Piezoelectric film laminate and manufacturing method thereof

By flattening the lower ScAlN film surface and ensuring the intermediate layer is thinner than 14% of its thickness, the piezoelectric film laminate addresses abnormal grain issues, maintaining piezoelectricity and reducing variations, thus improving the laminate's effectiveness.

JP2024158399AActive Publication Date: 2024-11-08DENSO CORP +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023073561
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

The presence of abnormal grains in ScAlN films with high Sc concentration leads to irregularities on the surface, affecting the intermediate layer and reducing piezoelectricity, either by making the intermediate layer too thick or too thin, which compromises the effective piezoelectricity of the laminate.

Method used

A piezoelectric film laminate is constructed with a lower ScAlN film having a maximum height smaller than the thickness of the intermediate layer, ensuring the intermediate layer is thinner than 14% of the lower ScAlN film, and the surface is flattened to suppress abnormal grain protrusion, using amorphous films for improved crystallinity and capacitance.

Benefits of technology

This approach maintains the piezoelectric constant d33 and prevents reductions and variations in piezoelectricity by containing abnormal grain effects, enhancing the laminate's performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158399000001_ABST
    Figure 2024158399000001_ABST
Patent Text Reader

Abstract

To provide a piezoelectric film laminate capable of suppressing reduction and variations of piezoelectricity caused by abnormal grains.SOLUTION: A piezoelectric film laminate comprises: an Si substrate 11; a lower layer ScAlN film 13 formed on one face 11a of the Si substrate 11; an intermediate layer 14 formed on one face 13a of the lower layer ScAlN film 13 at an opposite side of the Si substrate 11 and consisting of an amorphous film; and an upper layer ScAlN film 15 formed on one face 14a of the intermediate layer 14 at an opposite side of the lower layer ScAlN film 13. A maximum height Rz2 on one face 13a of the lower layer ScAlN film 13 is smaller than a film thickness of the intermediate layer 14 and less than 14% of a film thickness of the lower layer ScAlN film 13.SELECTED DRAWING: Figure 1B
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a piezoelectric film laminate in which a plurality of piezoelectric films are laminated on a substrate serving as a base material, and a method for manufacturing the same. [Background technology]

[0002] When a piezoelectric film is made of ScAlN, it is known that the piezoelectric constant can be increased by incorporating a high concentration of Sc, thereby improving the piezoelectric response (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5190841 Summary of the Invention [Problem to be solved by the invention]

[0004] However, while the piezoelectric constant can be increased by including Sc at a high concentration, it also increases the number of abnormal grains whose c-axes are randomly oriented. The abnormal grains are present in a state where they protrude from the surface of the ScAlN film, so that the surface of the ScAlN film is left with unevenness. For this reason, if an ScAlN film is formed on the ScAlN film through an intermediate layer made of an amorphous film, the intermediate layer is affected by the unevenness of the underlying ScAlN film. The intermediate layer is made of an insulating film and has a capacitance value, but if the intermediate layer is made thicker to alleviate the effect of the unevenness of the ScAlN film, an insulating film with a low capacitance value will exist between the ScAlN films, and the effective piezoelectricity of ScAlN will decrease. For this reason, it is not preferable to make the intermediate layer thick. On the other hand, if the intermediate layer is made thin, abnormal grains protrude from the intermediate layer, and the abnormal grains are inherited by the ScAlN film placed on the intermediate layer, reducing the piezoelectricity, or causing variation in the piezoelectricity due to the variation in the thickness of the intermediate layer.

[0005] In view of the above, an object of the present disclosure is to provide a piezoelectric film laminate capable of suppressing deterioration and variation in piezoelectricity caused by abnormal grains, and a manufacturing method thereof. [Means for solving the problem]

[0006] In order to achieve the above object, the invention described in claim 1 comprises: A piezoelectric film laminate, A substrate (11), A lower layer ScAlN film (13) formed on one surface (11a) of a substrate; an intermediate layer (14) formed on one surface (13a) of the lower ScAlN film opposite to the substrate; an upper layer ScAlN film (15) formed on one surface (14a) of the intermediate layer opposite to the lower layer ScAlN film; The maximum height (Rz2) on one surface of the lower ScAlN film is smaller than the film thickness of the intermediate layer, and is less than 14% of the film thickness of the lower ScAlN film.

[0007] In this way, the maximum height of one surface of the lower ScAlN film is smaller than the thickness of the intermediate layer, and is less than 14% of the thickness of the lower ScAlN film. In other words, by flattening one surface of the lower ScAlN film, the maximum height is made smaller than the thickness of the intermediate layer. This makes it possible to ensure the piezoelectric constant d33 and suppress the decrease and variation in piezoelectricity caused by abnormal grains.

[0008] The invention described in claim 8 is A method for manufacturing a piezoelectric film laminate, comprising the steps of: Providing a substrate (11); forming a lower layer ScAlN film (13) on one surface (11a) of a substrate; flattening a surface (13a) of the lower ScAlN film opposite to the substrate; forming an intermediate layer (14) on one surface of the lower ScAlN film; forming an upper layer ScAlN film (15) on a surface (14a) of the intermediate layer opposite to the lower layer ScAlN film; By forming the intermediate layer, the film thickness of the intermediate layer is made smaller than the maximum height (Rz2) of one side of the lower ScAlN film before planarization and larger than the maximum height of one side of the lower ScAlN film after planarization.

[0009] In this way, by flattening one surface of the lower ScAlN film, the thickness of the intermediate layer can be made smaller than the maximum height of one surface of the lower ScAlN film before flattening and larger than the maximum height of one surface of the lower ScAlN film after flattening. This makes it possible to ensure the piezoelectric constant d33 and suppress the decrease and variation in piezoelectricity caused by abnormal grains.

[0010] The reference symbols in parentheses attached to each component indicate an example of the correspondence between the component and specific components described in the embodiments described below. [Brief description of the drawings]

[0011] [Figure 1A] 1 is a cross-sectional view of a piezoelectric film laminate in a first embodiment. [Figure 1B] 1B is an explanatory diagram of the maximum height of each portion of the piezoelectric film laminate shown in FIG. 1A. [Diagram 2] FIG. 1 is a diagram showing the crystal structure of ScAlN. [Figure 3A] 3A to 3C are diagrams illustrating a manufacturing process of the piezoelectric film laminate in the first embodiment. [Figure 3B] 3B is a diagram showing a manufacturing process of the piezoelectric film laminate subsequent to FIG. 3A. FIG. [Figure 3C] 3C is a diagram showing a manufacturing process of the piezoelectric film laminate subsequent to FIG. 3B. [Figure 3D] 3D is a diagram showing a manufacturing process of the piezoelectric film laminate subsequent to FIG. 3C. [Figure 4] 10 is a cross-sectional view showing the relationship between the maximum height of one surface of the lower ScAlN film before planarization and the film thickness of the second intermediate layer. FIG. [Figure 5A] FIG. 13 is a view showing a surface AFM image of one surface of a lower ScAlN film. [Figure 5B]5B is a diagram showing the results of observing unevenness on one surface of the lower ScAlN film in a cross section taken along line VB-VB in FIG. 5A. FIG. [Figure 6] FIG. 13 is a graph showing the change in piezoelectric constant d33 with respect to the thickness of an amorphous film when an ScAlN film is formed on the amorphous film. [Figure 7] FIG. 11 is a cross-sectional view showing a state in which a second intermediate layer is formed thick and then flattened, and an upper ScAlN film is formed thereon. [Figure 8] FIG. 11 is a cross-sectional view of a piezoelectric film laminate in a second embodiment. [Figure 9A] 7A to 7C are diagrams illustrating a manufacturing process of a piezoelectric film laminate in the second embodiment. [Figure 9B] 9B is a diagram showing a manufacturing process of the piezoelectric film laminate subsequent to FIG. 9A. [Figure 9C] 9C is a diagram showing a manufacturing process of the piezoelectric film laminate subsequent to FIG. 9B. [Figure 10] 4 is an explanatory diagram of the maximum height of one surface of a second electrode film. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In the following embodiments, parts that are the same or equivalent to each other will be denoted by the same reference numerals.

[0013] (First embodiment) 1A and 1B, the piezoelectric film laminate 10 of this embodiment includes a Si substrate 11, a first intermediate layer 12, a lower ScAlN film 13, a second intermediate layer 14, and an upper ScAlN film 15. The piezoelectric film laminate 10 is formed by stacking these films in order.

[0014] The Si substrate 11 is a substrate mainly composed of Si, which is a semiconductor material. Substrates composed of semiconductor materials other than Si may be used. Although not described here, a TEOS (Tetraethyl orthosilicate) film or the like may be formed on one surface 11a of the Si substrate 11.

[0015] The first intermediate layer 12 is formed on one surface 11a of the Si substrate 11, and includes a layer serving as a base for ScAlN. The first intermediate layer 12 may have a multi-layered structure or a single-layered structure. If the first intermediate layer 12 is made of an amorphous film, the crystallinity of the ScAlN formed thereon can be improved. When the first intermediate layer 12 has a multi-layered structure, it is preferable that the outermost layer in contact with the ScAlN is made of an amorphous film. In this embodiment, the first intermediate layer 12 is made of an insulating material, and when it has a multi-layered structure, at least the outermost layer in contact with the ScAlN is made of an insulating material. The maximum height Rz1 of the surface 12a of the first intermediate layer 12 opposite to the Si substrate 11 shown in FIG. 1B is arbitrary, but it is preferable to set it to 0.5 nm or less because good piezoelectricity can be obtained even if the Sc concentration in the ScAlN formed in the upper layer is high.

[0016] Examples of amorphous films made of insulating materials include SiN (silicon nitride) film, TEOS film, silicon oxide film, HfOx (hafnium oxide) film, Mo (molybdenum) oxide film, Al2O3 film, etc. The first intermediate layer 12 of this embodiment is made of one or more of the amorphous films listed here.

[0017] Incidentally, "amorphous" refers to a state of matter that does not have a crystal structure, and is also called non-crystalline. The fact that the material constituting the film is amorphous can be confirmed by performing electron beam diffraction measurement on the film. When the measurement results show a halo pattern, the material constituting the film is amorphous. In addition, in this specification, "insulating" refers to an electrical resistivity, i.e., a volume resistivity of 10 4 This means that the resistance is Ω·m or more.

[0018] The maximum height Rz is the difference between the most protruding and most recessed points of the surface irregularities. The maximum height Rz is specified in JIS B 0601. The maximum height Rz can be measured by scanning the surface with an atomic force microscope, a stylus-type surface roughness meter, or the like. In addition, if another film is formed on the surface to be measured, the maximum height Rz can be measured by observing the cross section with a transmission electron microscope and determining the shape of the interface to be measured.

[0019] The lower ScAlN film 13 is a piezoelectric film mainly composed of ScAlN, i.e., scandium-containing aluminum nitride. The lower ScAlN film 13 is formed on one surface 12a of the first intermediate layer 12, i.e., on one surface 11a of the Si substrate 11 via the first intermediate layer 12. The surface 13a of the lower ScAlN film 13 opposite to the first intermediate layer 12 is flattened as shown in FIG. 1B, so that the maximum height Rz2 is smaller than the film thickness of the second intermediate layer 14 formed on the lower ScAlN film 13.

[0020] The Sc concentration of the lower ScAlN film 13 may be any concentration greater than 0 atomic % and less than or equal to 43 atomic %. Since the higher the Sc concentration, the higher the piezoelectricity, it is preferable to set the Sc concentration to 24 atomic % or more. However, if the Sc concentration is too high, abnormal grains are more likely to occur, so taking into account the amount of abnormal grains that occur, it is preferable for the Sc concentration to be 43 atomic % or less.

[0021] The lower ScAlN film 13 has a hexagonal crystal structure as shown in FIG. 2 and a polycrystalline structure having a plurality of crystal grains. When the plurality of crystal grains contain many c-axis oriented crystal grains in which the c-axis of the hexagonal crystal is oriented perpendicularly to one surface 13a of the lower ScAlN film 13, the piezoelectricity of the lower ScAlN film 13 becomes high. On the other hand, when the plurality of crystal grains contain many abnormal grains in which the c-axis of the hexagonal crystal is oriented randomly, the piezoelectricity of the lower ScAlN film 13 becomes low. There is a relationship in which the fewer the abnormal grains present in the lower ScAlN film 13, the more the c-axis oriented crystal grains present in the lower ScAlN film 13. For this reason, it is desirable to suppress the occurrence of abnormal grains in the ScAlN film 15. Therefore, by containing Sc, preferably at a high Sc concentration, the piezoelectricity is improved while the Sc concentration is suppressed to a level that does not reduce the piezoelectricity, and the Sc concentration is preferably set to 24 atomic % or more and 43 atomic % or less.

[0022] The Sc concentration is the ratio of the number of Sc atoms to the total number of Sc atoms and Al atoms, which is 100 atomic %. The atomic % indicates several hundredths of an atom. The Sc concentration is measured by RBS. RBS is an abbreviation for Rutherford Backscattering Spectrometry. The Sc concentration shown in this specification is a value measured using the following apparatus under the following measurement conditions.

[0023] Device name: National Electrostatics Corporation Pelletron 3SDH Measurement conditions RBS measurements Incident ions: 4He++ Incident energy: 2300keV Incident angle: 0deg Scattering angle: 160deg Specimen current: 13nA Beam diameter: 2mmφ In-plane rotation: None Irradiance: 70μC The second intermediate layer 14 is formed on one surface 13a of the lower ScAlN film 13, and includes a layer serving as a base for ScAlN. The thickness of the second intermediate layer 14 is set to 10 to 20 nm. The second intermediate layer 14 may be a laminated structure of multiple layers, or may be a single layer structure. If the second intermediate layer 14 is made of an amorphous film, the crystallinity of the ScAlN formed thereon can be improved. When the second intermediate layer 14 has a laminated structure, it is preferable that the outermost layer in contact with the ScAlN is made of an amorphous film. In this embodiment, the second intermediate layer 14 is made of an insulating material, and when it has a laminated structure of multiple layers, at least the outermost layer in contact with the ScAlN is made of an insulating material. The maximum height Rz3 of one surface 14a of the second intermediate layer 14 opposite the lower ScAlN film 13 shown in Figure 1B is approximately the same as the maximum height Rz2 of one surface 13a of the lower ScAlN film 13, that is, smaller than the film thickness of the second intermediate layer 14.

[0024] The shape of one surface 14a of the second intermediate layer 14 follows the shape of one surface 13a of the lower ScAlN film 13. Therefore, the maximum height Rz3 is equivalent to the maximum height Rz2. And, since the maximum height Rz2 is smaller than the film thickness of the second intermediate layer 14, all of the irregularities caused by abnormal grains formed on the one surface 13a of the lower ScAlN film 13 are contained within the film thickness of the second intermediate layer 14.

[0025] The upper ScAlN film 15 is formed on one surface 14a of the second intermediate layer 14. The upper ScAlN film 15 has a configuration similar to that of the lower ScAlN film 13. However, for the upper ScAlN film 15, the maximum height Rz4 of one surface 15a opposite to the second intermediate layer 14 shown in Fig. 1B does not need to be equal to the maximum height Rz2 of one surface 13a of the lower ScAlN film 13, and the maximum height Rz4 may be larger than the maximum height Rz2.

[0026] The piezoelectric film laminate 10 thus configured can be used, for example, as a piezoelectric filter. For example, a piezoelectric filter can be configured by joining electrodes (not shown) to the side surfaces of the lower ScAlN film 13 and the upper ScAlN film 15 in the lateral direction of the paper surface of FIG. 1 and incorporating them into a circuit.

[0027] In this embodiment, one surface 13a of the lower ScAlN film 13 is flattened to make the maximum height Rz2 smaller than the film thickness of the second intermediate layer 14. Therefore, even if the film thickness of the second intermediate layer 14 is not large, all of the irregularities caused by abnormal grains in the lower ScAlN film 13 can be contained within the film thickness of the second intermediate layer 14. In other words, the abnormal grains can be prevented from protruding from the second intermediate layer 14. Therefore, it is possible to obtain a piezoelectric film laminate 10 that can suppress the decrease and variation in piezoelectricity caused by abnormal grains.

[0028] Next, a method for manufacturing the piezoelectric film laminate 10 of this embodiment will be described with reference to Figures 3A to 3D and 4 to 7. In the figures, A1 indicates the film formation direction.

[0029] First, as shown in FIG. 3A, a Si substrate 11 is prepared, and a first intermediate layer 12 is formed on one surface 11a of the Si substrate 11. The Si substrate 11 may have a TEOS film formed on one surface 11a. For example, when the first intermediate layer 12 is a SiN film, the first intermediate layer 12 can be formed by a plasma CVD method or the like. In addition, a planarization process is performed on the one surface 12a side of the first intermediate layer 12 as necessary to reduce the maximum height Rz1 of the one surface 12a. For example, the one surface 12a of the first intermediate layer 12 can be planarized by etching using Ar plasma.

[0030] Next, as shown in FIG. 3B, the lower ScAlN film 13 is formed on the surface 12a of the first intermediate layer 12. For example, the lower ScAlN film 13 can be formed on the surface 12a of the first intermediate layer 12 by reactive DC sputtering. At this time, since the lower ScAlN film 13 contains Sc, abnormal grains protrude, making the surface 13a of the lower ScAlN film 13 an uneven surface. Then, as shown in FIG. 4, the maximum height Rz2 of the surface 13a at this time is still equal to or greater than the film thickness T of the second intermediate layer 14 to be formed later. According to an experiment, it has been confirmed that there is a correlation between the thickness of the ScAlN film and the maximum height Rz, and that the maximum height Rz is about 14% of the thickness of the ScAlN film. Here, the thickness of the lower ScAlN film 13 is several hundred nm, for example, 500 nm, and when the thickness is 500 nm, the maximum height Rz2 is 70 nm. For this reason, the maximum height Rz2 is larger than the film thickness of the second intermediate layer 14, which is 10 to 20 nm, and is equal to or greater than the film thickness of the second intermediate layer 14. Even if the thickness of the lower ScAlN film 13 is set to 100 nm, the maximum height Rz2 is 14 nm, and would be larger than that if the film thickness of the second intermediate layer 14 were to be set to about 10 nm. It is desirable to make the film thickness of the second intermediate layer 14 as thin as possible because the capacitance value can be increased as the film thickness is thinner, but it is difficult to make the film thin if the maximum height Rz2 is large.

[0031] Specifically, when a surface AFM image is taken of one surface 13a of the lower ScAlN film 13, a countless number of abnormal grains 20 are present as shown in FIG. 5A. When the unevenness of the surface 13a is observed in a cross section along the VB-VB line shown in this surface AFM image, the height of the unevenness is high at the location where the abnormal grains 20 are present as shown in FIG. 5B. If the second intermediate layer 14 is formed on the surface 13a in this state, the tip of the abnormal grain 20 protrudes from the second intermediate layer 14, so the second intermediate layer 14 needs to be thickened. However, since the second intermediate layer 14 is made of an insulating material and has a capacitance value, an insulating material with a low capacitance value is present between the lower ScAlN film 13 and the upper ScAlN film 15. This reduces the effective piezoelectricity of ScAlN, so it is not preferable to make the second intermediate layer 14 too thick, and it is preferable for the thickness to be 20 nm or less.

[0032] The change in the piezoelectric constant d33 when an ScAlN film is formed on an amorphous film with different thicknesses was analyzed by forming ScAlN films with three different Sc concentrations of 24 atomic %, 30 atomic %, and 40 atomic %, and the results shown in FIG. 6 were obtained. As shown in this figure, the higher the Sc concentration, the larger the piezoelectric constant d33, but the thicker the amorphous film, the smaller the piezoelectric constant d33. From the results shown in FIG. 5B, since the maximum height Rz2 of the one surface 13a in this state is about 51.14 nm, it is considered that the second intermediate layer 14 should be made about 70 nm thick. However, when the amorphous film is 70 nm thick, as shown by the arrow in the figure, the piezoelectric constant d33 when the Sc concentration is 40 atomic % is about 18 pC / N, and when the thickness is 20 nm, it is the same value as the piezoelectric constant d33 when the Sc concentration is 30 atomic %. In this way, the effect of increasing the Sc concentration is weakened, so it is not preferable to form a thick amorphous film.

[0033] On the other hand, it is also possible to form the second intermediate layer 14 made of an amorphous film while leaving the unevenness of the surface 13a, flatten the surface of the second intermediate layer 14, and thin the second intermediate layer 14 to suppress the decrease in piezoelectricity. However, in this case, as shown in FIG. 7, the film thickness of the second intermediate layer 14 may vary, and the second intermediate layer 14 may partially disappear, exposing the abnormal grains 20. The variation in the film thickness of the second intermediate layer 14 causes the piezoelectricity to vary, and the partial disappearance also causes the piezoelectricity to decrease. Furthermore, when the upper ScAlN film 15 is formed on the exposed abnormal grains 20, the abnormal grains 20 are inherited in the upper ScAlN film 15. Therefore, even when the thickly formed second intermediate layer 14 is flattened and thinned, the decrease in piezoelectricity is unavoidable.

[0034] For this reason, in this embodiment, as shown in FIG. 3C, a planarization process is performed on the one surface 13a of the lower ScAlN film 13 to make the one surface 13a a flat surface. Examples of the planarization process include milling, CMP (chemical mechanical polishing), etch-back, and wet etching. Milling can minimize the maximum height Rz3. In the case of etch-back, the etching rate may be set to be higher for the protruding portion than for the recessed portion. In the case of wet etching, the one surface 13a is planarized by isotropic etching. This planarization process reduces the maximum height Rz3 of the one surface 13a to less than 14% of the film thickness of the lower ScAlN film 13, which is smaller than the film thickness T of the second intermediate layer 14 to be formed later. According to an experiment, the maximum height Rz2 can be reduced to less than 10 nm, for example, 8 nm or less.

[0035] 3D, the second intermediate layer 14 is formed to a thickness of, for example, 10 to 20 nm, and then the upper ScAlN film 15 is formed on the first surface 14a. The second intermediate layer 14 can be formed by the same method as the first intermediate layer 12. The upper ScAlN film 15 can be formed by the same method as the lower ScAlN film 13. By forming the upper ScAlN film 15 in this manner, the piezoelectric film laminate 10 of this embodiment is completed.

[0036] As described above, in the piezoelectric film laminate 10 according to this embodiment, one surface 13a of the lower ScAlN film 13 is flattened, so that the maximum height Rz2 is made smaller than the film thickness T of the second intermediate layer 14. This makes it possible to ensure the piezoelectric constant d33 and suppress the decrease and variation in piezoelectricity caused by the abnormal grains 20.

[0037] In the piezoelectric film laminate 10 of this embodiment, the first intermediate layer 12 and the second intermediate layer 14 are made of amorphous films, which can improve the crystallinity of the lower ScAlN film 13 and the upper ScAlN film 15 formed thereon. In particular, it is preferable to use an HfOx film as the amorphous film, since this film has high amorphousness and can increase the capacitance value.

[0038] Second embodiment The first embodiment will be described. In this embodiment, electrode materials are disposed on both sides of the ScAlN film, and the rest is the same as in the first embodiment, so only the differences from the first embodiment will be described.

[0039] As shown in Fig. 8, in the piezoelectric film laminate 10 according to this embodiment, a first electrode film 31 is formed on a substrate 11, and a lower ScAlN film 13 is formed on one surface 31a thereof via a first intermediate layer 12. A second electrode film 32 is formed on one surface 13a of the lower ScAlN film 13, and an upper ScAlN film 15 is formed on one surface 32a thereof via a second intermediate layer 14. A third electrode film 33 is formed on one surface 15a of the upper ScAlN film 15. That is, the lower ScAlN film 13 is sandwiched between the first electrode film 31 and the second electrode film 32, and the upper ScAlN film 15 is sandwiched between the second electrode film 32 and the third electrode film 33.

[0040] The first electrode film 31, the second electrode film 32, and the third electrode film 33 are each made of one or more layers of electrode materials such as platinum (Pt), Mo, titanium (Ti), tungsten (W), and ruthenium (Ru). The first electrode film 31, the second electrode film 32, and the third electrode film 33 may all be made of the same electrode material, or may be made of different electrode materials.

[0041] Thus, even in a structure in which electrode materials are disposed on both sides of the ScAlN film, the surface 13a of the lower ScAlN film 13 is planarized before the process. The shape of the surface 32a of the second electrode film 32 formed on the lower ScAlN film 13 is inherited from the shape of the surface 13a of the lower ScAlN film 13 that serves as the base. If the unevenness of the surface 32a of the second electrode film 32 can be suppressed, the second intermediate layer 14 can be made thin, and the decrease and variation in piezoelectricity can be suppressed while maintaining the piezoelectric constant d33. Therefore, by planarizing the surface 13a of the lower ScAlN film 13, the same effect as in the first embodiment can be obtained.

[0042] The piezoelectric film laminate 10 thus configured is applied to, for example, a microphone. When used in a microphone, an opening is formed in the Si substrate 11 to form a membrane having a laminated structure of the first electrode film 31, the first intermediate layer 12, the lower ScAlN film 13, the second electrode film 32, the second intermediate layer 14, the upper ScAlN film 15, and the third electrode film 33. When pressure is applied to the membrane, polarization proportional to the pressure applied to the lower ScAlN film 13 and the upper ScAlN film 15 occurs based on the displacement. Conversely, when a voltage is applied to the lower ScAlN film 13 and the upper ScAlN film 15, the membrane is displaced based on the applied voltage, so that the membrane can be ultrasonically vibrated. As a result, the microphone is ultrasonically vibrated to output ultrasonic waves, and when ultrasonic waves are input, they can be detected.

[0043] The piezoelectric film laminate 10 thus configured can also be applied to, for example, a piezoelectric sensor. For example, the lower layer ScAlN film 13 and the upper layer ScAlN film 15, which are arranged with the second intermediate layer 14 sandwiched therebetween, are configured to form a parallel circuit as a pair of piezoelectric films. That is, the voltage change based on the displacement of the lower layer ScAlN film 13 is taken out from the first electrode film 31 and the second electrode film 32, and the voltage change based on the displacement of the upper layer ScAlN film 15 is taken out from the second electrode film 32 and the third electrode film 33. Then, a sensor output can be obtained by differentially amplifying these potentials. In this way, a parallel circuit is formed as a pair of piezoelectric films, thereby making it possible to obtain a piezoelectric sensor with high sensor sensitivity.

[0044] Next, a method for manufacturing the piezoelectric film laminate 10 of this embodiment will be described with reference to Figures 9A to 9C. In the figures, A1 indicates the film formation direction.

[0045] First, as shown in Fig. 9A, a Si substrate 11 is prepared, and a first electrode film 31 is formed thereon. For example, the first electrode film 31 is formed by reactive DC sputtering. Thereafter, the first intermediate layer 12 and the lower ScAlN film 13 are formed in the same manner as in Figs. 3A to 3C in the first embodiment, and then one surface 13a of the lower ScAlN film 13 is planarized.

[0046] Thereafter, as shown in FIG. 9B, the second electrode film 32 is formed on the surface 13a. For example, the second electrode film 32 is formed by reactive DC sputtering. At this time, since the surface 13a is planarized, the second electrode film 32 also inherits the shape of the surface 13a, and the unevenness of the surface 32a of the second electrode film 32 is suppressed. In other words, the maximum height Rz5 of the surface 32a of the second electrode film 32 shown in FIG. 10 is equal to the maximum height Rz2 of the surface 13a and is smaller than the film thickness T of the second intermediate layer 14.

[0047] Thereafter, as shown in FIG. 9C, the second intermediate layer 14 and the upper ScAlN film 15 are formed in the same manner as in FIG. 3D of the first embodiment. If necessary, a planarization process is performed on one surface 15a of the upper ScAlN film 15. The planarization process may be performed in the same manner as the planarization process on the one surface 13a of the lower ScAlN film 13. Then, a third electrode film 33 is formed on the one surface 15a of the upper ScAlN film 15. Although it is not necessary to perform a planarization process on the one surface 33a of the third electrode film 33, a planarization process may be performed. In this manner, the piezoelectric film laminate 10 of this embodiment is completed.

[0048] (Modification of the second embodiment) In the second embodiment, the first intermediate layer 12 and the second intermediate layer 14 are formed as a base while the first electrode film 31 and the second electrode film 32 are formed in order to improve the crystallinity of the lower ScAlN film 13 and the upper ScAlN film 15. Instead of this, if the first intermediate layer 12 and the second intermediate layer 14 are made of a conductive amorphous film, the first intermediate layer 12 and the second intermediate layer 14 can also fulfill the role of the first electrode film 31 and the second electrode film 32 while ensuring the crystallinity of the lower ScAlN film 13 and the upper ScAlN film 15. This simplifies the piezoelectric film laminate 10 and the manufacturing process, and reduces manufacturing costs, compared to the case where each layer is formed separately.

[0049] Metallic glasses can be used as such conductive amorphous films, such as an alloy composed of Zr-55%, Cu-30%, Al-10%, and Ni-5%, or an alloy composed of Pd-55%, Ni-30%, and P-10%.

[0050] (Other embodiments) Although the present disclosure has been described based on the above-described embodiment, it is not limited to the embodiment, and includes various modifications and modifications within the equivalent range. In addition, various combinations and forms, and other combinations and forms including only one element, more than one element, or less than one element, are also within the scope and concept of the present disclosure.

[0051] For example, the methods of forming the films and the method of planarizing the surface 13a of the lower ScAlN film 13 described in the above embodiments are merely examples, and other methods may be used. Furthermore, the constituent materials and thicknesses of the first intermediate layer 12 and the second intermediate layer 14 are also merely examples.

[0052] In addition, in each of the above embodiments, the piezoelectric film laminate 10 is constructed by forming each film on the Si substrate 11, but the base material for constructing the piezoelectric film laminate 10 does not necessarily have to be a substrate.

[0053] Furthermore, in each of the above embodiments, a structure including a lower ScAlN film 13 and an upper ScAlN film 15, that is, a structure including two layers of ScAlN films, has been given as an example. However, it is sufficient to include at least a lower ScAlN film 13 and an upper ScAlN film 15, and a structure including three or more layers of ScAlN films may also be used. Even in this case, in a structure in which an intermediate layer is disposed on a lower ScAlN film and an upper ScAlN film is disposed, the effects of each of the above embodiments can be obtained by planarizing one surface of the lower ScAlN film.

[0054] Furthermore, in each of the above embodiments, when a Si substrate 11 is used as the base material, a lower layer ScAlN film 13 is formed on the Si substrate 11 via a first intermediate layer 12, but depending on the material of the base material, the first intermediate layer 12 may be omitted and the lower layer ScAlN film 13 may be formed directly on one surface of the base material.

[0055] (In view of the present disclosure) The present disclosure described above can be understood from the following viewpoints, for example.

[0056] [First viewpoint] A piezoelectric film laminate, A substrate (11), a lower layer ScAlN film (13) formed on one surface (11a) of the substrate; an intermediate layer (14) formed on one surface (13a) of the lower ScAlN film opposite to the substrate; an upper layer ScAlN film (15) formed on one surface (14a) of the intermediate layer opposite to the lower layer ScAlN film, A piezoelectric film laminate, wherein the maximum height (Rz2) of the lower ScAlN film on the one surface is smaller than the thickness of the intermediate layer and is less than 14% of the thickness of the lower ScAlN film. [Second viewpoint] The piezoelectric film laminate according to the first aspect, wherein the intermediate layer is an amorphous film. [Third Perspective] The piezoelectric film laminate according to a second aspect, wherein the amorphous film is composed of one or more of a SiN film, a TEOS film, a silicon oxide film, a HfOx film, a Mo oxide film, and an Al2O3 film. [Fourth viewpoint] The piezoelectric film laminate according to a second aspect, wherein the amorphous film is conductive. [Fifth viewpoint] a first electrode film (31) formed between the substrate and the lower ScAlN film; a second electrode film (32) formed between the lower ScAlN film and the upper ScAlN film; The piezoelectric film laminate according to any one of the first to third aspects, further comprising a third electrode film (33) formed on a surface (15a) of the upper ScAlN film opposite the intermediate layer. [Sixth viewpoint] 6. The piezoelectric film laminate according to claim 5, wherein the first electrode film, the second electrode film, and the third electrode film are each composed of one or more layers of Pt, Mo, Ti, W, or Ru. [Seventh viewpoint] The piezoelectric film laminate according to any one of the first to sixth aspects, wherein the concentration of Sc contained in the lower ScAlN film is 24 atomic % to 43 atomic %. [Eighth viewpoint] A method for manufacturing a piezoelectric film laminate, comprising the steps of: Providing a substrate (11); forming a lower layer ScAlN film (13) on one surface (11a) of the substrate; planarizing a surface (13a) of the lower ScAlN film opposite to the substrate; forming an intermediate layer (14) on the one surface of the lower ScAlN film; forming an upper layer ScAlN film (15) on a surface (14a) of the intermediate layer opposite to the lower layer ScAlN film; A method for manufacturing a piezoelectric film laminate, wherein the intermediate layer is formed so that the film thickness of the intermediate layer is smaller than the maximum height (Rz2) of one surface of the lower layer ScAlN film before the planarization and larger than the maximum height of the one surface of the lower layer ScAlN film after the planarization. [Ninth viewpoint] The method for producing a piezoelectric film laminate according to an eighth aspect, wherein the planarization is performed by any one of milling, CMP, etch-back, and wet etching. [Explanation of symbols]

[0057] 10 Piezoelectric film laminate 11. Silicon substrate 12 First Middle Class 13 Lower layer ScAlN film 14 The second middle class 15 Upper ScAlN film 31~33 1st~3rd electrode film

Claims

1. A piezoelectric film laminate, A substrate (11), a lower layer ScAlN film (13) formed on one surface (11a) of the substrate; an intermediate layer (14) formed on one surface (13a) of the lower ScAlN film opposite to the substrate; an upper layer ScAlN film (15) formed on one surface (14a) of the intermediate layer opposite to the lower layer ScAlN film; A piezoelectric film laminate, wherein a maximum height (Rz2) of the lower ScAlN film on the one surface is smaller than a thickness of the intermediate layer and is less than 14% of a thickness of the lower ScAlN film.

2. The piezoelectric film laminate according to claim 1 , wherein the intermediate layer is an amorphous film.

3. The amorphous film may be a SiN film, a TEOS film, a silicon oxide film, a HfOx film, a Mo oxide film, or an Al 2 O 3 The piezoelectric film stack of claim 2 , which is comprised of any one or more of the films.

4. The piezoelectric film laminate according to claim 2 , wherein the amorphous film is electrically conductive.

5. a first electrode film (31) formed between the substrate and the lower ScAlN film; a second electrode film (32) formed between the lower ScAlN film and the upper ScAlN film; 2. The piezoelectric film laminate according to claim 1, further comprising: a third electrode film (33) formed on a surface (15a) of said upper ScAlN film opposite to said intermediate layer.

6. 6. The piezoelectric film laminate according to claim 5, wherein the first electrode film, the second electrode film, and the third electrode film are each composed of one or more layers of Pt, Mo, Ti, W, or Ru.

7. 7. The piezoelectric film laminate according to claim 1, wherein the concentration of Sc contained in said lower ScAlN film is 24 atomic % to 43 atomic %.

8. A method for manufacturing a piezoelectric film laminate, comprising the steps of: Providing a substrate (11); forming a lower layer ScAlN film (13) on one surface (11a) of the substrate; planarizing a surface (13a) of the lower ScAlN film opposite to the substrate; forming an intermediate layer (14) on the one surface of the lower ScAlN film; forming an upper layer ScAlN film (15) on a surface (14a) of the intermediate layer opposite to the lower layer ScAlN film; A method for manufacturing a piezoelectric film laminate, in which the intermediate layer is formed so that the film thickness of the intermediate layer is smaller than the maximum height (Rz2) of one surface of the lower ScAlN film before the planarization and larger than the maximum height of the one surface of the lower ScAlN film after the planarization.

9. The method for producing a piezoelectric film laminate according to claim 8 , wherein the planarization is performed by any one of milling, CMP, etch-back, and wet etching.

Citation Information

Patent Citations

  • Piezoelectric thin film, piezoelectric material, fabrication method of piezoelectric thin film and piezoelectric material, and piezoelectric resonator, actuator element and physical sensor using piezoelectric thin film

    JP2009010926A

  • Piezoelectric film laminate and method for manufacturing the same

    JP2023042851A

  • Packages with Organic Back Ends for Electronic Components

    US20210028766A1

  • Semiconductor structure and method for manufacturing thereof