Method of separating dissimilar bonded body
The method employs bubble nucleation and foaming stimuli to separate metal and resin bodies, addressing the challenge of strongly stabilized interfaces by enabling efficient recycling and reducing fragility, with minimal residual resin.
Patent Information
- Application Number
- JP2023073208
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing methods for joining metal and resin bodies without adhesives result in strongly stabilized bonded interfaces that are difficult to disassemble, hindering recycling and posing fragility risks during use.
A method involving bubble nucleation and foaming stimuli is used to separate metal and resin bodies by generating thermodynamic work at the bonded interface, utilizing a pressure container to impregnate the heterozygous body with a bubble nucleation gas and then heating it to a predetermined temperature to induce macroscopic volumetric expansion.
The method effectively decomposes the bonding interface, allowing for easy separation of metal and resin bodies while maintaining structural integrity during use and reducing environmental impact by minimizing residual resin on the metal body.
Smart Images

Figure 2024158209000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for separating a heterogeneous bonded body in which a metal body and a resin body are bonded to each other. [Background technology]
[0002] A technology that directly bonds a metal body and a resin body without using adhesives is attracting attention. For example, Patent Document 1 discloses a method for manufacturing electric and electronic components in which a metal surface is irradiated with laser light to form irregularities, and then a resin or the like is injection molded into the areas where the irregularities are formed; the irregularities formed on the metal surface enhance the anchoring effect. Patent Document 2 discloses a method for producing a composite molded article in which a joining surface of a metal molded article is roughened by continuous irradiation with laser light, thereby increasing the joining strength with a resin molded article.
[0003] Such a bonded structure has a strongly stabilized bonded interface and is not easily disassembled. However, in today's society where contributions to the realization of a resource-recycling society are essential, it is desirable to separate the heterogeneous bonded body into the metal body and the resin body and recycle each of them. Furthermore, when disposing of the product, it is necessary to be able to disassemble the bonded body by breaking down the stable bonded interface, while at the same time, it is necessary for the bonded body to be robust during use. Therefore, there is a demand for technology that can achieve both. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-294024 [Patent Document 2] JP 2015-142960 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a method for separating a metal body and a resin body, as required, from each other in a heterogeneous joined body in which a metal body and a resin body are joined. [Means for solving the problem]
[0006] The method for separating heterogeneous bonded bodies according to the present invention is a method for separating a metal body and a resin body from a heterogeneous bonded body in which a resin body is bonded to a rough surface of a metal body, and is characterized in that it comprises a bubble nucleation step of impregnating the heterogeneous bonded body with a bubble nucleation gas, and a foaming step of foaming the bubble nucleation gas impregnated in the heterogeneous bonded body.
[0007] In order to separate and break down a strongly stabilized bonded interface, it is necessary to generate thermodynamic work at the bonded interface, i.e., volume expansion, sufficient to overcome the condensation energy of the interface. In the present invention, a foaming phenomenon initiated by bubble nucleation induced by an external stimulus causes macroscopic volume expansion, thereby freely decomposing the bonded interface of a heterogeneous bonded structure. By separating the metal body and the resin body using multiple stimuli, with an external stimulus (bubble nucleation process) as the first stimulus and a foaming-inducing stimulus (foaming process) as the second stimulus, it is possible to prevent the heterogeneous bonded body from becoming brittle (accidental separation) during use, etc.
[0008] In the present invention, the bubble nucleation step may include sealing the heterogeneous conjugate and a bubble nucleation gas in a pressure-resistant vessel and creating a high pressure state in the pressure-resistant vessel. For example, the method may include the steps of sealing the heterogeneous conjugate and a bubble nucleation gas in a pressure vessel, creating a high pressure state inside the pressure vessel, and reducing the pressure inside the pressure vessel. By sealing the heterogeneous bond and a bubble nucleation gas (for example, carbon dioxide gas) in a pressure-resistant vessel and applying high pressure, the bubble nucleation gas is impregnated into the resin, and bubble nuclei are generated at the bonded interface.
[0009] In the present invention, the foaming step may involve heating the heterogeneous bonded body impregnated with the bubble nucleation gas in the bubble nucleation step to a predetermined temperature. For example, the method may include the steps of removing the heterogeneous conjugate impregnated with the bubble nucleation gas from the pressure vessel, and heating the heterogeneous conjugate impregnated with the bubble nucleation gas to a predetermined temperature. By subjecting the heterogeneous bonded body impregnated with the bubble nucleation gas to a heat treatment, the bubble nuclei that appeared in the bubble nucleation step expand, forming gaps at the bonded interface and reducing the strength.
[0010] For example, in the bubble nucleation step, the inside of the pressure-resistant vessel may be set to 10 MPa or more. This makes it easy to reduce the energy required to separate the metal body and the resin body in the foaming step even when the heating temperature is in the low temperature range. For example, in the foaming step, the predetermined temperature may be equal to or lower than the glass transition temperature of the resin constituting the resin body. This makes it easier to reduce the proportion of the resin body remaining on the surface of the metal body when the joint interface between the metal body and the resin body is decomposed and the heterogeneous joint body is disassembled. Effect of the Invention
[0011] According to the present invention, the bonding interface between the metal body and the resin body that constitute the heterogeneous bonded body is decomposed by multiple stimuli, so that the bonding strength between the metal body and the resin body is high when the heterogeneous bonded body is in use, and the metal body and the resin body can be separated when necessary, such as when discarding the body. [Brief description of the drawings]
[0012] [Figure 1] The heterozygote of this example is shown. [Diagram 2] The method for isolating heterozygotes in this example is shown below. [Diagram 3] The results of Test 1-1 (gas concentration impregnated in resin) are shown below. [Figure 4] The results of Test 1-2 (expansion ratio) are shown below. [Diagram 5] The results of test 2 (strength) are shown. [Figure 6] The results of Test 3 (resin body remaining rate) are shown. [Figure 7] The relationship between strength and resin body remaining rate is shown. [Figure 8] An example of the results of Test 4 (interface photograph using X-rays) is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The heterogeneous bonded body according to the present invention refers to a bond between a metal body and a resin body without the use of an adhesive. For example, the surface of a metal body is roughened by laser light irradiation or atmospheric pressure plasma treatment, etc. (for example, the formation of irregularities in Patent Document 1, and the formation of open holes, internal spaces, tunnel connecting paths, open spaces, etc. in Patent Document 2), and a resin body is injection molded or compression molded onto this roughened surface, with the resin body embedded in the roughened surface, thereby producing a heterogeneous joint body. For example, in a medical device in which the interface between a metal body and a resin body is bonded with an adhesive, if the metal body and the resin body are bonded without the use of adhesive, there is no risk of the adhesive leaking into medicines or other items inside the medical device. Such adhesive-free heterogeneous bonded bodies are expected to be used in a variety of applications, including medical devices, food packaging, and automobile parts.
[0014] The metal body is not particularly limited in its metal, and may be, for example, selected from aluminum or its alloys, iron, stainless steel, zinc, magnesium, copper, lead, tin, and alloys containing these. For example, the metal body may be manufactured by a die casting method, or may be anodized, plated, electrocoated, or the like.
[0015] The resin body is not particularly limited in terms of the resin, and examples thereof include thermoplastic resins, thermosetting resins, thermoplastic elastomers, amorphous resins, and crystalline resins. From the viewpoint of foaming the resin, however, amorphous resins are preferable. For example, examples of amorphous resins include polycarbonate, polyvinyl chloride, polystyrene, polymethyl methacrylate, acrylonitrile-butadiene-styrene, modified polyphenylene ether, polyethersulfone, polyetherimide, and polyamideimide; examples of thermosetting resins include epoxy resin, polyurethane, and phenolic resin; and examples of crystalline resins include polyethylene, polypropylene, polyamide, polyethylene terephthalate, polybutylene terephthalate, polyphenylene sulfide, polyether ether ketone, liquid crystal polymer, and polytetrafluoroethylene. The resin body may contain a known fibrous filler in addition to the resin. Examples of fibrous fillers include carbon fibers (e.g., pitch-based, rayon-based, lignin-based, etc.), inorganic fibers (e.g., glass fibers, basalt fibers, silica fibers, zirconia fibers, silicon nitride fibers, etc.), metal fibers (e.g., fibers made of stainless steel, aluminum, copper, etc.), and organic fibers (e.g., polyamide fibers, polyvinyl alcohol fibers, acrylic fibers, etc.), and there are no particular limitations on the amount of resin and fibrous filler to be mixed.
[0016] In the following, as the present embodiment, the metal body is an aluminum alloy (A5052, approximately 45×10×1.5 mm 3 , hereafter referred to as "Al"), and the resin body was polycarbonate containing 40% by weight of glass fiber (Panlite (registered trademark) G3440L1 BLK (manufactured by Teijin Limited), approximately 45 x 10 x 3 mm 3 Hereinafter, the heterologous conjugate (DLAMP (registered trademark) (manufactured by Daicel Miraize Co., Ltd.), hereinafter referred to as "Al-PC / GF40") will be used as an example for explanation. As shown in Fig. 1, the surface of the aluminum end was roughened by irradiating it with laser light. 2 ) is joined to PC / GF40 by injection insert molding.
[0017] In this specification, separation of a heterogeneous bonded body preferably means separating the metal body and the resin body constituting the heterogeneous bonded body so that each of them can be recycled. When the bonding interface between the metal body and the resin body is decomposed and the bonded body of different types is disassembled, if the proportion of the resin body remaining on the surface of the metal body is low, both the metal body and the resin body will have excellent recyclability. Furthermore, if the energy required to separate the metal body and the resin body is small, the environmental load of energy can be reduced.
[0018] FIG. 2 shows the method for isolating heterologous conjugates in this example, and the interface condition in the figure shows the concept of the present invention. The separation method includes a bubble nucleation step of impregnating the heterogeneous bonded body with a bubble nucleation gas, and a foaming step of foaming the bubble nucleation gas impregnated in the heterogeneous bonded body. While "homogeneous nucleation" refers to the generation of bubbles in a homogeneous solvent (such as in a liquid phase), "heterogeneous nucleation" refers to the generation of bubbles at a two-layer interface such as a solid surface, and the present invention is deeply related to this heterogeneous nucleation. The heterogeneous nucleation rate J is given by the following equation (1). F(θ) is the wetting angle factor, θ is the contact angle between the solid surface and the bubble, m' is a parameter that represents the wetting angle, m is the mass of one particle, γ is the surface tension, k B is the Boltzmann constant, T is the temperature, and P D is the internal pressure of the bubble, P C is the atmospheric pressure, and N is the number of particles per unit volume in the metastable state. TIFF2024158209000002.tif23166It is believed that bubble nucleation is likely to occur at the interface of heterogeneous bonded structures because the free energy barrier for bubble nucleation is low, creating a thermodynamically favorable condition. Based on this theory, by heating a gas-impregnated heterogeneous composite, bubbles are generated by utilizing the difference in the degree of gas saturation. Examples of the bubble nucleation gas include carbon dioxide and nitrogen. The bubble nucleation gas is preferably one having a high solubility in the resin, such as carbon dioxide. In the bubble nucleation step, the heterogeneous bond and a bubble nucleation gas are sealed in a pressure vessel, and the inside of the pressure vessel is brought to a high pressure state. After the pressure inside the pressure vessel has been kept at a high pressure for a predetermined period of time, the pressure is released to reduce the pressure. The slower the pressure reduction rate, the more the generated bubble nuclei can be prevented from foaming inside the pressure vessel. In the foaming step, the heterogeneous composite body impregnated with the bubble nucleation gas is removed from the pressure vessel and heated to a predetermined temperature. The following will explain this based on specific tests.
[0019] <Test 1-1: Impregnation test of bubble nucleation gas> An autoclave was used as a pressure-resistant vessel, and with the heterogeneous composite (Al-PC / GF40) placed inside the vessel, carbon dioxide gas was transferred from a tank to a cooling device and temporarily stored as a liquid. The gas was then sealed inside the vessel using the automatic control of a pressure pump. The pressure and temperature inside the pressure vessel were maintained at the specified levels using a pressure pump and autoclave, and the impregnation conditions for this test were an impregnation pressure of 5 MPa, 7.5 MPa, or 10 MPa, an impregnation temperature of 80°C, and an impregnation time of 24 hours. After 24 hours of impregnation, carbon dioxide gas was released and the pressure inside the pressure vessel was reduced over a period of 5 minutes. The method for calculating the concentration of carbon dioxide impregnated into the resin will be described later, but as for the change in carbon dioxide concentration with increasing impregnation time, from 0 to 18 hours of impregnation, it was impregnated in proportion to the time, but thereafter tended to increase gradually, and it was estimated that gas impregnation would reach saturation at 30 to 40 hours of impregnation, so the impregnation time in this test was set to 24 hours.
[0020] In the above impregnation test, the ratio of the amount of carbon dioxide impregnated into the resin (PC) is called the CO2 concentration G r The calculation method is shown in the following formula (2). w0 is the mass of the resin body, w p is the mass of the resin excluding the glass fiber, G a is the amount of gas impregnation. In one impregnation test, five pieces of Al-PC / GF40 were used for each impregnation pressure, and the weight of each sample was measured before and after the test to determine the amount of gas impregnation G. aThe carbon dioxide concentrations of the five samples were calculated using the above formula (2), and the average value was calculated. Figure 3 shows the results of the above impregnation test conducted five times, i.e., the CO2 concentration G in 25 samples for each impregnation pressure. r The average value and its standard deviation are shown.
[0021] As shown in FIG. 3, the change in carbon dioxide concentration indicates that the carbon dioxide concentration is proportional to the impregnation pressure. This is thought to be because as the impregnation pressure increases, the carbon dioxide gas concentration inside the pressure vessel becomes higher, and as a result, the gas concentration inside the resin increases. However, there is a limit to the gas concentration that can be impregnated into the resin, and as the pressure increases, the amount of impregnation becomes saturated, and the proportional trend ends at a certain pressure value.
[0022] <Test 1-2: Heating test after impregnation> After the pressure in the pressure vessel was reduced in the above impregnation test, the sample was removed from the pressure vessel and further heated on a hot plate. In this case, assuming that the bonding surface with PC / GF40 was on the front surface of the Al, the back surface of the Al was placed on the hot plate. The heating conditions were a heating temperature (hot plate temperature setting) of 110° C., 120° C., 130° C., 140° C., or 150° C., and a heating time of 180 seconds. The hot plate was preheated to a desired heating temperature.
[0023] In the above impregnation and heating test, the expansion ratio of the volume of the resin body by the carbon dioxide impregnated into the resin is called the expansion ratio X, and can be expressed by the following formula (3). ρ s is the specific gravity of the resin before the impregnation test, ρ f is the specific gravity of the resin body after the impregnation and heating (foaming) test. TIFF2024158209000004.tif23166When calculating the foaming ratio, it is necessary to determine the resin density before and after the test. The calculation method is shown in the following formulas (4) and (5), which incorporate approximate data from the average value of three randomly selected samples. The definitions of each symbol in formulas (4) and (5) are shown in Table 1 below. TIFF2024158209000005.tif23166TIFF2024158209000006.tif23166 [Table 1] After the above impregnation and heating tests, the volume of Al-PC / GF40 was measured using a specific gravity meter (MDS-300), and the data was used in the above formulas (4) and (5) to calculate the resin density. The resin densities before and after the tests were then substituted into the above formula (3) to calculate the expansion ratio. FIG. 4 shows the results of the expansion ratio. Each bar graph shows the average value for five samples. As shown in FIG. 4, the higher the impregnation pressure and the higher the heating temperature, the higher the expansion ratio.
[0024] <Test 2: Strength test> Using a universal testing machine (AGS-5kNX, manufactured by Shimadzu Corporation), the strength of the samples after the above-mentioned double stimulation (impregnation and heating test) was quantitatively measured. As comparative examples, strength tests were also carried out on samples in the initial state (before the impregnation test) and after a single stimulation (no heating after the impregnation test, or only heating without carrying out the impregnation test). For the strength test, the sample was fixed to a jig conforming to IS019095-3, two levels were attached, and a load was applied in a direction parallel to the sample interface. The strength test conditions were a load cell capacity of 5000 N and a tensile speed of 1 mm / min. After the strength test, the universal testing machine outputs a load-displacement diagram as data. The maximum load value in this load-displacement diagram is taken as the sample strength, and the results are shown in Figure 5. Each bar represents the average value for triplicate samples.
[0025] Looking at Figure 5 overall, for the samples after double stimulation, the higher the impregnation pressure and the higher the heating temperature, the lower the maximum load. As can be seen from Figures 3 and 4, this is thought to be because the higher the impregnation pressure, the more gas is impregnated into the resin, and the higher the heating temperature, the greater the expansion rate of the resin, making it easier to destroy the bond between the metal body and the resin body. Resins have a "melting point" at which the state of a substance changes from solid to liquid, and a "glass transition temperature" at which the substance transitions from a glassy state, in which the molecules are tightly bound, to a rubber-like state, in which the amorphous parts become more fluid, even in the same solid state. In Figure 5, the reason for the large decrease in strength when the heating temperature is 130°C or higher is that in the case of PC / GF40, the glass transition temperature is at approximately 130°C, and this temperature is the boundary where the mechanical properties change. In the temperature range above approximately 130°C, the resin transitions to a soft rubber-like state, relaxing the bonds at the interface, resulting in a decrease in strength. Looking closely at the results of the expansion ratio in Fig. 4 and the strength in Fig. 5, the expansion ratio at a heating temperature of 150°C shown in Fig. 4 was approximately 1.05 at an impregnation pressure of 5 MPa, approximately 1.10 at 7.5 MPa, and approximately 1.30 at 10 MPa, which was significantly higher in the high pressure range, whereas the strength at a heating temperature of 150°C shown in Fig. 5 was approximately 500 N at any impregnation pressure. On the other hand, the expansion ratio at 120°C was less than 1.05 at both impregnation pressures of 5 MPa and 7.5 MPa, and approximately 1.15 at 10 MPa, so the expansion ratio was high in the high pressure range, and the strength at a heating temperature of 120°C was also low in the high pressure range. From this, it is considered that the degree to which the expansion of the resin affects the interfacial strength changes depending on the heating temperature range.
[0026] <Test 3: Interface observation and image analysis> When the samples after the above impregnation and heating tests were subjected to the above strength test for tensile fracture, the amount of PC / GF40 remaining on the Al surface changed depending on the conditions. Therefore, the surface condition of the metal body was photographed using a digital microscope (VHX-7100) with a magnification of 20x and a VHX-E20 lens. After photographing, the area percentage of the resin remaining on the metal body surface was measured using the brightness analysis function of Image J. The threshold was set to 120, and the procedure was as follows: (1)Start Image J and open the image file. (2) Cut out only the joint part from the image. (3) Reduce the bit depth of the cropped image to 8 and display it in black and white. (4)Open Threshold and set the threshold to 120. (5) Open Analyze Particles and start the analysis to obtain the percentage of black area in the image. FIG. 6 shows the resin residue rate.
[0027] As can be seen from Figure 6, in the sample that was only heated, the proportion of residual resin gradually decreased as the heating temperature increased, and there was no significant change before and after the change in mechanical properties such as the glass transition point, remaining almost the same as the initial metal surface state. In contrast, in the samples after double stimulation, especially in the low-pressure range of impregnation pressures (5 MPa, 7.5 MPa), the proportion of residual resin after the glass transition point (approximately 130°C) increased sharply compared to before the transition point. This is thought to be related to bubble nucleation due to gas impregnation and the change in resin hardness before and after the glass transition point. Gas impregnation generates air bubbles in the resin (especially near the joint interface). In the subsequent heating process, if the heating temperature is higher than the glass transition point, the air bubbles are more likely to grow and the resin softens into a rubber-like material, reducing the strength of the material and making it more likely to break at locations other than the joint interface, resulting in an increase in the amount of residual material. On the other hand, if the heating temperature is below the glass transition point, the resin remains in a glassy state, making it easier to separate cleanly. In addition, in the sample that was only heated, no air bubbles were generated and the resin state did not change significantly. Therefore, even if the sample turned rubbery at a temperature higher than approximately 130°C, it would later return to a glassy state at room temperature, and it is believed that the residual amount did not change significantly from the initial state.
[0028] FIG. 7 shows the relationship between strength and the resin body remaining rate. The vertical axis indicates the relative strength, with the strength of the sample in its initial state (before the impregnation test) taken as 1. The closer the resin residual rate and relative strength are to 0, the less residual resin there is and the smaller the environmental load energy becomes. In this example, it was found that the double stimulation under the conditions of an impregnation pressure of 10 MPa and a heating temperature of 130°C resulted in the lowest proportion of PC / GF40 remaining on the Al surface after separation of Al and PC / GF40, and also resulted in a small environmental load energy.
[0029] <Test 4: X-ray observation> The state of bubbles near the bonded interface was observed by X-ray measurement. For X-ray measurement, the interface of the sample was cut into 2 × 10 × 2 mm pieces using a PCB cutter and manual precision polishing device. 3 It was molded into a square pillar. An example of an interface photograph taken using X-rays is shown in FIG. The left side of Figure 8 shows the initial state, and the right side shows a photograph of the interface after double stimulation under conditions of an impregnation pressure of 10 MPa and a heating temperature of 130°C. The lower part is Al, the upper part is PC / GF40, and the areas surrounded by triangles are traces of bubble nucleation and foaming. For example, under the conditions of an impregnation pressure of 5 MPa and a heating temperature of 140°C, and an impregnation pressure of 7.5 MPa and a heating temperature of 140°C, more bubble nucleation was observed on the resin body side than near the interface between the metal body and the resin body. When relating this to the results of the resin residual rate in Figure 6, it is believed that the proportion of residual resin was high because foaming and peeling frequently occurred in locations shifted from the joint interface. On the other hand, under the conditions of an impregnation pressure of 10 MPa and a heating temperature of 130°C, bubbles were observed near the interface as shown on the right side of Figure 8, and it is believed that peeling occurred at the bonding interface, resulting in little residual resin. In other words, in samples with a resin body residual rate close to 100%, cohesive failure occurred inside the resin body, while in samples in which a large number of air bubbles were generated at the bonding interface and interfacial peeling occurred, the resin body residual rate was thought to be low.
Claims
1. A method for separating a heterogeneous bonded body, in which a metal body and a resin body are respectively separated from a heterogeneous bonded body in which a resin body is bonded to a rough surface of a metal body, comprising the steps of: a bubble nucleation step of impregnating the heterogeneous bonded body with a bubble nucleation gas; and a foaming step of foaming the bubble nucleation gas impregnated in the heterogeneous conjugate.
2. 2. The method for separating heterogeneous conjugates according to claim 1, wherein said bubble nucleation step comprises sealing said heterogeneous conjugates and a bubble nucleation gas in a pressure-resistant vessel and creating a high-pressure state inside said pressure-resistant vessel.
3. 2. The method for separating heterogeneous conjugates according to claim 1, wherein said foaming step comprises heating the heterogeneous conjugate impregnated with the bubble nucleation gas in said bubble nucleation step to a predetermined temperature.
4. 3. The method for separating heterogeneous conjugates according to claim 2, wherein the pressure inside the pressure vessel is set to 10 MPa or more in the bubble nucleation step.
5. 4. The method for separating heterogeneous bonded bodies according to claim 3, wherein in the foaming step, the predetermined temperature is equal to or lower than a glass transition temperature of a resin constituting the resin body.
Citation Information
Patent Citations
Electric and electronic parts and manufacture thereof
JP1998294024A
Method of producing composite molded body
JP2015142960A