Method for manufacturing aluminum alloy-based cylinder block
By controlling the nickel content in recycled aluminum-silicon alloy cylinder blocks and using die casting and heat treatments, the method addresses the decrease in seizure resistance, maintaining wear resistance and mechanical properties.
Patent Information
- Application Number
- JP2023073324
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The use of recycled aluminum-silicon alloy materials in manufacturing cylinder blocks leads to a decrease in seizure resistance, primarily due to the formation of intermetallic compounds containing nickel.
A manufacturing method that uses recycled aluminum-silicon alloy with controlled nickel content (0.1% by mass or less) and optional dilution with virgin aluminum alloy to manage nickel content, combined with die casting and heat treatments, to suppress the formation of intermetallic compounds and maintain seizure resistance.
The method effectively suppresses the deterioration in seizure resistance of aluminum alloy cylinder blocks, ensuring they maintain wear resistance and mechanical properties.
Smart Images

Figure 2024158265000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing an aluminum alloy cylinder block, and more particularly to a method for manufacturing a cylinder block made of an aluminum-silicon alloy of a hypereutectic composition. [Background technology]
[0002] In recent years, aluminum alloys have been increasingly used for cylinder blocks in order to reduce the weight of internal combustion engines. Since high wear resistance is required for cylinder blocks, aluminum alloys containing a large amount of Si, i.e., aluminum-silicon alloys with hypereutectic composition, are considered promising as aluminum alloys for cylinder blocks. In cylinder blocks made of aluminum-silicon alloys, silicon crystal grains located on the sliding surfaces contribute to improving wear resistance. A cylinder block made of an aluminum-silicon alloy is disclosed in Patent Document 1, for example. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2004 / 002658 Summary of the Invention [Problem to be solved by the invention]
[0004] Recently, with the rise in environmental awareness, various efforts are being made to achieve carbon neutrality. In order to contribute to the realization of carbon neutrality, the applicant of the present application is actively promoting the use of recycled aluminum alloys.
[0005] However, according to the investigations of the present inventors, it has been found that when recycled materials are used to manufacture a cylinder block made of an aluminum-silicon alloy having a hypereutectic composition, the seizure resistance of the cylinder block may be reduced.
[0006] An embodiment of the present invention has been made in consideration of the above-mentioned problems, and its object is to suppress a decrease in seizure resistance in an aluminum alloy cylinder block manufactured using recycled materials. [Means for solving the problem]
[0007] This specification discloses a method for manufacturing an aluminum alloy cylinder block as described in the following items.
[0008] [Item 1] A method for manufacturing an aluminum alloy cylinder block, comprising the steps of: A process A of preparing a recycled aluminum alloy material containing 12% by mass or more and 20% by mass or less of Si; A step B of obtaining a molten metal having a Ni content of 0.1% by mass or less by using the recycled material as at least a part of a raw material; A step C of performing die casting using the molten metal; The manufacturing method includes the steps of:
[0009] A manufacturing method according to an embodiment of the present invention includes a step B of obtaining a molten metal using, as at least a part of a raw material, a recycled material of an aluminum alloy containing 12% by mass to 20% by mass of Si (i.e., an aluminum-silicon alloy having a hypereutectic composition), and the Ni content of the molten metal obtained in the step B is 0.1% by mass or less. This suppresses the generation of intermetallic compounds containing Ni in the manufactured cylinder block, and thus suppresses a decrease in the seizure resistance of the cylinder block.
[0010] [Item 2] 2. The method according to item 1, wherein the molten metal obtained in step B has a Zn content of 0.3 mass% or less.
[0011] From the viewpoint of preventing a decrease in seizure resistance, it is more preferable that the Zn content in the molten metal obtained in step B is 0.3 mass % or less.
[0012] [Item 3] 3. The method according to item 1 or 2, wherein the Ni content of the recycled material prepared in step A is 0.1% by mass or less.
[0013] In step A, by preparing a recycled material having a Ni content of 0.1 mass % or less, it becomes easy to adjust the Ni content of the molten metal obtained in step B to 0.1 mass % or less.
[0014] [Item 4] 4. The method according to any one of items 1 to 3, wherein the Ni content of the molten metal obtained in step B is less than 0.05% by mass.
[0015] From the viewpoint of preventing a decrease in seizure resistance, it is more preferable that the Ni content of the molten metal obtained in step B is less than 0.05 mass %.
[0016] [Item 5] 5. The method according to any one of items 1 to 4, wherein the molten metal obtained in step B has a Cu content of 3.0% by mass or more and 5.0% by mass or less.
[0017] The molten metal contains Cu, which improves the strength after heat treatment. The Cu content of the molten metal is, for example, 3.0 mass % or more and 5.0 mass % or less.
[0018] [Item 6] The step B is A step b1 of melting at least the recycled material to obtain a primary molten metal; A step b2 of performing a component analysis on the primary molten metal; 6. The method for producing a process according to any one of items 1 to 5, comprising:
[0019] The process B may include at least a process b1 of melting the recycled material to obtain a primary molten metal, and a process b2 of performing a component analysis on the primary molten metal. This makes it possible to determine whether the Ni content of the primary molten metal is 0.1 mass% or less, and therefore makes it easy to control the Ni content of the molten metal finally obtained in the process B.
[0020] [Item 7] The step B is 7. The method according to item 6, further comprising a step b3 of diluting the primary molten metal with a virgin aluminum alloy having a Ni content of less than 0.1% by mass when the Ni content of the primary molten metal is more than 0.1% by mass.
[0021] Step B may further include step b3 of diluting the primary molten metal with a virgin aluminum alloy having a Ni content of less than 0.1% by mass when the Ni content of the primary molten metal exceeds 0.1% by mass. By carrying out such step b3, the Ni content of the molten metal finally obtained in step B can be reduced, so that even if the Ni content of the primary molten metal exceeds 0.1% by mass, the Ni content of the molten metal finally obtained can be 0.1% by mass or less. Effect of the Invention
[0022] According to an embodiment of the present invention, it is possible to suppress a decrease in seizure resistance in an aluminum alloy cylinder block manufactured using recycled materials. [Brief description of the drawings]
[0023] [Figure 1] 1 is a perspective view showing a cylinder block 100 that can be manufactured by a manufacturing method according to an embodiment of the present invention. [Diagram 2] 2 is an enlarged schematic plan view of a sliding surface of a cylinder block 100. FIG. [Diagram 3] 2 is a flow chart of a manufacturing method according to an embodiment of the present invention. [Figure 4] 4 is a graph showing evaluation results of seizure properties for cylinder blocks of prototypes 1 and 2. [Diagram 5] 1 is a graph showing the calculation results of the liquid phase ratio for virgin material and recycled material. [Figure 6] 1 is a graph showing the calculation results of the composition of the liquid phase of recycled material. [Figure 7]1 is a graph showing DSC curves during the temperature rise process for virgin material and recycled material. [Figure 8] 1 is a graph showing the calculation results of the liquid phase ratio for a recycled material having the composition shown in Table 5 (Ni content of 0.1 mass %, Zn content of 0.3 mass %). [Figure 9] 13 is a flowchart showing another embodiment of step S2 for obtaining a molten metal. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. However, the present invention is not limited to the following embodiment.
[0025] First, an example of a cylinder block manufactured by the manufacturing method according to the embodiment of the present invention will be described. For example, a cylinder block 100 shown in Fig. 1 can be manufactured by the manufacturing method according to the embodiment of the present invention.
[0026] The cylinder block 100 is formed from an aluminum alloy containing Si, more specifically, an aluminum-silicon alloy of a hypereutectic composition.
[0027] 1, the cylinder block 100 has a wall portion (called a "cylinder bore wall") 103 that defines a cylinder bore 102, and a wall portion (called a "cylinder block outer wall") 104 that surrounds the cylinder bore wall 103 and forms the outer contour of the cylinder block 100. A water jacket 105 that holds a coolant is provided between the cylinder bore wall 103 and the cylinder block outer wall 104.
[0028] A surface 101 of a cylinder bore wall 103 on the cylinder bore 102 side is a sliding surface that comes into contact with a piston. This sliding surface 101 is shown enlarged in Fig. 2. Fig. 2 is a plan view showing the sliding surface 101 in schematic form.
[0029] 2, the cylinder block 100 has a plurality of silicon crystal grains 1, 2 and an intermetallic compound 4 on a sliding surface 101. These silicon crystal grains 1, 2 and the intermetallic compound 4 are dispersed in a matrix (alloy base material) 3 of a solid solution containing aluminum.
[0030] When a molten aluminum-silicon alloy with a hypereutectic composition is cooled, the silicon crystal grains that crystallize first are called "primary silicon grains," and the silicon crystal grains that crystallize next are called "eutectic silicon grains." Of the multiple silicon crystal grains 1 and 2 shown in FIG. 2, the relatively large silicon crystal grain 1 is a primary silicon grain. Also, the relatively small silicon crystal grain 2 located between the primary silicon grains is a eutectic silicon grain. There are two types of intermetallic compounds 4: those that crystallize when the molten alloy is cooled, and those that precipitate by heat treatment.
[0031] Since the sliding surface 101 of the cylinder block 100 has the above-mentioned structure, the cylinder block 100 can have excellent wear resistance.
[0032] The present inventors have investigated the use of recycled materials in the manufacture of cylinder blocks made of aluminum-silicon alloys with a hypereutectic composition, and have found that the use of recycled materials may reduce the seizure resistance of the cylinder block. After further investigation, the present inventors have found that the occurrence of seizure is caused by intermetallic compounds containing Ni (nickel). The present invention has been made based on the findings of the present inventors.
[0033] Hereinafter, a method for manufacturing a cylinder block according to an embodiment of the present invention will be described with reference to Fig. 3. Fig. 3 is a flowchart of the manufacturing method according to the embodiment of the present invention.
[0034] First, a recycled aluminum alloy material containing Si is prepared (step S1). This aluminum alloy is an aluminum-silicon alloy with a hypereutectic composition, and the Si content is specifically 12% by mass or more and 20% by mass or less (more preferably 16% by mass or more and 18% by mass or less).
[0035] Next, the recycled material prepared in step S1 is used as at least a part of the raw material to form a molten metal (step S2). The Ni content of the molten metal obtained in step S2 is equal to or less than a predetermined value, specifically, equal to or less than 0.1 mass%. The molten metal is formed by heating and melting the raw material in a melting furnace. Only recycled material may be used as the raw material (i.e., the front part of the raw material may be recycled material), or recycled material and virgin material may be used in combination. Using only recycled material as the raw material can further promote the use of recycled material.
[0036] Next, the obtained molten metal is subjected to die casting (step S3). That is, the molten metal is injected into a mold at high speed and pressure and cooled to form a molded body. At this time, by cooling the vicinity of the sliding surface at a high cooling rate (for example, 4°C / sec or more and 400°C / sec or less), a molded body having silicon crystal grains that contribute to wear resistance near the surface is obtained. This step S3 can be performed, for example, by using a casting device disclosed in Patent Document 1.
[0037] Next, the compact removed from the mold is subjected to one of the heat treatments called "T5", "T6" and "T7" (step S4). The T5 treatment is a treatment in which the compact is quenched by water cooling or the like immediately after being removed from the mold, then artificially aged at a predetermined temperature for a predetermined time to improve mechanical properties and stabilize dimensions, and then air-cooled. The T6 treatment is a treatment in which the compact is solution-treated at a predetermined temperature for a predetermined time after being removed from the mold, then water-cooled, then artificially aged at a predetermined temperature for a predetermined time, and then air-cooled. The T7 treatment is a treatment that causes overaging compared to the T6 treatment, and can achieve more dimensional stability than the T6 treatment, but the hardness is lower than that of the T6 treatment.
[0038] Next, the molded body is subjected to a predetermined machining process (step S5). Specifically, the mating surfaces with the cylinder head and the crankcase are ground.
[0039] Thereafter, the inner surface of the part of the molded body that will become the cylinder bore wall (i.e., the surface that will become the sliding surface) is processed to form a sliding surface (step S6), for example, by fine boring, honing, etching, or the like.
[0040] As described above, the manufacturing method according to the embodiment of the present invention includes step S2 of obtaining a molten metal by using recycled aluminum alloy material containing 12% by mass or more and 20% by mass or less of Si as at least a part of the raw material, and the Ni content of the molten metal obtained in step S2 is 0.1% by mass or less. As already explained, the occurrence of seizure is considered to be caused by intermetallic compounds containing Ni. By making the Ni content of the molten metal 0.1% by mass or less, the generation of intermetallic compounds containing Ni in the manufactured cylinder block is suppressed, and therefore the deterioration of the seizure resistance of the cylinder block is suppressed.
[0041] From the viewpoint of preventing deterioration of seizure resistance, it is more preferable that the molten metal obtained in step S2 have a Zn (zinc) content of 0.3 mass % or less. The effect of Zn on seizure will be described later.
[0042] For example, by preparing a recycled material with a Ni content of 0.1 mass % or less in step S1, it becomes easy to adjust the Ni content of the molten metal obtained in step S2 to 0.1 mass % or less.
[0043] From the viewpoint of preventing deterioration of seizure resistance, it is more preferable that the Ni content of the molten metal obtained in step S2 is less than 0.05% by mass. When the Ni content of the molten metal is less than 0.05% by mass, deterioration of seizure resistance can be prevented more reliably.
[0044] Although there is no particular restriction on the content of components other than Si and Ni in the molten metal obtained in step S2, the molten metal containing Cu (copper) improves the strength after heat treatment. The Cu content of the molten metal is, for example, 3.0 mass% or more and 5.0 mass% or less.
[0045] Here, the results of investigating the effect of using recycled materials on seizure resistance will be described.
[0046] First, a cylinder block of prototype 1 was manufactured using virgin material having the chemical composition shown in Table 1, and a cylinder block of prototype 2 was manufactured using recycled material having the chemical composition shown in Table 1.
[0047] [Table 1]
[0048] Next, the metal structures of prototypes 1 and 2 were observed using a scanning electron microscope (SEM) and wavelength dispersive X-ray analysis (EPMA). In prototype 2, an intermetallic compound formed of Al, Cu, and Ni (presumably Al7Cu4Ni, hereinafter sometimes referred to as "AlCuNi compound") was observed, but in prototype 1, no such intermetallic compound was observed.
[0049] Next, a reciprocating sliding test (SRV test) was carried out to evaluate the seizure properties of prototypes 1 and 2. The test conditions are as shown below, and the evaluation was carried out five times for each of prototypes 1 and 2. Counterpart: Barrel-shaped iron test piece with Sn-plated surface Stroke: 2000μm Frequency: 10Hz Heater temperature: 175℃ Oil: 10W-40 2500μl (soaking) Break-in time (50N constant): 1 minute Load: 600N Test time: Until burn-in occurs (maximum 30 minutes)
[0050] The evaluation results of image sticking characteristics are shown in Figure 4. An "X" in Figure 4 indicates the occurrence of image sticking. As shown in Figure 4, a clear difference was observed in the time until image sticking occurred between prototype 1 and prototype 2. Specifically, the time until image sticking occurred was shorter in prototype 2 than in prototype 1.
[0051] Next, for prototypes 1 and 2, the above-mentioned SRV test was stopped just before the occurrence of seizure, and the surface of the mating material was observed. In prototype 1, almost no material was found to have been transferred to the mating material, but in prototype 2, material was found to have been transferred to the mating material. The results of a component analysis of the transferred material in prototype 2 (chemical composition of the transferred material) are shown in Table 2. Table 3 also shows the results of calculating the amounts of other elements, assuming the amount of Al to be 100, for the chemical composition of the transferred material and the chemical composition of the recycled material that is the raw material for prototype 2.
[0052] [Table 2]
[0053] [Table 3]
[0054] From Tables 2 and 3, it can be seen that the composition of the transferred material contains more Ni and Cu than the composition of the recycled material (i.e., the original composition). This is thought to be due to the formation of AlCuNi compounds in the cylinder block of Prototype 2.
[0055] Next, for the virgin material and the recycled material, the proportion of the liquid phase near the melting point (specifically, 500 to 600°C) and the composition of the liquid phase were calculated using thermodynamic calculation software (product name: Thermo-Calc). Calculations were performed for each of the virgin material and the recycled material using the compositions shown in Table 4. As shown in Table 4, the contents of Zn, Mn, Ni, and Sn differ between the virgin material and the recycled material.
[0056] [Table 4]
[0057] FIG. 5 shows the calculation results of the liquid phase ratio for virgin material and recycled material. From FIG. 5, it can be seen that the melting characteristics are different between virgin material and recycled material. Specifically, at relatively low temperatures, the virgin material has a higher liquid phase ratio than the recycled material, but at 530 to 540°C, the liquid phase ratio is reversed. At 540 to 560°C, the recycled material has a 5 to 10% higher liquid phase ratio than the virgin material. The reason why the time until seizure occurred was short in the above-mentioned prototype 2 is thought to be due to such a difference in melting characteristics.
[0058] Figure 6 shows the calculation results for the liquid phase composition of recycled materials. Figure 6 shows the amounts of Al, Cu, Zn, Mn, Ni, and Sn when the total amount is set to 1.0 kg. From Figure 6, it is believed that the reversal of the high and low liquid phase ratio at 530-540°C is due to the melting of Ni (melting of intermetallic compounds containing Ni). It is also presumed that the melting of Zn also contributes.
[0059] Next, differential scanning calorimetry (DSC) was performed to verify whether the melting characteristics of the virgin material and recycled material, which have the compositions shown in Table 4, are actually different. Figure 7 shows the DSC curves during the temperature rise process.
[0060] From Figure 7, it can be seen that from around 530-540°C, differences in melting characteristics occur between virgin and recycled materials, with the recycled material showing a peak at a lower temperature than the virgin material. Thus, the evaluation results of the actual melting characteristics of virgin and recycled materials were generally consistent with the calculation results using thermodynamic calculation software.
[0061] As mentioned above, it was confirmed that the melting characteristics of virgin materials and recycled materials are different. As already explained, the difference in melting characteristics is considered to be caused by the presence or absence of the formation of AlCuNi compounds, and such a difference in melting characteristics is considered to be the cause of the difference in seizure characteristics.
[0062] As described above, in the manufacturing method according to the embodiment of the present invention, the Ni content of the molten metal obtained in step S2 is 0.1 mass% or less, so that the generation of AlCuNi compounds in the manufactured cylinder block is suppressed, and as a result, the deterioration of the seizure resistance of the cylinder block is suppressed. From the viewpoint of suppressing the deterioration of the seizure resistance, it is more preferable that the Ni content of the molten metal obtained in step S2 is less than 0.05 mass%.
[0063] As explained with reference to FIG. 6, it is presumed that the melting of Zn also contributes to the difference in melting characteristics. Therefore, from the viewpoint of suppressing a decrease in seizure resistance, it is more preferable that the Zn content of the molten metal obtained in step S2 be 0.3 mass % or less.
[0064] Figure 8 shows the results of calculating the liquid phase ratio near the melting point (specifically, 500 to 600°C) using thermodynamic calculation software (product name: Thermo-Calc) for recycled materials with the compositions shown in Table 5 (Ni content of 0.1 mass%, Zn content of 0.3 mass%). Figure 8 also shows the calculation results for virgin materials and recycled materials with the compositions shown in Table 4.
[0065] [Table 5]
[0066] From FIG. 8, it can be seen that the recycled material with the composition shown in Table 5 has melting characteristics close to those of virgin material.
[0067] Another embodiment of the step S2 of obtaining a molten metal will be described with reference to Fig. 9. The step S2 of obtaining a molten metal may include steps S21, S22, and S23 shown in Fig. 9.
[0068] 9, first, at least recycled materials are melted to obtain a primary molten metal (step S21). As the raw material, only recycled materials may be used (i.e., the front part of the raw material may be recycled materials), or recycled materials and virgin materials may be used in combination.
[0069] Next, the primary molten metal is subjected to a component analysis (step S22). As a method for the component analysis, various known methods can be used, for example, optical emission spectroscopy.
[0070] When the Ni content of the primary molten metal exceeds 0.1% by mass, the primary molten metal is diluted with virgin aluminum alloy material having a Ni content of less than 0.1% by mass (step S23). This allows the Ni content of the finally obtained molten metal to be 0.1% by mass or less. When the Ni content of the primary molten metal is 0.1% by mass or less, the primary molten metal becomes the final molten metal as it is. Note that after step S23, a component analysis may be performed on the diluted molten metal.
[0071] In this manner, step S2 may include step S21 of obtaining a primary molten metal and step S22 of performing a component analysis on the primary molten metal. This makes it possible to determine whether the Ni content of the primary molten metal is 0.1 mass% or less, making it easy to control the Ni content of the molten metal finally obtained in step S2.
[0072] Furthermore, as exemplified above, step S2 may further include step S23 of diluting the primary molten metal with a virgin material having a Ni content of less than 0.1% by mass when the Ni content of the primary molten metal exceeds 0.1% by mass. By carrying out such step S23, the Ni content of the molten metal finally obtained in step S2 can be reduced, so that even if the Ni content of the primary molten metal exceeds 0.1% by mass, the Ni content of the molten metal finally obtained can be 0.1% by mass or less.
[0073] As already explained, the Si content and Ni content of the molten metal obtained in step S2 are 12 mass% or more and 20 mass% or less (preferably 16 mass% or more and 18 mass% or less) and 0.1 mass% or less (preferably less than 0.05 mass%), respectively. The Zn content of the molten metal obtained in step S2 is preferably 0.3 mass% or less. Other components of the molten metal obtained in step S2 are not particularly limited, but a suitable example of the composition of the molten metal obtained in step S2 is as shown in Table 6.
[0074] [Table 6] [Industrial Applicability]
[0075] According to the embodiment of the present invention, it is possible to suppress the deterioration of seizure resistance in an aluminum alloy cylinder block manufactured using recycled materials. The cylinder block manufactured by the manufacturing method according to the embodiment of the present invention is suitably used for internal combustion engines of various transportation machines such as motorcycles. [Explanation of symbols]
[0076] 1: primary silicon grain, 2: eutectic silicon grain, 3: matrix, 4: intermetallic compound, 100: cylinder block, 101: sliding surface, 102: cylinder bore, 103: cylinder bore wall, 104: cylinder block outer wall, 105: water jacket
Claims
1. A method for manufacturing an aluminum alloy cylinder block, comprising the steps of: A step A of preparing a recycled aluminum alloy material containing 12% by mass or more and 20% by mass or less of Si; A step B of obtaining a molten metal having a Ni content of 0.1 mass% or less by using the recycled material as at least a part of a raw material; A step C of performing die casting using the molten metal; The manufacturing method includes the steps of:
2. The method according to claim 1 , wherein the molten metal obtained in step B has a Zn content of 0.3 mass % or less.
3. The method according to claim 1 or 2, wherein the Ni content of the recycled material prepared in the step A is 0.1 mass % or less.
4. The method according to claim 1 or 2, wherein the Ni content of the molten metal obtained in the step B is less than 0.05 mass%.
5. The method according to claim 1 or 2, wherein the Cu content of the molten metal obtained in the step B is 3.0 mass % or more and 5.0 mass % or less.
6. The step B comprises: A step b1 of melting at least the recycled material to obtain a primary molten metal; A step b2 of performing a component analysis on the primary molten metal; The method of claim 1 or 2, comprising:
7. The step B comprises: The method according to claim 6, further comprising a step b3 of diluting the primary molten metal with a virgin aluminum alloy having a Ni content of less than 0.1% by mass when the Ni content of the primary molten metal is more than 0.1% by mass.
Citation Information
Patent Citations
Method and device for vacuum die casting of aluminum alloy, and aluminum alloy product
WO2004002658A1