, R in formula (V) 9 , R 10 , R 11 may be the same as or different from each other.

[0041] The phosphorus-based antioxidant represented by formula (V) preferably includes the following: 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenzo[d,f][1,3,2]dioxaphosphepine, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenz[d,f][1,3,2]dioxaphosphepine, Oxaphosphepin, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propoxy]-4,8-di-t-butyl-2,10-dimethyl-12H-dibenzo[d,g][1,3,2]dioxaphosphocin, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxy]-4,8-di-t-butyl-2,10-dimethyl-12H-dibenzo[d,g][1,3,2]dioxaphosphocin and the like.

[0042] (Sulfur-based antioxidants (3)) An example of the sulfur-based antioxidant (3) is bis[2-methyl-4-{3-n-alkyl(C12 or C14)thiopropionyloxy}-5-t-butylphenyl]sulfide. The composition (A) may contain one type of sulfur-based antioxidant as the sulfur-based antioxidant (3), or may contain two or more types of sulfur-based antioxidants. From the viewpoint of improving heat coloration resistance and antioxidation properties, the sulfur-based antioxidant is preferably a sulfur-based antioxidant represented by the formula (VI): (R 14 -DS-C2H4CO2) m -E (VI) [In formula (VI), R 14 represents a linear alkyl group having 12 to 18 carbon atoms or a branched alkyl group having 12 to 18 carbon atoms, D represents a single bond or a -C2H4CO2- group, m represents an integer of 1 to 4, and E represents an m-valent alcohol residue having 5 to 18 carbon atoms. It is preferable that the antioxidant is a sulfur-based antioxidant represented by the formula:

[0043] In formula (VI), R 14is preferably a dodecyl group, a tetradecyl group, an octadecyl group, or the like. The alcohol residue in E refers to the portion of the alcohol other than the hydroxyl group. Examples of alcohols that provide the alcohol residue include dodecyl alcohol, tetradecyl alcohol, octadecyl alcohol, and pentaerythritol.

[0044] In particular, in the sulfur-based antioxidant represented by formula (VI), when D in formula (VI) is a single bond, R 14 is a dodecyl group, m is 4, and E is a pentaerythritol residue. 14 is a dodecyl group, a tetradecyl group, or an octadecyl group, m is 1, and E is the above R 14 Preferably, it is an alcohol residue having 12, 14 or 18 carbon atoms corresponding to the following formula:

[0045] When D is a -C2H4CO2- group, the alcohol residue and D are usually bonded via an ester group. Specifically, when E is monovalent, it is -C2H4CO2-Z.

[0046] Examples of the sulfur-based antioxidant represented by formula (VI) include 3,3'-thiodipropionic acid di-n-dodecyl ester, 3,3'-thiodipropionic acid di-n-tetradecyl ester, 3,3'-thiodipropionic acid di-n-octadecyl ester, and tetrakis(3-dodecylthiopropionic acid) pentaerythrityl ester.

[0047] In a preferred embodiment of the present invention, when the composition (A) forming the additive granule contains, as the antioxidant (a), a phenol-based antioxidant (1), a phosphorus-based antioxidant (2) and / or a sulfur-based antioxidant (3), the total amount of the phenol-based antioxidant (1), the phosphorus-based antioxidant (2) and / or the sulfur-based antioxidant (3) is preferably 25 to 100 mass%, more preferably 26 to 90 mass%, and even more preferably 27 to 80 mass%, based on the total amount of the composition (A).

[0048] In a more preferred embodiment of the present invention, when the composition (A) forming the additive granule contains, as the antioxidant (a), a phenol-based antioxidant (1) and a phosphorus-based antioxidant (2) and / or a sulfur-based antioxidant (3), the amount of the phenol-based antioxidant (1) relative to the total amount of the antioxidant (a) is preferably 5 to 30 mass%, more preferably 8 to 20 mass%, and even more preferably 10 to 15 mass%, and the total amount of the phosphorus-based antioxidant (2) and / or the sulfur-based antioxidant (3) relative to the total amount of the antioxidant (a) is preferably 70 to 95 mass%, more preferably 80 to 92 mass%, and even more preferably 85 to 90 mass%. Note that the composition (A) contains 40 to 100 mass% of the phenol-based antioxidant (1-1-1) relative to the total amount of the phenol-based antioxidant (1).

[0049] In a more preferred embodiment of the present invention, when the composition (A) forming the additive granule contains, as the antioxidant (a), a phenol-based antioxidant (1), a phosphorus-based antioxidant (2), and a sulfur-based antioxidant (3), the amount of the phenol-based antioxidant (1) relative to the total amount of the antioxidant (a) is preferably 10 to 15 mass%, more preferably 10 to 14 mass%, and even more preferably 11 to 14 mass%, the amount of the phosphorus-based antioxidant (2) is preferably 48 to 53 mass%, more preferably 49 to 52 mass%, and even more preferably 49 to 51 mass%, and the amount of the sulfur-based antioxidant (3) is preferably 35 to 40 mass%, more preferably 36 to 39 mass%, and even more preferably 36 to 38 mass%. Note that the composition (A) contains 40 to 100 mass% of the phenol-based antioxidant (1-1-1) relative to the total amount of the phenol-based antioxidant (1).

[0050] From the viewpoint of improving heat discoloration resistance and antioxidant properties, the phenolic antioxidant (1) is preferably a compound selected from the group consisting of phenolic antioxidants represented by formula (I) and phenolic antioxidants represented by formula (II). However, from the viewpoint of obtaining an additive granule having high fluidity, the phenolic antioxidant (1-1-1) is contained in an amount of 40 to 100 mass% based on the total amount of the phenolic antioxidant (1). From the viewpoint of improving heat coloration resistance and antioxidant properties, the phosphorus-based antioxidant (2) is preferably a compound selected from the group consisting of phosphorus-based antioxidants represented by formula (III), phosphorus-based antioxidants represented by formula (IV), and phosphorus-based antioxidants represented by formula (V), and is more preferably a phosphorus-based antioxidant represented by formula (III). From the viewpoint of improving heat coloration resistance and antioxidation properties, the sulfur-based antioxidant (3) is preferably a compound selected from the group consisting of sulfur-based antioxidants represented by formula (VI), in which D is a -C2H4CO2- group and R 14 is a dodecyl group, a tetradecyl group, or an octadecyl group, m is 1, and E is the above R 14 More preferred are sulfur-based antioxidants which are alcohol residues having 12, 14 or 18 carbon atoms corresponding to the following:

[0051] (Other additives) The composition (A) forming the additive granules may further contain various additives known in the art in addition to the antioxidant (a). Examples of such additives include at least one additive selected from the group consisting of neutralizers, lubricants, hindered amine light stabilizers, ultraviolet absorbers, metal soaps, antistatic agents, antiblocking agents, pigments, flame retardants, fillers, nucleating agents, plasticizers, processing aids, foaming agents, and emulsifiers. The composition (A) may further contain one of these additives, or may contain two or more of them in combination. The content of the above additives in the composition (A) is not particularly limited, but is preferably 10 to 75% by mass, more preferably 15 to 70% by mass, and even more preferably 20 to 65% by mass based on the total amount of the composition (A) from the viewpoint of processing stability.

[0052] Examples of the neutralizing agent include calcium stearate, zinc stearate, magnesium stearate, zinc oxide, synthetic hydrotalcite, natural hydrotalcite, calcium hydroxide, and the like.

[0053] Lubricants include oleamide, erucamide, and propylene glycol mono Stearate, stearyl stearate, sorbitan stearate, etc.

[0054] Examples of the hindered amine light stabilizer include bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate (melting point 81 to 86°C), bis(2,2,6,6-tetramethyl-4-piperidyl)ester, 2,2,6,6-tetramethyl-4-piperidyl methacrylate (melting point 58°C), poly[{6-(1,1,3,3,-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}-1,6-hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}] (melting point 100 to 135°C), and the like.

[0055] Examples of ultraviolet absorbers include 2-hydroxy-4-n-octyloxybenzophenone (melting point 45°C or higher), 2-(2H-benzotriazol-2-yl)-4,6-di-t-pentylphenol (melting point 77°C or higher), 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl-]-5-(octyloxy)phenol (melting point 87 to 89°C), 2-(2-hydroxy-5-methylphenyl)benzotriazole (melting point 127°C), 2-(3-t-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole (melting point 137°C), and 2,4-di-t-butylphenyl-3,5-di-t-butyl-4-hydroxybenzoate (melting point 192°C).

[0056] Metal soaps include fatty acid metal salts such as calcium stearate.

[0057] Examples of the antistatic agent include cationic surfactants such as quaternary ammonium salt type cationic surfactants, betaine type amphoteric surfactants, alkyl phosphate type anionic surfactants, primary amine salts, secondary amine salts, tertiary amine salts, quaternary amine salts, and pyridine derivatives; anionic surfactants such as sulfated oils, soaps, sulfated ester oils, sulfated amide oils, sulfated ester salts of olefins, fatty alcohol sulfate salts, alkyl sulfate salts, fatty acid ethyl sulfonates, alkyl naphthalene sulfonates, alkyl benzene sulfonates, succinic acid ester sulfonates, and phosphate salts; nonionic surfactants such as ethylene oxide adducts of partial fatty acid esters of polyhydric alcohols, ethylene oxide adducts of fatty alcohols, ethylene oxide adducts of fatty acids, ethylene oxide adducts of fatty aminos or fatty acid amides, ethylene oxide adducts of alkylphenols, ethylene oxide adducts of partial fatty acid esters of polyhydric alcohols, and polyethylene glycol; and amphoteric surfactants such as carboxylic acid derivatives and imidazoline derivatives.

[0058] Examples of the antiblocking agent include inorganic antiblocking agents such as aluminum silicate, synthetic silica, natural silica, zeolite, kaolin, and diatomaceous earth, and organic antiblocking agents such as crosslinked polymethyl methacrylic acid.

[0059] Examples of pigments include carbon black, titanium oxide, phthalocyanine pigments, quinacridone pigments, isoindolinone pigments, perylene or perinine pigments, quinophthalone pigments, diketopyrrolo-pyrrole pigments, dioxazine pigments, disazo condensation pigments, and benzimidazolone pigments.

[0060] Examples of the flame retardant include decabromobiphenyl, antimony trioxide, phosphorus-based flame retardants, and aluminum hydroxide.

[0061] Examples of the filler include calcium carbonate, silicates, glass fibers, talc, kaolin, mica, barium sulfate, carbon black, carbon fibers, zeolite, metal powders, and metal oxides.

[0062] Examples of nucleating agents include the sodium salt of α-naphthalenesulfonic acid, the magnesium salt of α-naphthalenesulfonic acid, the calcium salt of α-naphthalenesulfonic acid, the aluminum salt of α-naphthalenesulfonic acid, the sodium salt of 8-aminonaphthalenesulfonic acid, the sodium salt of benzenesulfonic acid, the magnesium salt of benzenesulfonic acid, the calcium salt of benzenesulfonic acid, the aluminum salt of benzenesulfonic acid, the calcium salt of 2,5-dichlorobenzenesulfonic acid, the magnesium salt of 2,5-dichlorobenzenesulfonic acid, the calcium salt of m-xylenesulfonic acid, and the aluminum salt of m-xylenesulfonic acid. Magnesium salt, benzoic acid (melting point 122°C), sodium benzoate (melting point 147°C), p-isopropylbenzoic acid, ot-butylbenzoic acid, pt-butylbenzoic acid, monophenylacetic acid (melting point 77°C), diphenylacetic acid, Li salt of diphenylacetic acid, Al salt, Na salt, Na salt of diphenylacetic acid, Mg salt of diphenylacetic acid, Ca salt of diphenylacetic acid, Ba salt of diphenylacetic acid, Al salt of diphenylacetic acid, Phenyldimethylacetic acid, Li salt of phenyldimethylacetic acid, Na salt of phenyldimethylacetic acid, Phenyldimethyl Mg salt of acetic acid, Ca salt of phenyldimethylacetate, Ba salt of phenyldimethylacetate, Mg salt of phthalic acid, Succinic acid (melting point 185°C), Li salt of succinic acid, Na salt of succinic acid, Mg salt of succinic acid, Ca salt of succinic acid, Ba salt of succinic acid, Glutaric acid (melting point 95-99°C), Li salt of glutaric acid, Na salt of glutaric acid, Mg salt of glutaric acid, Ca salt of glutaric acid, Ba salt of glutaric acid, Adipic acid (melting point 151-153°C), Suberic acid, Li salt of suberic acid, Na salt of suberic acid, Mg salt of suberic acid , Ca salt of suberic acid, Ba salt of suberic acid, Sebacic acid, Li salt of sebacic acid, Na salt of sebacic acid, Mg salt of sebacic acid, Ca salt of sebacic acid, Al salt of sebacic acid, Diphenylphosphinic acid (melting point 193-196°C), Li salt of diphenylphosphinic acid, Na salt of diphenylphosphinic acid, K salt of diphenylphosphinic acid, Ca salt of diphenylphosphinic acid, Mg salt of diphenylphosphinic acid, Al salt of diphenylphosphinic acid, Li salt of 4,4'-dichlorodiphenylphosphinic acid, 4,Examples of the dinaphthylphosphinic acid include a sodium salt of 4'-dimethyldiphenylphosphinic acid, dinaphthylphosphinic acid, a lithium salt of dinaphthylphosphinic acid, a sodium salt of dinaphthylphosphinic acid, a magnesium salt of dinaphthylphosphinic acid, a calcium salt of dinaphthylphosphinic acid, and an aluminum salt of dinaphthylphosphinic acid.

[0063] The plasticizer includes polyethylene glycol, polypropylene glycol, and the like.

[0064] Processing aids include ricinoleic acid, stearic acid, palmitic acid, lauric acid, and the like.

[0065] Examples of the foaming agent include chemical foaming agents and physical foaming agents. Examples of the chemical foaming agent include inorganic compounds and organic compounds. Examples of the inorganic compounds include hydrogen carbonates such as sodium hydrogen carbonate, and ammonium carbonate. Examples of the organic compounds include polycarboxylic acids, azo compounds, sulfonhydrazide compounds, nitroso compounds, p-toluenesulfonylsemicarbazide, and isocyanate compounds. Examples of the physical foaming agent include volatile organic compounds such as inert gases, butane, and pentane, and examples of the inert gas include carbon dioxide, nitrogen, argon, neon, and helium.

[0066] Examples of the emulsifier include polyoxyethylene sorbitan monolaurate, polyethylene glycol monolaurate, and sorbitan tristearate.

[0067] In a preferred embodiment of the present invention, the composition (A) contains 25 to 100 mass% of the antioxidant (a) based on the total amount of the composition (A). The antioxidant (a) contains a phenol-based antioxidant (1), a phosphorus-based antioxidant (2) and / or a sulfur-based antioxidant (3). The amount of the phenol-based antioxidant (1) contained in the antioxidant is preferably 2 to 30 mass% based on the total amount of the composition (A), and the amount of the phenol-based antioxidant (1-1-1) based on the total amount of the phenol-based antioxidant (1) is preferably 40 to 100 mass%.

[0068] [Additive granules] The additive granules of the present invention are granules formed from the composition (A). Examples of the shape of the additive granules include "pellets" obtained by granulation using a semi-dry extruder such as a single-screw or multi-screw melt extruder or a disk pelleter, "granules" obtained by stirring and granulating, and "flakes" obtained by granulation using a compression granulator such as a roller compactor. The shape of the additive granules mentioned above means the shape classified according to the definition described in JIS-Z8841 (1993) Section 10, Explanation Table 1, Shape and Name of Granules. The additive granules do not refer to a single granule, but rather to an aggregate of granules. Among the above shapes, "granules" are preferred from the viewpoints of excellent fluidity and excellent dispersibility in thermoplastic resins. Granular additive granules can be obtained by any method such as extrusion granulation and stirring granulation, but "granules" obtained by stirring and granulating the composition (A) are more preferred.

[0069] The method for producing the additive granules is not particularly limited, but examples thereof include a method in which composition (A) is stirred and granulated or extruded at an appropriate temperature range, for example, 40°C to 80°C, preferably 40°C to 70°C, and particularly preferably 40°C to 60°C.

[0070] Examples of equipment used for stirring granulation include high-speed rotating equipment such as a Henschel mixer, a super mixer, and a high-speed mixer, stirring mixer granulators such as a vertical granulator, and a tumbling fluidized coating device. Granulated materials may also be produced by the production method described in JP-A-2010-254958.

[0071] Examples of the stirring granulation method include a method in which the raw materials constituting the composition (A) are charged into a mixer such as a Henschel mixer and then stirred and mixed at high speed. Examples of the method for setting the temperature within the above range include a method of heating the Henschel mixer by attaching a hot water jacket to it, and a method of increasing the temperature by utilizing the shear heat generated by high-speed stirring.

[0072] The size of the additive granules is not particularly limited, but for example, when produced by stirring granulation, the median diameter (mass basis) is preferably 0.1 to 7 mm, more preferably 0.15 to 6 mm, even more preferably 0.18 to 6 mm, and even more preferably 0.20 to 6 mm. The median diameter (mass basis) is determined by mechanically sieving about 100 g of a sample using a low-tap shaker (for example, low-tap shaker RL-1, Kagaku Kyoeisha) for 15 minutes, with a shaking speed of 290 rpm / 60 Hz, a swing width of 25 mm, and a stroke rate of 156 tpm / 60 Hz.

[0073] As a method for producing an additive granule having the above-mentioned median diameter (mass basis), for example, a method using an agitation granulator having an agitation blade and an agitation granulator in which the clearance between the tip of the agitation blade and the wall surface inside the agitation granulator is adjusted to 30 mm or less can be mentioned. The additive granule having the above-mentioned median diameter (mass basis) is preferably in the form of a granule.

[0074] Examples of equipment used for extrusion granulation include single-screw or multi-screw melt extruders, and semi-dry extruders such as disk pelleters.

[0075] As an extrusion granulation method, for example, the raw materials constituting the composition (A) are mixed in a mixer such as a Henschel mixer or a super mixer to prepare a mixture, and the mixture is fed into an extruder from a hopper or the like, and the material temperature in the extruder is adjusted to 40°C to 80°C by the shear heat generation or heating equipment of the extruder, so that the material can be easily extruded to obtain a cylindrical granule. The extruded cylindrical granule can be cut to an appropriate length with a cutter or the like to obtain a pellet-shaped additive granule. By adjusting the diameter of the die, the extrusion speed, and the cutting speed, a pellet-shaped additive granule of any size can be produced, but from the viewpoint of dispersibility, it is preferable that the diameter is 2 to 5 mm and the length is 2 to 5 mm.

[0076] The additive granule of the present invention contains 40 to 100% by mass of the phenolic antioxidant (1-1-1) relative to the total amount of the phenolic antioxidant (1). The ratio of the amount of the phenolic antioxidant (1-1-1) relative to the total amount of the phenolic antioxidant (1) contained in the additive granule may be calculated, for example, from the charge ratio when producing the additive granule, or the amount of the phenolic antioxidant (1) contained in the additive granule may be identified and quantified by HPLC, and the amount of the phenolic antioxidant (1-1-1) may be calculated from the endothermic amount at the time of melting at about 124 to 127°C by DSC, and the ratio may be calculated from these amounts.

[0077] The additive granule according to one embodiment of the present invention is used by being blended with, for example, plastics, such as thermoplastic resins. The blending ratio of the additive granule to the plastic can be, for example, 0.005 to 10 parts by mass of the additive granule to 100 parts by mass of the plastic, preferably 0.01 to 5 parts by mass, more preferably 0.01 to 3 parts by mass. The present invention also provides a method for producing a plastic composition by blending the additive granule of the present invention with a plastic, preferably 0.005 to 10 parts by mass of the additive granule of the present invention with 100 parts by mass of the plastic, and the plastic composition. The plastic composition obtained by the above-mentioned manufacturing method has the advantage that, for example, the additive granule with high fluidity is added, and therefore the additive is uniformly dispersed. According to the present invention, a method for stabilizing a plastic can also be provided, which includes a step of blending 0.005 to 10 parts by mass of the additive granule of the present invention with 100 parts by mass of the plastic.

[0078] The plastic to which the additive granules are mixed is preferably a thermoplastic resin. The thermoplastic resin is not particularly limited as long as it is a commercially available resin, but examples thereof include polypropylene resins such as ethylene-propylene copolymers, polyethylene resins (high density polyethylene (HD-PE), low density polyethylene (LD-PE), linear low density polyethylene (LLDPE), etc.), methylpentene polymers, ethylene-ethyl acrylate copolymers, ethylene-vinyl acetate copolymers, polystyrenes (polystyrenes such as poly(p-methylstyrene) and poly(α-methylstyrene), acrylonitrile-styrene copolymers, acrylonitrile-butadiene-styrene copolymers, special acrylic rubber-acrylonitrile-styrene copolymers, acrylonitrile-chlorinated polyethylene-styrene copolymers, styrene-butadiene copolymers, etc.), chlorinated polyethylene, polychloroprene, chlorinated rubber, polyvinyl chloride, polychloride, etc. Examples of the resin include polyvinylidene fluoride, methacrylic resin, ethylene-vinyl alcohol copolymer, fluororesin, polyacetal, grafted polyphenylene ether resin, polyphenylene sulfide resin, polyurethane, polyamide, polyester resin (e.g., polyethylene terephthalate, polybutylene terephthalate, etc.), polycarbonate, polyacrylate, polysulfone, polyether ether ketone, polyether sulfone, aromatic polyester resin, diallyl phthalate prepolymer, silicone resin, 1,2-polybutadiene, polyisoprene, butadiene / acrylonitrile copolymer, ethylene-methyl methacrylate copolymer, etc., and from the viewpoint of good moldability, polyolefin resins such as polyethylene resins and polypropylene resins, and polystyrene resins are preferred, with polyolefin resins being more preferred.

[0079] Here, the polypropylene-based resin means a polyolefin-based resin containing a structural unit derived from propylene, and specific examples thereof include crystalline propylene homopolymer, propylene-ethylene random copolymer, propylene-α-olefin random copolymer, propylene-ethylene-α-olefin copolymer, polypropylene-based block copolymers consisting of a propylene homopolymer component or a copolymer component mainly consisting of propylene, and a copolymer component of propylene and ethylene and / or α-olefin, etc. When a polypropylene-based resin is used as the thermoplastic resin, one type of polypropylene-based resin may be used, or two or more types may be blended and used.

[0080] Examples of the α-olefin include α-olefins having 4 to 12 carbon atoms, such as 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene, and preferably 1-butene, 1-hexene, and 1-octene.

[0081] Examples of the propylene-α-olefin random copolymer include a propylene-1-butene random copolymer, a propylene-1-hexene random copolymer, and a propylene-1-octene random copolymer.

[0082] Examples of the propylene-ethylene-α-olefin copolymer include a propylene-ethylene-1-butene copolymer, a propylene-ethylene-1-hexene copolymer, and a propylene-ethylene-1-octene copolymer.

[0083] In the polypropylene block copolymer consisting of a propylene homopolymer component or a copolymer component mainly consisting of propylene, and a copolymer component of propylene and ethylene and / or α-olefin, examples of the copolymer component mainly consisting of propylene include a propylene-ethylene copolymer component, a propylene-1-butene copolymer component, a propylene-1-hexene copolymer component, etc., and examples of the copolymer component of propylene and ethylene and / or α-olefin include a propylene-ethylene copolymer component, a propylene-ethylene-1-butene copolymer component, a propylene-ethylene-1-hexene copolymer component, a propylene-ethylene-1-octene copolymer component, a propylene-1-butene copolymer component, a propylene-1-hexene copolymer component, a propylene-1-octene copolymer component, etc. The content of ethylene and / or an α-olefin having 4 to 12 carbon atoms in the copolymer component of propylene and ethylene and / or α-olefin is, for example, 0.01 to 20% by weight.

[0084] Examples of polypropylene block copolymers consisting of a propylene homopolymer component or a copolymer component mainly consisting of propylene and a copolymer component of propylene and ethylene and / or an α-olefin include propylene-ethylene block copolymers, (propylene)-(propylene-ethylene) block copolymers, (propylene)-(propylene-ethylene-1-butene) block copolymers, (propylene)-(propylene-ethylene-1-hexene) block copolymers, (propylene)-(propylene-1-butene) block copolymers, (propylene)-(propylene-1-hexene) block copolymers, (propylene-ethylene)-(propylene-ethylene-1-butene) block copolymers, polymer, (propylene-ethylene)-(propylene-ethylene-1-hexene) block copolymer, (propylene-ethylene)-(propylene-1-butene) block copolymer, (propylene-ethylene)-(propylene-1-hexene) block copolymer, (propylene-1-butene)-(propylene-ethylene) block copolymer, (propylene-1-butene)-(propylene-ethylene-1-butene) block copolymer, (propylene-1-butene)-(propylene-ethylene-1-hexene) block copolymer, (propylene-1-butene)-(propylene-1-butene) block copolymer, (propylene-1-butene)-(propylene-ethylene-1-hexene) block copolymer, (propylene-1-butene)-(propylene-1-butene) block copolymer, (propylene-1-butene)-(propylene-1-butene) block copolymer, (propylene-1-butene)-(propylene-1-hexene) block copolymer, and the like.

[0085] When a polypropylene-based resin is used as the thermoplastic resin, preferably, a crystalline propylene homopolymer, a polypropylene-based block copolymer consisting of a propylene homopolymer component or a copolymer component mainly consisting of propylene, and a copolymer component of propylene and ethylene and / or an α-olefin having 4 to 12 carbon atoms is used, and more preferably, a polypropylene-based block copolymer consisting of a propylene homopolymer component or a copolymer component mainly consisting of propylene, and a copolymer component of propylene and ethylene and / or an α-olefin having 4 to 12 carbon atoms is used.

[0086] Examples of methods for blending the additive granules with plastics include a method in which the additive granules and plastics are mixed and then melt-kneaded using a single-screw or multi-screw extruder, and a method in which the additive granules are added by feeding them into a solution obtained after polymerization of a thermoplastic resin, etc. The thermoplastic resin thus obtained can be processed into products such as films, molding materials, and pipes.

[0087] The additive granules of the present invention have good fluidity, and therefore, when blended with plastics such as thermoplastic resins, they are easy to handle, the amount of additive is unlikely to vary, and a highly uniform plastic composition can be produced. Furthermore, when the additive granules of the present invention are blended with plastics, the effect of the additive granules is uniformly exerted, and a thermoplastic resin composition having excellent heat coloring resistance can be obtained. EXAMPLES

[0088] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0089] The components used in the examples and comparative examples are listed below. Compound (1-1-1): 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5·5]undecane, which has a crystal structure that shows sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6° by X-ray diffraction measurement using X-rays of Cu-Kα wavelength. (The results of the X-ray diffraction measurement are shown in Figure 1. Note that the left end of the horizontal axis in Figures 1 and 2 is 4°.) Compound (1-1-2): 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5 5]undecane, which has a crystal structure that shows a sharp X-ray diffraction peak at a diffraction angle of 2θ = 7.9° when measured using X-rays with a Cu-Kα wavelength (Figure 2 shows the X-ray diffraction measurement result). Compound (2-1): Tris(2,4-di-t-butylphenyl)phosphite "Irgafos 168 (registered trademark)" (manufactured by BASF) Compound (3-1): 3,3'-thiodipropionic acid di-n-tetradecyl ester "Sumilizer TPM (registered trademark)" (manufactured by Sumitomo Chemical)

[0090] (Example 1: Production of additive granule A-1) Into a 10L high-speed mixer (manufactured by Fukae Powtec Co., Ltd.: model number FS-GS-10J), 187.5 g of compound (1-1-1), 750.0 g of compound (2-1), and 562.5 g of compound (3-1) were added. After addition, 50°C hot water was passed through the jacket of the high-speed mixer to heat up the stirring tank equipped with the high-speed mixer. Then, the rotation speed of the stirring blade was set to 450 rpm and the rotation speed of the chopper blade was set to 2000 rpm, and the compounds were mixed. Stirring was stopped when the agitator current reached 4.7 A, and additive granules A-1 having a median diameter (mass basis) of 241 μm was obtained.

[0091] (Comparative Example 2: Production of additive granule A-2) Additive granule A-2 was obtained in the same manner as in the production of additive granule A-1, except that compound (1-1-2) was used instead of compound (1-1-1) used in the production of additive granule A-1.

[0092] (Examples 2 to 3, Comparative Example 1) A total of 80.0 g of additive granules A-1 and / or additive granules A-2 in the proportions shown in Table 1 was placed in a 20 L plastic bag and mixed uniformly to obtain additive granules B-1 to B-3.

[0093] (Liquidity) 80.0 g of the obtained additive granules of Examples 1 to 3 and Comparative Examples 1 and 2 were each placed in a funnel (with a stopper) with an opening diameter of 95 mm and an outer leg diameter of 20 mm. The fluidity of the additive granules in the initial state when the stopper was removed was evaluated. After evaluating the initial state, the additive granules were stored in a thermo-hygrostat at a temperature of 35°C and a humidity of 80% RH for 7 days, and then the fluidity was evaluated in the same manner. The results are shown in Table 1. Liquidity Assessment Metrics ○: The entire amount flows down. ×: The entire amount did not flow down due to bridging phenomenon.

[0094] (Median diameter based on mass) The additive granules A-1 and A-2 were used as measurement samples, and 100 g of the sample was mechanically sieved using a low tap shaker RL-1 (Kagaku Kyoeisha) under the conditions of sieving time 15 minutes, shaking speed 290 rpm / 60 Hz, swing width 25 mm, and stroke number 156 tpm / 60 Hz to determine the median diameter based on mass. The median diameters of the additive granules A-1 and A-2 were within the range of 0.1 to 7 mm.

[0095] [Table 1]

[0096] The components used in the production examples are listed below. Compound (4-1): Calcium stearate "Calcium Stearate WLC (registered trademark)" (manufactured by Faci) Compound (5-1): Sodium benzoate "Sodium Benzoate 20M (registered trademark)" (manufactured by BASF) Compound (6-1): Hydrotalcite "DHT-4C (registered trademark)" (Kyowa Chemical Industry Co., Ltd.) Compound (7-1): Talc "Micron White 5000S (registered trademark)" (manufactured by Hayashi Kasei) Compound (8-1): Oleic acid amide "Kemamide VO (registered trademark)" (manufactured by PMC)

[0097] (Production example: Excipient granules A-3) A 100L high-speed mixer (manufactured by Fukae Powtec Co., Ltd.: model number FS-100) is charged with raw materials (total 15 kg) consisting of 8.9 parts by weight of compound (1-1-1), 35.7 parts by weight of compound (2-1), 26.8 parts by weight of compound (3-1), 25.0 parts by weight of compound (5-1), and 3.6 parts by weight of compound (6-1). The high-speed mixer is heated by passing hot water at 50°C through the jacket of the high-speed mixer. The rotation speed of the stirring blade inside the stirring tank of the high-speed mixer is set to 165 rpm (6 m / s as the blade tip speed) and the rotation speed of the chopper is set to 1500 rpm (10 m / s as the blade tip speed), and the high-speed mixer is operated for about 20 minutes while maintaining this state. In this way, the mixture of the raw materials is stirred and granulated to obtain additive granule A-3.

[0098] (Production example: Excipient granules A-4) Additive granule A-4 was obtained in the same manner as additive granule A-3, except that compound (1-1-2) was used instead of compound (1-1-1) used in additive granule A-3.

[0099] (Production example: Excipient granules A-5) A 100L high-speed mixer (manufactured by Fukae Powtec Co., Ltd.: model number FS-100) is charged with raw materials (total 15 kg) consisting of 9.6 parts by weight of compound (1-1-1), 38.2 parts by weight of compound (2-1), 29.1 parts by weight of compound (3-1), 19.3 parts by weight of compound (4-1), and 3.8 parts by weight of compound (7-1). The high-speed mixer is heated by passing hot water at 50°C through the jacket of the high-speed mixer. The rotation speed of the stirring blade inside the stirring tank of the high-speed mixer is set to 165 rpm (6 m / s as the blade tip speed) and the rotation speed of the chopper is set to 1500 rpm (10 m / s as the blade tip speed), and the high-speed mixer is operated for about 1 minute and 20 seconds while maintaining this state. In this way, additive granule A-5 is obtained by stirring and granulating the mixture consisting of the raw materials.

[0100] (Production example: Excipient granules A-6) Additive granule A-6 is obtained in the same manner as additive granule A-5, except that compound (1-1-2) is used instead of compound (1-1-1) used in additive granule A-5.

[0101] (Production example: Excipient granule A-7) A 100L high-speed mixer (manufactured by Fukae Powtec Co., Ltd.: model number FS-100) is charged with raw materials (total 15 kg) consisting of 3.9 parts by weight of compound (1-1-1), 15.4 parts by weight of compound (2-1), 11.5 parts by weight of compound (3-1), 7.7 parts by weight of compound (4-1), 46.1 parts by weight of compound (7-1), and 15.4 parts by weight of compound (8-1). The high-speed mixer is heated by passing hot water at 50°C through the jacket of the high-speed mixer. The rotation speed of the stirring blade inside the stirring tank of the high-speed mixer is set to 165 rpm (6 m / s as the blade tip speed) and the rotation speed of the chopper is set to 1500 rpm (10 m / s as the blade tip speed), and the high-speed mixer is operated for about 40 minutes while maintaining this state. In this way, additive granule A-7 is obtained by stirring and granulating the mixture consisting of the raw materials.

[0102] (Production example: Excipient granules A-8) Additive granule A-8 was obtained in the same manner as additive granule A-7, except that compound (1-1-2) was used instead of compound (1-1-1) used in additive granule A-7.

[0103] (Production example: Excipient granule A-9) In a 100L high-speed mixer (manufactured by Fukae Powtec Co., Ltd.: model number FS-100), raw materials consisting of 8.9 parts by weight of compound (1-1-1), 35.7 parts by weight of compound (2-1), 26.8 parts by weight of compound (3-1), 25.0 parts by weight of compound (5-1), and 3.6 parts by weight of compound (6-1) are mixed using a Henschel mixer. Then, this mixture is put into a disk pelleter (manufactured by Dalton Co., Ltd.: model number F-5) and operated. The pellet-shaped additive granule A-9 is obtained by extruding from the disk die under the roller and cutting immediately thereafter.

[0104] (Production example: Excipient granules A-10) Additive granule A-10 is obtained in the same manner as additive granule A-9, except that compound (1-1-2) is used instead of compound (1-1-1) used in additive granule A-9.

[0105] (Production example: Excipient granule A-11) In a 100L high-speed mixer (manufactured by Fukae Powtec Co., Ltd.: model number FS-100), raw materials consisting of 9.6 parts by weight of compound (1-1-1), 38.2 parts by weight of compound (2-1), 29.1 parts by weight of compound (3-1), 19.3 parts by weight of compound (4-1), and 3.8 parts by weight of compound (7-1) are mixed using a Henschel mixer. Then, this mixture is put into a disk pelleter (manufactured by Dalton Co., Ltd.: model number F-5) and operated. The pellet-shaped additive granule A-11 is obtained by extruding from the disk die under the roller and cutting immediately thereafter.

[0106] (Production example: Excipient granules A-12) Additive granule A-12 is obtained in the same manner as additive granule A-11, except that compound (1-1-2) is used instead of compound (1-1-1) used in additive granule A-11.

[0107] (Production example: Excipient granule A-13) The raw materials consisting of 3.9 parts by weight of compound (1-1-1), 15.4 parts by weight of compound (2-1), 11.5 parts by weight of compound (3-1), 7.7 parts by weight of compound (4-1), 46.1 parts by weight of compound (7-1), and 15.4 parts by weight of compound (8-1) are mixed using a Henschel mixer. Then, this mixture is put into a disk pelleter (manufactured by Dalton Co., Ltd.: model number F-5) and operated. The pellet-shaped additive granule A-13 is obtained by extruding from the disk die under the roller and cutting immediately thereafter.

[0108] (Production example: Excipient granule A-14) Additive granule A-14 is obtained in the same manner as additive granule A-13, except that compound (1-1-2) is used instead of compound (1-1-1) used in additive granule A-13.

[0109] The additive granules A-3, A-5, A-7, A-9, A-11 and A-13 obtained in the above manufacturing examples are considered to have the same initial and 7-day flowability as in Example 1. The additive granules A-4, A-6, A-8, A-10, A-12 and A-14 obtained in the above manufacturing examples are considered to have the same initial and 7-day flowability as in Comparative Example 2. [Industrial Applicability]

[0110] The present invention provides an additive granule having excellent flowability.

Claims

1. The additive granules are formed from a composition (A) containing an antioxidant (a) that contains a phenolic antioxidant (1), and contain 40 to 100 mass % of a phenolic antioxidant (1-1-1) that is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystal structure that shows sharp X-ray diffraction peaks at diffraction angles 2θ=4.2° and 2θ=10.6° in X-ray diffraction measurement using X-rays of Cu-Kα wavelength.

2. The additive granule according to claim 1, wherein the content of the phenolic antioxidant (1-1-1) is 40 to 100 mass% based on the total amount of the phenolic antioxidant (1-1) which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane contained in the phenolic antioxidant (1).

3. The additive granule according to claim 1, wherein in the phenolic antioxidant (1), the ratio of the amount of the phenolic antioxidant (1-1-1) to the amount of the phenolic antioxidant (1-1-2) which is 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane having a crystal structure which shows a sharp X-ray diffraction peak at a diffraction angle 2θ=7.9° in X-ray diffraction measurement using X-rays of Cu-Kα wavelength is (1-1-1):(1-1-2)=100:0 to 40:

60.

4. The additive granule according to claim 1, wherein the amount of the phenol-based antioxidant (1) contained in the composition (A) is 2 to 30 mass% based on the total amount of the composition (A).

5. The additive granule according to claim 1, wherein the amount of the antioxidant (a) contained in the composition (A) is 25 to 100 mass% based on the total amount of the composition (A).

6. The additive granule according to claim 1, wherein the antioxidant (a) further comprises a phosphorus-based antioxidant (2) and / or a sulfur-based antioxidant (3).

7. The additive granule according to claim 6, wherein the total amount of the phenol-based antioxidant (1), the phosphorus-based antioxidant (2) and / or the sulfur-based antioxidant (3) contained in the composition (A) is 25 to 100 mass% based on the total amount of the composition (A).

8. The additive granule according to claim 6, wherein the amount of the phenol-based antioxidant (1) is 5 to 30 mass% and the total amount of the phosphorus-based antioxidant (2) and / or the sulfur-based antioxidant (3) is 70 to 95 mass% based on the total amount of the antioxidant (a).

9. The additive granule according to claim 6, wherein the amount of the phenol-based antioxidant (1) is 10 to 15 mass%, the amount of the phosphorus-based antioxidant (2) is 48 to 53 mass%, and the amount of the sulfur-based antioxidant (3) is 35 to 40 mass%, based on the total amount of the antioxidant (a).

10. The additive granule according to claim 1, wherein the composition (A) further contains at least one additive selected from the group consisting of a neutralizing agent, a lubricant, a hindered amine light stabilizer, an ultraviolet absorber, a metal soap, an antistatic agent, an antiblocking agent, a pigment, a flame retardant, a filler, a nucleating agent, a plasticizer, a processing aid, a foaming agent, and an emulsifier.

11. The additive granule according to claim 1, wherein the additive granule has a median diameter (by mass) of 0.1 to 7 mm.

12. A method for producing a plastic composition, comprising a step of blending 0.005 to 10 parts by mass of the additive granule according to any one of claims 1 to 10 with respect to 100 parts by mass of plastic.

13. The method of claim 12, wherein the plastic is a thermoplastic resin.

14. The method for producing a plastic composition according to claim 12, wherein the plastic is a polyolefin-based resin.

Citation Information

Patent Citations

  • Hydroxyphenylpropionic acid ester having new crystalline structure

    JP1994087860A

  • Granules of hydroxyphenylpropionic acid ester

    JP2015157853A