Combing trowel and method for applying adhesive composition using the same
The comb trowel with specific dimensions addresses the challenges of water-based adhesive compositions by enhancing pot life and adhesive strength in high temperature and humidity environments, resulting in improved workability and water-resistant adhesion.
Patent Information
- Application Number
- JP2023072287
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
AI Technical Summary
Water-based adhesive compositions face challenges with high viscosity, poor workability, and reduced adhesive strength, especially in high temperature and high humidity environments, requiring improved pot life and water-resistant adhesiveness.
A comb trowel with specific dimensions and configurations is used to apply aqueous adhesive compositions, ensuring sufficient pot life and enhanced adhesive strength by alternately providing notches and closed portions, along with a construction method that includes applying the adhesive and laminating flooring.
The comb trowel improves workability and ensures a floor structure with excellent adhesive strength and water-resistant properties, even in summer conditions.
Smart Images

Figure 2024157745000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a comb trowel used primarily for an aqueous adhesive composition for flooring materials, a method for applying the adhesive composition using the comb trowel, and a floor structure formed by the application method. [Background technology]
[0002] Conventionally, organic solvent-based adhesive compositions have been widely used for on-site construction of flooring materials such as synthetic resin flooring materials. However, organic solvent-based adhesive compositions have problems such as the working environment, safety for the human body, and fire hazards due to the organic solvent, and in recent years, solventless adhesive compositions that do not use organic solvents and emulsion-type aqueous adhesive compositions have come to be used.
[0003] However, in general, solvent-free adhesive compositions have high viscosity and poor workability, and although low molecular weight plasticizers are sometimes blended to improve workability, there is a risk of reduced adhesive strength and bleeding contamination. In addition, when using an aqueous adhesive composition to install flooring at a site with a large installation area, the time from applying the aqueous adhesive composition to the base to attaching the flooring is long, and if the aqueous adhesive composition dries during this time, it will not be possible to attach it to the flooring or the adhesive strength will decrease, so the aqueous adhesive composition is required to have sufficient pot life (open time) after application.
[0004] In order to ensure sufficient working time after application of the aqueous adhesive composition, the applicant has proposed an aqueous polyurethane emulsion composition in which finely powdered silica and a thickener are blended with an aqueous polyurethane emulsion (Patent Document 1). The aqueous polyurethane emulsion composition of Patent Document 1 has a longer touch-dry time after application than conventional aqueous adhesive compositions, improving workability. On the other hand, a new method is required for fast drying of the aqueous adhesive composition and ensuring sufficient working time for work in the summer (high temperature and high humidity). In addition, aqueous adhesive compositions may have inferior water-resistant adhesion compared to organic solvent-based adhesive compositions, and there is a demand for improved water-resistant adhesion. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-152815 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above circumstances, and aims to improve workability by ensuring a sufficient pot life (open time) after application of an aqueous adhesive composition even in a summer environment (high temperature and humidity), and to improve the adhesive strength (water-resistant adhesion) of the aqueous adhesive composition. [Means for solving the problem]
[0007] As a result of intensive research, the present inventors have found that a comb trowel for an aqueous adhesive composition having the following specific comb portion and a method for applying the aqueous adhesive composition using the same are effective means for solving the problems of the present invention. The gist of the configuration of the present invention is as follows. [1] A comb trowel for use with an aqueous adhesive composition, the comb trowel having a comb portion with alternating notches and blocked portions at the end, The comb trowel is characterized in that the height of the notch is 2.5 to 6.0 mm, the width of the notch is 1.0 to 4.0 mm, the ratio of the height of the notch to the width of the notch (height / width) is 1.3 to 3.0, and the notch has a pitch of 4.0 to 12.0 mm and the comb portion is formed in plurality. [2] A comb trowel for use with an aqueous adhesive composition, the comb trowel having a comb portion at an end of which is provided with alternating notches and blocked portions, the aqueous adhesive composition is an aqueous urethane adhesive composition, The comb trowel is characterized in that the height of the notch is 2.5 to 6.0 mm, the width of the notch is 1.0 to 4.0 mm, the ratio of the height of the notch to the width of the notch (height / width) is 1.3 to 3.0, and the notch has a pitch of 4.0 to 12.0 mm and the comb portion is formed in plurality. [3] A comb trowel for use with an aqueous adhesive composition, the comb trowel having a comb portion with alternating notches and blocked portions at the end, the aqueous adhesive composition has a viscosity of 15,000 to 40,000 mPa s (12 rpm, 25°C, Brookfield viscometer), a TI value (viscosity at 6 rpm / viscosity at 12 rpm, 25°C, Brookfield viscometer) of 1.3 to 3.0, and a non-volatile content of 20 to 80 mass%; The comb trowel according to [1] or [2], characterized in that the height of the notch is 2.5 to 6.0 mm, the width of the notch is 1.0 to 4.0 mm, the ratio of the height of the notch to the width of the notch (height / width) is 1.3 to 3.0, and the pitch of the notch is 4.0 to 12.0 mm and the comb portion is formed in plurality. [4] A comb trowel for use with an aqueous adhesive composition, the comb trowel having a comb portion with alternating notches and blocked portions at the end, The aqueous adhesive composition is used for flooring materials, The comb trowel according to [1] or [2], characterized in that the height of the notch is 2.5 to 6.0 mm, the width of the notch is 1.0 to 4.0 mm, the ratio of the height of the notch to the width of the notch (height / width) is 1.3 to 3.0, and the pitch of the notch is 4.0 to 12.0 mm and the comb portion is formed in plurality. [5] Applying the aqueous adhesive composition to a substrate using the comb trowel described in [1] or [2]; A step of bonding the aqueous adhesive composition to a flooring material; Optionally, compressing the flooring. A construction method including the steps of carrying out the above in this order. [6] The construction method according to [5], wherein the moisture content of the base is 0 to 15 mass% (measured by a high-frequency capacitance moisture meter). [7] Applying the aqueous adhesive composition to a substrate using the comb trowel described in [1] or [2]; A step of bonding the aqueous adhesive composition to a flooring material; Optionally, compressing the flooring. A floor structure formed by a construction method including the steps of: Effect of the Invention
[0008] According to the embodiment of the comb trowel for the aqueous adhesive composition of the present invention and the application method using the same, when the aqueous adhesive composition is used, particularly as an adhesive composition for flooring, a sufficient pot life can be ensured after application of the aqueous adhesive composition, improving workability and allowing the production of a floor structure with excellent adhesive strength (water-resistant adhesion). [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is an overall view for explaining an outline of a comb trowel for use with an aqueous adhesive composition according to a first embodiment of the present invention. [Diagram 2] 1 is an enlarged front view of a comb portion of a comb trowel for use with an aqueous adhesive composition according to a first embodiment of the present invention. FIG. [Diagram 3] FIG. 2 is an overall view for explaining an outline of a comb trowel for use with an aqueous adhesive composition according to a second embodiment of the present invention. [Figure 4] FIG. 4 is an enlarged front view of a comb portion of a comb trowel for use with an aqueous adhesive composition according to a second embodiment of the present invention. [Diagram 5] FIG. 4 is an overall view for explaining an outline of a comb trowel for use with an aqueous adhesive composition according to a third embodiment of the present invention. [Figure 6] FIG. 4 is an enlarged front view of a comb portion of a comb trowel for use with an aqueous adhesive composition according to a third embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The comb trowel for use with the aqueous adhesive composition of the present invention and the application method and floor structure using the same will be described in detail below.
[0011] First, the comb trowel for an aqueous adhesive composition according to the first embodiment of the present invention will be described. Fig. 1 is an overall view for explaining the outline of the comb trowel for an aqueous adhesive composition according to the first embodiment of the present invention. Fig. 2 is an enlarged front view of the comb part of the comb trowel for an aqueous adhesive composition according to the first embodiment of the present invention.
[0012] As shown in FIG. 1, the comb trowel 1 for the aqueous adhesive composition according to the first embodiment of the present invention includes a plate-shaped main body 3 having a longitudinal direction L and a width direction (short direction) W perpendicular to the longitudinal direction L, and a comb-shaped comb portion 2 provided at an end of the main body 3 in the longitudinal direction L (one end of the longitudinal direction L and / or the other end opposite the one end) and / or an end of the width direction W (one end of the width direction W and / or the other end opposite the one end). In FIG. 1, the comb portion 2 is provided along the width direction W at one end of the longitudinal direction L of the main body 3. In the operation of applying the aqueous adhesive composition, an operator supplies the aqueous adhesive composition to the comb portion 2, holds the main body 3, and applies the aqueous adhesive composition to an object to be applied such as a base. Alternatively, an operator applies the aqueous adhesive composition to an object to be applied such as a base, and uses the comb portion 2 of the comb trowel 1 to level the aqueous adhesive composition.
[0013] The position of the comb portion 2 is on approximately the same plane as the flat plate-shaped main body 3. The comb portion 2 is formed at one end in the longitudinal direction L of the main body 3 over the entire width direction W, and the position of the tip portion 23, which is the end of the comb portion 2, is on approximately the same straight line over the entire width direction W of the main body 3.
[0014] 1 and 2, the comb portion 2 has alternating notches 21 and blocking portions 22, and a plurality of the notches 21 are formed at predetermined intervals. That is, blocking portions 22 are provided between adjacent notches 21. Each of the notches 21 functions as a comb of the comb portion 2. By alternately providing the notches 21 and blocking portions 22 in the comb portion 2, a comb (mountain) shape can be formed in the aqueous adhesive composition applied using the comb trowel 1 for the aqueous adhesive composition of the present invention.
[0015] The shape of the cutout 21 in a front view is not particularly limited, and examples thereof include an equilateral triangle, an isosceles triangle, a vertically elongated rectangle, a semi-ellipse, etc. In the comb trowel 1 for use with an aqueous adhesive composition, the cutout 21 is an isosceles triangle in a front view. The cutout 21 in a front view has a wide shape in which the width of the cutout 21 gradually increases toward the tip 23 of the comb portion 2.
[0016] 2, the cutout 21 has a predetermined height (total height) a and a predetermined width b in a front view. The cutouts 21, 21, 21... all have substantially the same height a and substantially the same width b in a front view. In this specification, the width of the cutout 21 refers to the width of the cutout 21 at the tip 23, which is the end of the comb portion 2.
[0017] In the comb trowel 1 for use with an aqueous adhesive composition of the present invention, the height a of the notch 21 is 2.5 to 6.0 mm, and the width b of the notch 21 is 1.0 to 4.0 mm. A plurality of notches 21 are formed at a predetermined pitch c. The pitch c of the notches 21 is preferably such that a plurality of notches are formed at equal intervals in order to stabilize adhesiveness. In the comb trowel 1 for use with an aqueous adhesive composition of the present invention, the pitch c of the notches 21 is 4.0 to 12.0 mm.
[0018] By having the height a of the cutout portion 21 be 2.5 to 6.0 mm, the width b of the cutout portion 21 be 1.0 to 4.0 mm, and the pitch c of the cutout portion 21 be 4.0 to 12.0 mm, it is possible to ensure sufficient pot life after application of the aqueous adhesive composition even in a summer environment (high temperature and humidity), improving workability, and also to improve the adhesive strength (water-resistant adhesion) of the aqueous adhesive composition.
[0019] The height a of the cutout 21 is not particularly limited as long as it is 2.5 to 6.0 mm, but is preferably 3.0 to 5.5 mm, and more preferably 3.5 to 5.0 mm, from the viewpoint of further extending the usable time in a summer (high temperature and high humidity) environment and further improving the adhesive strength. The width b of the cutout 21 is not particularly limited as long as it is 1.0 to 4.0 mm, but is preferably 1.5 to 3.0 mm, and more preferably 1.5 to 2.5 mm, from the viewpoint of further extending the usable time in a summer (high temperature and high humidity) environment and further improving the adhesive strength. The width b of the cutout 21 relative to the height a of the cutout 21 (height a / width b) is not particularly limited as long as it is 1.3 to 3.0, but is preferably 1.5 to 3.0, and more preferably 1.5 to 2.5, from the viewpoint of further extending the usable time in a summer (high temperature and high humidity) environment and further improving the adhesive strength. Furthermore, the pitch c of the cutouts 21 is not particularly limited as long as it is 4.0 to 12.0 mm, but from the viewpoints of further extending the pot life in a summer environment (high temperature and humidity) and further improving the adhesive strength, it is preferably 5.0 to 11.0 mm, and particularly preferably 6.0 to 10.0 mm.
[0020] Next, a comb trowel for an aqueous adhesive composition according to a second embodiment of the present invention will be described. The comb trowel for an aqueous adhesive composition according to the second embodiment has major components in common with the comb trowel for an aqueous adhesive composition according to the first embodiment, and therefore the same components as those of the comb trowel for an aqueous adhesive composition according to the first embodiment will be described using the same reference numerals. FIG. 3 is an overall view illustrating the outline of the comb trowel for an aqueous adhesive composition according to the second embodiment of the present invention. FIG. 4 is a front view showing an enlarged comb portion of the comb trowel for an aqueous adhesive composition according to the second embodiment of the present invention.
[0021] In the first embodiment of the comb trowel 1 for use with an aqueous adhesive composition, the shape of the cutout portion 21 when viewed from the front is an isosceles triangle. Instead, as shown in Figures 3 and 4, in the second embodiment of the comb trowel 12 for use with an aqueous adhesive composition, the shape is a semi-ellipse, more specifically, a vertically elongated semi-ellipse.
[0022] 4, in the comb trowel 12 for an aqueous adhesive composition, the cutout 21 also has a predetermined height (total height) a and a predetermined width b in a front view. Moreover, all of the multiple cutouts 21, 21, 21... have substantially the same height a and width b in a front view.
[0023] In the comb trowel 12 for use with an aqueous adhesive composition, the height a of the notch 21 is 2.5 to 6.0 mm, and the width b of the notch 21 is 1.0 to 4.0 mm. A plurality of notches 21 are formed at a predetermined pitch c. The pitch c of the notches 21 is preferably such that the plurality of notches are formed at equal intervals in order to stabilize adhesiveness. In the comb trowel 12 for use with an aqueous adhesive composition, the pitch c of the notches 21 is 4.0 to 12.0 mm.
[0024] Even in the comb trowel 12 for use with an aqueous adhesive composition, the height a of the cutout portion 21 is 2.5 to 6.0 mm, the width b of the cutout portion 21 is 1.0 to 4.0 mm, and the pitch c of the cutout portion 21 is 4.0 to 12.0 mm, so that a sufficient pot life can be ensured after application of the aqueous adhesive composition even in a summer environment (high temperature and humidity), improving workability, and also improving the adhesive strength (water-resistant adhesion) of the aqueous adhesive composition.
[0025] In the comb trowel 12 for the aqueous adhesive composition, the height a of the notch 21 is not particularly limited as long as it is 2.5 to 6.0 mm, but from the viewpoint of further extending the usable time in a summer (high temperature and high humidity) environment and further improving the adhesive strength, it is preferably 3.0 to 5.5 mm, and more preferably 3.5 to 5.0 mm. The width b of the notch 21 is not particularly limited as long as it is 1.0 to 4.0 mm, but from the viewpoint of further extending the usable time in a summer (high temperature and high humidity) environment and further improving the adhesive strength, it is preferably 1.5 to 3.0 mm, and more preferably 1.5 to 2.5 mm. The width b of the notch 21 relative to the height a of the notch 21 (height a / width b) is not particularly limited as long as it is 1.3 to 3.0, but from the viewpoint of further extending the usable time in a summer (high temperature and high humidity) environment and further improving the adhesive strength, it is preferably 1.5 to 3.0, and more preferably 1.5 to 2.5. Furthermore, the pitch c of the cutouts 21 is not particularly limited as long as it is 4.0 to 12.0 mm, but from the viewpoints of further extending the pot life in a summer environment (high temperature and humidity) and further improving the adhesive strength, it is preferably 5.0 to 11.0 mm, and particularly preferably 6.0 to 10.0 mm.
[0026] Next, a comb trowel for an aqueous adhesive composition according to a third embodiment of the present invention will be described. The comb trowel for an aqueous adhesive composition according to the third embodiment has major components in common with the comb trowel for an aqueous adhesive composition according to the first and second embodiments, and therefore the same components as those of the comb trowel for an aqueous adhesive composition according to the first and second embodiments will be described using the same reference numerals. FIG. 5 is an overall view illustrating the outline of the comb trowel for an aqueous adhesive composition according to the third embodiment of the present invention. FIG. 6 is an enlarged front view of the comb portion of the comb trowel for an aqueous adhesive composition according to the third embodiment of the present invention.
[0027] In the first embodiment of the comb trowel 1 for use with an aqueous adhesive composition, the shape of the cutout 21 when viewed from the front is an isosceles triangle. Instead, as shown in Figures 5 and 6, in the third embodiment of the comb trowel 13 for use with an aqueous adhesive composition, the cutout 21 has a quadrilateral shape, or more specifically, a vertically elongated rectangular shape.
[0028] 6, in the comb trowel 13 for an aqueous adhesive composition, the cutout 21 also has a predetermined height (total height) a and a predetermined width b in a front view. Moreover, all of the multiple cutouts 21, 21, 21... have substantially the same height a and width b in a front view.
[0029] In the comb trowel 13 for use with an aqueous adhesive composition, the height a of the notch 21 is 2.5 to 6.0 mm, and the width b of the notch 21 is 1.0 to 4.0 mm. A plurality of notches 21 are formed at a predetermined pitch c. The pitch c of the notches 21 is preferably such that the plurality of notches are formed at equal intervals in order to stabilize adhesiveness. In the comb trowel 13 for use with an aqueous adhesive composition, the pitch c of the notches 21 is 4.0 to 12.0 mm.
[0030] Even in the comb trowel 13 for use with an aqueous adhesive composition, the height a of the cutout portion 21 is 2.5 to 6.0 mm, the width b of the cutout portion 21 is 1.0 to 4.0 mm, and the pitch c of the cutout portion 21 is 4.0 to 12.0 mm, so that a sufficient pot life can be ensured after application of the aqueous adhesive composition even in a summer environment (high temperature and humidity), improving workability, and also improving the adhesive strength (water-resistant adhesion) of the aqueous adhesive composition.
[0031] In the comb trowel 13 for the aqueous adhesive composition, the height a of the notch 21 is not particularly limited as long as it is 2.5 to 6.0 mm, but from the viewpoint of further extending the usable time in a summer (high temperature and high humidity) environment and further improving the adhesive strength, it is preferably 3.0 to 5.5 mm, and more preferably 3.5 to 5.0 mm. The width b of the notch 21 is not particularly limited as long as it is 1.0 to 4.0 mm, but from the viewpoint of further extending the usable time in a summer (high temperature and high humidity) environment and further improving the adhesive strength, it is preferably 1.5 to 3.0 mm, and more preferably 1.5 to 2.5 mm. The width b of the notch 21 relative to the height a of the notch 21 (height a / width b) is not particularly limited as long as it is 1.3 to 3.0, but from the viewpoint of further extending the usable time in a summer (high temperature and high humidity) environment and further improving the adhesive strength, it is preferably 1.5 to 3.0, and more preferably 1.5 to 2.5. Furthermore, the pitch c of the cutouts 21 is not particularly limited as long as it is 4.0 to 12.0 mm, but from the viewpoints of further extending the pot life in a summer environment (high temperature and humidity) and further improving the adhesive strength, it is preferably 5.0 to 11.0 mm, and particularly preferably 6.0 to 10.0 mm.
[0032] Next, the aqueous adhesive composition using the comb trowel of the present invention (for example, comb trowel 1 for an aqueous adhesive composition which is the first embodiment of the present invention, comb trowel 12 for an aqueous adhesive composition which is the second embodiment of the present invention, and comb trowel 13 for an aqueous adhesive composition which is the third embodiment of the present invention) will be described. The aqueous adhesive composition described below is an aqueous adhesive composition suitable for application using the comb trowel of the present invention described above, and any conventionally known aqueous adhesive composition can be selected and used. The aqueous adhesive composition used with the comb trowel of the present invention is preferably an aqueous urethane adhesive composition from the viewpoints of ensuring a sufficient pot life after application of the aqueous adhesive composition and improving the adhesive strength (water-resistant adhesion) of the aqueous adhesive composition.
[0033] The viscosity (12 rpm) of the aqueous adhesive composition is preferably 15,000 to 45,000 mPa·s, more preferably 18,000 to 40,000 mPa·s, and particularly preferably 20,000 to 35,000 mPa·s. The TI value (viscosity at 6 rpm / viscosity at 12 rpm) of the aqueous adhesive composition is preferably 1.3 to 3.0, more preferably 1.3 to 2.5, and particularly preferably 1.4 to 2.0. The non-volatile content (solid content) of the aqueous adhesive composition is preferably 20 to 80 mass%, more preferably 30 to 70 mass%, and particularly preferably 40 to 50 mass%. When the viscosity (12 rpm), TI value, and non-volatile content of the aqueous adhesive composition are within these ranges, the aqueous adhesive composition is easily spread when applied to the surface of the base using the comb trowel of the present invention, maintains an appropriate comb (mountain) shape, and reduces the decrease in adhesive strength even when the pot life is extended. In this specification, the viscosity of the aqueous adhesive composition is a value measured at 25°C using a Brookfield type rotational viscometer 1 minute after the start of rotation. The TI value (thixotropic index) of the aqueous adhesive composition is the ratio of the viscosity at 6 rpm to the viscosity at 12 rpm (viscosity at 6 rpm / viscosity at 12 rpm, 25°C, Brookfield type rotational viscometer). The non-volatile content (solid content) of the aqueous adhesive composition and the aqueous polyurethane emulsion composition described below is a value calculated from the change in mass of the composition after placing 2.5 g of the composition in an aluminum cylindrical container with an inner diameter of 60 mm and placing it in an oven at 105°C for 3 hours.
[0034] The components of the aqueous urethane adhesive composition will be described. The aqueous urethane adhesive composition is a composition containing an aqueous polyurethane emulsion in which an aqueous polyurethane resin is dispersed in water (hereinafter, sometimes simply referred to as an "aqueous polyurethane emulsion composition").
[0035] The aqueous polyurethane emulsion composition can be obtained by dispersing the reactants in water during and / or after reacting (a) an organic polyisocyanate, (b) a polymer polyol, (c) an active hydrogen-containing compound having an anionic group, (d) a chain extender, (e) a neutralizing agent, and optionally (f) an adhesion promoter.
[0036] (a) Organic polyisocyanate Organic polyisocyanates are compounds having two or more isocyanate groups in one molecule. Examples of organic polyisocyanates include aromatic polyisocyanates in which an isocyanate group is bonded to an aromatic hydrocarbon, aromatic aliphatic polyisocyanates in which an aromatic ring is present and an isocyanate group is bonded to an aliphatic hydrocarbon group, aliphatic polyisocyanates made of chain-like aliphatic hydrocarbons, and alicyclic polyisocyanates made of cyclic aliphatic hydrocarbons. These may be used alone or in combination of two or more.
[0037] Examples of aromatic polyisocyanates include 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, and mixtures thereof (diphenylmethane diisocyanates (MDIs)); 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, and mixtures thereof (toluene diisocyanates (TDIs)); phenylene diisocyanate, diphenyl diisocyanate, naphthalene diisocyanate, and diphenyl ether diisocyanate.
[0038] The aromatic aliphatic polyisocyanate may be xylylene diisocyanate. The aliphatic polyisocyanate may be hexamethylene diisocyanate, pentamethylene diisocyanate, propylene diisocyanate, or butylene diisocyanate. The alicyclic polyisocyanate may be cyclohexane diisocyanate, methylene bis(cyclohexyl isocyanate), or isophorone diisocyanate.
[0039] Further examples of the organic polyisocyanate include carbodiimide-modified, biuret-modified, allophanate-modified, and isocyanurate-modified polyisocyanates described above, and polymethylene polyphenyl polyisocyanates (crude MDI, polymeric MDI), which are oligomers of polyisocyanates.
[0040] Of these organic polyisocyanates, alicyclic polyisocyanates, aliphatic polyisocyanates, and araliphatic polyisocyanates are preferred.
[0041] (b) Polymer polyol Examples of polymeric polyols include polyester polyols, polycarbonate polyols, polyoxyalkylene polyols, hydrocarbon polyols, poly(meth)acrylic polyols, animal and plant polyols, and copolyols thereof. In this specification, "polymeric" means that the number average molecular weight in terms of polystyrene measured by gel permeation chromatography is 1,000 or more, and "low molecular" means that the number average molecular weight in terms of polystyrene measured by gel permeation chromatography is less than 1,000. In this specification, "(meth)acrylic" means "acrylic and / or methacrylic".
[0042] The number average molecular weight of the polymer polyol, calculated as polystyrene by gel permeation chromatography, is preferably 1,000 to 100,000, more preferably 1,000 to 30,000, and particularly preferably 1,000 to 20,000. If the number average molecular weight of the polymer polyol is less than 1,000, the physical properties of the resulting aqueous polyurethane emulsion composition after curing tend to be poor. On the other hand, if the number average molecular weight of the polymer polyol exceeds 100,000, the viscosity of the resulting aqueous polyurethane emulsion composition tends to be high.
[0043] Examples of polyester polyols include polycarboxylic acids such as succinic acid, adipic acid, sebacic acid, azelaic acid, terephthalic acid, isophthalic acid, orthophthalic acid, hexahydroterephthalic acid, hexahydroisophthalic acid, hexahydroorthophthalic acid, naphthalenedicarboxylic acid, and trimellitic acid, esters of the above polycarboxylic acids, and polycarboxylic anhydrides, and at least one of these polycarboxylic acids and ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentanediol, and the like. Examples of the polyester polyol or polyesteramide polyol include those obtained by dehydration condensation reaction with one or more of low molecular weight polyols such as diethyl glycol, 1,8-octanediol, 1,9-nonanediol, diethylene glycol, dipropylene glycol, 1,4-cyclohexanedimethanol, ethylene oxide or propylene oxide adduct of bisphenol A, trimethylolpropane, glycerin, pentaerythritol, etc., low molecular weight polyamines such as butylenediamine, hexamethylenediamine, xylylenediamine, isophoronediamine, etc., and low molecular weight amino alcohols such as monoethanolamine, diethanolamine, etc. Also included are lactone-based polyester polyols obtained by ring-opening polymerization of cyclic ester (lactone) monomers such as ε-caprolactone, γ-valerolactone, etc., using low molecular weight polyols, low molecular weight polyamines, and low molecular weight amino alcohols as initiators.
[0044] Examples of polycarbonate polyols include those obtained by the dehydrochlorination reaction of the low molecular weight polyols used in the synthesis of the polyester polyols with phosgene, or the transesterification reaction of the low molecular weight polyols with diethylene carbonate, dimethyl carbonate, diethyl carbonate, or diphenyl carbonate.
[0045] Examples of the polyoxyalkylene polyol include polyoxyethylene polyols, polyoxypropylene polyols, polyoxybutylene polyols, polyoxytetramethylene polyols, and poly-(oxyethylene)-(oxypropylene)-random or block copolymer polyols, which are obtained by ring-opening addition polymerization or copolymerization (hereinafter, "polymerization or copolymerization" may be referred to as copolymerization) of one or more cyclic ether compounds such as ethylene oxide, propylene oxide, butylene oxide, and tetrahydrofuran, using as initiators low molecular weight polyols, low molecular weight polyamines, low molecular weight amino alcohols, and polycarboxylic acids used in the synthesis of the polyester polyols, sorbitol, mannitol, sucrose, glucose, and other sugar-based low molecular weight polyhydric alcohols, and low molecular weight polyhydric phenols such as bisphenol A and bisphenol F. Examples of the polyoxyalkylene polyol include polyester ether polyols and polycarbonate ether polyols using as initiators the polyester polyols and polycarbonate polyols. In addition, the polyoxyalkylene polyol may be a polyol obtained by reacting these various polyols with an organic isocyanate in an excess of hydroxyl groups relative to the isocyanate groups, resulting in a hydroxyl group at the molecular end. The number of alcoholic hydroxyl groups in the polyoxyalkylene polyol is not particularly limited, but is preferably 2 or more, more preferably 2 to 4, and particularly preferably 2 to 3 on average per molecule.
[0046] If necessary, polyoxyalkylene monools such as polyoxypropylene monools obtained by ring-opening addition polymerization of cyclic ether compounds such as propylene oxide using low molecular weight monoalcohols such as methyl alcohol, ethyl alcohol, and propyl alcohol as an initiator can also be used.
[0047] In this specification, the term "polyoxyalkylene-based" in the polyoxyalkylene-based polyol and the polyoxyalkylene-based monool means that 50% by mass or more of the portion excluding the hydroxyl group in 1 mole of the molecule is composed of polyoxyalkylene. Therefore, the remaining portion may be modified with other structures such as ester, urethane, polycarbonate, polyamide, poly(meth)acrylate, polyolefin, etc. The portion composed of polyoxyalkylene is not particularly limited as long as it is 50% by mass or more, but is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more.
[0048] Examples of the hydrocarbon polyol include polyolefin polyols such as polybutadiene polyol and polyisoprene polyol; polyalkylene polyols such as hydrogenated polybutadiene polyol and hydrogenated polyisoprene polyol; and halogenated polyalkylene polyols such as chlorinated polypropylene polyol and chlorinated polyethylene polyol.
[0049] As the poly(meth)acrylic polyol, one obtained by high-temperature continuous polymerization reaction of an ethylenically unsaturated compound containing at least a hydroxyl group-containing (meth)acrylic monomer in the presence or absence of a polymerization initiator, preferably at 150 to 350°C, more preferably at 210 to 250°C, by a known radical polymerization method such as batch or continuous polymerization, is suitable because the molecular weight distribution of the reaction product is narrow and the viscosity is low. The poly(meth)acrylic polyol may be one obtained by polymerizing one type of hydroxyl group-containing (meth)acrylic monomer, may be one obtained by copolymerizing two or more types of hydroxyl group-containing (meth)acrylic monomer, or may be one obtained by copolymerizing one or more types of hydroxyl group-containing (meth)acrylic monomer with an ethylenically unsaturated compound (other ethylenically unsaturated compound) other than the hydroxyl group-containing (meth)acrylic monomer. Among these, poly(meth)acrylic polyols obtained by copolymerizing one or more hydroxyl group-containing (meth)acrylic monomers with one or more ethylenically unsaturated compounds other than these are preferred because it is easy to adjust the hydroxyl group content of the poly(meth)acrylic polyol. In the copolymerization, it is particularly preferred to use the hydroxyl group-containing (meth)acrylic monomers so that the average number of hydroxyl groups per molecule of the poly(meth)acrylic polyol is 1.2 to 4.0. Among these, poly(meth)acrylic polyols having a number average molecular weight of 1,000 to 30,000 in terms of polystyrene by gel permeation chromatography are preferred, and poly(meth)acrylic polyols having a number average molecular weight of 2,000 to 15,000 are particularly preferred. The glass transition temperature (Tg) of the poly(meth)acrylic polyol is preferably 0°C or lower, more preferably -70 to -20°C, and particularly preferably -70 to -30°C.
[0050] As the hydroxyl group-containing (meth)acrylic monomer, an alcoholic hydroxyl group-containing (meth)acrylic monomer is preferred because it has good reactivity with the isocyanate group of the organic polyisocyanate.Specific examples include hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate; monoacrylates of polyhydric alcohols such as pentaerythritol tri(meth)acrylate, glycerin mono(meth)acrylate, pentaerythritol di(meth)acrylate monostearate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, and polypropylene glycol mono(meth)acrylate; and polyacrylates with residual hydroxyl groups.
[0051] Other ethylenically unsaturated compounds include ethylene, propylene, isobutylene, butadiene, chloroprene, vinyl chloride, vinylidene chloride, (meth)acrylic acid, vinyl acetate, styrene, 2-methylstyrene, divinylbenzene, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, behenyl (meth)acrylate, benzyl (meth)acrylate, glycidyl (meth)acrylate, tripropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylol (meth)acrylate, dimethyl ... Examples of the acrylates include diolpropane tri(meth)acrylate, polyurethane di(meth)acrylate, acrylic acid dimer, polyester poly(meth)acrylate, 1,6-hexanediol di(meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, lauryl (meth)acrylate, isodecyl (meth)acrylate, isooctyl (meth)acrylate, tridecyl (meth)acrylate, neopentyl glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate. Among these, the ethylenically unsaturated compound is preferably a (meth)acrylic compound such as a (meth)acrylic acid ester compound monomer, acrylamide, methacrylamide, or acrylonitrile, and more preferably methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, or 2-ethylhexyl (meth)acrylate. These may be used alone or in combination of two or more. Also, one or more (meth)acrylic monomers having 9 or less carbon atoms may be used in combination with one or more (meth)acrylic monomers having 10 or more carbon atoms.
[0052] Examples of the animal and vegetable polyols include castor oil polyols.
[0053] The above-mentioned various polymer polyols can be used alone or in combination of two or more. Among these polymer polyols, polyoxyalkylene polyols are preferred, and polyoxytetramethylene polyols are particularly preferred, in that they provide good water-resistant adhesion to the aqueous polyurethane emulsion composition.
[0054] (c) Active hydrogen-containing compound having an anionic group The active hydrogen-containing compound having an anionic group is a compound having one or more anionic groups and one or more active hydrogens (groups) in the compound. The active hydrogens (groups) of the active hydrogen-containing compound having an anionic group are reacted with the isocyanate group of the organic polyisocyanate to introduce an anionic group into the urethane prepolymer, so that the isocyanate group-containing urethane prepolymer having an anionic group is easily emulsified and dispersed in water. Examples of the active hydrogen-containing compound having an anionic group include an active hydrogen-containing compound having a carboxyl group and an active hydrogen-containing compound having a sulfone group. These can be used alone or in combination of two or more.
[0055] Examples of active hydrogen-containing compounds having a carboxyl group include 2,2-dimethylolpropionic acid (DMPA), 2,2-dimethylolbutanoic acid (DMBA), 2,2-dimethylolpentanoic acid, 2,2-dimethylolhexanoic acid, 2,2-dimethylolheptanoic acid, 2,2-dimethyloloctanoic acid, 2,2-dimethylolnonanoic acid, and 2,2-dimethyloldecanoic acid.
[0056] Examples of active hydrogen-containing compounds having a sulfone group include dihydroxybutanesulfonic acid, dihydroxypropanesulfonic acid, N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid, N,N-bis(2-hydroxyethyl)-2-aminobutanesulfonic acid, 1,3-phenylenediamine-4,6-disulfonic acid, diaminobutanesulfonic acid, diaminopropanesulfonic acid, 3,6-diamino-2-toluenesulfonic acid, 2,4-diamino-5-toluenesulfonic acid, N-(2-aminoethyl)-2-aminoethanesulfonic acid, 2-aminoethanesulfonic acid, and N-(2-aminoethyl)-2-aminobutanesulfonic acid.
[0057] Of these, 2,2-dimethylolpropionic acid (DMPA) and 2,2-dimethylolbutanoic acid (DMBA) are preferred because the isocyanate group-containing urethane prepolymer having an anionic group is more easily emulsified and dispersed in water, and the aqueous polyurethane emulsion composition has better water-resistant adhesion.
[0058] (d) Chain extender The chain extender is a compound having active hydrogen (groups) therein, and reacts (chain extends) with the isocyanate group of the isocyanate group-containing urethane prepolymer having an anionic group to polymerize the isocyanate group-containing urethane prepolymer having an anionic group. By polymerizing the isocyanate group-containing urethane prepolymer having an anionic group to form a polyurethane resin having an anionic group, the cured product formability of the aqueous polyurethane emulsion composition is improved, and the cured product of the aqueous polyurethane emulsion composition has particularly excellent water-resistant adhesion.
[0059] Examples of the chain extender include amine compounds such as ethylenediamine, 1,4-tetramethylenediamine, 2-methyl-1,5-pentanediamine, 1,4-butanediamine, 1,6-hexamethylenediamine, 1,4-hexamethylenediamine, 3-aminomethyl-3,5,5-trimethylcyclohexylamine, 1,3-bis(aminomethyl)cyclohexane, xylylenediamine, piperazine, adipoylhydrazide, hydrazine (including hydrates), isophoronediamine, 2,5-dimethylpiperazine, diethylenetriamine, and triethylenetetramine; diol compounds such as ethylene glycol, propylene glycol, 1,4-butanediol, and 1,6-hexanediol; polyalkylene glycols such as polyethylene glycol; low molecular weight polyols; low molecular weight amino alcohols; and water. These can be used alone or in combination of two or more. When water is used as the chain extender, the water, which is the dispersion medium, also serves as the chain extender. Among these, primary diamines are preferred because of their excellent solubility in water and reactivity with the isocyanate groups of the isocyanate group-containing urethane prepolymer having an anionic group, and hydrazine (including hydrates) and isophorone diamine are particularly preferred.
[0060] (e) Neutralizing agent In order to improve the emulsification and dispersion of the isocyanate group-containing urethane prepolymer having an anionic group in water, it is preferable to neutralize the anionic group in the isocyanate group-containing urethane prepolymer having an anionic group using a neutralizing agent. By neutralizing the anionic group with the neutralizing agent, the anionic group becomes an anionic group salt, improving the affinity with water, and the isocyanate group-containing urethane prepolymer having an anionic group becomes easily emulsified and dispersed in water.
[0061] Examples of the neutralizing agent include organic amines such as ammonia, ethylamine, trimethylamine, triethylamine, methyldiethylamine, tripropylamine, N-methylmorpholine, methyldiisopropylamine, ethyldiisopropylamine, diisopropylethylamine, tributylamine, triethanolamine, N-methyldiethanolamine, N-phenyldiethanolamine, monoethanolamine, dimethylethanolamine, diethylethanolamine, morpholine, and 2-amino-2-ethyl-1-propanol; alkali metals such as lithium, potassium, and sodium; and inorganic alkalis such as sodium hydroxide and potassium hydroxide. These can be used alone or in combination of two or more. Among these, volatile tertiary amines are preferred, and ammonia, trimethylamine, and triethylamine are particularly preferred, because they improve the storage stability of the aqueous polyurethane emulsion composition and can be removed by volatilization during drying and curing of the aqueous polyurethane emulsion composition, thereby preventing a decrease in water resistance.
[0062] (f) Adhesion promoter The adhesion promoter is a compound having an active hydrogen (group) reactive with the isocyanate group of the isocyanate group-containing urethane prepolymer having an anionic group and a hydrolyzable (crosslinkable) silyl group, and is used as necessary. The compound having an active hydrogen (group) reactive with the isocyanate group and a hydrolyzable silyl group is reacted with the isocyanate group of the isocyanate group-containing urethane prepolymer having an anionic group to introduce the hydrolyzable silyl group into the polyurethane resin having an anionic group, so that the cured product of the aqueous polyurethane emulsion composition has particularly excellent water-resistant adhesion. That is, the hydrolyzable silyl group in the polyurethane resin having an anionic group reacts chemically with the undercoat material or floor material to improve adhesion, and the hydrolyzable silyl groups condense with each other to polymerize the polyurethane resin having an anionic group to improve water resistance. Examples of adhesion promoters include aminosilane coupling agents and mercaptosilane coupling agents. These can be used alone or in combination of two or more.
[0063] Examples of aminosilane coupling agents include aminomethyltriethoxysilane, N-(2-aminoethyl)aminomethyltrimethoxysilane, aminomethyldiethoxysilane, N-(2-aminoethyl)methyltributoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminoisobutyltrimethoxysilane, N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, and N-(2-aminoethyl)-3-amino-2-methylpropyltrimethoxysilane.
[0064] Examples of mercaptosilane coupling agents include 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylethyldimethoxysilane, 3-mercaptopropylethyldiethoxysilane, 3-mercaptopropyldimethylmethoxysilane, 2-mercaptoethylmethyldimethoxysilane, 2-mercaptoethyltrimethoxysilane, and 2-mercaptoethyltriethoxysilane.
[0065] Among these, aminosilane coupling agents are preferred because they have high reactivity with the isocyanate groups of the isocyanate group-containing urethane prepolymer having an anionic group and provide excellent water-resistant adhesion to the aqueous polyurethane emulsion composition.
[0066] The content of silicon atoms of hydrolyzable silyl groups in the polyurethane resin having an anionic group is not particularly limited, but is preferably 0.01 to 3.0 mass%, more preferably 0.1 to 3.0 mass%, and particularly preferably 0.3 to 2.0 mass%. If the content of silicon atoms of hydrolyzable silyl groups in the polyurethane resin having an anionic group is less than 0.01 mass%, the adhesion to the base material (particularly, inorganic materials) may decrease, and if the content of silicon atoms of hydrolyzable silyl groups exceeds 3.0 mass%, the storage stability of the aqueous polyurethane emulsion composition may decrease.
[0067] The total amount of the chain extender and adhesion promoter used is preferably in a molar ratio to the isocyanate groups of the isocyanate group-containing urethane prepolymer having an anionic group (number of moles of isocyanate groups of the isocyanate group-containing urethane prepolymer having an anionic group / total number of moles of active hydrogen (groups) of the chain extender and adhesion promoter) of 1.0 to 1.3 / 1.0, more preferably 1.0 to 1.2 / 1.0, and particularly preferably 1.0 to 1.1 / 1.0.
[0068] In the aqueous urethane adhesive composition of the present invention, finely divided silica and a thickener can be optionally blended with the above-mentioned aqueous polyurethane emulsion composition, if necessary.
[0069] By blending the fine powder silica in the aqueous polyurethane emulsion composition, the use of the comb trowel of the present invention contributes to improving the water-resistant adhesion of the aqueous polyurethane emulsion composition and ensuring sufficient pot life, and also contributes to obtaining excellent adhesion even when the aqueous polyurethane emulsion composition is applied to a substrate with a high water content. Note that a substrate with a high water content means a substrate with a water content of more than 8% by mass. In addition, by imparting thixotropy to the aqueous polyurethane emulsion composition, the comb shape after application of the aqueous adhesive composition can be sufficiently maintained even when the height of the notch of the comb part is larger than the width of the notch and the comb has a high mountain shape, as in the comb trowel of the embodiment of the present invention. Examples of the fine powder silica include fumed silica (hydrophilic silica, hydrophobic silica). Among these, hydrophilic silica is preferred because of its good dispersibility in the aqueous polyurethane emulsion composition. Examples of commercially available fumed silica include "Aerosil 130", "Aerosil 200", "Aerosil 300", and "Aerosil R106" manufactured by Nippon Aerosil Co., Ltd., "Reolosil QS-102", "Reolosil MT-10", and "Reolosil DM-10" manufactured by Tokuyama Corporation, and "CAB-O-SIL" and "CAB-O-SPERSE" manufactured by Cabot Corporation. These may be used alone or in combination of two or more. The average primary particle size of the finely powdered silica is preferably 1 to 100 nm, and more preferably 1 to 50 nm, in order to improve water-resistant adhesion even on a substrate with a high water content, and the BET specific surface area of the finely powdered silica is preferably 10 to 500 m. 2 / g, 50-500m 2 Finely divided silica also has the effect of increasing the viscosity of the aqueous polyurethane emulsion composition when blended with the aqueous polyurethane emulsion composition, similar to the thickener described below, but since finely divided silica has effects other than increasing the viscosity that differ from those of the thickener, it is not included in the thickener described below in this specification.
[0070] The amount of the fine powder silica is preferably 3.0 to 10 parts by mass, particularly preferably 4.5 to 9.0 parts by mass, based on 100 parts by mass of the aqueous polyurethane emulsion composition (theoretical solid content of the aqueous polyurethane resin). If the amount of the fine powder silica is less than 3.0 parts by mass, sufficient water-resistant adhesion tends not to be obtained, and if it exceeds 10 parts by mass, the touch-dry time after application of the aqueous polyurethane emulsion composition becomes shorter, making it impossible to ensure sufficient pot life, and workability tends to decrease.
[0071] By incorporating the thickener into the aqueous polyurethane emulsion composition, even if the aqueous polyurethane emulsion composition is applied to a substrate having a low water content, the aqueous polyurethane emulsion composition is less likely to absorb water into the substrate by using the comb trowel of the present invention, and the aqueous polyurethane emulsion composition is less likely to dry after application, thereby contributing to a longer pot life. A substrate having a low water content means a substrate having a water content of 5% by mass or less. Examples of thickeners include polyvinyl alcohol (PVA), sodium poly(meth)acrylate, alkali swelling type (meth)acrylic emulsion, carboxymethyl cellulose (CMC), methyl cellulose (MC), hydroxyethyl cellulose (HEC), hydroxypropyl cellulose (HPC), polyvinyl alcohol, and synthetic smectite. These can be used alone or in combination of two or more. Among these, sodium poly(meth)acrylate is preferred from the viewpoints of more reliably ensuring the pot life after application of the aqueous polyurethane emulsion composition and obtaining storage stability.
[0072] The blending amount of the thickener is preferably 1.0 to 3.5 parts by mass, particularly preferably 1.5 to 3.0 parts by mass, relative to 100 parts by mass of the aqueous polyurethane emulsion composition (theoretical solid content of the aqueous polyurethane resin). If the blending amount of the thickener is less than 1.0 part by mass, when the substrate to be coated has a low water content, the touch-dry time after coating of the aqueous polyurethane emulsion composition is shortened, and sufficient pot life cannot be secured, which tends to reduce workability, and the storage stability of the aqueous polyurethane emulsion composition tends to decrease. On the other hand, if the blending amount exceeds 3.5 parts by mass, when the aqueous polyurethane emulsion composition is applied to a substrate with a high water content, sufficient water-resistant adhesion tends not to be obtained.
[0073] The blending ratio of finely powdered silica to the thickener (finely powdered silica / thickener) is preferably a mass ratio of 1.0 to 6.0 / 1.0, particularly preferably 2.0 to 5.0 / 1.0, from the viewpoint of achieving a well-balanced improvement in the water-resistant adhesion and ensuring a sufficient pot life of the aqueous polyurethane emulsion composition.
[0074] Next, a method for producing the aqueous polyurethane emulsion composition used in the present invention will be described. The composition containing the aqueous polyurethane emulsion used in the present invention is a composition in which an aqueous polyurethane resin is dispersed in water, and the method for producing the composition can be a conventional method, and is not particularly limited. Specifically, the composition can be produced by, for example, the method described in JP-A-2020-152815.
[0075] The average particle size of the aqueous polyurethane resin (emulsion) is preferably 10 to 1,000 nm, more preferably 20 to 500 nm, and particularly preferably 40 to 400 nm. If the average particle size of the aqueous polyurethane resin (emulsion) is less than 10 nm, the water-resistant adhesion after application of the aqueous polyurethane emulsion composition tends to decrease, and if the average particle size exceeds 1,000 nm, the storage stability of the aqueous polyurethane emulsion composition tends to decrease. In this specification, the average particle size is a value determined by particle size distribution measurement by laser diffraction scattering method.
[0076] In addition to the above components, the aqueous polyurethane emulsion composition can use additives other than the above-mentioned fine silica powder and thickeners, as long as the object of the present invention is not impaired.Specific examples of additives include adhesion promoters other than the above-mentioned adhesion promoters, antifoaming agents, leveling agents, antioxidants, ultraviolet absorbers, fillers, and preservatives.Each of these additives can be used alone or in combination of two or more.
[0077] Specific examples of other adhesion promoters include epoxy silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3,4-epoxycyclohexylethyltrimethoxysilane, 3,4-epoxycyclohexyltriethoxysilane, and 3,4-epoxycyclohexylethylmethyldimethoxysilane; vinyl groups or (meth)acryloxypropyltrimethoxysilane such as vinyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, vinylmethyldimethoxysilane, and 3-methacryloxypropyltrimethoxysilane; Examples of the coupling agents include unsaturated hydrocarbon silane coupling agents having an acrylyl group, and hydrocarbon silane coupling agents such as methyl silicate, methyltrimethoxysilane, ethyltrimethoxysilane, butyltrimethoxysilane, octyltrimethoxysilane, dodecyltrimethoxysilane, phenyltrimethoxysilane, dimethyldimethoxysilane, diethyldimethoxysilane, dibutyldimethoxysilane, diphenyldimethoxysilane, trimethylmethoxysilane, triethylmethoxysilane, and triphenylmethoxysilane, and ureidosilane coupling agents such as 3-ureidopropyltriethoxysilane.
[0078] Specific examples of the defoaming agent include silicone-based defoaming agents such as mineral oil-based nonionic surfactants, polydimethylsiloxane oil, EO- or PO-modified dimethyl silicone or dimethyl silicone emulsion, mineral oil, and alcohol-based defoaming agents such as acetylene alcohol.
[0079] By applying an aqueous adhesive composition to a substrate using the trowel of the present invention instead of a solvent-based urethane adhesive composition using an organic solvent, a sufficient pot life can be ensured after application of the aqueous adhesive composition even in a summer environment (high temperature and humidity), and the adhesive strength of the aqueous adhesive composition can be improved. In particular, when a solvent-based urethane adhesive composition is applied to a substrate with a high water content, the adhesive strength tends to decrease, but when an aqueous adhesive composition is applied to a substrate with a high water content using the trowel of the present invention, the water-resistant adhesion can be improved.
[0080] In addition, the comb trowel of the present invention is suitable for applying an aqueous adhesive composition rather than a solvent-based urethane adhesive composition, and the use of an aqueous adhesive composition provides an excellent working environment and prevents sick house syndrome, resulting in an excellent indoor environment.
[0081] Next, a construction method using the comb trowel of the present invention will be described. The construction method includes the following steps (1) to (3).
[0082] (1) A step of applying an aqueous adhesive composition to a substrate using the comb trowel of the present invention. (2) A step of attaching the aqueous adhesive composition to a flooring material (3) Optionally, compressing the flooring. A construction method including the steps of carrying out the above in this order.
[0083] The application method of the present invention will be further described. First, the process of applying the aqueous adhesive composition to the substrate using the comb trowel of the present invention will be described. The substrate surface to which the aqueous adhesive composition is applied is adjusted to be even using a substrate conditioner such as level mortar. In this case, if there is any unnecessary matter such as dust on the substrate surface, it is removed in advance. If the substrate surface is not uneven, the substrate conditioner need not be used. Next, an appropriate amount of the aqueous adhesive composition is applied to the substrate surface, and the aqueous adhesive composition is spread evenly on the substrate surface using the comb trowel of the present invention. Next, the process of attaching the aqueous adhesive composition to the flooring material will be described. A predetermined flooring material is attached without gaps on the aqueous adhesive composition (adhering surface) that has been evenly spread on the substrate surface. There is no need to provide a pot time (open time) for the purpose of volatilization of water (dispersion medium) after application of the aqueous adhesive composition until attachment, and the flooring material can be attached immediately after application of the aqueous adhesive composition. After attachment of the flooring material, the surface of the flooring material can be optionally pressed using a pressing tool such as a roller. By pressing the surface of the flooring material, the aqueous adhesive composition is sufficiently crushed, improving the adhesion between the base and the flooring material, and reducing unevenness on the surface of the flooring material. By using a construction method including such steps, a floor structure is formed in which the base, the aqueous adhesive composition (adhesive layer), and the flooring material are integrated in this order.
[0084] Examples of the substrate include substrates mainly used in buildings, such as concrete, mortar, stone, metal, ceramic, wood, and resin. Among these, water-absorbent substrates such as concrete, mortar, and wood can be suitably used in that sufficient pot life can be ensured and excellent water-resistant adhesion can be obtained by applying an aqueous adhesive composition such as an aqueous urethane adhesive composition (an aqueous urethane adhesive composition optionally containing fine powder silica and a thickener as necessary) using the comb trowel of the present invention. When the moisture content of the substrate is 0 to 15% by mass, particularly 0 to 12% by mass, the above-mentioned effects of the present invention tend to be easily exhibited. In this specification, the moisture content of the substrate is a value measured by a high-frequency capacitance moisture meter.
[0085] Examples of flooring materials include flooring materials that are primarily used in buildings, such as stone tiles, ceramic tiles, metal plates, wood plates, resin sheets, and resin tiles. EXAMPLES
[0086] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0087] <Synthesis Example 1> In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen seal tube, and a heating / cooling device, 344 g of polytetramethylene ether glycol (PTG 2000, number average molecular weight 2,000, manufactured by Hodogaya Chemical Co., Ltd.), 126 g of isophorone diisocyanate (IPDI), and 0.03 g of dibutyltin dilaurate (DBTDL) were charged and stirred while flowing nitrogen gas into the reaction vessel, and reacted for 2 hours at 80° C. Next, after cooling this reaction liquid to 50° C., 23.5 g of dimethylolpropionic acid (DMPA), 17.7 g of triethylamine (TEA), and 194 g of acetone were added and stirred to react for 3 hours. Further, 216g of acetone was added to this reaction liquid and cooled to 30℃, 8.5g of 3-aminopropyltriethoxysilane was added and stirred, a mixture of 10g of hydrazine monohydrate, 103g of isopropyl alcohol (IPA) and 778g of water was added and stirred at high speed, and the acetone and IPA were distilled off from this liquid to obtain an aqueous polyurethane emulsion composition. The obtained aqueous polyurethane emulsion composition had a nonvolatile content of 41% by mass, a viscosity at 25℃ of 110mPa s (B-type rotational viscometer, 60 rpm), and an average particle size of 78nm.
[0088] <Preparation Example 1> Nitrogen gas was passed through a mixing vessel equipped with a stirrer, a thermometer, and a nitrogen seal tube, and 1,000 g of the aqueous polyurethane emulsion composition of Synthesis Example 1 was charged and stirred, and 35.3 g of fumed silica (Reolosil QS-102, Tokuyama Corporation) as fine powder silica, 7.5 g of sodium polyacrylate (Aron A-20L, Toagosei Co., Ltd.) as a thickener, and 0.5 g of a silicone-based defoamer (KS-66, Shin-Etsu Chemical Co., Ltd.) as a defoamer were charged and stirred to prepare an aqueous adhesive composition (aqueous urethane adhesive composition). The aqueous urethane adhesive composition had a nonvolatile content of 43% by mass, a viscosity of 45,000 mPa·s at 6 rpm at 25°C, a viscosity of 27,200 mPa·s at 12 rpm at 25°C, and a thixotropic index (TI value: viscosity at 6 rpm / viscosity at 12 rpm, 25°C, B-type rotational viscometer) of 1.67.
[0089] <Example 1> As the comb trowel for the aqueous adhesive composition, the comb trowel for the aqueous adhesive composition of the first embodiment was used. Specifically, the comb trowel for the aqueous adhesive composition of the present invention was used, in which the height (total height) of the comb teeth (notches of the comb teeth) was 4 mm, the width of the comb teeth (notches of the comb teeth) was 2 mm, the ratio (height / width) of the height of the comb teeth (notches of the comb teeth) to the width of the comb teeth (notches of the comb teeth) was 2, the pitch of the comb teeth (notches of the comb teeth) was 8 mm, and the comb shape was an isosceles triangle, and the following tests were performed using the comb trowel for the aqueous adhesive composition of the present invention.
[0090] <Comparative Example 1> Instead of the above-mentioned comb trowel for the aqueous adhesive composition of the present invention, a comb trowel (JIS A 5536:2015 "Adhesives for Floor Finishing Materials" 6.2b)1) was used, in which the height (total height) of the comb teeth (notches in the comb teeth) is 2 mm, the width of the comb teeth (notches in the comb teeth) is 2 mm, the ratio (height / width) of the height of the comb teeth (notches in the comb teeth) to the width of the comb teeth (notches in the comb teeth) is 1, the pitch of the comb teeth (notches in the comb teeth) is 5 mm, and the shape of the comb teeth is an isosceles triangle, was used to carry out the following tests.
[0091] [Test Method] (1) Peel adhesion strength The peel adhesion strength was measured according to JIS A 5536:2015 "Adhesives for floor finishing materials" 6.3.3 Peel adhesion strength. The floor material used was Viewista (manufactured by Tajima Roofing Co., Ltd.), the adhesive used was the aqueous urethane adhesive composition of Preparation Example 1, and the base material used was a flexible board (water content 3.7% by mass) measuring 150 mm in length, 70 mm in width, and 5 mm in thickness. The amount of application of the aqueous urethane adhesive composition was approximately 245 g / m2 using the comb trowel of Example 1 and Comparative Example 1. 2 The time from application of the aqueous urethane adhesive composition to attachment of the flooring material (potable time (open time)) was 5 minutes, 20 minutes, and 40 minutes, and the temperature and humidity were 23°C 50% RH and 35°C 70% RH. The moisture content of the flexible board was measured using a high-frequency capacitance moisture meter (HI-520, Kett Electric Laboratory Co., Ltd.) with the target material being mortar, thickness correction set to 10 mm, and temperature correction set to AUTO.
[0092] (2) Peel adhesion strength (wet surface) [Normal] Peel adhesion strength was measured in accordance with JIS A 5536:2015 "Adhesives for Floor Finishing Materials" 6.3.3 Peel Adhesion Strength. The flooring material used was Viewista (manufactured by Tajima Roofing Co., Ltd.), the adhesive used was the aqueous urethane adhesive composition of Preparation Example 1, and the base material used was a mortar board (water content 10.4% by mass) measuring 150 mm in length, 70 mm in width, and 10 mm in thickness. The mortar board was immersed in water at 23°C for 24 hours, and after removal, its surface was wiped with a rag so that the adhesive surface was wet. The amount of application of the aqueous urethane adhesive composition was approximately 245 g / m2 using a comb trowel in Example 1 and Comparative Example 1. 2 The time from application of the aqueous urethane adhesive composition to attachment of the flooring material (open time) was 2 minutes, and the temperature and humidity were 23°C and 50% RH. The moisture content of the mortar board was measured using a high-frequency capacitance moisture meter (HI-520, Kett Electric Laboratory Co., Ltd.) with the target material being mortar, the thickness correction being 10 mm, and the temperature correction being AUTO. [Submersion in water] Peel adhesion strength was measured according to JIS A 5536:2015 "Adhesives for floor finishing materials" 6.3.3 Peel adhesion strength. The test specimens were prepared in the same condition as for peel adhesion strength (wet surface), and then immersed in water at 23°C for 7 days, and then wiped with a cloth after removal.
[0093] (3) Height of floor finishing material (exterior) The aqueous urethane adhesive composition of Preparation Example 1 was applied to a flexible board (water content 4.5% by mass) of 280 mm length x 200 mm width x 5 mm thickness using the comb trowels of Example 1 and Comparative Example 1, and after 5 minutes of pot life (open time), a PVC sheet (transparent vinyl mat, manufactured by Nitori Co., Ltd.) was attached as a flooring material. After the flooring material was attached, a 60 mm wide hand roller was used to press the flooring material back and forth twice with a load of about 50 N, and the material was cured at 23°C and 50% RH for 2 days. The height of the flooring material from the flexible board after curing (the difference between the height between the flexible board surface and the flooring surface of the part coated with the aqueous urethane adhesive composition and the height between the flexible board surface and the flooring surface of the part not coated with the aqueous urethane adhesive composition, i.e., the height of the adhesive layer of the part coated with the aqueous urethane adhesive composition) was measured using a microscope. The moisture content of the flexible board was measured using a high-frequency capacitance moisture meter (HI-520, Kett Electric Laboratory) with the target material being mortar, thickness correction set to 10 mm, and temperature correction set to AUTO.
[0094] In Reference Examples 1 and 2, instead of the aqueous urethane adhesive composition of Preparation Example 1, a solvent-based urethane adhesive composition, Auton Floor Grip S (manufactured by Auto Chemical Industry Co., Ltd.), was used as the adhesive composition, and the pot life (open time) was set to 20 minutes, but the same test as for the height (appearance) of the floor finishing material was performed, and the height of the flooring material from the flexible board after curing was measured with a microscope. In Reference Example 1, the comb trowel of Example 1 was used, and in Reference Example 2, the comb trowel of Comparative Example 1 was used.
[0095] The test results are shown in Tables 1 and 2.
[0096] [Table 1]
[0097] [Table 2]
[0098] From Table 1, Example 1 had a higher peel strength than Comparative Example 1, and was excellent in workability because it could extend the working time. Comparative Example 1 was unable to attach the flooring material after 40 minutes of working time at 23°C 50% RH and after 20 minutes of working time at 35°C 70% RH. Therefore, it was found that Comparative Example 1 was inferior in workability because it was necessary to attach the flooring material in a short time after applying the aqueous urethane adhesive composition, especially in the summer with high temperature and humidity. This is presumably because the aqueous urethane adhesive composition was applied with the comb trowel of Comparative Example 1, the aqueous urethane adhesive composition dried before the flooring material was attached, and a hardened film was generated on the surface of the aqueous urethane adhesive composition, making it impossible to attach the flooring material. In addition, it was found that Example 1 had a higher peel strength (wet surface) than Comparative Example 1 in terms of normal adhesive strength, so it had good adhesive strength even when the substrate was wet or had a high moisture content, and had excellent water-resistant adhesive strength because it had high adhesive strength when immersed in water. Furthermore, when the aqueous urethane adhesive composition was applied with the comb trowel of Example 1, the height of the flooring after installation was 0.56 mm from the flexible board (base material), which was lower than that of the comb trowel of Comparative Example 1, resulting in an overall less noticeable appearance of the flooring. The comb trowel of Comparative Example 1 uses a trowel with a lower tooth height than the comb trowel of Example 1, but with the comb trowel of Comparative Example 1, the aqueous urethane adhesive composition dried quickly, and it is presumed that a hardened film was formed on the surface of the aqueous urethane adhesive composition, which was not sufficiently crushed even when pressed.
[0099] As can be seen from Table 2, in Reference Example 1, in which the solvent-based urethane adhesive composition was applied using the comb trowel of Example 1, the height of the flooring after installation was 1.86 mm from the flexible board (base material), which was higher than in Reference Example 2, in which the solvent-based urethane adhesive composition was applied using the comb trowel of Comparative Example 1, resulting in an appearance in which the entire flooring stands out (the applied area was slightly higher and looked wavy, and felt wavy to the touch).From the above, it can be seen that the comb trowel of the present invention is a comb trowel that is suitable for applying an aqueous adhesive composition rather than a solvent-based urethane adhesive composition.
[0100] As described above, the comb trowel of the present invention can be used as an aqueous adhesive composition for flooring materials, and is particularly suitable as an aqueous adhesive composition for flooring materials for buildings. In addition, by applying the aqueous adhesive composition using the comb trowel of the present invention to a base and attaching a flooring material, a floor structure with excellent water-resistant adhesion can be formed. [Explanation of symbols]
[0101] 1, 12, 13 Comb iron 2 Comb section 21 Notch (comb) 22 Occlusion
Claims
1. A comb trowel for use with an aqueous adhesive composition, the comb trowel having alternating notches and plugs at its ends, The comb trowel is characterized in that the height of the notch is 2.5 to 6.0 mm, the width of the notch is 1.0 to 4.0 mm, the ratio of the height of the notch to the width of the notch (height / width) is 1.3 to 3.0, and the pitch of the notch is 4.0 to 12.0 mm and the comb portion is formed in plurality.
2. A comb trowel for use with an aqueous adhesive composition, the comb trowel having alternating notches and plugs at its ends, the aqueous adhesive composition is an aqueous urethane adhesive composition, The comb trowel is characterized in that the height of the notch is 2.5 to 6.0 mm, the width of the notch is 1.0 to 4.0 mm, the ratio of the height of the notch to the width of the notch (height / width) is 1.3 to 3.0, and the pitch of the notch is 4.0 to 12.0 mm and the comb portion is formed in plurality.
3. A comb trowel for use with an aqueous adhesive composition, the comb trowel having alternating notches and plugs at its ends, the aqueous adhesive composition has a viscosity of 15,000 to 40,000 mPa s (12 rpm, 25°C, Brookfield viscometer), a TI value (viscosity at 6 rpm / viscosity at 12 rpm, 25°C, Brookfield viscometer) of 1.3 to 3.0, and a non-volatile content of 20 to 80 mass%; The comb trowel according to claim 1 or 2, characterized in that the height of the notch is 2.5 to 6.0 mm, the width of the notch is 1.0 to 4.0 mm, the ratio of the height of the notch to the width of the notch (height / width) is 1.3 to 3.0, and the notch has a pitch of 4.0 to 12.0 mm and is formed in plurality at the comb portion.
4. A comb trowel for use with an aqueous adhesive composition, the comb trowel having alternating notches and plugs at its ends, The aqueous adhesive composition is used for flooring materials, The comb trowel according to claim 1 or 2, characterized in that the height of the notch is 2.5 to 6.0 mm, the width of the notch is 1.0 to 4.0 mm, the ratio of the height of the notch to the width of the notch (height / width) is 1.3 to 3.0, and the notch has a pitch of 4.0 to 12.0 mm and is formed in plurality at the comb portion.
5. Applying the aqueous adhesive composition to a substrate using the comb trowel according to claim 1 or 2; A step of bonding the aqueous adhesive composition to a flooring material; Optionally, compressing the flooring. A construction method including the steps of carrying out the above in this order.
6. The construction method according to claim 5, wherein the moisture content of the base is 0 to 15% by mass (measured by a high-frequency capacitance moisture meter).
7. Applying the aqueous adhesive composition to a substrate using the comb trowel according to claim 1 or 2; A step of bonding the aqueous adhesive composition to a flooring material; Optionally, compressing the flooring. A floor structure formed by a construction method including the steps of:
Citation Information
Patent Citations
Adhesive composition for flooring material
JP2020152815A