Polyisocyanate composition, adhesive resin composition and adhesive resin cured material
A polyisocyanate composition combining aliphatic and alicyclic diisocyanates with specific properties addresses the strength and flexibility issues of urethane-based adhesives, providing enhanced adhesive strength and heat resistance.
Patent Information
- Application Number
- JP2023073274
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing adhesives with urethane bonds lack the high strength of epoxy adhesives while maintaining flexibility, and alicyclic isocyanates used for quick-drying properties result in brittle cured resin products, limiting their use.
A polyisocyanate composition containing a mixture of aliphatic and alicyclic diisocyanates with specific molecular weight and isocyanurate groups, along with additional functional groups, is developed to enhance adhesive strength, durability, and heat resistance.
The composition achieves high König hardness, tensile strength, elongation, and shear adhesive strength, maintaining performance under high temperatures and improving durability.
Smart Images

Figure 2024158243000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyisocyanate composition, an adhesive resin composition, and a cured adhesive resin product. [Background technology]
[0002] In recent years, adhesives have become popular as an alternative to rivets and bolts for bonding metals and plastics together and for bonding different materials. Adhesives used in such fields are required to have long-term durability and heat resistance, as well as the ability to achieve high adhesive strength. In addition, everyday products that support us, such as electrical appliances, displays, and automobiles, are becoming more highly functional, and there is a demand for products with higher strength, higher performance, higher heat resistance, and higher durability.
[0003] For example, adhesives having urethane bonds are characterized by high flexibility and excellent impact resistance, and are therefore used as elastic adhesives that can stretch by 35% or more (see, for example, Patent Document 1).
[0004] However, adhesives with urethane bonds have a breaking strength of about 2-6 MPa when the adhesive is cured, which is inferior in strength to general epoxy adhesives that have a breaking strength of several tens of MPa. Therefore, there is a demand for adhesives that combine the elasticity of urethane with the high strength of epoxy adhesives. However, until now there has been no adhesive with a urethane bond that has the same level of high strength as epoxy adhesives.
[0005] Some paints contain alicyclic isocyanates to improve quick drying, but no consideration has been given to their adhesive strength or coating strength (see, for example, Patent Document 2). It is generally known that the use of alicyclic isocyanates makes the resin cured product harder, but on the other hand, it also makes the resin brittle, so its use has been limited. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 03-084159 [Patent Document 2] International Publication No. 2005 / 082966 Summary of the Invention [Problem to be solved by the invention]
[0007] As the fields in which adhesives are used expand, there is a demand for polyisocyanate compositions that are excellent in adhesive strength and durability, as well as adhesive resin compositions and adhesive resin cured products that use the same. The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a polyisocyanate composition having excellent adhesive strength, durability, and heat resistance, and an adhesive resin composition and an adhesive resin cured product using the same. [Means for solving the problem]
[0008] That is, the present invention includes the following aspects. [1] A polyisocyanate composition containing a polyisocyanate derived from at least one of an aliphatic diisocyanate and an alicyclic diisocyanate and having an isocyanurate group, wherein the polyisocyanate has a value represented by the following formula (I) of 31 or more and 55 or less, and the polyisocyanate has a weight average molecular weight of 500 or more and 1,200 or less. [B / (A+B)]×100 (I) (In formula (I), A is the weight of the constituent component derived from the aliphatic diisocyanate, and B is the weight of the constituent component derived from the alicyclic diisocyanate.) [2] The polyisocyanate composition according to [1], wherein the polyisocyanate composition has an average number of isocyanate groups of 2.6 or more and 3.8 or less. [3] The polyisocyanate composition according to [1] or [2], wherein the polyisocyanate composition has an isocyanate group content of 19.3 mass% or more in a solvent-free state. [4] The polyisocyanate composition according to any one of [1] to [3], wherein the alicyclic diisocyanate is isophorone diisocyanate. [5] The polyisocyanate composition according to any one of [1] to [4], which contains at least one of a urethane group, an allophanate group, a urea group, a biuret group, and a uretdione group in addition to an isocyanurate group, and has a value represented by the following formula (II) of 0.70 or more. c / (c+d+e+f+g+h) (II) (In formula (II), c is the number of moles of isocyanurate groups, d is the number of moles of urethane groups, e is the number of moles of allophanate groups, f is the number of moles of urea groups, g is the number of moles of biuret groups, and h is the number of moles of uretdione groups.) [6] The polyisocyanate composition according to any one of [1] to [5], wherein the polyisocyanate composition has a viscosity of 20,000 mPa·s or less at 25° C. [7] The polyisocyanate composition according to any one of [1] to [6], wherein the polyisocyanate composition has a solid content of 60% or more. [8] The polyisocyanate composition according to any one of [1] to [7], wherein the polyisocyanate composition forms a cured resin film having a Konig hardness of 110 or more at 23° C., provided that the cured resin film is a cured resin film having a thickness of 40 μm, which is formed by applying the polyisocyanate composition onto glass and curing the applied film at 23° C. for 168 hours. [9] An adhesive resin composition comprising the polyisocyanate composition according to any one of [1] to [8] and a crosslinkable functional group-containing compound.
[10] The adhesive resin composition according to [9], wherein the cured product 1 has a Konig hardness of 140 or more in an environment at 23° C. The cured product 1 is an adhesive resin cured product having a film thickness of 40 μm, which is obtained by applying the adhesive resin composition onto glass, heating at 80° C. for 30 minutes, and then curing at 23° C. for 168 hours.
[11] The adhesive resin composition according to [9] or
[10] , wherein the tensile strength of the cured product 2 is 62 MPa or more at a chuck distance of 20 mm and a peeling speed of 20 mm / min in an environment of 23°C, provided that the cured product 2 is an adhesive resin cured product obtained by applying the adhesive resin composition to a release film to a thickness of 40 μm, heating at 80°C for 30 minutes, and curing at 23°C for 168 hours.
[12] The adhesive resin composition according to any one of [9] to
[11] , wherein the adhesive resin composition is prepared using a crosslinkable functional group-containing compound having a Tg of 0°C or higher in a 60°C environment with a chuck distance of 20 mm and a peeling speed of 20 mm / min, and the cured product 2 has a tensile strength of 26 MPa or higher. However, the cured product 2 is an adhesive resin cured product obtained by applying the adhesive resin composition to a release film to a thickness of 40 μm, heating at 80°C for 30 minutes, and curing at 23°C for 168 hours.
[13] The adhesive resin composition according to any one of [9] to
[12] , wherein the cured product 2 produced using a crosslinkable functional group-containing compound having a Tg of 0°C or higher has an elongation of 7% or more in a tensile test in an environment of 60°C with a chuck distance of 20 mm and a peeling speed of 20 mm / min. The cured product 2 is an adhesive resin cured product obtained by applying the adhesive resin composition to a release film to a thickness of 40 μm, heating at 80°C for 30 minutes, and curing at 23°C for 168 hours.
[14] The adhesive resin composition according to any one of [9] to
[13] , wherein the adhesive resin composition has a shear adhesive strength of 19 MPa or more when measured at a test speed of 50 mm / min on a test piece produced under the following conditions. [Test piece manufacturing conditions] Two electrodeposited plates, each 20 mm wide and 100 mm long, are bonded together using the adhesive resin composition. The bonded area of the two electrodeposited plates is 5 mm x 20 mm. After bonding, the plates are heated at 80°C for 30 minutes and then aged at 23°C for 336 hours to produce a test piece.
[15] The adhesive resin composition according to any one of [9] to
[14] , wherein the adhesive resin composition contains a silane coupling agent, and the amount of the silane coupling agent per 100 parts by mass of the total solid content of the adhesive resin composition is 0.01 parts by weight or more and 5.0 parts by weight or less.
[16] The adhesive resin composition according to any one of [9] to
[15] , wherein the crosslinkable functional group-containing compound contains at least one functional group selected from the group consisting of a hydroxyl group, a carboxyl group, and an amino group, and has a glass transition temperature of 0°C or higher and 100°C or lower.
[17] A cured adhesive resin comprising the polyisocyanate composition according to any one of [1] to [8] and a crosslinkable functional group-containing compound.
[18] The adhesive resin cured product according to
[17] , having a gel fraction of 90% or more. Effect of the Invention
[0009] According to the present invention, it is possible to provide a polyisocyanate composition having excellent adhesive strength, durability and heat resistance, and an adhesive resin composition and an adhesive resin cured product using the same. In the present invention, excellent adhesive strength is evaluated by the Konig hardness of a cured resin film formed from the polyisocyanate composition, and the gel fraction, Konig hardness, tensile strength at 23° C., elongation at 23° C., tensile strength and shear adhesive strength at 60° C. of a cured product formed from an adhesive resin composition containing the polyisocyanate composition. In addition, for the evaluation of heat resistance, the result of tensile strength in a 60° C. environment is adopted as a simplified evaluation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In this specification, the term "polyol" refers to a compound having two or more hydroxyl groups (-OH) in one molecule. In addition, in this specification, the term "polyisocyanate" refers to a reaction product in which a plurality of monomer compounds each having two or more isocyanate groups (-NCO) are bonded together. In this specification, unless otherwise specified, "(meth)acrylic" includes both methacrylic and acrylic, and "(meth)acrylate" includes both methacrylate and acrylate.
[0011] <Polyisocyanate composition> The present embodiment is a polyisocyanate composition that contains a polyisocyanate derived from an aliphatic diisocyanate and an alicyclic diisocyanate and has an isocyanurate group.
[0012] <Physical properties of polyisocyanate> The polyisocyanate is derived from at least one of an aliphatic diisocyanate and an alicyclic diisocyanate. In one embodiment of the present invention, the polyisocyanate is a mixture of a polyisocyanate synthesized from an aliphatic diisocyanate and a polyisocyanate synthesized from an alicyclic diisocyanate. In one embodiment of the present invention, the polyisocyanate may be a reaction product obtained by reacting an aliphatic diisocyanate with an alicyclic diisocyanate through an isocyanurate reaction.
[0013] Polyisocyanates have isocyanurate groups in their molecular structure.
[0014] The polyisocyanate has a value represented by the following formula (I) of 31 or more and 55 or less, preferably 33 or more and 53 or less, and more preferably 34 or more and 51 or less. [B / (A+B)]×100 (I) (In formula (I), A is the weight of the constituent component derived from an aliphatic diisocyanate, and B is the weight of the constituent component derived from an alicyclic diisocyanate.)
[0015] The polyisocyanate in which the value of formula (I) satisfies the above range means that the weight of the constituent component derived from the aliphatic diisocyanate is equal to or greater than the weight of the constituent component derived from the alicyclic diisocyanate. The use of an alicyclic diisocyanate can impart high hardness to the resulting cured product, but if the amount is too large, the resulting cured product is likely to be brittle. As a result of extensive research, the present inventors have found that when an aliphatic diisocyanate and an alicyclic diisocyanate are used in combination to obtain a polyisocyanate whose ratio of the formula (I) satisfies the above range, the resulting cured product has high adhesive strength, excellent breaking strength in a high temperature environment, and exhibits durability.
[0016] When determining the value of (I) from the polyisocyanate composition, it is determined from the composition at the time of synthesis or the blend composition, or it is calculated by separating the constituent components derived from the aliphatic diisocyanate and the constituent components derived from the alicyclic diisocyanate from the polyisocyanate composition, or it is calculated by using a combination of H-NMR, C-NMR, IR, MS, and GPC. As a method for separating the constituent components derived from the aliphatic diisocyanate and the constituent components derived from the alicyclic diisocyanate from the polyisocyanate composition, for example, fractional distillation by high performance liquid chromatography (HPLC), GPC, thin film distillation or the like may be used.
[0017] The polyisocyanate has a weight average molecular weight of 500 or more and 1,200 or less, preferably 600 or more and 1,100 or less, and more preferably 650 or more and 1,000 or less.
[0018] When a polyisocyanate composition containing a polyisocyanate having a weight average molecular weight equal to or greater than the above lower limit is cured, a polyisocyanate cured product having excellent tensile strength and elongation can be obtained. On the other hand, when a polyisocyanate composition containing a polyisocyanate having a weight average molecular weight equal to or less than the above upper limit is cured, a polyisocyanate cured product having excellent adhesive strength, tensile strength of the cured resin film, and adhesive durability can be obtained.
[0019] [Method for measuring weight average molecular weight] The weight average molecular weight of the polyisocyanate can be measured, for example, by gel permeation chromatography (hereinafter sometimes abbreviated as "GPC"). The weight average molecular weight of the polyisocyanate can be adjusted by appropriately selecting the weight average molecular weight of the aliphatic polyisocyanate and alicyclic polyisocyanate used as raw materials.
[0020] (Aliphatic diisocyanate or alicyclic diisocyanate) Examples of aliphatic diisocyanates include, but are not limited to, 1,4-diisocyanatobutane, 1,5-diisocyanatopentane (PDI), ethyl (2,6-diisocyanato)hexanoate, 1,6-diisocyanatohexane (hereinafter sometimes abbreviated as "HDI"), 1,9-diisocyanatononane, 1,12-diisocyanatododecane, 2,2,4- or 2,4,4-trimethyl-1,6-diisocyanatohexane, etc. These aliphatic diisocyanates may be used alone or in combination of two or more.
[0021] Examples of alicyclic diisocyanates include, but are not limited to, isophorone diisocyanate (IPDI), 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane (hereinafter sometimes abbreviated as "hydrogenated XDI"), 1,3- or 1,4-diisocyanatocyclohexane, 3,5,5-trimethyl-1-isocyanato-3-(isocyanatomethyl)cyclohexane (hereinafter sometimes abbreviated as "IPDI"), 4-4'-diisocyanato-dicyclohexylmethane (hereinafter sometimes abbreviated as "hydrogenated MDI"), 2,5- or 2,6-diisocyanatomethylnorbornane, etc. These alicyclic diisocyanates may be used alone or in combination of two or more.
[0022] These aliphatic diisocyanates and alicyclic diisocyanates may be used alone, or two or more of them may be used in combination.
[0023] As the aliphatic diisocyanate, HDI and PDI are preferred, and HDI is more preferred, and as the alicyclic diisocyanate, isophorone diisocyanate is preferred.
[0024] In the production of polyisocyanates, in addition to the diisocyanates described above, isocyanate monomers such as those shown below may be further used. (1) Aromatic diisocyanates such as diphenylmethane-4,4'-diisocyanate (MDI), 1,5-naphthalene diisocyanate, tolylene diisocyanate (TDI), xylylene diisocyanate (XDI), and m-tetramethylxylylene diisocyanate (TMXDI). (2) Triisocyanates such as 4-isocyanatomethyl-1,8-octamethylene diisocyanate (hereinafter sometimes referred to as "NTI"), 1,3,6-hexamethylene triisocyanate (hereinafter sometimes referred to as "HTI"), bis(2-isocyanatoethyl) 2-isocyanatoglutarate (hereinafter sometimes referred to as "GTI"), and lysine triisocyanate (hereinafter sometimes referred to as "LTI").
[0025] <Physical properties of polyisocyanate composition> The polyisocyanate composition has an average number of isocyanate functional groups (average number of NCO groups) of preferably 2.6 or more and 3.8 or less, more preferably 2.8 or more and 3.8 or less, more preferably 2.9 or more and 3.7 or less, and even more preferably 3.0 or more and 3.6 or less, from the viewpoint of improving the curability, tensile strength, adhesive strength, and durability of the cured product to be produced. The average number of isocyanate functional groups in the polyisocyanate composition can be measured by the method described in the Examples below.
[0026] The polyisocyanate composition preferably has an isocyanate group content of 19.3 mass % or more, more preferably 19.5 mass % or more, and even more preferably 20.0 mass % or more, in a solvent-free state.
[0027] The polyisocyanate composition contains at least one of urethane groups, allophanate groups, urea groups, biuret groups, and uretdione groups in addition to isocyanurate groups, and the value represented by the following formula (II) is preferably 0.70 or more, more preferably 0.75 or more, more preferably 0.80 or more, more preferably 0.85 or more, and even more preferably 0.90 or more. The upper limit of the value of formula (II) is not particularly limited, and is, for example, 1.0 or less, 0.99 or less, or 0.98 or less.
[0028] c / (c+d+e+f+g+h) (II) (In formula (II), c is the number of moles of isocyanurate groups, d is the number of moles of urethane groups, e is the number of moles of allophanate groups, f is the number of moles of urea groups, g is the number of moles of biuret groups, and h is the number of moles of uretdione groups.)
[0029] Use of a polyisocyanate composition satisfying formula (II) can impart a high elongation to the resulting cured product.
[0030] In formula (II), the values of c, d, e, f, g, and h are, for example, 1 H-nuclear magnetic resonance (NMR) spectroscopy, 13 It can be calculated by C-NMR spectroscopy, infrared absorption (IR) spectroscopy, and mass spectrometry (MS).
[0031] The viscosity of the polyisocyanate composition at 25° C. is preferably 20,000 mPa·s or less, more preferably 9,000 mPa·s or less, more preferably 8,000 mPa·s or less, more preferably 7,000 mPa·s or less, and even more preferably 6,500 mPa·s or less. The lower limit of the viscosity of the polyisocyanate composition at 25° C. is not particularly limited, but is, for example, 10 mPa·s or more, 20 mPa·s or more, or 30 mPa·s or more.
[0032] The viscosity of the polyisocyanate composition at 25°C is, for example, 10 mPa·s or more and 10,000 mPa·s or less, 20 mPa·s or more and 9,000 mPa·s or less, 30 mPa·s or more and 8,000 mPa·s or less, 30 mPa·s or more and 7,000 mPa·s or less, or 30 mPa·s or more and 6,500 mPa·s or less.
[0033] When the viscosity at 25° C. is in the above range, it is preferable to use as little solvent as possible in the polyisocyanate composition of the present embodiment from the viewpoints of the environment and carbon neutrality.
[0034] The viscosity of the polyisocyanate composition at 25°C can be measured at 25°C, for example, using an E-type viscometer (manufactured by Tokimec Inc.).
[0035] The solids content of the polyisocyanate composition is preferably 60% or more, more preferably 65% or more, and even more preferably 68% or more. The solids content of the polyisocyanate composition can be measured by the method described in the Examples below.
[0036] In one embodiment of the present invention, the polyisocyanate composition comprises a polyisocyanate derived from at least one of an aliphatic diisocyanate and an alicyclic diisocyanate. In one embodiment of the present invention, the polyisocyanate composition includes polyisocyanate 1 derived from at least one of an aliphatic diisocyanate and an alicyclic diisocyanate, and polyisocyanate 2 derived from an aromatic diisocyanate. When polyisocyanate 1 and polyisocyanate 2 are contained, the proportion of polyisocyanate 1 in the total amount of polyisocyanate 1 and polyisocyanate 2 is preferably 60 mass% or more, more preferably 70 mass% or more, even more preferably 80 mass% or more, particularly preferably 90 mass% or more, and especially preferably 95 mass% or more.
[0037] <Production method of polyisocyanate> In one embodiment of the present invention, the polyisocyanate can be produced by mixing a polyisocyanate synthesized from an aliphatic diisocyanate and a polyisocyanate synthesized from an alicyclic diisocyanate. In one embodiment of the present invention, the polyisocyanate can be produced by reacting an aliphatic diisocyanate with an alicyclic diisocyanate via an isocyanuration reaction.
[0038] Examples of catalysts for deriving a polyisocyanate having an isocyanurate group from either or both of an aliphatic diisocyanate and an alicyclic diisocyanate include commonly used isocyanuration reaction catalysts.
[0039] The isocyanurate reaction catalyst is not particularly limited, but is preferably a catalyst having basicity in general. Specific examples of the isocyanurate reaction catalyst include the following. 1) Hydroxides of tetraalkylammonium such as tetramethylammonium, tetraethylammonium, and tetrabutylammonium, and organic weak acid salts such as acetates, propionates, octylates, caprates, myristates, and benzoates of the above tetraalkylammonium. 2) Hydroxides of aryltrialkylammonium such as benzyltrimethylammonium and trimethylphenylammonium, and organic weak acid salts such as acetates, propionates, octylates, caprates, myristates, and benzoates of the above aryltrialkylammonium. 3) Hydroxyalkylammonium hydroxides, such as trimethylhydroxyethylammonium, trimethylhydroxypropylammonium, triethylhydroxyethylammonium, and triethylhydroxypropylammonium, and organic weak acid salts, such as acetates, propionates, octylates, caprates, myristates, and benzoates of the above hydroxyalkylammoniums. 4) Metal salts, such as tin, zinc, lead, etc., of alkyl carboxylic acids, such as acetic acid, propionic acid, caproic acid, octylic acid, capric acid, and myristic acid. 5) Metal alcoholates such as sodium and potassium. 6) Aminosilyl group-containing compounds such as hexamethylenedisilazane. 7) Mannich bases. 8) Mixtures of tertiary amines and epoxy compounds. 9) Phosphorus compounds such as tributylphosphine.
[0040] Among these, from the viewpoint of preventing the production of unnecessary by-products, the isocyanurate reaction catalyst is preferably a quaternary ammonium hydroxide or a weak organic acid salt of a quaternary ammonium, and more preferably a tetraalkylammonium hydroxide, a weak organic acid salt of a tetraalkylammonium, an aryltrialkylammonium hydroxide, or a weak organic acid salt of an aryltrialkylammonium.
[0041] The upper limit of the amount of the isocyanurate reaction catalyst used is preferably 1000 ppm by mass, more preferably 500 ppm by mass, and even more preferably 100 ppm by mass, based on the mass of the charged aliphatic diisocyanate or alicyclic diisocyanate. On the other hand, the lower limit of the amount of the isocyanurate reaction catalyst used is not particularly limited, and may be, for example, 5 ppm by mass.
[0042] The isocyanurate reaction temperature is preferably from 50° C. to 120° C., and more preferably from 55° C. to 90° C. By keeping the isocyanurate reaction temperature at or below the upper limit, coloration of the polyisocyanate tends to be more effectively suppressed.
[0043] When a desired conversion rate (the ratio of the mass of the polyisocyanate produced in the isocyanuration reaction to the mass of the charged aliphatic diisocyanate or alicyclic diisocyanate) is reached, the isocyanuration reaction is stopped by adding an acidic compound (e.g., phosphoric acid, an acidic phosphoric acid ester, etc.). In order to obtain polyisocyanate, it is necessary to stop the reaction at an early stage. However, since the reaction rate of the isocyanurate reaction is very fast at the early stage, it is difficult to stop the reaction at an early stage, and therefore the reaction conditions, particularly the amount and method of adding the catalyst, must be carefully selected. For example, a method of adding the catalyst in portions at regular intervals is recommended as a suitable method.
[0044] Therefore, the conversion rate of the isocyanurate reaction to obtain a polyisocyanate is preferably 10% or more and 60% or less, more preferably 12% or more and 55% or less, and even more preferably 14% or more and 50% or less. By setting the conversion rate of the isocyanurate reaction to the upper limit or less, the viscosity of the polyisocyanate can be made lower. By setting the conversion rate of the isocyanurate reaction to the lower limit or more, the reaction terminating operation can be more easily carried out.
[0045] When deriving a polyisocyanate having an isocyanurate group, a monohydric to hexahydric alcohol can be used in addition to an aliphatic diisocyanate or an alicyclic diisocyanate. Examples of the monohydric to hexahydric alcohol include polyhydric alcohols such as monoalcohols, diols, triols, and tetraols.
[0046] Examples of monoalcohols include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, n-pentanol, n-hexanol, n-octanol, n-nonanol, 2-ethylbutanol, 2,2-dimethylhexanol, 2-ethylhexanol, cyclohexanol, methylcyclohexanol, and ethylcyclohexanol.
[0047] Examples of diols include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2-methyl-1,2-propanediol, 1,5-pentanediol, 2-methyl-2,3-butanediol, and Examples of the hexanediol include hexanediol, 1,6-hexanediol, 1,2-hexanediol, 2,5-hexanediol, 2-methyl-2,4-pentanediol, 2,3-dimethyl-2,3-butanediol, 2-ethyl-hexanediol, 1,2-octanediol, 1,2-decanediol, 2,2,4-trimethylpentanediol, 2-butyl-2-ethyl-1,3-propanediol, and 2,2-diethyl-1,3-propanediol. Examples of triols include glycerin and trimethylolpropane. An example of the tetraols is pentaerythritol.
[0048] <Physical properties of cured resin film> In one embodiment of the present invention, the cured resin film produced from the polyisocyanate composition preferably has a Konig hardness of 110 or more, more preferably 120 or more, more preferably 130 or more, more preferably 140 or more, preferably 148 or more, more preferably 150 or more, and even more preferably 152 or more in a 23°C environment. The cured resin film was a coating film having a thickness of 40 μm, which was prepared by applying the polyisocyanate composition onto glass and curing the composition at 23° C. for 168 hours.
[0049] <Adhesive resin composition> This embodiment is an adhesive resin composition comprising the polyisocyanate composition of the present invention and a crosslinkable functional group-containing compound.
[0050] ≪Crosslinkable functional group-containing compound≫ The crosslinkable functional group-containing compound preferably contains at least one functional group selected from the group consisting of a hydroxyl group, a carboxyl group, and an amino group. The crosslinkable functional group-containing compound is preferably a compound having a glass transition temperature of 0°C or higher and 100°C or lower. The crosslinkable functional group-containing compound may be any compound that contains a crosslinkable functional group capable of reacting with the isocyanate group of the polyisocyanate composition. The crosslinkable functional group-containing compound is preferably a polyol or a compound having an amino group as a functional group.
[0051] The amino group, which is a functional group contained in the crosslinkable functional group-containing compound, is preferably a primary amino group or a secondary amino group. The secondary amino group is preferably an amino group derived from an aspartic acid ester polyamine.
[0052] Specific examples of the crosslinkable functional group-containing compound include acrylic polyol, polycarbonate polyol, polyester polyol, polyether polyol, epoxy polyol, fluorine polyol, polyolefin polyol, polyurethane polyol, polyamine, and the like.
[0053] Among these, one or more polyols selected from the group consisting of acrylic polyols, polycarbonate polyols, polyester polyols, polyether polyols, epoxy polyols, polyolefin polyols, and polyurethane polyols, each having a weight-average molecular weight of 500 or more and 100,000 or less, are preferred, and acrylic polyols, polyester polyols, polyether polyols, polycarbonate polyols, and aspartic acid ester polyamines, each having a weight-average molecular weight of 500 or more and 100,000 or less, are more preferred.
[0054] [Acrylic polyol] The acrylic polyol is not particularly limited, but examples thereof include those obtained by copolymerizing a single or mixture of an ethylenically unsaturated bond-containing monomer having a hydroxy group with a single or mixture of other ethylenically unsaturated bond-containing monomers copolymerizable therewith.
[0055] The ethylenically unsaturated bond-containing monomer having a hydroxy group is not particularly limited, but examples thereof include hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate. These may be used alone or in combination of two or more. Among them, hydroxyethyl acrylate or hydroxyethyl methacrylate is preferred.
[0056] Examples of other ethylenically unsaturated bond-containing monomers copolymerizable with the above monomers include the following (1) to (5), which may be used alone or in combination of two or more.
[0057] (1) Methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate (meth)acrylate esters such as decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, benzyl (meth)acrylate, and cyclohexyl (meth)acrylate.
[0058] (2) Unsaturated carboxylic acids, such as acrylic acid, methacrylic acid, maleic acid, and itaconic acid.
[0059] (3) Monomers having an epoxy group, such as acrylamide, methacrylamide, N,N-methylenebisacrylamide, diacetone acrylamide, diacetone methacrylamide, maleic acid amide, maleimide, 1,2-epoxy-4-vinylcyclohexane, allyl glycidyl ether, 4-hydroxybutyl acrylate glycidyl ether, etc. Unsaturated amides, such as N-methylolacrylamide, diacetone acrylamide, dimethylaminopropyl acrylamide, etc.
[0060] (4) Vinyl monomers such as glycidyl methacrylate, styrene, vinyl toluene, vinyl acetate, acrylonitrile, dibutyl fumarate, N-vinylpyrrolidone, N-vinylcaprolactam, and acryloylmorpholine.
[0061] (5) Vinyl monomers having a hydrolyzable silyl group, such as vinyltrimethoxysilane, vinylmethyldimethoxysilane, and γ-(meth)acryloxypropyltrimethoxysilane.
[0062] [Polycarbonate polyol] The polycarbonate polyol is not particularly limited, but examples thereof include the following (1) to (4). (1) Dialkyl carbonates such as dimethyl carbonate. (2) Alkylene carbonates such as ethylene carbonate. (3) Diaryl carbonates such as diphenyl carbonate. (4) A product obtained by condensation polymerization of low molecular weight carbonate compounds such as those described in (1) to (3) above.
[0063] Commercially available polycarbonate polyols include, for example, Duranol T5650E (number average molecular weight 500), T5650J (number average molecular weight 800), T5651 (number average molecular weight 1000), and T5652 (number average molecular weight 2000), all manufactured by Asahi Kasei Corporation.
[0064] [Polyester polyol] The polyester polyol can be obtained, for example, by subjecting a dibasic acid, or a mixture of two or more kinds, and a polyhydric alcohol, or a mixture of two or more kinds, to a condensation reaction.
[0065] Examples of the dibasic acid include carboxylic acids such as succinic acid, adipic acid, dimer acid, maleic anhydride, phthalic anhydride, isophthalic acid, terephthalic acid, and 1,4-cyclohexanedicarboxylic acid.
[0066] Examples of the polyhydric alcohol include ethylene glycol, propylene glycol, diethylene glycol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, trimethylpentanediol, cyclohexanediol, trimethylolpropane, glycerin, pentaerythritol, 2-methylolpropanediol, and ethoxylated trimethylolpropane.
[0067] Alternatively, for example, polycaprolactones obtained by ring-opening polymerization of lactones such as ε-caprolactone with polyhydric alcohols can also be used as polyester polyols.
[0068] [Polyether polyol] The polyether polyols are not particularly limited, but examples thereof include the following (1) to (3).
[0069] (1) Polyether polyols obtained by random or block addition of an alkylene oxide or a mixture of alkylene oxides to a polyhydric hydroxy compound or a mixture of polyhydric hydroxy compounds using a catalyst.
[0070] Examples of the catalyst include hydroxides (lithium, sodium, potassium, etc.), strong basic catalysts (alcoholates, alkylamines, etc.), composite metal cyanide complexes (metal porphyrins, zinc hexacyanocobaltate complexes, etc.), and the like. Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, cyclohexene oxide, and styrene oxide.
[0071] (2) Polyether polyols obtained by reacting a polyamine compound with an alkylene oxide. Examples of the polyamine compound include ethylenediamines. Examples of the alkylene oxide include the same as those exemplified in (1).
[0072] (3) Polymer polyols obtained by polymerizing acrylamide or the like using the polyether polyols obtained in (1) or (2) as a medium.
[0073] Examples of the polyhydric hydroxy compound include the following compounds (i) to (vi).
[0074] (i) Diglycerin, ditrimethylolpropane, pentaerythritol, dipentaerythritol, etc.
[0075] (ii) Sugar alcohol compounds such as erythritol, D-threitol, L-arabinitol, ribitol, xylitol, sorbitol, mannitol, galactitol, and rhamnitol.
[0076] (iii) Monosaccharides such as arabinose, ribose, xylose, glucose, mannose, galactose, fructose, sorbose, rhamnose, fucose, and ribosaccharides.
[0077] (iv) Disaccharides such as trehalose, sucrose, maltose, cellobiose, gentiobiose, lactose, and melibiose.
[0078] (v) Trisaccharides such as raffinose, gentianose, and melezitose.
[0079] (vi) Tetrasaccharides such as stachyose.
[0080] [Epoxy polyol] Examples of epoxy polyols include novolac-type epoxy polyols, β-methylepicro-type epoxy polyols, cyclic oxirane-type epoxy polyols, glycidyl ether-type epoxy polyols, glycol ether-type epoxy polyols, epoxy-type aliphatic unsaturated compounds, epoxidized fatty acid esters, ester-type polyvalent carboxylic acids, aminoglycidyl-type epoxy polyols, halogenated epoxy polyols, and resorcin-type epoxy polyols, as well as resins obtained by modifying these epoxy polyols with amino compounds, polyamide compounds, or the like.
[0081] [Polyolefin polyol] The polyolefin polyol is not particularly limited, but examples thereof include polybutadiene having two or more hydroxyl groups, hydrogenated polybutadiene, polyisoprene, and hydrogenated polyisoprene.
[0082] The number of hydroxyl groups statistically possessed by one molecule of the polyol (hereinafter, sometimes referred to as the "average number of hydroxyl groups") is preferably at least 2. When the average number of hydroxyl groups of the polyol is at least 2, there is a tendency that the decrease in the crosslink density of the coating film obtained by curing the one-component coating composition of the present embodiment can be further suppressed.
[0083] [Polyurethane polyol] The polyurethane polyol is not particularly limited, but can be obtained, for example, by reacting a polyol not containing a carboxy group with an isocyanate component in a conventional manner.
[0084] Examples of the polyol not containing a carboxy group include low molecular weight ones such as ethylene glycol and propylene glycol, and high molecular weight ones such as acrylic polyol, polyester polyol, polyether polyol, etc.
[0085] [Polyamine] The polyamine is not particularly limited, but is preferably one having two or more primary amino groups and / or secondary amino groups in one molecule. The amino groups of the polyamine are preferably secondary amines.
[0086] Specific examples of polyamines include, but are not limited to, diamines such as ethylenediamine, propylenediamine, butylenediamine, triethylenediamine, hexamethylenediamine, 4,4'-diaminodicyclohexylmethane, piperazine, 2-methylpiperazine, and isophoronediamine; chain polyamines having three or more amino groups such as bishexamethylenetriamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentamethylenehexamine, and tetrapropylenepentamine; cyclic polyamines such as 1,4,7,10,13,16-hexaazacyclooctadecane, 1,4,7,10-tetraazacyclodecane, 1,4,8,12-tetraazacyclopentadecane, 1,4,8,11-tetraazacyclotetradecane, and aspartic acid ester amines; and aliphatic polyamines, with aspartic acid ester polyamines being preferred.
[0087] [Content ratio of compound containing crosslinkable functional group] In the adhesive resin composition of the present embodiment, the content of the above-mentioned polyisocyanate composition is preferably 0.01 parts by mass or more and 200.0 parts by mass or less, more preferably 0.03 parts by mass or more and 180.0 parts by mass or less, and even more preferably 0.05 parts by mass or more and 160.0 parts by mass or less, relative to 100 parts by mass of the crosslinkable functional group-containing compound.
[0088] The adhesive resin composition of the present embodiment preferably contains a silane coupling agent. The amount of the silane coupling agent to be blended relative to 100 parts by mass of the total solid content of the adhesive resin composition is preferably 0.01 parts by weight or more and 5.0 parts by weight or less. By containing the silane coupling agent in an amount within the above numerical range, the adhesive resin composition of the present embodiment can further improve the shear adhesive strength of the adhesive resin cured product obtained, and can further suppress lifting and peeling at the adherend interface during heating and humidification. Here, "100 parts by weight of the total solid content of the adhesive resin composition" is the total amount of the polyisocyanate composition and the crosslinkable functional group-containing compound.
[0089] Examples of silane coupling agents include, but are not limited to, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, ureidopropyltriethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, methyltriethoxysilane, and methyltrimethoxysilane.
[0090] The content of the silane coupling agent is preferably 0.01 parts by mass or more and 5.00 parts by mass or less, more preferably 0.01 parts by mass or more and 3.00 parts by mass or less, even more preferably 0.01 parts by mass or more and 2.00 parts by mass or less, even more preferably 0.01 parts by mass or more and 1.00 parts by mass or less, even more preferably 0.01 parts by mass or more and 0.70 parts by mass or less, and particularly preferably 0.03 parts by mass or more and 0.60 parts by mass or less, relative to 100 parts by mass of the total solids content of the adhesive resin composition.
[0091] The adhesive resin composition of the present embodiment may further contain other additives. Other additives include, for example, curing catalysts, solvents, pigments (extender pigments, colored pigments, metallic pigments, etc.), silica fillers, adhesion-imparting resins, photopolymerization initiators, ultraviolet absorbers, light stabilizers, radical stabilizers, yellowing inhibitors that suppress coloring during the baking process, coating surface adjusters, flow adjusters, pigment dispersants, defoamers, thickeners, film-forming assistants, and the like.
[0092] The curing catalyst may be a basic compound or a Lewis acid compound. Examples of the basic compound include metal hydroxides, metal alkoxides, metal carboxylates, metal acetylacetinates, hydroxides of onium salts, onium carboxylates, halides of onium salts, metal salts of active methylene compounds, onium salts of active methylene compounds, aminosilanes, amines, phosphines, etc. As the onium salts, ammonium salts, phosphonium salts, or sulfonium salts are preferable. Examples of the Lewis acid compound include an organotin compound, an organozinc compound, an organotitanium compound, and an organozirconium compound.
[0093] Examples of the solvent include 1-methylpyrrolidone, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, dipropylene glycol monomethyl ether, propylene glycol monomethyl ether, 3-methoxy-3-methyl-1-butanol, ethylene glycol diethyl ether, diethylene glycol diethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dipropylene glycol dimethyl ether (DPDM), propylene glycol dimethyl ether, methyl ethyl ketone, acetone, and the like. Examples of the solvent include methyl isobutyl ketone, propylene glycol monomethyl ether acetate, ethanol, methanol, iso-propanol, 1-propanol, iso-butanol, 1-butanol, tert-butanol, 2-ethylhexanol, cyclohexanol, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, ethyl acetate, isopropyl acetate, butyl acetate, toluene, xylene, pentane, iso-pentane, hexane, iso-hexane, cyclohexane, solvent naphtha, mineral spirits, etc. These solvents may be used alone or in combination of two or more.
[0094] In addition, known pigments (extender pigments, colored pigments, metallic pigments, etc.), ultraviolet absorbers, light stabilizers, radical stabilizers, yellowing inhibitors that suppress coloring during the baking process, coating surface conditioners, flow conditioners, pigment dispersants, defoamers, thickeners, and film-forming aids can be appropriately selected and used.
[0095] <Method for producing adhesive resin composition> The adhesive resin composition can be produced by a conventional method, for example, a melt-kneading method using a general mixer such as a Banbury mixer, a single screw extruder, a twin screw extruder, a co-kneader, or a multi-screw extruder, or a method in which each component is dissolved or dispersed and mixed, then coated on a substrate film with a coater or the like, and the solvent is then removed by heating.
[0096] <Physical properties of the cured product> In one embodiment of the present invention, the adhesive resin composition is applied onto glass, heated at 80°C for 30 minutes, and then aged at 23°C for 168 hours to obtain a cured adhesive resin having a film thickness of 40 µm, which preferably has the following physical properties: In one embodiment of the present invention, the Konig hardness of the cured product 1 in a 25° C. environment is preferably 140 or more, more preferably 142 or more, and even more preferably 144 or more.
[0097] In one embodiment of the present invention, the adhesive resin composition is applied onto a release film to a thickness of 40 μm, heated at 80° C. for 30 minutes, and then cured at 23° C. for 168 hours to obtain a cured adhesive resin product, which preferably has the following physical properties: In one embodiment of the present invention, the tensile strength of the cured product 2 produced using a crosslinkable functional group-containing compound having a Tg of 0°C or higher in an environment of 23°C with a chuck distance of 20 mm and a peeling speed of 20 mm / min is preferably 62 MPa or more, more preferably 64 MPa or more, more preferably 66 MPa or more, more preferably 68 MPa or more, and even more preferably 70 MPa or more. In one embodiment of the present invention, the tensile strength of the cured product 2 produced using a crosslinkable functional group-containing compound having a Tg of 0°C or higher in a 60°C environment with a chuck distance of 20 mm and a peeling speed of 20 mm / min is preferably 26 MPa or higher, more preferably 27 MPa or higher, more preferably 28 MPa or higher, and even more preferably 30 MPa or higher. In one embodiment of the present invention, the tensile elongation of the cured material 2 produced using a crosslinkable functional group-containing compound having a Tg of 0°C or higher in a 60°C environment with a chuck distance of 20 mm and a peeling speed of 20 mm / min is preferably 7% or higher, more preferably 8% or higher, and even more preferably 9% or higher.
[0098] In one embodiment of the present invention, the shear adhesive strength of a test piece produced under the following conditions, measured at a test speed of 50 mm / min, is preferably 19 MPa or more, more preferably 19.5 MPa or more, even more preferably 20 MPa or more, and most preferably 21 MPa or more. [Test piece manufacturing conditions] Two electrodeposited plates, each 20 mm wide and 100 mm long, are bonded together using the adhesive resin composition. The bonded area of the two electrodeposited plates is 5 mm x 20 mm. After bonding, the plates are heated at 80°C for 30 minutes and then aged at 23°C for 336 hours to produce a test piece.
[0099] In one embodiment of the present invention, the cured adhesive resin comprises a polyisocyanate composition and a compound containing a crosslinkable functional group. In one embodiment of the present invention, the adhesive resin cured product has a gel fraction of 90% or more. When the gel fraction is 90% or more, the adhesive strength of the cured product can be maintained and the durability is excellent. The gel fraction of the adhesive resin cured product is measured by the method described in the examples below. EXAMPLES
[0100] <Synthesis of polyisocyanate> [Synthesis Example 1] Synthesis of polyisocyanate P1 In a four-neck flask equipped with a thermometer, stirring blade, and reflux condenser, 100 parts by mass of HDI was charged under a nitrogen stream, and the temperature inside the reactor was maintained at 61°C while stirring. 0.02 parts by mass of isobutanol and 0.0030 parts by mass of tetramethylammonium caprate were added, and after 3.8 hours, when the conversion rate reached 22% by mass, phosphoric acid was added to stop the reaction. After filtering the reaction liquid, unreacted HDI was removed using a thin-film evaporator to obtain an isocyanurate-type polyisocyanate (hereinafter sometimes referred to as "polyisocyanate P1"). The NCO content was 23.3% by mass, and the weight-average molecular weight was 7.32 x 10 2 The average number of isocyanate groups was 3.28. The presence of isocyanurate groups was confirmed by NMR measurement, and it was confirmed that isocyanurate groups were the main component.
[0101] [Synthesis Example 2] Synthesis of polyisocyanate P2 In a four-neck flask equipped with a thermometer, stirring blade, and reflux condenser, 100 parts by mass of IPDI (isophorone diisocyanate) was charged under a nitrogen stream, and the temperature inside the reactor was maintained at 72°C while stirring. 0.0030 parts by mass of tetramethylammonium caprate was added, and after 5.0 hours, phosphoric acid was added to stop the reaction. The reaction liquid was filtered, and unreacted IPDI was removed using a thin-film evaporator to obtain an isocyanurate-type polyisocyanate (hereinafter sometimes referred to as "polyisocyanate P2"). The NCO content was 17.37% by mass, and the weight-average molecular weight was 8.75 x 10 2 The average number of isocyanate groups was 3.22. The presence of isocyanurate groups was confirmed by NMR measurement, and it was confirmed that isocyanurate groups were the main component.
[0102] [Synthesis Example 3] Synthesis of polyisocyanate P3 In a four-neck flask equipped with a thermometer, stirring blade, and reflux condenser, 80 parts by mass of HDI and 20 parts by mass of IPDI (isophorone diisocyanate) were charged under a nitrogen gas flow, the temperature inside the reactor was maintained at 71°C with stirring, 0.0040 parts by mass of tetramethylammonium caprate was added, and after 5.0 hours, phosphoric acid was added to stop the reaction. The reaction liquid was filtered, and unreacted HDI and IPDI were removed using a thin-film evaporator to obtain an isocyanurate-type polyisocyanate (hereinafter sometimes referred to as "polyisocyanate P3"). The NCO content was 21.4% by mass, and the weight-average molecular weight was 8.42 x 10 2 The average number of isocyanate groups was 3.26. The presence of isocyanurate groups was confirmed by NMR measurement, and it was confirmed that isocyanurate groups were the main component.
[0103] [Synthesis Example 4] Synthesis of polyisocyanate P4 In a four-neck flask equipped with a thermometer, stirring blade, and reflux condenser, 70 parts by weight of HDI, 30 parts by weight of IPDI (isophorone diisocyanate), and 10 parts by weight of trifunctional polycaprolactone triol 3PO-1 (manufactured by Daicel Corporation, Plaxel 303, number average molecular weight Mn300) were added under a nitrogen gas flow, and the temperature inside the reactor was maintained at 62°C while stirring. The reaction was stopped when the yield reached 46%. After filtering the reaction liquid, unreacted HDI and IPDI were removed using a thin-film distillation apparatus to obtain a polyisocyanate (hereinafter referred to as "polyisocyanate P4"). The NCO content of the obtained P4 was 19.21% by mass, and the weight average molecular weight was 4.55 x 10 3 It was.
[0104] [Synthesis Example 5] Synthesis of polyisocyanate P4 In a four-neck flask equipped with a thermometer, stirring blade, and reflux condenser, 63 parts by weight of HDI, 37 parts by weight of IPDI (isophorone diisocyanate), and 10 parts by weight of trifunctional polycaprolactone triol 3PO-1 (manufactured by Daicel Corporation, Plaxel 303, number average molecular weight Mn300) were added under a nitrogen gas flow, and the temperature inside the reactor was maintained at 62°C while stirring. The reaction was stopped when the yield reached 45%. After filtering the reaction liquid, unreacted HDI and IPDI were removed using a thin-film distillation apparatus to obtain a polyisocyanate (hereinafter referred to as "polyisocyanate P4"). The NCO content of the obtained P4 was 18.21% by mass, and the weight average molecular weight was 4.75 x 10 3 It was.
[0105] <Preparation of polyisocyanate composition> Example 1 In a four-neck flask equipped with a thermometer, stirring blade, and reflux condenser, 65 g of polyisocyanate P1 and 35 g of polyisocyanate P2 were mixed under nitrogen gas flow, and butyl acetate was added in a ratio of 70% solids weight, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pa-1. For polyisocyanate composition Pa-1, A (weight of components derived from aliphatic diisocyanate), B (weight of components derived from alicyclic diisocyanate), value of formula (I), weight average molecular weight Mw, NCO (%) (as is), NCO (%) (excluding solvent), average number of NCO groups, value of formula (II), Konig hardness of the coating, solids (%), and viscosity are shown in Table 1. The same applies to the following examples and comparative examples.
[0106] For Example 1, the value of formula (I) was calculated from the blending ratio of A and B. For the subsequent Examples and Comparative Examples, the value of formula (I) was calculated in the same manner.
[0107] For Example 1, the value of formula (II) is calculated by dividing the resulting polyisocyanate composition by 1 H-nuclear magnetic resonance (NMR) spectroscopy, 13The values of c, d, e, f, g, and h were calculated after analysis by C-NMR spectroscopy. In formula 1, the value of formula (II) is expressed as ◎ if it is 0.90 or more, 0.80 or more but less than 0.90 if it is 〇, 0.75 or more but less than 0.80 if it is 〇△, 0.70 or more but less than 0.75 if it is △, and less than 0.70 if it is ×.
[0108] Example 2 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 60 g of polyisocyanate P1 and 40 g of polyisocyanate P2 were mixed under a nitrogen gas flow, and butyl acetate was added in a proportion such that the solid content weight was 70%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pa-2.
[0109] Example 3 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 55 g of polyisocyanate P1 and 45 g of polyisocyanate P2 were mixed under a nitrogen gas flow, and butyl acetate was added in a proportion such that the solid content weight was 70%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pa-3.
[0110] Example 4 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 50 g of polyisocyanate P1 and 50 g of polyisocyanate P2 were mixed under a nitrogen gas flow, and butyl acetate was added in a proportion such that the solid content weight was 70%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pa-4.
[0111] Example 5 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 g of polyisocyanate P3 and 37 g of polyisocyanate P2 were mixed under a nitrogen gas flow, butyl acetate was added in a proportion such that the solid content weight was 70%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pa-5.
[0112] Example 6 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 60 g of polyisocyanate P1 and 40 g of polyisocyanate P2 were mixed under a nitrogen gas flow, and butyl acetate was added in a proportion such that the solid content weight was 85%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pa-6.
[0113] Example 7 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 55 g of polyisocyanate P1 and 45 g of polyisocyanate P2 were mixed under a nitrogen gas flow, and butyl acetate was added in a proportion such that the solid content weight was 85%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pa-7.
[0114] Example 8 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 50 g of polyisocyanate P1 and 50 g of polyisocyanate P2 were mixed under a nitrogen gas flow, and butyl acetate was added in a proportion such that the solid content weight was 85%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pa-8.
[0115] Comparative Example 1 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 g of polyisocyanate P1 was mixed under a nitrogen stream, and butyl acetate was added in a proportion such that the solid content weight was 70%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pb-1.
[0116] Comparative Example 2 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 g of polyisocyanate P2 was mixed under a nitrogen stream, and butyl acetate was added in a proportion such that the solid content weight was 70%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pb-2.
[0117] Comparative Example 3 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 75 g of polyisocyanate P1 and 25 g of polyisocyanate P2 were mixed under a nitrogen gas flow, and butyl acetate was added in a proportion such that the solid content weight was 70%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pb-3.
[0118] Comparative Example 4 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 40 g of polyisocyanate P1 and 60 g of polyisocyanate P2 were mixed under a nitrogen gas flow, and butyl acetate was added in a proportion such that the solid content weight was 70%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pb-4.
[0119] Comparative Example 5 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 g of polyisocyanate P4 was mixed under a nitrogen stream, and butyl acetate was added in a proportion such that the solid content weight was 70%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pb-5.
[0120] Comparative Example 6 In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 g of polyisocyanate P5 was mixed under a nitrogen stream, and butyl acetate was added in a proportion such that the solid content weight was 70%, and the mixture was stirred for 1 hour to obtain polyisocyanate composition Pb-6.
[0121] <Production of Compound Containing Crosslinkable Functional Group> [Synthesis Example 5] (Production of acrylic polyol for preparing adhesive composition) A four-neck flask equipped with a stirrer, a thermometer, a cooling tube, and a nitrogen gas inlet was charged with 29 parts by mass of propylene glycol monomethyl ether, and heated to 112°C under nitrogen gas aeration. After reaching 112°C, the nitrogen gas aeration was stopped, and a mixture consisting of 22.3 parts by mass of 2-hydroxyethyl methacrylate, 10.0 parts by mass of methyl methacrylate, 26.1 parts by mass of butyl acrylate, 40.3 parts by mass of styrene, 1.3 parts by mass of acrylic acid, and 2 parts by mass of 2,2'-azobis(isobutyronitrile) was dropped over 6 hours. Next, the mixture was stirred for 3 hours while flowing nitrogen gas at 115°C, and then cooled to 60°C, and a butyl acetate solution was added to obtain a solution of acrylic polyol A1 for preparing an adhesive composition with a solid content of 60% by mass. The acrylic polyol for preparing the adhesive composition has a glass transition temperature Tg of 29.8°C, a hydroxyl value relative to the resin solid content of 139 mgKOH / g, and a weight average molecular weight Mw of 2.46 × 10 4 It was.
[0122] <Production of adhesive resin composition and cured adhesive resin film> Pa-1 was mixed with the acrylic polyol A1, which was the main component, at a ratio of NCO / OH=1, and 0.2 parts by mass of a silane coupling agent KBM403 (manufactured by Shin-Etsu Chemical Co., Ltd.) was added to 100 parts by mass of the acrylic polyol A1. Then, butyl acetate was mixed at a ratio of 45% solid content and stirred to prepare an adhesive resin composition. The obtained butyl acetate solution with a solid content of 45% was applied to a peel-treated PET film with an applicator so that the thickness after drying was 40 μm, and the film was dried at 80° C. for 30 minutes, and then stored in a 23° C. / 50% RH environment for 7 days to obtain a cured film of the adhesive resin composition. Pa-2 to Pb-5 were also prepared in the same manner.
[0123] <Methods for measuring various physical properties> -Method of measuring tensile strength and elongation at 23℃ The cured film test piece of the adhesive resin composition prepared by the above method was cut to a width of 10 mm and a length of 100 mm, and set in a tensile tester so that the gripping distance was 20 m. The tensile strength and elongation were measured at a speed of 20 mm / min in an environment of 23°C. Pa-2 to Pb-5 were also measured in the same manner.
[0124] -Measuring method for tensile strength and elongation in 60℃ environment As a simple evaluation to confirm heat resistance, the tensile strength and elongation were measured in a 60°C environment. The cured film test piece of the adhesive resin composition prepared by the above method was cut to a width of 10 mm and a length of 100 mm, and set in a tensile tester so that the gripping distance was 20 mm. The tensile strength and elongation were measured at a speed of 20 mm / min in an environment of 60°C. Pa-2 to Pb-5 were also measured in the same manner.
[0125] ·Measuring method for Konig hardness of polyisocyanate film The polyisocyanate P-a1 obtained on the glass was applied to the glass with an applicator to a thickness of 40 μm, and stored in an environment of 23°C and 60% RH for 168 hours to obtain a polyisocyanate resin film on the glass. The Konig hardness (times) of the obtained film at 23°C was measured. Pa-2 to Pb-5 were also measured by the same method.
[0126] -Measurement of Konig hardness of cured adhesive resin film Pa-1 was mixed with acrylic polyol A1, a crosslinkable functional group-containing compound, at a ratio of NCO / OH=1, and 0.2 parts by mass of silane coupling agent KBM403 (manufactured by Shin-Etsu Chemical Co., Ltd.) was added to acrylic polyol A1: 100 parts by mass, and butyl acetate was added to prepare an adhesive resin composition. The obtained butyl acetate solution with a solid content of 45% was applied to glass with an applicator so that the thickness after drying was 40 μm, dried at 80 ° C for 30 minutes, and then stored in a 23 ° C / 50% RH environment for 7 days, and the Konig hardness (times) of the adhesive resin cured film obtained was measured. Pa-2 to Pb-5 were also measured by the same method.
[0127] Shear adhesion measurement method The adhesive resin composition obtained above was attached to two electrodeposited plates of JIS G 3141 (SPCC, SD) with a width of 20 mm and a length of 100 mm so that the adhesive area was 5 mm x 20 m. After aging for 336 hours at 23°C, the shear adhesive strength was measured at a speed of 50 mm / min. Pa-2 to Pb-5 were also measured by the same method.
[0128] Adhesion durability evaluation The adhesive resin composition obtained above was laminated to two electrodeposited plates of 20 mm width x 100 mm length so that the adhesive area was 5 mm x 20 mm, dried at 80°C for 30 minutes, aged at 23°C for 336 hours, then placed at 70°C for 1000 hours, removed and cooled, and the shear adhesive strength was measured at a speed of 50 mm / min. The measured value was evaluated as ◯ when it maintained 70% or more of the value before the application, △ when it maintained 50% or more but less than 70%, and × when it maintained less than 50%.
[0129] Gel fraction measurement method Approximately 0.1 to 0.2 g of the obtained adhesive resin cured film was collected, wrapped in a mesh sheet, immersed in acetone for 24 hours, and dried at 105°C for 1 hour. The gel fraction was calculated as follows: 100 x (sample weight after drying) / (sample weight before acetone application). Pa-2 to Pb-5 were also measured in the same manner.
[0130] Isocyanate group content First, 1 g or more and 2 g or less of a measurement sample was precisely weighed out into a flask (Wg). Next, 20 mL of toluene was added to dissolve the measurement sample, and then 20 mL of a 2N toluene solution of di-n-butylamine was added and mixed, followed by leaving the mixture at room temperature for 15 minutes.
[0131] Then, 70 mL of isopropyl alcohol was added and mixed. Then, this liquid was titrated with 1N hydrochloric acid solution (Factor F) as an indicator. The titration value obtained was designated as V2 mL. Next, the titration value obtained without the polyisocyanate sample was designated as V1ml. Next, the isocyanate group content (NCO%) (mass%) of the polyisocyanate composition was calculated from the following formula. Note that the NCO% values calculated without the solvent and with the solvent were used.
[0132] In Table 1, the isocyanate group content calculated without the solvent is indicated as "NCO% (excluding solvent)", and the isocyanate group content calculated with the solvent is indicated as "NCO% (as is)". Isocyanate group content (mass%) = (V1-V2) x F x 42 / (W x 1000) x 100
[0133] Number average molecular weight and weight average molecular weight The number average molecular weight and weight average molecular weight are those measured by gel permeation chromatography (GPC) using the following apparatus, using polystyrene as a standard.
[0134] (Measurement conditions) Equipment: Tosoh Corporation, HLC-802A Column: Tosoh Corporation, G1000HXL x 1 G2000HXL x 1 G3000HXL x 1 Carrier: Tetrahydrofuran Detection method: Differential refractometer
[0135] Average number of isocyanate functional groups The average number of isocyanate functional groups (average NCO number) of the polyisocyanate composition was calculated by the following formula. In the formula, "Mn" means number average molecular weight, and the value measured in "Physical Properties 2" above was used. "NCO%" is the value calculated as NCO% (excluding solvent) in "Physical Properties 1" above. Average number of isocyanate functional groups = (Mn x NCO% x 0.01) / 42
[0136] Glass transition temperature Tg The glass transition temperature of the crosslinkable functional group-containing compound was measured by the following method. The organic solvent and water in the crosslinkable functional group-containing compound solution were evaporated under reduced pressure, and the vacuum-dried product was measured using a differential scanning calorimeter (DSC) at a heating rate of 5°C / min, and the value was used as the glass transition temperature.
[0137] Solid content of polyisocyanate composition The solid content of the polyisocyanate composition was determined as follows. First, an aluminum dish with a bottom diameter of 38 mm was precisely weighed. Next, about 1 g of the polyisocyanate composition produced in the Examples and Comparative Examples was precisely weighed on the aluminum dish (W1). Next, the polyisocyanate composition was adjusted to a uniform thickness. Next, the polyisocyanate composition placed on the aluminum dish was kept in an oven at 150°C for 1 hour. Next, after the aluminum dish reached room temperature, the polyisocyanate composition remaining on the aluminum dish was precisely weighed (W2). Next, the solid content (mass%) of the polyisocyanate composition was calculated from the following formula.
[0138] Solid content of polyisocyanate composition (mass%)=W2 / W1×100
[0139] [Table 1]
[0140] As shown in the above results, when the polyisocyanate compositions of Examples 1 to 8 were used, cured products excellent in adhesive strength and adhesive durability were obtained. When Examples 1 to 8 were used, it was confirmed that they had high tensile strength both under 23°C and 60°C conditions. Since they had high tensile strength even under 60°C conditions, it was confirmed that they had heat resistance.
[0141] In Comparative Example 1, in which only an aliphatic diisocyanate was used, the Konig hardness, tensile strength, elongation percentage, and shear adhesive strength were all lower than those in the Examples. Comparative Example 2, in which only an alicyclic diisocyanate was used, exhibited high tensile strength under conditions of 60° C., but did not exhibit adhesion durability. Comparative Example 4, in which the amount of alicyclic diisocyanate was greater than that of aliphatic diisocyanate, also exhibited high tensile strength at 60° C., but had poor adhesion durability. In Comparative Examples 3 and 5, in which the values of formula (I) were lower than the lower limit of the present invention, the Konig hardness, tensile strength, elongation and shear adhesive strength were all lower than those of the Examples. In Comparative Example 6, in which the weight average molecular weight of the polyisocyanate exceeded 1200, the Konig hardness, tensile strength, elongation percentage, and shear adhesive strength were all lower than those in the Examples.
Claims
1. A polyisocyanate composition containing a polyisocyanate derived from at least one of an aliphatic diisocyanate and an alicyclic diisocyanate and having an isocyanurate group, The polyisocyanate has a value represented by the following formula (I) of 31 or more and 55 or less, The polyisocyanate composition, wherein the polyisocyanate has a weight average molecular weight of 500 or more and 1,200 or less. [B / (A+B)]×100...(I) (In formula (I), A is the weight of the constituent component derived from the aliphatic diisocyanate, and B is the weight of the constituent component derived from the alicyclic diisocyanate.)
2. The polyisocyanate composition according to claim 1, wherein the polyisocyanate composition has an average number of isocyanate groups of 2.6 or more and 3.8 or less.
3. The polyisocyanate composition according to claim 1 or 2, wherein the polyisocyanate composition has an isocyanate group content of 19.3 mass% or more in a solvent-free state.
4. The polyisocyanate composition according to claim 1 or 2, wherein the alicyclic diisocyanate is isophorone diisocyanate.
5. The polyisocyanate composition according to claim 1 or 2, which contains at least one of a urethane group, an allophanate group, a urea group, a biuret group, and a uretdione group in addition to an isocyanurate group, and has a value represented by the following formula (II) of 0.70 or more. c / (c+d+e+f+g+h)...(II) (In formula (II), c is the number of moles of isocyanurate groups, d is the number of moles of urethane groups, e is the number of moles of allophanate groups, f is the number of moles of urea groups, g is the number of moles of biuret groups, and h is the number of moles of uretdione groups.)
6. The polyisocyanate composition according to claim 1 or 2, wherein the polyisocyanate composition has a viscosity of 20,000 mPa·s or less at 25° C.
7. The polyisocyanate composition according to claim 1 or 2, wherein the polyisocyanate composition has a solids content of 60% or more.
8. The polyisocyanate composition according to claim 1 or 2, wherein the polyisocyanate composition forms a cured resin film having a Konig hardness of 110 or more in an environment at 25° C. The cured resin film is a cured resin film having a thickness of 40 μm, which is formed by applying the polyisocyanate composition onto glass and curing the applied film at 23° C. for 168 hours.
9. An adhesive resin composition comprising the polyisocyanate composition according to claim 1 or 2 and a crosslinkable functional group-containing compound.
10. The adhesive resin composition according to claim 9, wherein the adhesive resin composition has a Konig hardness of 140 or more in a cured product 1 at 23° C. The cured product 1 is an adhesive resin cured product having a film thickness of 40 μm, which is obtained by applying the adhesive resin composition onto glass, heating at 80° C. for 30 minutes, and then curing at 23° C. for 168 hours.
11. 10. The adhesive resin composition according to claim 9, wherein the adhesive resin composition is prepared using a crosslinkable functional group-containing compound having a Tg of 0° C. or higher in an environment of 23° C. with a chuck distance of 20 mm and a peeling speed of 20 mm / min, and the cured product 2 has a tensile strength of 62 MPa or higher. However, the cured product 2 is an adhesive resin cured product obtained by applying the adhesive resin composition to a release film to a thickness of 40 μm, heating at 80° C. for 30 minutes, and curing at 23° C. for 168 hours.
12. 10. The adhesive resin composition according to claim 9, wherein the adhesive resin composition is prepared using a crosslinkable functional group-containing compound having a Tg of 0° C. or higher in a 60° C. environment with a chuck distance of 20 mm and a peeling speed of 20 mm / min, and the cured product 2 has a tensile strength of 27 MPa or higher. However, the cured product 2 is an adhesive resin cured product obtained by applying the adhesive resin composition to a release film to a thickness of 40 μm and curing the applied adhesive resin composition at 23° C. for 168 hours.
13. The adhesive resin composition according to claim 9, wherein the adhesive resin composition is prepared using a crosslinkable functional group-containing compound having a Tg of 0° C. or higher and has a tensile elongation of 7% or more in a 60° C. environment with a chuck distance of 20 mm and a peeling speed of 20 mm / min. The cured product 2 is an adhesive resin cured product obtained by applying the adhesive resin composition to a release film to a thickness of 40 μm and curing the applied adhesive resin composition at 23° C. for 168 hours.
14. The adhesive resin composition according to claim 9, wherein the adhesive resin composition has a shear adhesive strength of 19 MPa or more, measured at a test speed of 50 mm / min on a test piece produced under the following conditions. [Test piece manufacturing conditions] Two electrodeposited plates of 20 mm width x 100 mm length are bonded together using the adhesive resin composition. At this time, the bonding area of the two electrodeposited plates is 5 mm x 20 mm. After bonding, the plates are heated at 80°C for 30 minutes and then aged at 23°C for 336 hours to produce a test piece.
15. The adhesive resin composition according to claim 9, wherein the adhesive resin composition contains a silane coupling agent, and the amount of the silane coupling agent per 100 mass parts of total solids of the adhesive resin composition is 0.01 parts by weight or more and 5.0 parts by weight or less.
16. The adhesive resin composition according to claim 9, wherein the crosslinkable functional group-containing compound contains at least one functional group selected from the group consisting of a hydroxyl group, a carboxyl group, and an amino group, and has a glass transition temperature of 0°C or higher and 100°C or lower.
17. A cured adhesive resin comprising the polyisocyanate composition according to claim 1 or 2 and a crosslinkable functional group-containing compound.
18. 18. The adhesive resin cured product according to claim 17, having a gel fraction of 90% or more.
Citation Information
Patent Citations
Polyisocyanate composition
JP2002293873A
Polyisocyanate composition, coating composition and cured article
JP2015127368A
Light-resistant polyurethane composition
JP2015517018A
Polyisocyanate composition, coating composition and aqueous adhesive composition
JP2020070440A
Coating composition comprising a bicyclo-orthoester-functional compound, an isocyanate-functional compound, and a thiol-functional compound
US20020123600A1