Apparatus and method for producing semiconductor nanoparticle
The semiconductor nanoparticle manufacturing apparatus and method address the challenges of controlling particle size and dispersibility by using a flow synthesis system with ligand concentration control, enabling cadmium-free production with improved dispersibility and emission properties.
Patent Information
- Application Number
- JP2023073541
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing semiconductor nanoparticles face challenges in controlling particle size, composition, and dispersibility, particularly when using water-soluble ligands, and often involve the use of cadmium, which is undesirable from a safety perspective.
A semiconductor nanoparticle manufacturing apparatus and method that utilizes flow synthesis with a detection and control system to manage the concentration of water-soluble ligands, allowing for cadmium-free production with high luminescent properties and dispersibility, by incorporating a raw material supply, heating, detection, and ligand supply system.
The method suppresses aggregation and particle size variation, ensuring high dispersibility and narrow half-width emission spectra, suitable for applications in bioimaging and bioassays.
Smart Images

Figure 2024158386000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an apparatus and method for producing semiconductor nanoparticles. [Background technology]
[0002] Semiconductor nanoparticles are nanometer-sized microcrystals produced by chemical synthesis, and unlike bulk materials, they have the advantage that physical quantities such as band gap energy can be adjusted according to the particle size. Semiconductor nanoparticles, also known as quantum dots, are attracting attention as next-generation light-emitting materials that can adjust the band gap energy, i.e., the emission wavelength, according to not only the material composition but also the particle size due to their quantum size effect.
[0003] Another luminescence characteristic of semiconductor nanoparticles is that, unlike phosphors and fluorescent dyes, they have a narrow half-width. There are two main physical properties that affect the half-width. The first is that, as mentioned above, the emission wavelength can be adjusted according to the particle size, so the particle size distribution contributes to the half-width. The second is that there are few crystal defects. When there are crystal defects, defect levels are generated and energy is released at a lower energy level than the original band gap energy. If there are many such defect levels, energy is released at various levels, resulting in a wide half-width.
[0004] Conventionally, the so-called hot soap method, in which an ion source of an element constituting the nanoparticle is reacted in an organic solvent, is known as a method for producing semiconductor nanoparticles. However, for application to bioscience fields such as bioimaging and bioassays, a process of substituting an organic ligand bonded to the periphery of the semiconductor nanoparticle with a water-soluble ligand and a process of coating with an amphiphilic polymer as a dispersant for the semiconductor nanoparticle are required, which makes the process complicated.
[0005] In response to this, development of semiconductor nanoparticles using a hydrothermal synthesis method has also been considered. That is, a method has been proposed in which the ion sources and water-soluble ligands that constitute the nanoparticles are dissolved in an aqueous solution, and the ion sources are reacted by heating in a closed vessel to synthesize semiconductor nanoparticles (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2019-34873 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the above method (Patent Document 1), it is necessary to heat the semiconductor nanoparticles at a temperature at which the water-soluble ligand used as a dispersant is easily thermally decomposed, and there is a problem that the ligand concentration varies during the formation process of the semiconductor nanoparticles, making it difficult to control the particle size, composition, and dispersibility. In addition, although semiconductor nanoparticles containing cadmium have been available in the past, it is desired to avoid the use of cadmium from the viewpoint of safety.
[0008] The present disclosure is intended to solve the above-mentioned problems in the related art, and has an object to provide a method for producing cadmium-free semiconductor nanoparticles that have high luminescence properties and dispersibility. [Means for solving the problem]
[0009] In order to achieve the above-mentioned object, the semiconductor nanoparticle manufacturing apparatus according to the present disclosure is a semiconductor nanoparticle manufacturing apparatus that performs flow synthesis of semiconductor nanoparticles from a raw material solution containing a water-soluble ligand, a cation source, and an anion source, and includes a raw material supply unit that supplies the raw material solution, a heating unit that is connected in series to the raw material supply unit and heats the raw material solution, a detection unit that is branched before and after the heating unit and detects the amount of ligand in the solution before and after heating, a control unit that controls the amount of ligand based on the result detected by the detection unit, and a ligand supply unit that supplies a ligand solution in accordance with the control unit.
[0010] Furthermore, the method for producing semiconductor nanoparticles according to the present disclosure is a method for producing semiconductor nanoparticles by synthesizing semiconductor nanoparticles from a raw material solution containing a water-soluble ligand, a cation source, and an anion source, and includes a raw material supplying step of supplying the raw material solution, a heating step of separating the solutions before and after the heating step and detecting the amounts of ligand in each of the solutions before and after the separation, a control step of controlling the amount of ligand based on the results detected in the detection step, and a ligand supplying step of supplying a ligand solution in accordance with the control step. Effect of the Invention
[0011] As described above, the semiconductor nanoparticle manufacturing apparatus according to the present disclosure can provide semiconductor nanoparticles that are suppressed in aggregation, have reduced particle size variation, and are highly dispersible. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic diagram showing a configuration of a manufacturing apparatus for semiconductor nanoparticles according to a first embodiment. [Diagram 2] 1 is a flowchart of a method for producing semiconductor nanoparticles according to the first embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The semiconductor nanoparticle manufacturing apparatus according to the first embodiment is an apparatus for manufacturing semiconductor nanoparticles that performs flow synthesis of semiconductor nanoparticles from a raw material solution containing a water-soluble ligand, a cation source, and an anion source, and includes a raw material supply unit that supplies the raw material solution, a heating unit that is connected in series to the raw material supply unit and heats the raw material solution, a detection unit that is branched before and after the heating unit and detects the amount of ligand in the solution before and after heating, a control unit that controls the amount of ligand based on the result detected by the detection unit, and a ligand supply unit that supplies a ligand solution in accordance with the control unit.
[0014] In a second aspect of the semiconductor nanoparticle manufacturing apparatus, in the above-mentioned first aspect, the detection unit includes a mechanism for evaluating the difference in peak intensity between peaks corresponding to the molecular weight of the ligand in the raw material solution and the compound solution produced in the heating unit, the control unit includes a mechanism for controlling the amount of ligand introduced based on the value detected in the detection unit, and the ligand supply unit is provided in parallel to the heating unit, connected in a manner that it joins with the compound solution produced in the heating unit, and may include a mechanism for supplying the ligand in response to the control unit.
[0015] A third embodiment of the method for producing semiconductor nanoparticles is a method for producing semiconductor nanoparticles by flow synthesis of semiconductor nanoparticles from a raw material solution containing a water-soluble ligand, a cation source, and an anion source, and includes a raw material supplying step of supplying the raw material solution, a heating step of separating the solutions before and after the heating step and detecting the amounts of ligand in each of the solutions before and after the separation, a control step of controlling the amount of ligand based on the results detected in the detection step, and a ligand supplying step of supplying a ligand solution in accordance with the control step.
[0016] A fourth aspect of the method for producing semiconductor nanoparticles is the third aspect, wherein the detection step includes evaluating the difference in peak intensity between peaks corresponding to the molecular weight of the ligand in the raw material solution and the compound solution generated in the heating section, the control step includes controlling the amount of ligand to be introduced based on the value detected in the detection step, and the ligand supply step may include supplying the ligand to the compound solution generated in the heating step in accordance with the control step.
[0017] A fifth aspect of the method for producing semiconductor nanoparticles is the method for producing semiconductor nanoparticles according to the third or fourth aspect, wherein the ligand is water-soluble and may contain a mercapto group or a disulfide group.
[0018] A sixth aspect of the method for producing semiconductor nanoparticles is any one of the third to fifth aspects, in which the raw material solution does not need to contain cadmium.
[0019] A seventh aspect of the method for producing semiconductor nanoparticles is any one of the third to sixth aspects, wherein the detection step is carried out by detecting a peak intensity I pre The peak intensity I of the peak due to the ligand of the compound solution generated during the heating process heat Ratio I heat / I pre may be 0.8 or more.
[0020] Hereinafter, an apparatus and method for producing semiconductor nanoparticles according to an embodiment will be described with reference to the accompanying drawings, in which substantially identical components are given the same reference numerals.
[0021] (Embodiment 1) Fig. 1 is a schematic diagram showing the configuration of a manufacturing apparatus for semiconductor nanoparticles according to the present embodiment 1. Fig. 2 is a flowchart showing the manufacturing method for semiconductor nanoparticles. As shown in FIG. 1 and FIG. 2, the semiconductor nanoparticle manufacturing apparatus according to the first embodiment includes a raw material supplying section, a heating section, a detection section, a control section, and a ligand supplying section. The raw material supplying section includes a raw material solution tank 101 and a liquid delivery pump 103, and supplies the raw material solution 11. The heating section is connected in series to the liquid delivery pump 103 of the raw material supplying section, includes a heating device 106 and a heating reactor 107, and heats the raw material solution 11. The detection section is branched before and after the heating device of the heating section, includes a T-shaped mixer 104 for fractionation, an on-off valve 105, a cooling device 108 for cooling the solution after heating, a cooling reactor 109, and a molecular weight evaluation device 110, and detects the amount of ligand in the solution before and after heating. The control section includes a calculation device 111 and a control device 112. The ligand supplying section includes a ligand solution tank 102 and a liquid delivery pump. The control section controls the amount of ligand by the ligand supplying section based on the result detected by the detection section.
[0022] Furthermore, as shown in FIG. 2, the method for producing semiconductor nanoparticles according to the first embodiment includes a raw material solution preparation step P1 before the raw material solution is delivered, a raw material supply step P2, a raw material solution heating step P3, a detection step P4, a ligand supply step P5, and a cooling step P6 for recovery. The method for producing semiconductor nanoparticles will be described in relation to the above-mentioned semiconductor nanoparticle production apparatus. In the raw material supply step P2, a raw material solution tank 101 and a liquid delivery pump 103 are provided. In the raw material solution heating step P3, a heating device 106 and a heating reactor 107 are provided. In the detection step P4, a T-shaped mixer 104 for fractionation, an on-off valve 105, a cooling device 108 for cooling the solution after heating, a cooling reactor 109, a molecular weight evaluation device 110, a calculation device 111, and a control device 112 are provided. In addition, in the ligand supply step P5, a ligand solution tank 102 and a liquid delivery pump are provided. In addition, in the cooling step P6 for recovery, a cooling device 108, a cooling reactor 109, and a back pressure valve 113 are provided.
[0023] Each step of the method for producing semiconductor nanoparticles will be described below.
[0024] The raw material solution preparation step P1 is a step of mixing a water-soluble ligand, a cation source compound as raw materials, and an anion source compound with water, respectively, to prepare a raw material solution 11. In Fig. 1, the raw material solution 11 is illustrated as a precursor solution obtained by mixing all of the water-soluble ligand aqueous solution, the cation source aqueous solution, and the anion source aqueous solution, but it is also possible to prepare each aqueous solution, mix them sequentially in a mixing device such as a T-shaped mixer equipped with each tank and liquid delivery pump, and then supply them to the heating step.
[0025] The water-soluble ligand is water-soluble and contains a mercapto group (thiol group: -SH) or a disulfide group (-SS-). In addition, although there is no particular limitation, a material containing one or more water-soluble functional groups such as carboxylic acid, amine, amide, hydroxyl group, and sulfonic acid is preferable. As the ligand, for example, mercaptopropionic acid, thioglycolic acid, thiolactic acid, mercaptoethanol, thioglycerin, aminoethanethiol, mercaptopropanesulfonic acid, N-acetyl-L-cysteine, L-cysteine, cysteamine, lipoic acid, triazinethiols, etc. can be used. In addition, a combination of multiple types of these can be used instead of one type.
[0026] The cation source is not particularly limited as long as it is water-soluble and does not contain cadmium, and examples of the cation source include zinc, indium, copper, silver, gallium, and magnesium, and not only one of these but also a combination of multiple types of these can be used. In addition, the raw material for the cation source can be the chloride, bromide, sulfide, acetate, nitrate, perchlorate, sulfate, etc. of the above-mentioned cation source. This makes it possible to make the cation source cadmium-free.
[0027] The anion source is not particularly limited as long as it is water-soluble, but for example, sulfur, selenium, tellurium, etc. can be used, and a combination of multiple types of these can be used instead of one type. In addition, as the raw material for the anion source, sodium salts, potassium salts, sodium hydride salts, potassium hydride salts of the above-mentioned anion sources, and solutions in which metallic selenium and tellurium are reduced with a reducing agent can be used.
[0028] The raw material supply step P2 is a step of supplying the raw material solution 11 to the heating step P3. As described above, the raw material solution 11, which is a mixture of the water-soluble ligand, cation source, and anion source, is supplied to the heating step by a liquid supply pump. It is also possible to supply aqueous solutions of the ligand, cation source, and anion source by a liquid supply pump, mix them sequentially using a T-shaped mixer, and supply them to the heating step. In this case, however, it is necessary to mix the ligand and cation source first, and then mix them with the anion source. If the cation source and anion source are mixed first, precipitates will immediately occur, making it impossible to produce semiconductor nanoparticles. The raw material supply tank 101 and the liquid delivery pump 103 are not particularly limited, but must be selected according to the required flow rate and pressure.
[0029] The heating step P3 is a step in which the solution in the heating reactor 107, which is a continuous flow path supplied from the raw material supply step P2, is heated by the heater 106. In this step, semiconductor nanoparticles are formed. The heating temperature in P3 is not particularly limited as long as it is a temperature at which semiconductor nanoparticles are formed, and can be, for example, 100° C. or higher and 200° C. or lower. The heating time can be adjusted by the raw material supply concentration, flow rate, and length of the heating reactor, and is not particularly limited as long as it is the time required for semiconductor nanoparticles to be formed and grow to the desired size, but can be, for example, from 0.01 minute (0.6 seconds) to 40 minutes.
[0030] The detection process P4 is a process in which the solution is sampled by opening an on-off valve 105 at the end of a T-shaped mixer 104 that can branch the raw material solution before and after the heating reactor in the continuous flow path, the molecular weight of the ligand is detected by a molecular weight evaluation device 110, and the result is fed back to the ligand supply process as necessary by an arithmetic device 111 and a control device 112. The molecular weight evaluation device 110 may be, for example, a liquid chromatography mass spectrometry method. The peak intensity I pre and the peak intensity I of the peak corresponding to the molecular weight due to the ligand after heating heat and the ratio I heat / I pre When the ratio is 0.8 or less, the amount of ligand supply can be calculated and fed back by the control device.
[0031] The ligand supplying step P5 is a step of supplying a ligand solution in response to feedback from the detection step P4. The ligand supply tank 102 and the liquid delivery pump 103 are not particularly limited, but should be selected according to the required flow rate and pressure. The ligand can be supplied and mixed through a T-shaped mixer 104 into the continuous flow path heated in the heating step P3.
[0032] The cooling step P6 is a step of stopping the growth of semiconductor nanoparticles by cooling the solution in the continuous flow path heated in the heating step P3 in the cooling reactor 109 with the cooling device 108. The cooling temperature in the cooling step P6 is not particularly limited as long as it is a temperature at which the growth of the semiconductor nanoparticles can be stopped, and the cooling temperature can be, for example, 0°C or higher and 5°C or lower. Furthermore, the cooling time is not particularly limited as long as it is a time that can stop the growth of the semiconductor nanoparticles, but can be, for example, from 0.1 minute (6 seconds) to 10 minutes.
[0033] Examples and comparative examples of experiments conducted by the inventors will be described below.
[0034] (Example) Semiconductor nanoparticles were produced by the following production method: N-acetyl-L-cysteine was selected as the ligand, zinc as the cation source, and tellurium as the anion source.
[0035] <Raw material solution preparation process P1> (1) The ultrapure water was stirred under a nitrogen atmosphere, and the dissolved oxygen concentration was confirmed to be 0.2 mg / L. All subsequent steps were then carried out under a nitrogen atmosphere. (2) To prepare a zinc ion source, zinc chloride (Kanto Chemical, special grade) and N-acetyl-L-cysteine (Kishida Chemical, special grade) were dissolved in the ultrapure water. (3) After that, the pH of the Zn ion solution was adjusted with potassium hydroxide (Wako Pure Chemical Industries, special grade). (4) Next, a Te ion source was prepared by dissolving sodium hydrogen telluride. (5) Then, the amount of Te ion source was adjusted and added to the Zn ion solution, and the pH of the precursor solution was adjusted with hydrochloric acid (Kanto Chemical, special grade) to prepare a raw material solution. (6) Furthermore, N-acetyl-L-cysteine (Kishida Chemical, special grade) was dissolved in the ultrapure water as a ligand supplying solution.
[0036] <Raw material supply process P2> The raw material solution was placed in a sealed container and fed using a plunger pump at a flow rate of 2.0 ml / min.
[0037] <Heating process P3> The heating device was set to 190° C., and the raw material solution was heated in the heating reactor for 4 minutes.
[0038] <Detection process P4> The solution was sampled by opening the on-off valve before the heating reactor in the continuous flow path, and the peak corresponding to the molecular weight of the ligand in the raw solution was evaluated. Next, the on-off valve before the heating reactor was closed, and the on-off valve after the heating reactor was opened to sample the solution, and the peak corresponding to the molecular weight of the ligand after heating was evaluated. From these results, the ratio of the peaks corresponding to the molecular weight of the ligand before and after heating was calculated using a computing device, and the result was 0.78.
[0039] <Coordination child supply process P5> As a result of feedback from the results obtained in P4, the ligand solution was delivered at a flow rate of 0.2 ml / min.
[0040] <Cooling process P6> The cooling device was set to 0° C., and the heated solution was cooled in a cooling reactor for 1 minute. Through the above steps, the semiconductor nanoparticles according to the example were obtained. The obtained solution was transparent.
[0041] <Evaluation of light emission characteristics> The emission spectrum of the obtained reaction solution was measured using a quantum efficiency measurement system (QE-2000, manufactured by Otsuka Electronics Co., Ltd.), and emission was confirmed. In the semiconductor nanoparticles according to the embodiment, the peak wavelength and half width (full width at half maximum of the emission peak) of the emission spectrum were 488 nm and 38.9 nm, respectively.
[0042] <Absorption spectrum evaluation> The absorption spectrum of the resulting reaction solution was measured using an ultraviolet-visible spectrophotometer (UV-mini-1240: manufactured by Shimadzu Corporation). The absorbance at 525 nm was 0.005.
[0043] (Comparative Example) The procedure was the same as that described in the Examples, except that no ligand solution was supplied in the ligand supplying step P4 in the Examples. The ratio of the peak intensities of the peaks corresponding to the molecular weight before and after heating was 0.78.
[0044] <Evaluation of light emission characteristics> The emission characteristics were measured in the same manner as in Example 1, and emission was confirmed. In the semiconductor nanoparticles according to Example 1, the peak wavelength and half width (full width at half maximum of the emission peak) of the emission spectrum were 488 nm and 41.4 nm, respectively.
[0045] <Absorption spectrum evaluation> The absorption spectrum was measured in the same manner as in Example 1. The absorbance at 525 nm was 0.010.
[0046] Comparing the Examples and Comparative Examples, the ratio of the peaks corresponding to the molecular weight of the ligand before and after heating is 0.7 or less in both cases, and the amount of the ligand is reduced. This means that the ligand is thermally decomposed by heating, and the function of the ligand as a dispersant is reduced. In contrast, it is believed that in the Examples, the dispersibility is improved and the absorbance is reduced by supplying the ligand solution. Accordingly, it can be seen that the half width is reduced even at the same emission peak wavelength. From the above, it is possible to synthesize semiconductor nanoparticles having high dispersibility and a narrow half-width in any of the semiconductor nanoparticles according to the examples.
[0047] In addition, the present disclosure includes appropriate combinations of any of the various embodiments and / or examples described above, and can achieve the effects of each embodiment and / or example. [Industrial Applicability]
[0048] According to the semiconductor nanoparticle manufacturing apparatus and manufacturing method of the present disclosure, it is possible to provide semiconductor nanoparticles that suppress aggregation, suppress particle size variation, and have high dispersibility, and can be used for bioimaging and bioassays with a high S / N ratio. The semiconductor nanoparticles according to the present disclosure can also be used as luminescent materials for sensors and displays other than biological applications. [Explanation of symbols]
[0049] 11 Raw material solution 12 Ligand solution 101 Raw material solution tank 102 Ligand solution tank 103 Liquid delivery pump 104 T-shaped mixer 105 On-off valve 106 Heating device 107 Heating Reactor 108 Cooling device 109 Cooling Reactor 110 Molecular weight evaluation device 111 Arithmetic equipment 112 Control device 113 Backpressure valve P1 Raw material preparation process P2 Raw material supply process P3 Heating process P4 Evaluation process P5 Coordination child supply process P6 Cooling process
Claims
1. An apparatus for producing semiconductor nanoparticles, which performs flow synthesis of semiconductor nanoparticles from a raw material solution containing a water-soluble ligand, a cation source, and an anion source, comprising: A raw material supply unit that supplies the raw material solution; a heating unit connected in series to the raw material supply unit and configured to heat the raw material solution; a detection unit which is branched before and after the heating unit and detects the amount of the ligand in the solution before and after heating; A control unit that controls the amount of the ligand based on the result detected by the detection unit; a ligand supply unit that supplies a ligand solution in accordance with the control unit; An apparatus for producing semiconductor nanoparticles comprising:
2. The detection unit is A mechanism for evaluating the difference in peak intensity between the peak corresponding to the molecular weight of the ligand in the raw material solution and the compound solution generated in the heating section is included; The control unit is a mechanism for controlling the amount of ligand to be introduced based on the value detected by the detection unit; The ligand supplying unit is provided in parallel to the heating section, The compound solution generated in the heating section is connected to the compound solution generated in the heating section. A mechanism for supplying a ligand in response to the control unit; The apparatus for producing semiconductor nanoparticles according to claim 1 .
3. A method for producing semiconductor nanoparticles, comprising synthesizing semiconductor nanoparticles from a raw material solution containing a water-soluble ligand, a cation source, and an anion source, the method comprising the steps of: A raw material supplying step of supplying the raw material solution; heating the raw material solution; a detection step of sampling the solutions before and after the heating step and detecting the amounts of the ligand in each of the samples before and after the sampling; a control step of controlling the amount of the ligand based on the result detected in the detection step; a ligand supplying step of supplying a ligand solution in accordance with the control step; A method for producing semiconductor nanoparticles, comprising:
4. The detection step includes: The method includes a step of evaluating a difference in peak intensity between a peak corresponding to a molecular weight of a ligand in a raw material solution and a compound solution generated in a heating section, The control step includes: A step of controlling the amount of ligand to be introduced based on the value detected in the detection step, The ligand supplying step includes: supplying a ligand to the compound solution generated in the heating step in response to the control step; The method for producing semiconductor nanoparticles according to claim 3 .
5. The ligand is water-soluble and contains a mercapto group or a disulfide group. The method for producing semiconductor nanoparticles according to claim 3 or 4.
6. The raw material solution does not contain cadmium. The method for producing semiconductor nanoparticles according to claim 3 or 4.
7. In the detection step Peak intensity I of the peak due to the ligand of the raw material solution pre On the other hand, the peak intensity I of the peak due to the ligand of the compound solution generated in the heating step heat Ratio I heat / I pre is equal to or greater than 0.8; The flow synthesis method according to claim 3 or 4.
Citation Information
Patent Citations
JP34873A