Silicone rubber hose

The silicone rubber hose addresses kink resistance, heat resistance, and thread detachment issues by balancing forces through inclined knitting rows, enhancing flexibility and durability for milking and chemical cleaning applications.

JP2024158071AActive Publication Date: 2024-11-08TOYOX CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023072927
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

Existing milking hoses made of silicone rubber face issues with kink resistance, heat resistance, flexibility, and thread detachment, leading to handling difficulties, increased strain on dairy cows, and reduced lifespan, which are exacerbated by automation demands and chemical cleaning processes.

Method used

A silicone rubber hose with a durometer A hardness of 35 to 85, tear strength of 5 to 60 N/mm, and a viscoelastic recovery rate to permanent strain rate ratio of 2.2 or more, featuring a braid wound between inner and outer layers with inclined knitting rows to balance forces and prevent thread detachment, while maintaining flexibility and transparency.

Benefits of technology

The hose exhibits excellent kink resistance, heat resistance, and flexibility, preventing thread detachment and maintaining shape under twisting, with improved durability and longevity, especially in milking and chemical cleaning environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158071000001_ABST
    Figure 2024158071000001_ABST
Patent Text Reader

Abstract

To provide a silicone rubber hose with excellent kink resistance and heat resistance and good flexibility and transparency.SOLUTION: A silicone rubber hose H1 is manufactured from a highly elastic silicone rubber with a durometer A hardness of 35 to 85 measured in accordance with JIS-K-6253 and a tear strength (Sa) of 5 to 60 N / mm measured in accordance with JIS-K-6252, and a ratio (viscoelastic recovery rate / permanent set rate) of a viscoelastic recovery rate defined by the following formula (1) to a permanent set rate defined by the following formula (2) is 2.2 or more: viscoelastic recovery rate={(elongation deformation amount-stress residual deformation recovery amount-residual set amount) / elongation deformation amount}×100 ...(1); permanent set rate=(residual set amount / elongation deformation amount)×100 ...(2).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silicone rubber hose having excellent kink resistance, heat resistance, flexibility and transparency, for use in, for example, the food, beverage, medical equipment, chemical and other industries, and in particular to a milking hose. [Background technology]

[0002] Tubes and hoses used in the medical, food industry, industrial parts, and other fields require flexibility, transparency, and kink resistance, and have traditionally been made of polyvinyl chloride resin. However, in recent years, due to growing concern about environmental issues, tubes and hoses made of silicone rubber instead of polyvinyl chloride resin have been developed (Patent Document 1).

[0003] For milking purposes, flexible milking hoses are used in milking machines used in milking work to extract milk from dairy cows, etc. Milking hoses are used between the milking head attached to the udder of the dairy cow, etc., and the milking machine main body that generates suction force to collect milk, and for piping inside the milking machine main body. In order to improve workability and to avoid putting a strain on the udder when a milking hose is used between the milking head and the milking machine main body, flexibility is required for the milking hose. In addition, the milking hose is required to be kink-resistant.

[0004] As milking hoses, typically, tubes formed with a thick wall from silicone rubber or the like, or tubes formed from soft resins are known. Such tubes are solid cylindrical. For example, Patent Document 2 discloses a resin composition containing an amorphous α-olefin polymer, a petroleum resin, and an amorphous α-olefin polymer, and a tube made of the resin composition, and discloses that the tube has excellent kink resistance and heat resistance and can be used for milking purposes. Patent Document 2 also discloses a multi-layer tube in which layers made of linear low-density polyethylene resins with different moduli and polyolefin elastomer layers are laminated, and discloses that the tube suppresses the elution of material components, is flexible, and can be used for milking purposes. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-54052 A [Patent Document 2] JP 2003-129188 A Summary of the Invention [Problem to be solved by the invention]

[0006] From the viewpoint of milking in particular, a heavy milking hose is not only difficult to handle during milking, but also places a burden on the udders of dairy cows, etc., and is therefore undesirable. That is, there is a demand for lighter milking hoses. A tubular (solid cylindrical) milking hose as described in the above patent document needs to be relatively thick-walled to prevent kinking when bent, and it is difficult to reduce the weight. Furthermore, as attempts to automate milking work are being made, if a milking hose is easily damaged, milking work becomes impossible and the health of dairy cows, etc. is easily harmed, and therefore there is a demand for milking hoses with a long life.

[0007] In addition, in conventional silicone reinforced hoses, if the silicone rubber of the inner and outer layers is softened to make it easier to use, when a pulling force acts in the axial direction of the silicone reinforced hose or when the entire hose expands due to a change in internal pressure, the inner and outer layers expand and contract in the axial direction, but the expansion rate of the braid material is significantly lower than that of silicone rubber, and in addition, silicone rubber has high releasability and lubricity, so the braid moves more easily than other rubbers or constituent resins. Therefore, every time the silicone reinforced hose expands and contracts, the braid gradually moves from the axial end of the silicone reinforced hose and the thread comes out, causing a problem that the pressure resistance of the part where the thread comes out is significantly reduced.

[0008] Furthermore, in the connection structure of a silicone reinforced hose, the pressure resistance of the connection end arranged at the axial end of the silicone reinforced hose drops significantly due to the above-mentioned braid coming loose, so that the braid is likely to break between the connection end and the connection fitting, in which case the connection fitting must be discarded together with the broken hose, resulting in a problem of high cost of hose replacement. Therefore, in order to prevent the braid from coming loose, it is conceivable to insert the connection end of the reinforced hose into the outer circumferential surface of the nipple and then strongly tighten it from the outside with a tightening tool to reduce the diameter, thereby pinching the blade so that it does not move.

[0009] However, in this case, when the fastener is tightened strongly, the silicone rubber sandwiched between the fastener and the nipple is pushed out, causing a step between the inner surface of the nipple and the inner surface of the hose, causing problems such as the fluid transported through the hose remaining in the step or increasing the resistance inside the pipe. In addition, as a means for preventing the braid from coming loose, it is possible to increase the adhesion between the inner and outer layers by applying a silicone rubber-based primer to the surface of the braid, but this increases the cost.

[0010] The tubes and silicone-reinforced hoses of the prior art were not fully satisfactory in terms of kink resistance and heat resistance. Under such circumstances, the problem that the present invention aims to solve is to provide a hose that is excellent in kink resistance and heat resistance, and has good flexibility and transparency. A milking hose is particularly preferable. Furthermore, it is intended to prevent the braid from coming loose, to increase the rigidity of the silicone rubber hose against twisting to prevent the silicone rubber hose from being crushed due to twisting, and to prevent the hose connection end from breaking with a simple structure, even for a silicone rubber hose molded from a silicone rubber with excellent flexibility. [Means for solving the problem]

[0011] As a result of extensive research, the present inventors have discovered that the above problems can be solved by the silicone rubber hose of the present invention. The silicone rubber hose of the present invention is manufactured using silicone rubber with excellent elasticity, having a durometer A hardness of 35 to 85 measured in accordance with JIS-K-6253 and a tear strength (Sa) of 5 to 60 N / mm measured in accordance with JIS-K-6252, and is formed by wrapping a braid between an inner layer and an outer layer, the silicone rubber hose comprising the inner layer made of silicone rubber extruded by an extrusion molding device, the braid formed in layers by knitting into a tubular shape by a knitting machine along the outer peripheral surface of the inner layer, and the outer layer made of silicone rubber extruded on the outside of the braid, which are laminated together, the warp knitted rows of the knitted braid are wound in a spiral shape at an angle from the axial direction of the hose, and the weft knitted rows are wound in a spiral shape so as to be perpendicular to the warp knitted rows, and the silicone rubber constituting the inner layer and the outer layer has a ratio of viscoelastic recovery defined by the following formula (1) to permanent set defined by the following formula (2) (viscoelastic recovery / permanent set) of 2.2 or more. Viscoelastic recovery rate = {(elongation deformation amount - stress residual deformation recovery amount - residual strain amount) / elongation deformation amount} × 100 (1) Permanent set rate = (residual set amount / elongation deformation amount) × 100 (2) Effect of the Invention

[0012] According to the present invention, it is possible to provide a silicone rubber hose that has excellent kink resistance, heat resistance, flexibility, and transparency. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a partially cutaway front view of a silicone rubber hose according to a first embodiment of the present invention. [Diagram 2] FIG. 4 is a partially cutaway front view of a silicone rubber hose according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] (First embodiment) A first embodiment of the present invention will be described below with reference to Fig. 1. A silicone rubber hose H1 (see Fig. 1) according to the first embodiment of the present invention is made of silicone rubber having a durometer A hardness of 35 to 85 measured in accordance with JIS-K-6253 and a tear strength (Sa) of 5 to 60 N / mm measured in accordance with JIS-K-6252. The durometer A hardness and tear strength were measured by subjecting uncured millable silicone rubber to a curing reaction in an environment of 200°C for 2 hours and measuring the results according to the methods specified by the respective JIS standards.

[0015] By setting the silicone rubber hardness in this range, it is possible to obtain a product that is highly resistant to kinking and does not lose much flexibility. If the hardness is less than 35, the product will have good flexibility but will be prone to kinking, while if the hardness is more than 85, the product will be too hard and will be less user-friendly than metal flexible piping.

[0016] Furthermore, the silicone rubber constituting the silicone rubber hose H1 of this embodiment has a ratio of viscoelastic recovery defined by the following formula (1) to the permanent set defined by the following formula (2) (viscoelastic recovery / permanent set) of 2.2 or more, preferably 2.25 or more, more preferably 2.3 or more, and even more preferably 2.5 or more. If this value is too low, the kink resistance may deteriorate. Viscoelastic recovery rate = {(elongation deformation amount - stress residual deformation recovery amount - residual strain amount) / elongation deformation amount} × 100 (1) Permanent set rate = (residual set amount / elongation deformation amount) × 100 (2)

[0017] Here, the elongation deformation amount, stress residual deformation recovery amount, and residual strain amount are values ​​determined from an elastic hysteresis test of the resin composition, and the elongation deformation amount represents the deformed length of the silicone rubber when it is elongated to a predetermined length (state A). The stress residual deformation recovery amount represents the change in the deformed length of the silicone rubber from state A to state B when the tensile load is gradually reduced from state A to zero (state B). The residual strain represents the deformed length of the silicone rubber when it is left to stand in a free state for a certain period of time after state B (state C).

[0018] The elastic hysteresis test of silicone rubber is carried out by the following method. (1) Before curing, millable silicone rubber is press-molded at 160°C and then cured in an environment of 200°C for 2 hours to produce a sheet with a thickness of 0.5 mm. (2) From the sheet, a dumbbell-shaped No. 1 test piece (gauge length = 40 mm) is prepared in accordance with JIS-K-6251. (3) The test piece is subjected to the following operations (i) to (iii) at a temperature of 23° C. using a tensile tester (Strograph R, manufactured by Toyo Seiki Seisaku-sho, Ltd.). (4)(i) The test piece is stretched to a stretch deformation rate of 100% (gauge length 80 mm) at a crosshead speed of 500 mm / min (stretch deformation amount = 40 mm). (5)(ii) Immediately after extension, the test piece is contracted at a crosshead speed of 500 mm / min until the tensile stress becomes zero. (6)(iii) Measure the gauge length when the tensile stress becomes zero, and calculate the difference between that length and the gauge length of 80 mm when the elongation deformation rate is 100%, and use this value as the stress residual deformation recovery amount. (7)(4) Immediately after the tensile stress of the test piece becomes zero, leave the test piece at rest in a free state at 23°C for 5 minutes, and measure the gauge length. The difference between the gauge length and the gauge length of 40 mm before the test is calculated, and this value is regarded as the amount of residual strain.

[0019] The silicone rubber hose H1 of this embodiment has excellent heat resistance, transparency, and kink resistance, and can be used for various molded products.

[0020] The silicone rubber used to manufacture the silicone rubber hose H1 of this embodiment has a tear strength (measured according to JIS-K-6252) of 5 to 60 N / mm after pre-curing millable silicone rubber is press-molded at 160°C and then cured in an environment of 200°C for 2 hours. If the tear strength is less than 5 N / mm, the deformation does not return when the hose is bent or stretched, causing dimensional deviation, which causes the wall thickness to change and makes it difficult to handle, and there is a concern that the hose may tear from the point where the wall thickness has changed, which is undesirable. Furthermore, if the tear strength is greater than 60 N / mm, the hose is difficult to deform and difficult to handle, and the rebound elasticity when bent and used is large, which reduces workability, which is undesirable.

[0021] In the silicone rubber hose H1 of this embodiment, the inner and outer layers made of silicone rubber that meets a specific range of physical properties expand and contract in the axial direction of the hose, and the cylindrically knitted braid also expands and contracts in the same direction. Furthermore, when the entire hose is twisted in the circumferential direction, the forces acting on the two intersecting braided rows are balanced, and the hose maintains its cylindrical shape. In addition, by reducing the diameter with the liner sandwiched between the outer circumferential surface of the hose connection end and the tightening tool, the tightening tool is protected from direct contact with the outer circumferential surface of the hose connection end.

[0022] As shown in Fig. 1, silicone rubber hose H1 is formed by integrating inner layer 1 and outer layer 2 by knitting braid 3 into a cylindrical shape between them to form a layered structure. Fig. 1 shows a case in which a liner 5 is placed over the outer circumferential surface of connection end 4 of silicone rubber hose H1, and a nipple portion 7a of a fitting 7 is connected by reducing the diameter of the liner 5 from the outside using a tightening tool 6.

[0023] The inner layer 1 and outer layer 2 are manufactured using silicone rubber, which has excellent flexibility as its main component. First, the inner layer 1 is extruded using a known extrusion molding device, and then the braid 3, which will be described later, is woven along its outer peripheral surface using a knitting machine (not shown). The outer layer 2 is then extruded and laminated on the outside of the braid 3.

[0024] The braid 3 thus knitted is made of reinforcing threads or fibers such as polyester, nylon, or aramid fiber, and is made of warp knit rows 3a extending in the axial direction of the silicone rubber hose H1 and weft knit rows 3b intersecting the warp knit rows 3a and extending in the circumferential direction of the silicone rubber hose H1, knitted in an elastic manner. The warp knit rows 3a and weft knit rows 3b are knitted in such a way that the warp knit rows 3a are parallel to the axial direction of the hose H, and the weft knit rows 3b are perpendicular to the warp knit rows 3a, or, as shown in Fig. 1, the braids are wound in a spiral shape at a predetermined angle inclined from the axial direction of the silicone rubber hose H1 so that the forces acting on the warp knit rows 3a and weft knit rows 3b are balanced with respect to the twist of the silicone rubber hose H1. The crossing angle of the warp knit rows 3a and weft knit rows 3b may be inclined at any angle other than the approximately right angle shown in the figure.

[0025] Considering that the silicone rubber hose H1 will be used particularly in food processing machines and medical equipment, the liner 5 is preferably made of a material that is safe from the standpoint of food hygiene and has excellent heat resistance, such as hard or semi-hard silicone rubber, fluororesin, nylon resin, etc. Using these materials, the liner 5 is formed into a cylindrical shape having approximately the same outer diameter as or slightly larger than the outer diameter of the connection end 4 of the silicone rubber hose H1, or into a double cylindrical shape having a horizontally oriented approximately U-shaped cross section.

[0026] The liner 5 is formed into a roughly cylindrical shape, and a crimped pipe 6a of a fastener 6 described later is placed over the outside of this cylindrical liner 5a. The crimped pipe 6a is then crimped to reduce its diameter, whereby the connection end 4 of the silicone rubber hose H1 is connected to a nipple portion 7a of a fitting 7 described later.

[0027] The crimping pipe 6a of the fastener 6 is made of a rigid material such as stainless steel or aluminum that undergoes compressive deformation when radially pressurized by, for example, a driven or manual hydraulic crimping machine (not shown) but does not return to its original shape when subjected to a repulsive force from the silicone rubber hose H1, and is formed in a cylindrical shape covering the outer peripheral surface of the connection end 4 of the silicone rubber hose H1.

[0028] The crimped pipe 6a of the fastener 6 is made of a rigid material such as stainless steel or aluminum that undergoes compressive deformation when radially pressurized by, for example, a driven or manual hydraulic crimping machine (not shown) but does not return to its original shape when subjected to a repulsive force from the silicone rubber hose H1, and is formed in a cylindrical shape covering the outer peripheral surface of the connection end 4 of the silicone rubber hose H1.

[0029] The above-mentioned joint 7 is made of hard synthetic resin or metal, and has a bamboo-shoot-shaped nipple portion 7a formed at its axial tip end, and a connecting means 8 for connecting to another device provided at its base end. In the example shown in Fig. 1, the inner surface 7b at the tip end of the nipple portion 7a is inclined so that its wall thickness gradually becomes thinner toward the tip.

[0030] Furthermore, as a connection means 8 to another device, for example a flange portion 8a as disclosed in Utility Model Registration No. 3061574 is integrally formed, this flange portion 8a and a flange portion 8b of the other device are arranged opposite each other and a sealing material 8c such as an O-ring is sandwiched between the two, and these two flange portions 8a, 8b are connected and tightened with a clamp 8d, thereby closely attaching and detaching them.

[0031] As a result of the above, when a tensile force acts in the axial direction of the silicone rubber hose H1 of this embodiment, or when the entire silicone rubber hose H1 expands due to a change in internal pressure and expands or contracts in the axial direction of the silicone rubber hose H1, the warp knit rows 3a and weft knit rows 3b of the tubularly knitted braid 3 also expand or contract in the same direction. As a result, it is possible to prevent threads from coming loose from the braid 3. In particular, since the knitting is performed by knitting the braid (reinforcing threads, reinforcing fibers) in alternating vertical and horizontal directions as shown in Figure 1, it is possible to dramatically prevent threads from coming loose compared to a braid wound in a spiral shape.

[0032] Furthermore, even if the entire silicone rubber hose H1 is twisted in the circumferential direction, the forces acting on the intersecting warp knitted rows 3a and weft knitted rows 3b are balanced and the silicone rubber hose H1 maintains its cylindrical shape. As a result, the rigidity of the silicone rubber hose H1 against twisting is increased, and the silicone rubber hose H1 can be prevented from collapsing due to twisting.

[0033] Furthermore, by reducing the diameter of the silicone rubber hose H1 with the liner 5 sandwiched between the outer circumferential surface of the connection end 4 and the fastener 6, the fastener 6 is protected from direct contact with the outer circumferential surface of the connection end 4. As a result, even in a hose made of silicone rubber with excellent flexibility, the connection end 4 can be prevented from breaking with a simple structure.

[0034] Furthermore, as shown in FIG. 1, when the connection end 4 of the silicone rubber hose H1 is reduced in diameter by crimping the crimped pipe 6a, a space S into which the silicone rubber is pushed out is defined at the base end of the crimped pipe 6a, and when the tip inner surface 7b of the nipple portion 7a of the fitting 7 is inclined, even if the crimped pipe 6a is tightly tightened to reduce the diameter, no step is created between the tip inner surface 7b and the inner surface 4a of the hose connection end 4, preventing the transported fluid from remaining and the resistance inside the pipe from increasing.

[0035] The silicone rubber of this embodiment may contain other resins, rubber / elastomer components, additives, etc., as necessary. Examples of other resins include polyethylene resins such as high-density polyethylene, medium-density polyethylene, low-density polyethylene, and linear low-density polyethylene (LLDPE), ethylene copolymer resins such as ethylene-vinyl acetate copolymer resin, ethylene-acrylate copolymer resin, ethylene-methacrylate copolymer resin, and ethylene-styrene copolymer resin, homopolypropylene resin, block polypropylene resin, polybutene resin, poly-4-methyl-pentene-1 resin, polystyrene resin, polyester resin, polyamide resin, polyphenylene ether resin, polyacetal resin, and polycarbonate resin. Examples of rubber / elastomer components include natural rubber; polybutadiene; liquid polybutadiene; polyacrylonitrile rubber; acrylonitrile-butadiene copolymer rubber; partially hydrogenated acrylonitrile-butadiene copolymer rubber; ethylene-based rubbers with an ethylene unit content of 70 mol% or more, such as ethylene-propylene rubber, ethylene-butene rubber, ethylene-hexene rubber, and ethylene-octene rubber; fluororubber; urethane rubber; isobutylene-isoprene copolymer rubber; non-crosslinked olefin-based thermoplastic elastomers, partially crosslinked olefin-based thermoplastic elastomers, and fully crosslinked olefin-based thermoplastic elastomers.

[0036] Examples of additives include antioxidants, antioxidants, antiozone deterioration agents, stabilizers such as ultraviolet absorbers and light stabilizers, lubricants, fillers, flame retardants, high-frequency processing aids, antistatic agents, internal release agents, colorants, dispersants, antiblocking agents, and antifogging agents.

[0037] Examples of the lubricant include wax, higher alcohol, fatty acid, fatty acid metal salt, fatty acid amide, carboxylate, phosphoric acid ester, sulfonic acid metal salt, acid ester metal salt, acrylic resin, fluorine-containing resin, and silicone. Two or more of these may be used in combination.

[0038] Examples of the wax include petroleum waxes such as paraffin wax and microcrystalline wax; vegetable waxes such as rice wax; mineral waxes such as montan wax; and synthetic waxes such as polyethylene wax and low molecular weight polypropylene.

[0039] Examples of the higher alcohol include lauryl alcohol, myristyl alcohol, palmityl alcohol, stearyl alcohol, behenyl alcohol, oleyl alcohol, erucyl alcohol, and 12-hydroxystearyl alcohol.

[0040] Examples of the fatty acid include lauric acid, palmitic acid, stearic acid, behenic acid, oleic acid, erucic acid, linoleic acid and ricinoleic acid.

[0041] Examples of the fatty acid metal salts include salts of fatty acids such as lauric acid, palmitic acid, stearic acid, behenic acid, oleic acid, erucic acid, linoleic acid, and ricinoleic acid with metals such as Li, Na, Mg, Al, K, Ca, Zn, Ba, and Pb.Specific examples of the fatty acid metal salts include lithium stearate, sodium stearate, calcium stearate, and zinc stearate.

[0042] Examples of the fatty acid amides include lauric acid amide, palmitic acid amide, stearic acid amide, oleic acid amide, erucic acid amide, methylene bisstearic acid amide, ethylene bisstearic acid amide, ethylene bisoleic acid amide, and stearyl diethanol amide.

[0043] Examples of the carboxylic acid esters include esters of carboxylic acids such as aliphatic carboxylic acids (acrylic acid, crotonic acid, isocrotonic acid, fumaric acid, maleic acid, succinic acid, aconitic acid, etc.), fatty acids (lauric acid, palmitic acid, stearic acid, behenic acid, oleic acid, erucic acid, linoleic acid, ricinoleic acid, etc.), and oxycarboxylic acids (lactic acid, malic acid, tartaric acid, citric acid, etc.) with alcohols such as aliphatic alcohols (myristyl alcohol, palmityl alcohol, stearyl alcohol, behenyl alcohol, 12-hydroxystearyl alcohol, etc.), aromatic alcohols (benzyl alcohol, β-phenylethyl alcohol, phthalyl alcohol, etc.), and polyhydric alcohols (glycerin, diglycerin, polyglycerin, sorbitan, sorbitol, propylene glycol, polypropylene glycol, polyethylene glycol, pentaerythritol, trimethylolpropane, etc.). Specific examples of carboxylates include glycerin monooleate, glycerin dioleate, polyethylene glycol monostearate, and citrate distearate.

[0044] Examples of the phosphoric acid ester include monoalkyl esters, dialkyl esters and trialkyl esters of phosphoric acid and higher alcohols.

[0045] Examples of the acrylic resin include polymers mainly composed of structural units derived from acrylic acid esters such as acrylic acid, methyl acrylate, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate, and structural units derived from methacrylic acid esters such as methacrylic acid, methyl methacrylate, ethyl methacrylate, butyl methacrylate, and 2-ethylhexyl methacrylate.Specific examples of the acrylic resin include an acrylic resin manufactured by Mitsubishi Chemical under the trade name Metablen, and an acrylic resin manufactured by Kaneka under the trade name Kane Ace.

[0046] Examples of the above-mentioned metal sulfonates include sodium stearyl sulfonate, sodium lauryl sulfonate, sodium dodecylbenzenesulfonate, sodium dodecylnaphthalenesulfonate, potassium stearylsulfonate, potassium lauryl sulfonate, dibutyl sodium sulfosuccinate, di-2-ethylhexyl sodium sulfosuccinate, disodium lauryl sulfosuccinate, and 2-sodium lauryl polyoxyethylene sulfosuccinate.

[0047] Examples of the acid ester metal salts include sulfates such as sodium lauryl sulfate and potassium lauryl sulfate; and phosphates such as sodium lauryl phosphate and potassium lauryl phosphate.

[0048] Examples of the above-mentioned fluorine-containing resins include fluorine-containing olefins such as tetrafluoroethylene, hexafluoropropylene, fluoroalkylethylene and perfluoroalkylvinylether; fluorine-containing alkyl acrylates such as perfluoroalkyleneacrylate and perfluoromethalkyleneacrylate; and polymers having as their main unit a structural unit derived from a fluorine-containing compound such as fluorine-containing alkyl methacrylate.Specific examples of the fluorine-containing resins include polytetrafluoroethylene and perfluoro(polyoxypropylene ethyl ether).

[0049] The silicone rubber hose H1 of the present embodiment can be used as piping for oil, various chemicals, air, various gases, water, etc. in the fields of various industrial vehicles, such as automobiles, construction machinery, agricultural machinery, and railway cars; various industrial and mining machinery, such as machine tools, construction machinery, agricultural machinery, mining machinery, industrial robots, chemical plants, coating machines, chemical transfer machines, food industry machinery, and hydraulic tools; and ships.

[0050] Specific examples of the silicone rubber hose H1 of this embodiment include automobile hoses such as filler hoses, evaporation hoses, fuel hoses, vapor emission hoses, in-tank fuel hoses, power steering hoses, air conditioning hoses, radiator hoses, heater hoses, transmission oil cooler hoses, engine oil cooler hoses, brake hoses, turbocharger drain hoses, fuel injection hoses, air conditioning hoses, air duct hoses, air intake hoses, vacuum control hoses, and air pollution control hoses; hoses for hydraulic machines, hoses for pneumatic machines, hoses for centralized lubrication equipment, hoses for painting equipment, hoses for chemical plants, hoses for transferring solvents and chemical liquids, hoses for transferring various liquefied gases, hoses for food-related machines, hoses for beverage-related machines, hoses for chemical plants, and the like. Examples of the hoses include hoses for various industrial machines and vehicles such as hoses for academic equipment, hoses for spinning machines, hoses for packing machines, hoses for printing machines, hoses for transmission machines, hoses for water treatment devices, hoses for fluid elements, hoses for industrial robots, hoses for industrial vehicles, hoses for agricultural machines, hoses for construction machines, hoses for machine tools, hoses for injection molding machines, hoses for labor-saving machines, hoses for air tools such as air drivers and air hammers, hoses for moving parts, hoses for air pressure / electrical signals, hoses for air pressure / signals, hoses for equipment that require heat resistance, high insulation, and high frequency characteristics, hoses for spot welding equipment, steam hoses, agricultural spray hoses, brewing hoses, diving hoses, bandless oil hoses, gas tubing hoses, air brake hoses, gas station hoses, tanker hoses, rotary hoses, and fire extinguisher hoses; hoses for medical equipment such as various infusion hoses and intake and exhaust hoses. In particular, the hoses are preferable as milking hoses.

[0051] The silicone rubber hose H1 according to the present embodiment described above can provide the following effects. That is, in the silicone rubber hose H1 of the present embodiment, as the inner and outer layers made of silicone rubber expand and contract in the axial direction of the hose, the tubular knitted braid also expands and contracts in the same direction, preventing the braid from coming loose. Therefore, compared to conventional hoses in which the braid is prone to coming loose when the silicone of the inner and outer layers is softened, the pressure resistance of the entire hose can be maintained high and rupture can be prevented, and manufacturing costs can be reduced compared to hoses in which the adhesion between the inner and outer layers is increased by applying a silicone rubber-based primer to the surface of the braid, for example.

[0052] Furthermore, when the entire hose is twisted in the circumferential direction, the forces acting on the two intersecting braided rows are balanced and the hose maintains its cylindrical shape, increasing the rigidity of the hose against twisting and preventing the hose from collapsing due to twisting. It also has high durability against cleaning with chemicals used in milking, and has a long life. Not only for milking, but when used in industries that use cleaning with chemicals, it can be used with a much longer life than conventional products.

[0053] Second embodiment Next, a second embodiment of the present invention will be described with reference to Fig. 2. A silicone rubber hose H2 according to the second embodiment of the present invention (see Fig. 2) is manufactured in a manner different from that of the silicone rubber hose H1 of the first embodiment. Other configurations are the same as those of the first embodiment, so description thereof will be omitted. The silicone rubber hose H2 of this embodiment is manufactured by forming a liner 105 that covers the outer peripheral surface of the connection end 4 of the silicone rubber hose H2 into a double cylindrical shape having a substantially horizontal U-shaped cross section, and fitting this double cylindrical liner 105b to the connection end 4.

[0054] The silicone rubber hose H2 of this embodiment provides the same effects as the silicone rubber hose H1 of Embodiment 1. Furthermore, since the inner circumferential surface of the connection end 4 of the silicone rubber hose H2 contacts the barb-like nipple portion 7a of the joint 7 via the inner cylindrical portion of the double cylindrical liner 105b, there is an advantage that the inner circumferential surface of the connection end 4 of the silicone rubber hose H2 is less likely to be damaged by this barb-like nipple portion 7a.

[0055] 2, a general belt-shaped hose band 106d is wound around the outside of the liner 5 as the fastener 106, thereby reducing the diameter of the liner 5 and the hose connection end 4. However, this is not limited to this, and the diameter may be reduced by crimping the crimped pipe 6a as in the manufacturing method of the silicone rubber hose H1 of the first embodiment, or conversely, a general belt-shaped hose band 106d may be used for the silicone rubber hose H1 of the first embodiment.

[0056] 2, in this embodiment, a cylindrical connecting tube portion 108e is protruded as a connecting means 108 to another device provided on the base end side of the joint 7, and a coupling portion 108f such as a screw is formed on the outer circumferential surface of the connecting tube portion 108e. Note that this is not limited to this, and the connecting means 8 to another device in the manufacturing method in the first embodiment may be used, or conversely, the connecting means 108 to another device shown in the second embodiment may be used for the manufacturing method in the first embodiment.

[0057] Third embodiment Next, a third embodiment of the present invention will be described. The silicone rubber hose according to the third embodiment of the present invention is manufactured in a different manner from the silicone rubber hose H1 of the first embodiment. Other configurations and effects are the same as those of the first embodiment, so descriptions are omitted. The silicone rubber hose according to this embodiment is manufactured by configuring the silicone rubber hose H1 of the first embodiment without covering the outer peripheral surface with a liner 5.

[0058] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments, and various modifications are possible without departing from the gist of the present invention. EXAMPLES

[0059] The present invention will be described in more detail below with reference to examples and comparative examples. In the examples, the physical properties of the silicone rubber hose were measured by the following methods.

[0060] 1. Viscoelastic recovery rate / permanent set rate In the examples, the ratio of viscoelastic recovery to permanent set of the silicone rubber constituting the silicone rubber hose (viscoelastic recovery / permanent set) was determined by determining the elongation deformation amount, stress residual deformation recovery amount, and residual strain amount according to the following procedures (i) to (iv), and then calculating the viscoelastic recovery and permanent set according to the following formulas (1) and (2). (i) Silicone rubber was press-molded at 160°C, and then cured for 2 hours at 200°C to produce a sheet with a thickness of 0.5 mm. (ii) From the produced sheet, a dumbbell-shaped No. 1 test piece (gauge length = 40 mm) as specified in JIS-K-6251 was prepared. (iii) The prepared test pieces were subjected to the following operations using a tensile testing machine (Strograph R, manufactured by Toyo Seiki Seisaku-Sho, Ltd.). (a) The test piece was stretched at a crosshead speed of 500 mm / min to a stretch deformation rate of 100% (gauge length = 80 mm) (stretch deformation amount = 40 mm). (b) Immediately after the test piece was stretched, it was contracted at a crosshead speed of 500 mm / min until the tensile stress reached zero. (c) The gauge length was measured when the tensile stress of the test piece became zero, and the difference between the measured gauge length and the gauge length of 80 mm when the elongation deformation rate was 100% was calculated. This value was regarded as the stress residual deformation recovery amount. (iv) The test piece whose tensile stress had become zero was immediately allowed to stand for 5 minutes in a free state at a temperature of 23°C after the tensile stress had become zero, and the gauge length was measured. The difference between the measured gauge length and the gauge length of 40 mm before the test was calculated, and this value was regarded as the amount of residual strain. Viscoelastic recovery rate = {(elongation deformation amount - stress residual deformation recovery amount - residual strain amount) / elongation deformation amount} × 100 (1) Permanent set rate = (residual set amount / elongation deformation amount) × 100 (2)

[0061] 2.Hardness Before curing, the millable silicone rubber was press molded at 160°C and then cured for 2 hours in a 200°C environment to produce a sheet with a thickness of 2 mm. The durometer hardness (Duro-A) of the sheet was measured according to JIS-K-6253.

[0062] 3. Kink resistance The molded silicone rubber hose (inner diameter 25.4 mm, outer diameter 35.5 mm) was wound around a 50 mm cylinder in an atmosphere of 23° C. and evaluated according to the following criteria.

[0063] 4.Transparency The pre-cured millable silicone rubber was press molded at 160° C., and then subjected to a curing reaction for 2 hours in an environment of 200° C. to produce a sheet having a thickness of 1 mm. The haze of the sheet was measured according to JIS-K-7105.

[0064] 5. Presence or absence of holes A pressure-resistant nipple was inserted into one end of a molded silicone rubber hose (inner diameter 25.4 mm, outer diameter 35.5 mm) and the end was sealed off by tightening it with a band. Air was continuously supplied into the inside of the hose from the other end, and the state of the reinforcing thread was confirmed when the hose burst due to pressure from inside the hose.

[0065] 6. Tear strength Before curing, Millable silicone rubber was press molded at 160°C, and then cured for 2 hours in an environment of 200°C. Measurements were then carried out according to JIS-K-6251.

[0066] (Measurement results) Each of the silicone rubber hoses of Examples 1 to 8 and Comparative Examples 1 to 5 shown in Table 1 below was installed in actual milking equipment at multiple dairy farms (Dairy Farm A to Dairy Farm D) and monitored and evaluated during daily milking work. These milking hoses were loaned for monitoring purposes without disclosing composition information, etc., and all of them were collected after the monitoring period. The "hardness" in Table 1 refers to durometer A hardness. The "hose characteristics" in Table 1 refers to the ratio of viscoelastic recovery rate to permanent set rate (the above-mentioned formula (1) / formula (2)). Examples 1 to 6 are silicone rubber hoses with a "hardness" of 35 to 80, a "tear strength" of 8 to 58 N / mm, and a "hose characteristic" of 2.2 to 2.8. Comparative Example 1 had a "tear strength" of more than 60. Comparative Example 2 had a "tear strength" of less than 5. Comparative Example 3 had a "hose characteristic" of less than 2.2.

[0067] Regarding the "manufacturing method" in Table 1, "1" is a silicone rubber hose manufactured by the manufacturing method shown in the first embodiment, "2" is a silicone rubber hose manufactured by the manufacturing method shown in the second embodiment, and "3" is a silicone rubber hose manufactured by the manufacturing method shown in the third embodiment. The "commercially available tube" in Comparative Example 4 is a commercially available milking hose, which is Sangohan's FEP Site Tube (product number 3316FEPTB16T, inner diameter 25.4 mm), and the "commercially available hose" in Comparative Example 5 is a commercially available milking hose, which is Sangohan's SB Hose (product number SB100 16B, inner diameter 25.4 mm).

[0068] [Table 1]

[0069] According to the monitor evaluation, the silicone rubber hoses of Examples 1 to 8 were rated as being lighter and easier to handle than the conventional thick-walled hoses / tube-shaped milking hoses (Comparative Examples 4 and 5) in terms of flexibility and lightness, which are related to the ease of handling of the milking equipment.

[0070] Table 2 below shows the evaluation results of the life span of the silicone rubber hoses of Examples 1-8 and the silicone rubber hoses / tubes of Comparative Examples 1-5.

[0071] The "kink resistance" in Table 2 was evaluated according to the following criteria. ○: The outer diameter of the hose wrapped around the cylindrical body is 50% or more of the original outer diameter. △: The outer diameter of the hose wrapped around the cylindrical body is between 30% and 50% smaller than the original outer diameter. ×: The outer diameter of the hose wrapped around the cylinder is less than 30% of the original outer diameter.

[0072] The "transparency" in Table 2 was judged by evaluating the measured haze according to the following criteria. Good: Haze is less than 70%. ×: Haze is greater than 70%.

[0073] The "washing durability" (lifespan) in Table 2 was judged by having 10 monitored dairy farms use silicone rubber hoses / tubes for up to two months, and if a part of the hose wall hardened or deformed to the point that it became difficult to use, if the hose wall broke and started leaking, or if cracks became noticeable in the hose wall, etc., it was judged that the hose could no longer be used and had reached the end of its lifespan, and was rated as x. If no cracks were observed and the hose was still usable, but some of the hose showed signs of hardening or deformation, it was rated as △. If no such notable findings were observed and the hose was the same as the original, it was rated as ○. Naturally, some of the hoses deteriorated before the two months had passed.

[0074] The "presence or absence of voids" in Table 2 was evaluated according to the following criteria. Yes: The reinforcing thread does not break at the hose rupture point. None: Reinforcing thread breaks at the hose rupture point.

[0075] [Table 2]

[0076] One silicone rubber hose from each Example, a total of 80 hoses, and one silicone rubber hose / tube from each Comparative Example, a total of 50 hoses / tubes, were monitored. One month after the start of monitoring, the hose / tube from the Comparative Example had samples rated △, samples that had reached the end of their life, and samples rated × or had come loose in any of the evaluation items. On the other hand, the silicone rubber hoses from each Example had samples rated △ after two months, and no samples rated × were observed during the two-month monitoring period.

[0077] As shown in Table 2, it was found that the silicone rubber hoses of each Example had excellent kink resistance, were transparent, and had a long life compared to the hoses of Comparative Examples 1 to 3. Furthermore, it was found that the silicone rubber hoses of each Example had no loss of reinforcing threads and were prevented from bursting compared to the hoses of Comparative Examples 4 and 5, and could be used continuously for milking work for a long period of time, making them highly economical.

[0078] When the silicone rubber hose of each embodiment is used as a milking hose, deterioration occurs in relation to the manner of use during cleaning work. Milking hoses are frequently cleaned inside after use to prevent the growth of dirt and germs. A high-temperature (60°C to 80°C) cleaning liquid containing acid or alkali is used for this internal cleaning work. In addition, in order to increase the cleaning efficiency, not only is the cleaning liquid continuously flowed during cleaning work, but the cleaning liquid is intermittently sent into the inside of the hose in a splash-like manner together with air by utilizing the negative pressure of the milking device. In addition, during this cleaning work, the silicone rubber hose takes a bent posture. Then, the high-temperature cleaning liquid that flows into the inside of the hose in a splash-like manner does not collide much with the hose wall in the straight part of the silicone rubber hose, while the cleaning liquid collide violently with the inside of the hose wall in the curved part of the silicone rubber hose. As a result, the silicone rubber hose is exposed to the high-temperature cleaning liquid in a specific part. Therefore, the bent part of this silicone rubber hose is easily deteriorated when it is cleaned. [Explanation of symbols]

[0079] 1 Inner layer 2 Outer layer 3 braid 3a warp knit row 3b Horizontal knitting row 4 Connection end 5 Liner H1, H2 Silicone Rubber Hose

Claims

1. A silicone rubber hose is manufactured using highly elastic silicone rubber having a durometer A hardness of 35 to 85 as measured in accordance with JIS-K-6253 and a tear strength (Sa) of 5 to 60 N / mm as measured in accordance with JIS-K-6252, and has a braid wound between an inner layer and an outer layer, a silicone rubber hose comprising: an inner layer made of silicone rubber extruded by an extrusion molding device; a braid formed in a layer by knitting into a tubular shape by a knitting machine along the outer peripheral surface of the inner layer; and an outer layer made of silicone rubber extruded on the outside of the braid, the warp knitted rows of the knitted braid are wound in a spiral shape at a predetermined angle from the axial direction of the hose, and the weft knitted rows are wound in a spiral shape so as to be perpendicular to the warp knitted rows, and the silicone rubber constituting the inner layer and the outer layer has a ratio of viscoelastic recovery defined by the following formula (1) to permanent set defined by the following formula (2) (viscoelastic recovery rate / permanent set rate) of 2.2 or more: Viscoelastic recovery rate={(elongation deformation amount−stress residual deformation recovery amount−residual strain amount) / elongation deformation amount}×100 (1) Permanent set rate=(residual set amount / elongation deformation amount)×100 (2)

2. 2. A silicone rubber hose according to claim 1, wherein the outer peripheral surface of the connecting end of the hose is covered with a liner, the diameter of which is reduced from the outside by a fastener, and the connecting end of the hose is connected to a fitting.

3. 2. The silicone rubber hose according to claim 1, which is used for milking.

Citation Information

Patent Citations

  • Special silicone tube for automatic milking production line of dairy cows

    CN212971131U

  • Olefin-based resin composition, tube and hose

    JP2004285299A

  • Silicone rubber composition, its production method and its molded article

    JP2005171004A

  • Silicone reinforced hose

    JP2010054052A

  • Silicone rubber-based curable composition and molded body

    JP2018053237A