Method for producing roadbed material and apparatus for producing roadbed material, and method for recovering carbon dioxide

The method addresses the limitations of existing carbon dioxide fixation technologies by using fresh concrete sludge water to produce roadbed materials with high calcium carbonate content, enhancing versatility and efficiency in carbon dioxide recovery and utilization.

JP2024158503APending Publication Date: 2024-11-08SUMITOMO OSAKA CEMENT CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023073748
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing methods for carbon dioxide fixation lack versatility and require complex operations, such as adjusting humidity or using large-scale equipment, limiting their applicability and efficiency.

Method used

A method involving the use of fresh concrete sludge water to contact base materials like crushed stone and recycled aggregates, with carbon dioxide-containing gas, to produce roadbed materials while capturing and fixing carbon dioxide, utilizing a contact device, reaction vessel, flue, and dust collector.

Benefits of technology

This method enables the production of roadbed materials with high calcium carbonate content, efficiently recovering carbon dioxide and reducing waste, with the recovered calcium carbonate being suitable for construction applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158503000005
    Figure 2024158503000005
  • Figure 2024158503000001
    Figure 2024158503000001
  • Figure 2024158503000002
    Figure 2024158503000002
Patent Text Reader

Abstract

To provide a method and an apparatus for producing a roadbed material by a simple operation, which is highly versatile in that it can be applied to a wide variety of materials, and a method for recovering carbon dioxide.SOLUTION: A method for producing a roadbed material comprises a first contacting step in which ready-mixed concrete sludge water 1 and a base material are contacted, a second contacting step in which the contained component and carbon dioxide-containing gas are contacted, a third contacting step in which the carbon dioxide-containing gas and ready-mixed concrete sludge water 2 are contacted, and a recovering step in which a reactant containing calcium carbonate is collected by a dust collector. An apparatus for producing the roadbed material comprises a contacting device with which the first contacting step is performed, a reaction vessel with which the second contacting step is performed, a gas duct and a spray nozzle with which the third contacting step is performed, and the dust collector, and a method for recovering carbon dioxide comprises the first contacting step, the second contacting step, the third contacting step, and the recovering step.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for producing a roadbed material, and a method for recovering carbon dioxide. [Background technology]

[0002] In recent years, interest in global warming has increased, and there is a demand for reducing the amount of carbon dioxide emitted into the atmosphere. At various facilities such as power plants, incinerators, cement plants, steelworks, and factory facilities, the amount of exhaust gas containing carbon dioxide emitted into the atmosphere during operation has been reduced and recovered. In particular, reducing the amount of carbon dioxide emitted from cement plants is considered to be an urgent issue.

[0003] For example, Patent Document 1 proposes a method for fixing carbon dioxide, which is characterized by accumulating materials obtained by crushing waste concrete, exposing the materials to conditions in which dry and wet conditions are alternated for a predetermined period of time, and taking in and fixing carbon dioxide in the air into the materials. Patent Document 2 also proposes a method for fixing carbon dioxide, which includes a contacting step in which a carbon dioxide-containing gas is brought into contact with a powdery or granular material having a predetermined particle size, which is made of a cementitious hardened body, at a temperature of 75 to 110°C, and the relative humidity of the gas is adjusted according to the adjustment of the moisture content of the powdery or granular material. [Prior art documents] [Patent documents]

[0004] Patent Document 1: JP 2009-028581 A Patent Document 2: JP 2020-131076 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to provide a manufacturing method and manufacturing apparatus that are highly versatile and can be applied to a wide variety of materials, and that can manufacture roadbed materials through simple operations, as well as a method for recovering carbon dioxide. [Means for solving the problem]

[0006] In order to solve the above problems, the present invention provides the following method for producing a roadbed material. 1. A first contact step of obtaining a content containing the fresh concrete sludge water 1 and the base material by contacting the fresh concrete sludge water 1 with the base material; A second contact step of obtaining a roadbed material containing the base material and calcium carbonate by contacting the content with a carbon dioxide-containing gas; A third contact step in which the carbon dioxide-containing gas is contacted with the fresh concrete sludge water 2 to obtain a reaction product containing calcium carbonate; and a recovery step of recovering the reaction product containing calcium carbonate with a dust collector; Equipped with A manufacturing method for roadbed materials.

[0007] Furthermore, the present invention provides the following method for producing a roadbed material as a preferred embodiment. 2. The method for producing a roadbed material according to the above item 1, wherein the base material is at least one material selected from the group consisting of crushed stone, crushed sand, recycled aggregate derived from waste asphalt, and recycled crushed stone derived from waste concrete. 3. A method for producing a roadbed material as described in 1 or 2 above, wherein the contact between the ready-mixed concrete sludge water 1 and the substrate is carried out by spraying the ready-mixed concrete sludge water 1. 4. The method for producing a roadbed material according to the above item 3, wherein the amount of the fresh concrete sludge water 1 sprayed per 100 parts by mass of the base material is 0.1 parts by mass or more and 15 parts by mass or less. 5. The method for producing a roadbed material according to the above item 1 or 2, wherein the contact between the content and the carbon dioxide-containing gas is carried out in a reaction vessel. 6. A method for producing a roadbed material as described in 5 above, in which the contact between the carbon dioxide-containing gas and the fresh concrete sludge water 2 is carried out by spraying the fresh concrete sludge water 2 into a flue through which the carbon dioxide-containing gas discharged from the reaction vessel passes. 7. A method for producing a roadbed material as described in 1 or 2 above, wherein the ready-mixed concrete sludge water 1 and the ready-mixed concrete sludge water 2 are supplied from a single ready-mixed concrete sludge water supply facility. 8. A method for producing a roadbed material as described in 1 or 2 above, wherein the fresh concrete sludge water 1 and the fresh concrete sludge water 2 are supernatant water obtained by removing solids from fresh concrete sludge, or sludge water containing the solids. 9. The method for producing a roadbed material according to the above 8, wherein the fresh concrete sludge water 1 and the fresh concrete sludge water 2 are the supernatant water. 10. A method for producing a roadbed material as described in 1 or 2 above, wherein the temperature of the carbon dioxide-containing gas in the second contact step is 10°C or higher and 90°C or lower. 11. 1 m of the carbon dioxide-containing gas in the third contact step 3 3. The method for producing a roadbed material according to the above 1 or 2, wherein the supply amount of the fresh concrete sludge water 2 per hour is 0.5 kg / h or more and 600 kg / h or less. 12. A method for producing a roadbed material as described in 1 or 2 above, wherein the roadbed material is a base material having a surface coated with the calcium carbonate.

[0008] The present invention provides the following roadbed material manufacturing apparatus. 13. A contact device for contacting the fresh concrete sludge water 1 with a substrate to obtain a content containing the fresh concrete sludge water 1 and the substrate; A reaction vessel for obtaining a roadbed material containing the base material and calcium carbonate by contacting the content with a carbon dioxide-containing gas; a flue through which the carbon dioxide-containing gas discharged from the reaction vessel passes; A spray nozzle for supplying fresh concrete sludge water 2 to the flue; and a dust collector for recovering a reaction product containing calcium carbonate obtained by contacting the carbon dioxide-containing gas in the flue with the fresh concrete sludge water 2; A roadbed material manufacturing device comprising:

[0009] The present invention also provides the following method for recovering carbon dioxide. 14. A first contact step of obtaining a content containing the fresh concrete sludge water 1 and the base material by contacting the fresh concrete sludge water 1 with the base material; a second contact step of contacting the mixture with a carbon dioxide-containing gas to react carbon dioxide contained in the carbon dioxide-containing gas to obtain a reaction product containing calcium carbonate; A third contact step in which the carbon dioxide contained in the carbon dioxide-containing gas is reacted with the carbon dioxide-containing gas to obtain a reaction product containing calcium carbonate by contacting the carbon dioxide-containing gas with the fresh concrete sludge water 2; and a recovery step of recovering the reaction product containing calcium carbonate obtained in the third contact step with a dust collector; A method for capturing carbon dioxide, comprising: Effect of the Invention

[0010] According to the present invention, it is possible to provide a manufacturing method and manufacturing apparatus that are highly versatile and can be applied to a wide variety of materials, and that can manufacture roadbed materials through simple operations, as well as a method for recovering carbon dioxide. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a flow diagram showing a preferred example of a roadbed material manufacturing apparatus according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention (hereinafter, sometimes referred to as "the present embodiment") will be described. The present invention is not limited to the following embodiment, and can be implemented with any modification within the scope that does not impair the effects of the invention. In this specification, the expression "AA to BB" for a numerical range means "AA or more and BB or less". In this specification, the numerical values ​​related to "above", "below" and "to" in the description of a numerical range are numerical values ​​that can be arbitrarily combined. For example, when a certain numerical range is described as "CC to DD" and "EE to FF", the numerical ranges "CC to FF" and "EE to DD" are also included.

[0013] [Method of manufacturing roadbed materials] The method for manufacturing a roadbed material of this embodiment is as follows: A first contact step of obtaining a content containing the fresh concrete sludge water 1 and the base material by contacting the fresh concrete sludge water 1 with the base material; A second contact step of obtaining a roadbed material containing the base material and calcium carbonate by contacting the content with a carbon dioxide-containing gas; A third contact step in which the carbon dioxide-containing gas is contacted with the fresh concrete sludge water 2 to obtain a reaction product containing calcium carbonate; and a recovery step of recovering the reaction product containing calcium carbonate with a dust collector; Equipped with That is it.

[0014] As mentioned above, there is a demand for reducing the amount of carbon dioxide emitted into the atmosphere, and reducing carbon dioxide emissions is an urgent issue, so it is extremely important that materials have high versatility so that they can be used with a wide variety of materials. There is also a demand for materials that can be solved with minor measures, such as simple modifications to existing facilities or the installation of small facilities, and that can be handled with easy work.

[0015] However, the technology described in Patent Document 1 requires the collection site to be moistened by showering with water, which requires large-scale treatment equipment and complicated work. The technology described in Patent Document 2 requires the complicated work of adjusting the relative humidity of the carbon dioxide-containing gas. Furthermore, both of the technologies described in Patent Documents 1 and 2 are only intended to use materials derived from concrete, and are therefore lacking in versatility.

[0016] The present inventors have been studying methods for capturing carbon dioxide, and have found that, depending on the material used in the method for capturing carbon dioxide, it can be a suitable material for roadbed material. In other words, by using a material used as a base material for roadbed material as the material to be used, and by simply contacting the base material with fresh concrete sludge water and with a carbon dioxide-containing gas, it has been found that not only can carbon dioxide be captured, but the base material used for capturing carbon dioxide can also be effectively used as a roadbed material. As described above, according to the method for manufacturing roadbed material of the present embodiment, roadbed material can be manufactured with minor adjustments and easy work, and carbon dioxide can be captured at the same time.

[0017] According to the method for manufacturing roadbed material of this embodiment, by contacting the carbon dioxide-containing gas with fresh concrete sludge water, it is possible to further recover carbon dioxide from the carbon dioxide-containing gas and reduce the amount of fresh concrete sludge that is normally discarded as waste.

[0018] Hereinafter, the method for manufacturing a roadbed material according to this embodiment will be described with reference to FIG. Fig. 1 is a flow diagram showing a preferred embodiment of the roadbed material manufacturing apparatus of this embodiment. The flow diagram shown in Fig. 1 shows that the roadbed material manufacturing apparatus is equipped with a contact device (first contact tank) that obtains a content containing fresh concrete sludge water 1 and a base material by a first contact step of contacting the fresh concrete sludge water 1 with a base material, and a reaction vessel (second contact tank) that obtains a roadbed material containing a base material and calcium carbonate by a second contact step of contacting the content obtained in the first contact step with a carbon dioxide-containing gas. In addition, the roadbed material manufacturing apparatus of this embodiment is also shown to be equipped with a flue through which the carbon dioxide-containing gas discharged from the reaction vessel passes, a spray nozzle that supplies fresh concrete sludge water 2 to the flue, and a dust collector that collects a reaction product containing calcium carbonate obtained by contacting the carbon dioxide-containing gas with the fresh concrete sludge water 2 in the flue.

[0019] In Fig. 1, a first contact step between the fresh concrete sludge water 1 and the substrate is performed in a contact device (first contact tank), the contents obtained in the first contact step are supplied to a reaction vessel (second contact tank), a second contact step between the contents and a carbon dioxide-containing gas is performed, and a roadbed material containing a substrate and calcium carbonate is obtained, and the fresh concrete sludge water 2 is supplied to the carbon dioxide-containing gas used in the second contact step, and a third contact step between the carbon dioxide-containing gas and the fresh concrete sludge water 2 is performed, and a reaction product containing calcium carbonate is obtained. Here, the carbon dioxide-containing gas is discharged from the reaction vessel and passes through a flue, and the fresh concrete sludge water 2 is supplied through a spray nozzle in the flue to perform the third contact step, and the calcium carbonate reaction product obtained by contact between the carbon dioxide-containing gas and the fresh concrete sludge water 2 in the flue is collected by a dust collector. FIG. 1 also shows that after the base material is crushed in the crushing facility, the crushed base material is moved to a base material yard by a transfer belt conveyor, and that the base material is transported from the base material yard using a transport vehicle such as a dump truck, and is supplied to a contact device (first contact tank) by the transport belt conveyor.

[0020] [First contact step] The method for producing a roadbed material of the present embodiment includes a first contact step of obtaining an inclusion containing the fresh concrete sludge water 1 and the base material by contacting the fresh concrete sludge water 1 with the base material. The contents obtained in the first contact step contain the fresh concrete sludge water 1 and the base material, and considering that they are obtained by contact between the fresh concrete sludge water 1 and the base material, the fresh concrete sludge water 1 is in a form in which the fresh concrete sludge water 1 is coated (adhered) to at least a portion of the surface of the base material.

[0021] (base material) The substrate used in the manufacturing method of this embodiment can be used without any particular limitation as long as it is a material that can be used as a roadbed material. For example, materials generally called crushed stone, crushed sand, recycled aggregate derived from asphalt waste, and recycled crushed stone derived from concrete waste are preferably exemplified. For example, as shown in FIG. 1, the substrate may be crushed in a crushing facility as necessary before use, and the crushing facility can crush the substrate into a size according to the desired roadbed material.

[0022] As for the crushed stone, any of the single-grained crushed stone (No. 1 to No. 7), crusher run (C-20 to C-40), and grain-adjusted crushed stone (M-25 to M-40) specified in JIS A5001:2008 can be used. Standard products include crushed stone for concrete specified in JIS A5005:2020. In addition, non-standard crushed stone that is equivalent to these crushed stones can also be used as crushed stone. The crushed sand can be the crushed sand for concrete specified in JIS A5005: 2020. It is also possible to use non-standard crushed sand that is equivalent to crushed sand as crushed sand.

[0023] As the recycled aggregate, any of recycled aggregates for concrete H, M, and L specified in JIS A5021:2018, JIS A5022:2018, and JIS A5023:2018 can be used. In addition, non-standard materials that are equivalent to these recycled aggregates can also be used as recycled aggregate.

[0024] Examples of the recycled crushed stone include the above-mentioned crushed stone, recycled crushed stone (for example, RC-40, etc.) using recycled material of grain-adjusted crushed stone, and recycled grain-adjusted crushed stone (for example, RM-30, etc.).

[0025] (reducing agent) The substrate used in the manufacturing method of this embodiment may dissolve hexavalent chromium when it comes into contact with water. In this case, it is preferable to use a chemical (mainly a reducing agent) to reduce the amount of hexavalent chromium dissolved. This is because hexavalent chromium can be detoxified by reducing it to trivalent chromium, and the safety of the substrate as a roadbed material can be improved. Therefore, when the amount of hexavalent chromium dissolved from the substrate does not meet, for example, the soil environmental standards, it is effective to use a reducing agent.

[0026] The reducing agent can be used without any particular limitation as long as it can reduce hexavalent chromium to trivalent chromium and detoxify it. For example, iron compounds such as iron hydroxide, iron chloride, iron fluoride, iron bromide, iron sulfate, iron nitrate, iron phosphate, iron thiocyanate, iron citrate, iron fumarate, and iron gluconate are preferably mentioned, and among them, divalent iron compounds (ferrous compounds) of these are preferable.

[0027] The amount of the reducing agent used is, for example, preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, and the upper limit is preferably 30 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of the base material. Within the above range, hexavalent chromium can be reduced and detoxified more efficiently.

[0028] (Fresh concrete sludge water 1) Ready-mixed concrete plants generate ready-mixed concrete sludge that contains cement, such as leftover concrete that is produced in excess of the order amount and not shipped, returned concrete that is not used by the supplier and returned, and dissolved products of these, washing wastewater generated by washing equipment such as mixer trucks, etc. In the method for manufacturing roadbed material of this embodiment, the ready-mixed concrete sludge generated in the ready-mixed concrete plant in this way can be used as ready-mixed concrete sludge water 1.

[0029] Ready-mixed concrete sludge 1 typically contains water, calcium components such as calcium hydroxide that dissolves in water, and sludge solids (mainly hydration products, aggregate fine particles, etc. (mainly metals such as silica, aluminum, iron, etc. and contents of these metals, as well as calcium carbonate)). The solids are sometimes removed from the ready-mixed concrete sludge, and the resulting mixture is separated into supernatant water containing calcium hydroxide, etc., and sludge water containing sludge solids (mainly hydration products, aggregate fine particles, etc.). In this case, either the supernatant water or the sludge water can be used as the ready-mixed concrete sludge water 1, and when a spray nozzle is used, the supernatant water is preferred from the viewpoint of preventing clogging of the spray nozzle.

[0030] Regardless of whether the fresh concrete sludge water used in the system of this embodiment is the above-mentioned supernatant water or sludge water, the solids concentration in the fresh concrete sludge water is preferably 40 mass% or less, more preferably 20 mass% or less, even more preferably 10 mass% or less, and even more preferably 5 mass% or less.

[0031] As described above, calcium hydroxide is dissolved in the ready-mixed concrete sludge water 1 as calcium content, but calcium hydroxide also exists as solid content due to its low solubility. Calcium content also includes calcium carbonate and the like, and exists mainly as solid content. Thus, the ready-mixed concrete sludge water 1 used in the manufacturing method of this embodiment includes calcium content such as calcium hydroxide and calcium carbonate as solid content, and sludge solid content (mainly including hydration products, aggregate fine particles, etc.) as described above. Then, among these solid content, calcium hydroxide contained as calcium content becomes calcium carbonate by contacting with carbon dioxide in the second contact step as described above. In this way, a roadbed material is obtained and carbon dioxide can be collected.

[0032] From the viewpoint of promoting the production of calcium carbonate, the solids concentration in the fresh concrete sludge water 1 is preferably 0.001 mass % or more, more preferably 0.0015 mass % or more, and even more preferably 0.002 mass % or more. From the same viewpoint, the particle size of the solids in the fresh concrete sludge water 1 is preferably 1000 μm or less, more preferably 100 μm or less, even more preferably 10 μm or less, still more preferably 1 μm or less, and particularly preferably 0.1 μm or less.

[0033] In the case where the fresh concrete sludge water 1 used in the manufacturing method of this embodiment is the above-mentioned supernatant water, the calcium concentration contained in the fresh concrete sludge water 1 is usually 100 mg / L or more, preferably 250 mg / L or more, more preferably 500 mg / L or more, and further preferably 800 mg / L or more. The higher the upper limit, the better, and there is no particular restriction, but it is usually 1500 mg / L or less. In addition, when the ready-mixed concrete sludge water 1 is the above-mentioned sludge water, the concentration of calcium contained in the ready-mixed concrete sludge water is usually 1000 mg / L or more, preferably 10000 mg / L or more, more preferably 100000 mg / L or more, and further preferably 300000 mg / L or more. The higher the upper limit, the better, and there is no particular restriction, but it is usually 3000000 mg / L or less.

[0034] Furthermore, the ready-mixed concrete sludge water 1 may be a mixture obtained by mixing the above solids obtained from the ready-mixed concrete sludge 1 with water, from which the solids have been removed. The above solids include calcium components such as calcium hydroxide, and the hydration products mainly contained in the solids include calcium components such as calcium hydroxide and calcium silicate hydrate. Therefore, the mixture from which the solids have been removed still contains calcium components that have dissolved from the solids into the water, making it possible to convert more calcium from the ready-mixed concrete sludge 1 into calcium carbonate.

[0035] (Contact between fresh concrete sludge water 1 and substrate) There are no particular limitations on the method for contacting the ready-mixed concrete sludge water 1 with the substrate, so long as they come into contact with each other. Preferred examples of the method include a method in which the ready-mixed concrete sludge water 1 is sprayed onto the substrate to bring the water into contact with the substrate, and a method in which the substrate is poured into the ready-mixed concrete sludge water 1 to bring the water into contact with the substrate.

[0036] Also, when a method of spraying the above-mentioned fresh concrete sludge water 1 onto the substrate and bringing it into contact with the substrate is adopted, the concrete sludge water 1 will be coated (adhered) to at least a portion of the substrate surface, although this can vary depending on the spraying method, spray amount, etc. More specifically, the fresh concrete sludge water 1 may be coated (adhered) to a portion of the substrate surface, or the fresh concrete sludge water 1 may be coated (adhered) to the entire substrate surface.

[0037] When a method is adopted in which the substrate is brought into contact with the fresh concrete sludge water 1, the contents containing the fresh concrete sludge water 1 and the substrate, obtained by contacting the fresh concrete sludge water 1 with the substrate, will vary depending on the relationship between the depth of the fresh concrete sludge water 1 and the dimensions of the substrate, as well as the method of introduction, but will have the fresh concrete sludge water 1 coated (adhered) to at least a portion of the surface of the substrate, similar to the case of spraying as described above.

[0038] Therefore, in any contact method, the inclusions are in a form in which at least a part of the surface of the substrate is coated (adhered) with the concrete sludge water 1. The coating (adhesion) of the surface of the substrate with the concrete sludge water 1 may be a physical coating (adhesion) or a chemical coating (adhesion).

[0039] In the case of contacting by spraying, contact can be performed by preparing a minor tool required for spraying, such as a spray nozzle described later, and the location of spraying can be determined arbitrarily, which is effective in terms of work efficiency. For example, FIG. 1 shows contacting by spraying as a preferred embodiment of the manufacturing method of this embodiment. In the manufacturing method of this embodiment, spraying of the ready-mixed concrete sludge water 1 may be performed at one location, for example, in the contact device (first contact tank), or as shown in FIG. 1, in addition to the contact device (first contact tank), in a base material yard where the base material is stored, during transportation using a transport vehicle, etc., when moving to the contact device (first contact tank) using a belt conveyor, or in a reaction vessel (second contact tank).

[0040] Although this method is more difficult to coat (adhere) the entire surface of the substrate with the fresh concrete sludge water 1 than the method of putting the substrate into contact with the fresh concrete sludge water 1, it has the advantage of making it easier to bring the fresh concrete sludge water 1 into contact with the substrate without excess or deficiency. In addition, it is also advantageous in that the amount of water used can be easily adjusted by the amount sprayed, making it easier to make contact as desired. In addition, since the fine particles (droplets) gather and cover (adhere) the surface of the base material, the calcium content contained in the fine particles (droplets) can come into contact with carbon dioxide more efficiently. Therefore, it is possible to produce roadbed material as efficiently as in the case of the method of putting the base material into the ready-mixed concrete sludge water 1 and contacting it, and also to collect carbon dioxide.

[0041] In order to more reliably bring the ready-mixed concrete sludge water 1 into contact with the substrate, it is effective to put the substrate into the ready-mixed concrete sludge water 1. On the other hand, when the substrate is put into contact with the ready-mixed concrete sludge water 1, a tank is required to store the ready-mixed concrete sludge water and to put the substrate in, and heavy metals may be eluted from the substrate into the tank. In addition, since it is more difficult to adjust the degree of contact than with the above-mentioned spraying, it may be difficult to meet the desired properties of the roadbed material.

[0042] Taking these factors into consideration, in the manufacturing method of this embodiment, the contact method in the first contact step may be a method suitable for the circumstances; however, taking into consideration work efficiency, ease of adjustment, etc., a method in which the fresh concrete sludge water 1 is sprayed onto the substrate to bring it into contact therewith is more preferable.

[0043] When the ready-mixed concrete sludge water 1 is sprayed, the concentration of solids and particle size of the solids contained in the ready-mixed concrete sludge water 1, and the concentration of calcium contained in the ready-mixed concrete sludge water 1 when the ready-mixed concrete sludge water 1 is the above-mentioned supernatant water, should be within the above ranges. If they are within the above ranges, clogging of the tool used for spraying (for example, the spray nozzle described later) can be suppressed, and a roadbed material can be produced that is stable over a longer period of time. In addition, as described above, by making it easier to coat (adhere) the surface of the base material as fine particles (droplets), the calcium contained in the fine particles (droplets) can come into contact with carbon dioxide more efficiently, making it possible to produce roadbed material more efficiently and to collect carbon dioxide.

[0044] When the ready-mixed concrete sludge water 1 is sprayed, the amount of the ready-mixed concrete sludge water 1 sprayed per 100 parts by mass of the substrate is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1.0 parts by mass or more, with the upper limit being preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less. When the amount of the ready-mixed concrete sludge water 1 sprayed is within the above range, the ready-mixed concrete sludge water 1 can be more efficiently contacted with the substrate, so that the roadbed material can be more efficiently produced and carbon dioxide can be recovered.

[0045] Ready-mixed concrete sludge water 1 may be stored in a ready-mixed concrete sludge water tank, as shown in Fig. 1, and contact may be made by spraying via a spray nozzle as necessary. For example, as shown in Fig. 1, a ready-mixed concrete sludge water supply facility equipped with one ready-mixed concrete sludge water tank may be provided to supply the water to a plurality of spray nozzles, or one spray nozzle may be provided with one ready-mixed concrete sludge water supply facility depending on the location of the spray nozzles. Also, as shown in Fig. 1, ready-mixed concrete sludge water 1 and ready-mixed concrete sludge water 2, which will be described later, may be supplied from one ready-mixed concrete sludge water supply facility.

[0046] When spraying the ready-mixed concrete sludge water 1, the tool used for spraying can be any tool capable of spraying the ready-mixed concrete sludge water 1, and it is preferable to use a spray nozzle in consideration of ease of handling and availability. Other details of the spray nozzle will be described later.

[0047] [Second Contact Step] The method for producing a roadbed material of this embodiment includes a second contact step in which the inclusions obtained in the first contact step are contacted with a carbon dioxide-containing gas to obtain a roadbed material containing the base material and calcium carbonate.

[0048] The roadbed material containing a base material and calcium carbonate obtained by the second contact step is not particularly limited in its form as long as it contains a base material and calcium carbonate, but preferably has a form in which calcium carbonate is coated (attached) to at least a part of the surface of the base material. As described above, the inclusion obtained in the first contact step preferably has a form in which the fresh concrete sludge water 1 is attached (coated) to at least a part of the surface of the substrate. In the inclusion in which the fresh concrete sludge water 1 is coated (attached) to at least a part of the surface of the substrate, calcium carbonate is generated by the reaction between the calcium content contained in the fresh concrete sludge water 1 and the carbon dioxide contained in the carbon dioxide-containing gas, and a roadbed material is obtained in which at least a part of the surface of the substrate is coated (attached) with calcium carbonate. In addition, the fresh concrete sludge water contains, in addition to calcium carbonate that is already present by reacting with carbon dioxide in the air, metals such as silica, aluminum, and iron, and compounds of these metals that are difficult to react with the carbon dioxide-containing gas. Therefore, the roadbed material is one in which these components contained in the fresh concrete sludge water are also coated (attached) to the surface of the substrate.

[0049] In the manufacturing method of this embodiment, a roadbed material is thus obtained, and carbon dioxide is consumed in a reaction with the calcium content adhered to at least a portion of the surface of the base material and recovered as calcium carbonate.

[0050] In the second contact step, the contact between the inclusions and the carbon dioxide-containing gas is preferably carried out in a reaction vessel (second contact tank) as shown in Fig. 1. By carrying out the second contact step in this manner, the inclusions come into contact with carbon dioxide more efficiently, and therefore the roadbed material can be produced more efficiently. In Fig. 1, carbon dioxide is supplied from the lower part of the reaction vessel (second contact vessel), and although not shown, carbon dioxide may be exhausted from at least one of the upper part of the reaction vessel (second contact vessel) and the upper part of the contact device (first contact vessel). By supplying and exhausting carbon dioxide in this manner, the contact between the contents and carbon dioxide can be made more efficient.

[0051] (carbon dioxide-containing gas) The carbon dioxide-containing gas used in the manufacturing method of the present embodiment can be any gas containing carbon dioxide without any particular limitation. For example, as shown in Fig. 1, exhaust gas (also called "combustion exhaust gas") discharged from various factory facilities is a typical example.

[0052] The concentration of carbon dioxide contained in these carbon dioxide-containing gases is, for example, usually 8 to 15% by volume for combustion exhaust gas from a power plant, usually 1 to 30% by volume for combustion exhaust gas from a precast concrete (PCa) product factory, asphalt factory, or incinerator, usually 15 to 30% by volume for combustion exhaust gas from a cement factory, usually 20 to 30% by volume for exhaust gas from an ironworks, and usually 1 to 10% by volume for exhaust gas from a drying furnace for aggregates to be used in asphalt mixtures at asphalt mixture factories. In the manufacturing method of this embodiment, any combustion exhaust gas can be used as the carbon dioxide-containing gas.

[0053] Among the above, in consideration of the use of the ready-mixed concrete sludge water 1, the combustion exhaust gas discharged in the firing process in a precast concrete (PCa) product factory is preferable. The production method of this embodiment can be carried out in the various types of factory equipment by installing a contactor and a reaction vessel (corresponding to the first contact tank and the second contact tank in FIG. 1 ), which are the production apparatus of this embodiment described below, in the various types of factory equipment.

[0054] The temperature conditions of the carbon dioxide-containing gas (combustion exhaust gas) cannot be generalized as they can vary depending on which exhaust gas is used, but the temperature at the point where the ready-mixed concrete sludge water 1 is supplied is preferably 10°C or higher, more preferably 15°C or higher, and even more preferably 20°C or higher, with the upper limit being preferably 100°C or lower, more preferably 95°C or lower, even more preferably 80°C or lower, and even more preferably 70°C or lower. Furthermore, when using a large amount of substrate, for example 100 kg or more, the temperature is preferably 10° C. or higher, more preferably 15° C. or higher, even more preferably 20° C. or higher, even more preferably 45° C. or higher, and particularly preferably 55° C. or higher, and the upper limit is preferably 100° C. or lower, more preferably 95° C. or lower, and even more preferably 80° C. or lower. When the temperature conditions are within the above range, the roadbed material can be obtained more efficiently.

[0055] The amount of carbon dioxide-containing gas to be supplied cannot be generally determined because it varies depending on the amount of the contained material to be treated, the size of the reaction vessel in which the second contact step is performed, etc., but for example, the amount of carbon dioxide-containing gas to be supplied per ton of the contained material is preferably 3 Nm 3 / h or more, preferably 10Nm 3 / h or more, more preferably 50Nm 3 / h or more, with the upper limit preferably being 2500 Nm 3 / h or less, preferably 2000Nm 3 / h or less, more preferably 1500Nm 3 / h or less.

[0056] [Third Contact Step] The method for producing a roadbed material in this embodiment then includes a third contact step in which the carbon dioxide-containing gas is contacted with the fresh concrete sludge water 2 to obtain a reaction product containing calcium carbonate.

[0057] The carbon dioxide-containing gas used in the second contact step is usually finally discharged to the atmosphere, but before being discharged to the atmosphere, in the third contact step, the carbon dioxide-containing gas is brought into contact with the fresh concrete sludge water 2 to obtain a reaction product containing calcium carbonate. In the third contact step, the carbon dioxide-containing gas is brought into contact with the fresh concrete sludge water 2 to obtain a reaction product containing calcium carbonate. Therefore, in the third contact step, it becomes possible to further recover carbon dioxide from the carbon dioxide-containing gas from which carbon dioxide has been recovered in the second contact step.

[0058] The ready-mixed concrete sludge water 2 used in the third contact step has the same properties as the ready-mixed concrete sludge water 1 described above, and is the same as that described for the ready-mixed concrete sludge water 1 described above.

[0059] The ready-mixed concrete sludge water 2 may have properties different from those of the ready-mixed concrete sludge water 1, or may be the same as the ready-mixed concrete sludge water 1. When the same ready-mixed concrete sludge water as the ready-mixed concrete sludge water 1 is used, the ready-mixed concrete sludge water 1 and the ready-mixed concrete sludge water 2 may be supplied from a single ready-mixed concrete sludge water supply facility (or may be supplied from a single ready-mixed concrete sludge water tank), as shown in Fig. 1, for example.

[0060] (Contact between carbon dioxide-containing gas and fresh concrete sludge water 2) The method of contacting the carbon dioxide-containing gas with the fresh concrete sludge water 2 is not particularly limited as long as it is a method that brings the carbon dioxide-containing gas into contact with the fresh concrete sludge water 2, and it is preferable to spray the fresh concrete sludge water 2 into the carbon dioxide-containing gas. More specifically, considering that the carbon dioxide-containing gas is usually released into the atmosphere through a flue, it is preferable to spray the fresh concrete sludge water 2 into the flue through which the carbon dioxide-containing gas used in the second contact step passes. When the second contact step is carried out in a reaction vessel, the carbon dioxide-containing gas becomes the gas discharged from the reaction vessel.

[0061] When the carbon dioxide-containing gas is brought into contact with the fresh concrete sludge water 2 by spraying the fresh concrete sludge water 2, the fresh concrete sludge water 2 and the carbon dioxide in the carbon dioxide-containing gas come into contact with each other easily, and carbon dioxide can be efficiently taken into the fresh concrete sludge water 2. Furthermore, the calcium content contained in the fresh concrete sludge water 2 is more likely to react with carbon dioxide, which promotes the production of reaction products containing calcium carbonate and also promotes the recovery of carbon dioxide.

[0062] When spraying the fresh concrete sludge water 2, the amount of fresh concrete sludge water 2 supplied to the flue cannot be generalized because it varies depending on the flow rate of the exhaust gas passing through the flue, the size of the flue, etc., but it is recommended to spray the amount of fresh concrete sludge water 2 per 1 m of exhaust gas. 3 The supply amount per unit time is preferably 0.5 kg / h or more and 600 kg / h or less. From the viewpoint of more efficiently promoting the production of a reaction product containing calcium carbonate, the supply amount is preferably 5 kg / h or more, more preferably 10 kg / h or more, even more preferably 20 kg / h or more, and even more preferably 100 kg / h or more, and the upper limit is preferably 500 kg / h or less. In addition, when a plurality of spray nozzles are provided, the above supply amount is the supply amount supplied from all the spray nozzles.

[0063] The ready-mixed concrete sludge water 2 may be stored in a ready-mixed concrete sludge water tank as shown in Fig. 1, and may be sprayed and brought into contact with the ready-mixed concrete sludge water 2 via a spray nozzle as necessary. As described above, ready-mixed concrete sludge water 1 and 2 may have the same properties, and therefore the ready-mixed concrete sludge water 1 and 2 may be supplied from one ready-mixed concrete sludge water tank as shown in Fig. 1, that is, one ready-mixed concrete sludge water tank may be shared and supplied from one ready-mixed concrete sludge water supply facility. In addition, when a plurality of spray nozzles are used as the spray nozzles used in the third contact step, a single ready-mixed concrete sludge water tank may be provided and the water may be supplied to a plurality of spray nozzles as shown in Fig. 1, or one ready-mixed concrete sludge water supply facility may be provided for one spray nozzle depending on the location of the spray nozzle.

[0064] When spraying the fresh concrete sludge water 2, the tool used for spraying can be any tool capable of spraying the fresh concrete sludge water 2, and it is preferable to use a spray nozzle in consideration of ease of handling and availability. Other details of the spray nozzle will be described later.

[0065] (roadbed material) The roadbed material obtained as described above contains a base material and calcium carbonate, and preferably has calcium carbonate coated (attached) to the surface of the base material. Calcium carbonate may be coated (attached) to a part of the surface of the base material, or may be coated (attached) to the entire surface. Either way, it can be suitably used as a roadbed material.

[0066] The roadbed material obtained by the method for producing a roadbed material of this embodiment is suitable for use as a substitute for single materials conventionally used as roadbed materials, such as crushed stone, slag, cut gravel, sand, etc. When used for these purposes, by receiving mass balance certification for the carbon dioxide fixed as calcium carbonate in the base material, it becomes possible to contribute to carbon neutralization according to the amount of carbon dioxide fixed in the roadbed material obtained by the method for producing a roadbed material of this embodiment.

[0067] (Reactants containing calcium carbonate) In the method for producing a roadbed material of this embodiment, a reaction product containing calcium carbonate is obtained as a by-product by the third contact step. The reaction product containing calcium carbonate mainly contains calcium carbonate generated by a reaction between the carbon dioxide contained in the carbon dioxide-containing gas and the calcium content contained in the fresh concrete sludge water 2. The reaction product containing calcium carbonate obtained in the third contact step can be collected, for example, by using a dust collector as described below.

[0068] The purity of calcium carbonate contained in the reaction product containing calcium carbonate is usually 90% by mass or more, and further 92% by mass or more, or 95% by mass or more. Thus, in the method for producing a roadbed material of this embodiment, the reaction product containing calcium carbonate obtained as a by-product has an extremely high purity of calcium carbonate and becomes a calcium carbonate powder having high quality.

[0069] The reaction product containing calcium carbonate recovered by the production method of the present embodiment can be suitably used for applications such as fillers used in cement compositions, mortar, concrete, asphalt, and the like, and building materials.

[0070] The calcium carbonate produced by the production method of this embodiment can be used alone or in a mixture with other fillers such as calcium carbonate. In addition, when used for the above-mentioned applications, by obtaining mass balance certification for calcium carbonate, it becomes possible to contribute to carbon neutralization according to the amount of calcium carbonate obtained by the production method of this embodiment used.

[0071] Fresh concrete sludge water also contains sodium, sulfur, etc., so the reaction product containing calcium carbonate may also contain impurities resulting from these. The content of impurities contained in the reaction product containing calcium carbonate is usually about 10% by mass or less, and furthermore 8% by mass or less, 5% by mass or less, 3% by mass or less, or 1% by mass or less. Since the content of impurities is so low, there is no problem in using it for the above-mentioned purposes.

[0072] [Road base material manufacturing equipment] The roadbed material manufacturing apparatus of this embodiment is A contacting device for contacting the fresh concrete sludge water 1 with a substrate to obtain a content containing the fresh concrete sludge water 1 and the substrate; A reaction vessel for obtaining a roadbed material containing the base material and calcium carbonate by contacting the content with a carbon dioxide-containing gas; a flue through which the carbon dioxide-containing gas discharged from the reaction vessel passes; A spray nozzle for supplying fresh concrete sludge water 2 to the flue; and a dust collector for recovering a reaction product containing calcium carbonate obtained by contacting the carbon dioxide-containing gas in the flue with the fresh concrete sludge water 2; The idea is to provide the following:

[0073] [Contact device] The contact device can be used without any particular restrictions as long as it can bring the fresh concrete sludge water 1 into contact with the base material. For example, a device of the type shown in Figure 1 having a container for temporarily storing the base material and a spray nozzle on the top of the container can be used.

[0074] In the contact device shown in Fig. 1, the container portion is shown to have a structure in which the inlet at the top is large and the outlet at the bottom is small. Examples of such shapes include a shape combining a prism and a pyramid, or a shape combining a cylinder and a cone, and containers such as silos and hoppers can be used. By using a contact device having such a shape, it is easy to efficiently bring the ready-mixed concrete sludge water 1 into contact with the base material, and the contents including the ready-mixed concrete sludge water 1 and the base material can be more easily supplied to the reaction container.

[0075] (Spray nozzle for spraying fresh concrete sludge water 1) The contact device preferably includes a spray nozzle for spraying the fresh concrete sludge water 1 onto the substrate to bring it into contact therewith. The fresh concrete sludge water 1 sprayed onto the substrate by the spray nozzle is sprayed onto the substrate as tiny particles, which tend to adhere to the surface of the substrate as tiny particles (droplets), allowing the calcium contained in the tiny particles (droplets) to come into contact with carbon dioxide more efficiently, enabling the roadbed material to be produced more efficiently and also enabling the carbon dioxide to be recovered.

[0076] The spray nozzle is not particularly limited as long as it is a nozzle capable of spraying the ready-mixed concrete sludge water 1, and it is possible to use any commercially available spray nozzle. For example, it is possible to use a one-fluid nozzle that sprays only the ready-mixed concrete sludge water 1, or a multi-fluid nozzle such as a two-fluid nozzle that sprays the ready-mixed concrete sludge water 1 together with a gas such as air as necessary. Furthermore, it is possible to use a nozzle having a mechanism for making the spray particles finer by generating ultrasonic waves (also called an "ultrasonic spray nozzle") as necessary.

[0077] The spray pattern of the spray nozzle can be adopted without any particular limitation, and representative examples include full cone, hollow cone, flat (fan shape), solid (straight), etc. The spray angle of the spray nozzle can also be adopted without any particular limitation, and is preferably 60° or more, more preferably 90° or more, with the upper limit being preferably 145° or less, more preferably 140° or less. As the spray nozzle, from the viewpoint of ensuring a better spray state and promoting the reaction between the calcium content and carbon dioxide due to contact with carbon dioxide in the second contact step, it is preferable to use a spray nozzle having a hollow cone with a large spray angle or a flat (fan-shaped) spray pattern.

[0078] The hole diameter of the spray nozzle for the fresh concrete sludge water 1 cannot be generalized as it can vary depending on the number of spray holes the spray nozzle has, the amount of fresh concrete sludge water 1 supplied, etc., but from the viewpoint of ensuring a better spraying condition, it is preferably 0.1 mm or more, more preferably 0.5 mm or more, and even more preferably 1.0 mm or more, with the upper limit being preferably 10 mm or less, more preferably 5.0 mm or less, and even more preferably 3.0 mm or less.

[0079] The finer the spray particles of the fresh concrete sludge water 1 sprayed from the spray nozzle, the better from the viewpoint of promoting the reaction between the calcium content and carbon dioxide. The particle diameter of the spray particles is preferably 1000 μm or less, more preferably 500 μm or less, even more preferably 100 μm or less, and even more preferably 50 μm or less.

[0080] In the manufacturing method of this embodiment, the number of spray nozzles to be installed cannot be generalized because it can vary depending on the size of the spray nozzle, the diameter and number of the spray holes of the spray nozzle, and the supply amount of the fresh concrete sludge water 1, but it is preferable to have at least one spray nozzle on the upper part of the contact device (first contact tank) in which the first contact step between the fresh concrete sludge water 1 and the base material is performed, as shown in Fig. 1. That is, the upper part of the contact device (first contact tank) may have one spray nozzle, or may have two or more spray nozzles as necessary.

[0081] As shown in Fig. 1, the spray nozzle may be provided not only in the contact device (first contact tank) but also in other locations. For example, after the substrate is crushed in the crushing facility, the spray nozzle may be provided on a belt conveyer when the crushed substrate is moved to a substrate yard by a transfer belt conveyer, during transport (for example, in a transport vehicle) from the substrate yard (substrate shipping base) to a manufacturing equipment site (transport belt conveyer within the site), on a belt conveyer when the substrate is transported within the manufacturing equipment site to the contact device (first contact tank), etc.

[0082] Moreover, the gas may be provided in a location that is not intended for contact between the fresh concrete sludge water 1 and the base material, for example, as shown in FIG. 1, in a supply line for supplying carbon dioxide-containing gas from various factory facilities (immediately before the supply port to the reaction vessel (second contact tank)), or inside the reaction vessel (second contact tank).

[0083] (Other jigs) As other tools, the contact device is preferably equipped with a partition tool such as a knife gate at the bottom of the contact device to keep the base material in the contact device and ensure the contact time with the fresh concrete sludge water 1. In addition, in order to quantitatively supply the contents containing the fresh concrete sludge water 1 and the base material to the reaction vessel, it is preferable that the reaction vessel is provided with a quantitative supply valve such as a rotary valve.

[0084] [Reaction vessel] The reaction vessel can be used without any particular limitation as long as it can contact the contents obtained in the contact device with the carbon dioxide-containing gas. For example, as shown in Fig. 1, a vessel having the same structure as the vessel part of the contact device, that is, a vessel having a large inlet at the top and a small outlet at the bottom, may be used.

[0085] It is also preferable that the reactor has a supply port and a discharge port for the carbon dioxide-containing gas, and the supply port is preferably provided at the bottom of the reactor as shown in Fig. 1. It is also preferable that the discharge port is provided at the top of the reactor. By providing the discharge port in this way, it becomes easier to efficiently contact the contents with the carbon dioxide-containing gas.

[0086] [Flute] A flue is a pipe that allows carbon dioxide-containing gas to pass through. A flue usually refers to a pipe or duct that guides exhaust gas from power plants, cement plants, precast concrete (PCa) product plants, asphalt plants, steel mills, incinerators, and other factory facilities, as well as the boilers and other equipment installed in these facilities, to a chimney.

[0087] The flue refers not only to the piping for leading the exhaust gas discharged from the factory equipment directly to the chimney, but also to the piping from the reaction vessel to the dust collector after the exhaust gas (gas containing carbon dioxide) is extracted from the chimney and passed through the reaction vessel, and further to the piping of the exhaust gas discharged from the factory equipment after passing through the dust collector, as shown in Figure 1. Therefore, when a spray nozzle, which will be described later, is provided in the flue, the spray nozzle can be provided not only to the piping for leading the exhaust gas discharged from the factory equipment directly to the chimney, but also to the piping from the reaction vessel to the dust collector after the exhaust gas (gas containing carbon dioxide) is extracted from the chimney and passed through the reaction vessel, and further to the piping of the exhaust gas discharged from the factory equipment after passing through the dust collector.

[0088] The flue is not particularly limited as long as it can pass exhaust gas containing carbon dioxide, and may be a newly installed flue, or, in consideration of reducing equipment costs, may be an existing flue installed to exhaust exhaust gas discharged from power plants, cement plants, precast concrete (PCa) product factories, asphalt factories, steelworks, incinerators, and other factory equipment, and boilers and the like installed in these various facilities. Considering that the manufacturing apparatus of this embodiment uses ready-mixed concrete sludge water, it is preferable to use an existing flue installed in a precast concrete (PCa) product factory to exhaust exhaust gas as the flue. Therefore, it is preferable that the manufacturing apparatus of this embodiment is incorporated into the precast concrete (PCa) product factory.

[0089] [Spray nozzle for supplying fresh concrete sludge water 2] The manufacturing apparatus of this embodiment includes a spray nozzle for supplying the ready-mixed concrete sludge water 2 in the third contact step. As described above, the ready-mixed concrete sludge water 2 can be the same as the ready-mixed concrete sludge water 1. Therefore, as the spray nozzle used for supplying the ready-mixed concrete sludge water 2, the spray nozzle described above for supplying the ready-mixed concrete sludge water 1 can be used.

[0090] The number of spray nozzles to be installed cannot be generalized as it varies depending on the size of the spray nozzle, the diameter and number of the spray ports of the spray nozzle, the amount of fresh concrete sludge water 2 supplied, and the dimensions of the flue, but it is sufficient to have one or more, and the upper limit is usually 10 or less, preferably 8 or less, and more preferably 5 or less.

[0091] There are no particular limitations on the location of the spray nozzle as long as it can supply fresh concrete sludge water 2 to the flue, but it is preferable to install it directly in the flue as shown in Fig. 1. In this case, if the vertical cross section of the flue is circular, the installation location of the spray nozzle is preferably on the semicircle in the upper half of the circle (within ±90° when the uppermost point is 0°), more preferably within ±60°, even more preferably within ±30°, still more preferably within ±15°, and particularly preferably at the uppermost point. Furthermore, if the flue is a square duct, the same applies as in the case of the circular pipe (or duct) described above. When multiple spray nozzles are provided, the multiple spray nozzles may be provided on a circle of the same cross section, or may be provided one after the other at the uppermost point in the direction in which the exhaust gas flows.

[0092] [Dust collection device] The manufacturing apparatus of this embodiment includes a dust collector that collects a reaction product containing calcium carbonate obtained by contacting the carbon dioxide-containing gas in the flue with the fresh concrete sludge water 2. As the dust collector, various types of dust collectors can be used, such as electrostatic precipitators such as dry electrostatic precipitators and wet electrostatic precipitators, and filter dust collectors (bag filters), etc. In the system of this embodiment, a filter dust collector (bag filter) is preferred in view of reducing electricity consumption and ease of handling.

[0093] The dust collector may be provided at a location where a reaction product containing calcium carbonate generated by contact of the carbon dioxide-containing gas with the fresh concrete sludge water 2 in the flue (third contact step) can be collected. For example, as shown in FIG. 1, the dust collector may be provided before the exhaust gas (carbon dioxide-containing gas) discharged from the reaction vessel joins the piping of the exhaust gas discharged from the plant equipment, or may be provided from the joining point where the exhaust gas (carbon dioxide-containing gas) discharged from the reaction vessel joins the piping of the exhaust gas discharged from the plant equipment to the chimney. In the latter case, when a spray nozzle is used, the spray nozzle may be provided in the flue before the joining, or may be provided after the joining and upstream of the dust collector. From the viewpoint of making the size of the dust collector smaller, it is preferable that the dust collector be provided before the joining, as shown in FIG. 1.

[0094] The dust collector is provided to recover a reactant containing calcium carbonate produced in the third contact step, as shown in Fig. 1, i.e., may be provided separately from a dust collector for exhaust gas discharged from the factory facility (corresponding to the "dust collector in the factory facility" in Fig. 1), or may share the same dust collector as the dust collector provided in the factory facility as in the latter case described above. From the viewpoint of obtaining a reactant (calcium carbonate) of higher quality, it is preferable that the dust collector is provided separately from a dust collector for exhaust gas discharged from the factory facility (dust collector in the factory facility) as shown in Fig. 1.

[0095] The filters used in the filtration dust collection device (bag filter) can be any filter made of materials such as polypropylene, nylon, acrylic, polyester, cotton, wool, heat-resistant nylon, glass fiber, and PTFE (polytetrafluoroethylene), and functional filters such as electrostatic filters can also be used. The bag filter may have a brushing means, and preferred examples of such means include a pulsating counter pressure type and a pulse jet type, with the pulse jet type being preferred.

[0096] [Other devices] The manufacturing apparatus of this embodiment is equipped with the above-mentioned contact device, reaction vessel, flue, spray nozzle for supplying ready-mixed concrete sludge water 2, and dust collection device, and may be equipped with other devices and equipment as necessary.

[0097] (Ready-mixed concrete sludge water supply equipment) For example, as shown in Fig. 1, a concrete sludge water supply facility having a ready-mixed concrete sludge water tank for storing ready-mixed concrete sludge water can be provided. By providing the ready-mixed concrete sludge water, the ready-mixed concrete sludge water can be stored once and then supplied in the required amount in the first contact step, improving the operational stability of the manufacturing apparatus of this embodiment.

[0098] Temporarily storing ready-mixed concrete sludge water in a ready-mixed concrete sludge water tank not only makes it easier to respond to fluctuations in the required amount, but also makes it easier to spray a constant amount from a spray nozzle when one is used. This stabilizes the contact between the ready-mixed concrete sludge water and the base material, making it easier to homogenize the contents and homogenize the roadbed material.

[0099] The ready-mixed concrete sludge water tank can be used without any particular restriction as long as it is capable of storing sludge water, and may be one that is installed either above ground or underground, such as an above-ground storage tank or an underground storage tank, and may be selected from various roof-type storage tanks called fixed roof types and floating roof types, as well as horizontal and vertical storage tanks such as horizontal cylindrical types and vertical cylindrical types. In addition, the ready-mix concrete sludge water tank may be a new tank or an existing tank may be reused.

[0100] The ready-mix concrete sludge water tank is preferably equipped with an agitator, which can suppress solidification of the ready-mix concrete sludge water, which may contain solids. The ready-mix concrete sludge water tank may also be equipped with a retarder supplying tool to inhibit the solidification of the solids. There are no particular limitations on the type of retarder supplying tool, and any device such as a drug metered supplying device may be used. As the retarder, any agent that can inhibit the solidification of the solids may be used without particular limitations, and examples of such retarders include gluconates, citric acid and its salts, and tartaric acid and its salts.

[0101] The ready-mixed concrete sludge water tank may also be equipped with various instrumentation such as a level gauge and a control valve that adjusts the amount of ready-mixed concrete sludge water supplied to the ready-mixed concrete sludge water tank using the level gauge.

[0102] The ready-mixed concrete sludge water supply facility may include, in addition to the ready-mixed concrete sludge water tank, instrumentation such as a flow meter, a flow control valve, etc. When there are multiple supply destinations for the ready-mixed concrete sludge water, each supply destination may be provided with instrumentation.

[0103] The ready-mixed concrete sludge water supply equipment has at least a ready-mixed concrete sludge water tank, and preferably has the above-mentioned various instrumentation devices, as well as piping to the supply destinations of the spray nozzles, etc. As described above, for example, when there are a plurality of spray nozzles, one ready-mixed concrete sludge water supply equipment may supply ready-mixed concrete sludge water to a plurality of spray nozzles, or ready-mixed concrete sludge water may be supplied to each spray nozzle, i.e., a plurality of ready-mixed concrete sludge water supply equipment may be provided.

[0104] In addition, as the fresh concrete sludge water, fresh concrete sludge water 1 and 2 are used, and a fresh concrete sludge water supply facility may be provided for each of the fresh concrete sludge water 1 and 2, or one fresh concrete sludge water supply facility may be provided for the fresh concrete sludge water 1 and 2.

[0105] (Substrate receiving and transport equipment) As shown in FIG. 1, the manufacturing apparatus of this embodiment may include a crushing facility for crushing received substrates as necessary, a substrate yard for temporarily storing substrates in order to load them onto a transport vehicle, and various types of belt conveyors, such as a transfer belt conveyor for transporting substrates from the crushing facility to the substrate yard and a transport belt conveyor for transporting substrates from the substrate yard to the contact device. The types of these facilities, belt conveyors, etc. may be appropriately selected from known types. Also, Fig. 1 shows a preferred embodiment, and it goes without saying that these facilities, belt conveyors, transport vehicles, etc. may be adopted as necessary.

[0106] [Method of capturing carbon dioxide] The carbon dioxide recovery method of the present embodiment includes: A first contact step of obtaining a content containing the fresh concrete sludge water 1 and the base material by contacting the fresh concrete sludge water 1 with the base material; a second contact step of contacting the mixture with a carbon dioxide-containing gas to react carbon dioxide contained in the carbon dioxide-containing gas to obtain a reaction product containing calcium carbonate; A third contact step in which the carbon dioxide contained in the carbon dioxide-containing gas is reacted with the carbon dioxide-containing gas to obtain a reaction product containing calcium carbonate by contacting the carbon dioxide-containing gas with the fresh concrete sludge water 2; and a recovery step of recovering the reaction product containing calcium carbonate obtained in the third contact step with a dust collector; It includes the following.

[0107] According to the method for producing a roadbed material of the present embodiment, not only can the roadbed material be produced as described above, but also carbon dioxide can be captured. The method for capturing carbon dioxide of the present embodiment focuses on this point.

[0108] The first contact step, the second contact step, the third contact step, and the objects of contact in these contact steps, such as the fresh concrete sludge water, the base material, and the carbon dioxide-containing gas, are the same as those described in the above-mentioned method for producing a roadbed material. Various conditions during contact are also the same as those described in the above-mentioned method for producing a roadbed material. The dust collector and the reactant containing calcium carbonate in the recovery step are also the same as those described in the method for producing roadbed material. EXAMPLES

[0109] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples in any way.

[0110] Example 1 A contact device (first contact tank), a reaction vessel (second contact tank), a flue, a dust collector and a chimney in a roadbed material manufacturing apparatus having the configuration shown in FIG. 1 were used. Crushed stone (particle size: 13 mm or less (13 mm sieve processed product)) was used as the base material, and 1000 g of crushed stone was charged from the top of the contact device (first contact tank). Next, 15 g of ready-mixed concrete sludge water 1 (calcium concentration: 900 mass ppm, solids concentration: 3 mass%) was supplied while being sprayed through a spray nozzle (nozzle hole diameter: 0.05 mmφ) to bring the ready-mixed concrete sludge water 1 into contact with the crushed stone (first contact step), thereby obtaining an inclusion containing the ready-mixed concrete sludge water 1 and the crushed stone. The obtained inclusion was supplied to a reaction vessel (second contact tank), and then 0.03 m of a carbon dioxide-containing gas (carbon dioxide concentration: 3% by volume) at 25°C was added. 3 / h, and the contents were contacted with the carbon dioxide-containing gas (second contact step) at a temperature of 25°C to obtain a roadbed material containing the base material and calcium carbonate. The amount of carbon dioxide consumed in the second contact process to produce the roadbed material was calculated as the amount of carbon dioxide recovered, which was 0.3 kg-CO2 / t-base material. The amount of carbon dioxide recovered was calculated based on the exhaust gas flow rate (m 3 / s) × supply time (s) × (carbon dioxide concentration at reactor inlet - carbon dioxide concentration at reactor outlet) × specific gravity of carbon dioxide (kg / m 3 ) / mass of substrate (tons).

[0111] After the second contact step, the carbon dioxide-containing gas passes through a flue (diameter: 100 mm, flow rate: 0.24 m 3 Fresh concrete sludge water 2 (calcium concentration: 900 mass ppm, solids concentration: 22 mass ppm, solids particle size: 1-10 μm) was supplied to a suction vessel (air conditioner) ...

[0112] Comparative Example 1 The same procedure was followed as in Example 1, except that water was used instead of the fresh concrete sludge water 1 and 2. The amount of carbon dioxide consumed in the second contact step was calculated as the amount of carbon dioxide recovered in the same manner as in Example 1, and was less than 0.1 kg-CO2 / t-base material. No calcium carbonate powder was obtained. The above measurement results and the various conditions in the examples are shown in Table 1.

[0113] Example 2 A roadbed material was obtained in the same manner as in Example 1, except that the crushed stone was replaced with recycled crushed stone (particle size: 40 mm or less (40 mm sieve-treated product)) and the amount of ready-mixed concrete sludge water 1 was changed to 61.7 g. The amount of carbon dioxide recovered was 3.3 kg-CO2 / t-substrate, and the powder recovered by the dust collector (bag filter) was analyzed and confirmed to be calcium carbonate powder (purity: 96%). The above measurement results and the various conditions used in the examples are shown in Table 1.

[0114] Comparative Example 2 Example 2 was conducted in the same manner as Example 2, except that water was used instead of the fresh concrete sludge water 1 and 2. The amount of carbon dioxide consumed in the second contact step was calculated as the amount of carbon dioxide recovered in the same manner as Example 2, resulting in 2.6 kg-CO2 / t-base material. No calcium carbonate powder was obtained. The above measurement results and the various conditions in the example are shown in Table 1.

[0115] Example 3 In Example 1, the roadbed material was obtained in the same manner as in Example 1, except that the crushed stone was replaced with crushed sand (particle size: 2.85 mm or less), the amount of fresh concrete sludge water 1 used was 15 g, and the fresh concrete sludge water 2 was supplied while spraying at a flow rate of 2 g / min (0.12 kg / h). The amount of carbon dioxide recovered was 0.5 kg-CO2 / t-substrate, and the powder recovered by the dust collector (bag filter) was analyzed and confirmed to be calcium carbonate powder (purity: 93%). The above measurement results and the various conditions used in the examples are shown in Table 1.

[0116] Comparative Example 3 Example 3 was the same as Example 3, except that water was used instead of the fresh concrete sludge water 1 and 2. The amount of carbon dioxide consumed in the second contact step was calculated as the amount of carbon dioxide recovered in the same manner as in Example 3, and was less than 0.1 kg-CO2 / t-base material. No calcium carbonate powder was obtained. The above measurement results and the conditions in the examples are shown in Table 1.

[0117] Example 4 In Example 1, the roadbed material was obtained in the same manner as in Example 1, except that crushed stone was used as recycled aggregate (particle size: 40 mm or less), the amount of fresh concrete sludge water 1 used was 15 g, and the fresh concrete sludge water 2 was supplied while spraying at a flow rate of 20 g / min (1.2 kg / h). The amount of carbon dioxide recovered was 0.3 kg-CO2 / t-substrate, and the powder recovered by the dust collector (bag filter) was analyzed and confirmed to be calcium carbonate powder (purity: 94%). The above measurement results and the various conditions used in the examples are shown in Table 1.

[0118] Comparative Example 4 Example 4 was conducted in the same manner as in Example 4, except that water was used instead of the fresh concrete sludge water 1 and 2. The amount of carbon dioxide consumed in the second contact step was calculated as the amount of carbon dioxide recovered in the same manner as in Example 4, and was less than 0.1 kg-CO2 / t-base material. No calcium carbonate powder was obtained. The above measurement results and the various conditions in the examples are shown in Table 1.

[0119] [Table 1]

[0120] From the results of Examples 1 to 4, it was confirmed that the method for producing a roadbed material of the present embodiment makes it possible to efficiently obtain a roadbed material containing a base material and calcium carbonate. A comparison between Example 1 and Comparative Example 1 shows that by using the fresh concrete sludge water 1 in the first contact step, the amount of carbon dioxide recovered is three times or more, that is, a roadbed agent in which three times or more calcium carbonate is coated (adhered) to the surface of the base material is obtained. A comparison between Example 2 and Comparative Example 2 shows that the amount of carbon dioxide recovered is improved by 27%, that is, a roadbed agent in which 1.27 times more calcium carbonate is coated (adhered) to the surface of the base material is obtained. Also, it shows that Example 3 and Comparative Example 3, and Example 4 and Comparative Example 4 also show that roadbed materials in which five times or more and three times more calcium carbonate are coated (adhered) to the surface of the base material, respectively, are obtained.

[0121] Moreover, it was confirmed that the reaction product containing calcium carbonate obtained by the third contact step had a calcium carbonate purity of 93 to 96%, and was a calcium carbonate powder having high quality. On the other hand, in the comparative example in which the fresh concrete sludge water 2 was not used, a reaction product containing calcium carbonate was not obtained. Note that the carbon dioxide concentration of the carbon dioxide-containing gas used in the third contact step was 3% by volume or less because part of the carbon dioxide was consumed in the second contact step.

[0122] As described above, it has been confirmed that the method for producing roadbed material according to the present embodiment has high versatility that can be applied to a wide variety of materials such as crushed stone and recycled crushed stone, and can produce roadbed material by the simple contacting operation of the first contacting step to the third contacting step, and can also capture carbon dioxide. Furthermore, it has been confirmed that high-quality calcium carbonate can be obtained, and at the same time, carbon dioxide can be captured when obtaining calcium carbonate. Therefore, it has been confirmed that the method for manufacturing roadbed material of this embodiment can efficiently capture carbon dioxide by including not only the first and second contact steps but also the third contact step, and therefore can be suitably used as a method for capturing carbon dioxide as it is.

[0123] (Examples 5 to 8) In Example 1, only the third contact step was carried out, changing the carbon dioxide-containing gas to the conditions shown in Table 2. The measurement results of the reaction products containing calcium carbonate obtained in Examples 5 to 8 are shown in Table 2.

[0124] [Table 2] * The amount of fresh concrete sludge water 2 supplied is 1 m3 of carbon dioxide-containing gas in the third contact step. 3 / h is the supply amount of fresh concrete sludge water 2.

[0125] According to the results of Examples 5 to 8, it was confirmed that, within the above-mentioned condition range, the purity of calcium carbonate was extremely high, at 91% or more, and a high-quality calcium carbonate powder could be obtained. It was also confirmed that the purity of calcium carbonate tends to improve when the supply amount of the fresh concrete sludge water 2 is increased.

[0126] Example 9 A contact device (first contact tank) and a reaction vessel (second contact tank) in a roadbed material manufacturing apparatus having the configuration shown in FIG. 1 were used. Recycled crushed stone (grain size: 40 mm or less) was used as the base material, and 1000 kg of recycled crushed stone was charged from the top of the contact device (first contact tank). Next, 10 kg of ready-mixed concrete sludge water 1 (calcium concentration: 900 mass ppm, solids concentration: 3 mass%) was supplied while spraying through a spray nozzle (nozzle hole diameter: 0.5 mmφ) to bring the ready-mixed concrete sludge water 1 into contact with the crushed stone (first contact step), thereby obtaining an inclusion containing the ready-mixed concrete sludge water 1 and the crushed stone. The obtained inclusion was supplied to a reaction vessel (second contact tank), and then 300 m of a carbon dioxide-containing gas (carbon dioxide concentration: 3% by volume) at 60°C was poured into the reaction vessel. 3 / h, and the contents were contacted with the carbon dioxide-containing gas (second contact step) at a temperature of 60°C to obtain a roadbed material containing the base material and calcium carbonate. The amount of carbon dioxide consumed in the second contact process to produce roadbed material was calculated as the amount of carbon dioxide recovered, which was 5.1 kg-CO2 / t-base material.

[0127] After the second contact step, the carbon dioxide-containing gas passes through a flue (diameter: 100 mm, flow rate: 270 m 3Fresh concrete sludge water 2 (calcium concentration: 900 mass ppm, solids concentration: 22 mass ppm, solids particle size: 1-10 μm) was supplied to a 13,500 kg / h (40°C) tank through a spray nozzle (nozzle hole diameter: 0.5 mmφ) while being sprayed at a flow rate of 13,500 kg / h (spray particle size: 10-50 μm), and contact between the carbon dioxide-containing gas and the fresh concrete sludge water 2 (third contact step) was carried out. The powder collected by the dust collector (bag filter) was analyzed and confirmed to be calcium carbonate powder (purity: 92%). The above measurement results and various conditions in the examples are shown in Table 3.

[0128] (Examples 10 to 12) Example 9 was the same as Example 9, except that the supply amount and temperature of the carbon dioxide-containing gas were set to the conditions shown in Table 3. The amount of carbon dioxide consumed in the second contact step was calculated as the amount of carbon dioxide recovered in the same manner as in Example 9, and the results are shown in Table 3. In addition, when the powder recovered in the dust collector (bag filter) was analyzed, it was confirmed to be calcium carbonate powder. The purity of the calcium carbonate powder and the various conditions in the example are shown in Table 3.

[0129] [Table 3]

[0130] Even in Examples 9 to 12, which use 1,000 times the amount of base material compared to Examples 1 to 4, it was confirmed that the roadbed material manufacturing method of this embodiment can efficiently produce a roadbed material containing the base material and calcium carbonate.

[0131] (Examples 13 and 14) The same procedure was followed as in Example 9, except that the supply amount and temperature of the carbon dioxide-containing gas were set to the conditions shown in Table 4, and the second contact step was carried out. The amount of carbon dioxide consumed was calculated as the amount of carbon dioxide recovered in the same manner as in Example 9, and the results are shown in Table 4.

[0132] [Table 4]

[0133] From the results of Examples 13 and 14, it was confirmed that the method for producing a roadbed material of this embodiment can efficiently produce a roadbed material containing a base material and calcium carbonate, even in Examples 13 and 14, which use 1000 times the amount of base material compared to Examples 1 to 4. It was also confirmed that calcium carbonate of the same purity as in Examples 9 to 12 can be obtained even if the temperature of the carbon dioxide-containing gas is set lower than that in Examples 9 to 12.

Claims

1. A first contact step of obtaining a content containing the fresh concrete sludge water 1 and the base material by contacting the fresh concrete sludge water 1 with the base material; A second contact step of obtaining a roadbed material containing the base material and calcium carbonate by contacting the content with a carbon dioxide-containing gas; A third contact step in which the carbon dioxide-containing gas is contacted with the fresh concrete sludge water 2 to obtain a reaction product containing calcium carbonate; and a recovery step of recovering the reaction product containing calcium carbonate with a dust collector; Equipped with A manufacturing method for roadbed materials.

2. 2. The method for producing a roadbed material according to claim 1, wherein the base material is at least one material selected from the group consisting of crushed stone, crushed sand, recycled aggregate derived from waste asphalt, and recycled crushed stone derived from waste concrete.

3. The method for manufacturing a roadbed material according to claim 1 or 2, wherein the contact between the ready-mixed concrete sludge water 1 and the substrate is carried out by spraying the ready-mixed concrete sludge water 1.

4. The method for manufacturing a roadbed material according to claim 3, wherein the amount of the fresh concrete sludge water 1 sprayed relative to 100 parts by mass of the base material is 0.1 parts by mass or more and 15 parts by mass or less.

5. The method for producing a roadbed material according to claim 1 or 2, wherein the contact between the content and the carbon dioxide-containing gas is carried out in a reaction vessel.

6. The method for producing a roadbed material according to claim 5, wherein the contact between the carbon dioxide-containing gas and the fresh concrete sludge water 2 is carried out by spraying the fresh concrete sludge water 2 into a flue through which the carbon dioxide-containing gas discharged from the reaction vessel passes.

7. 3. The method for manufacturing a roadbed material according to claim 1, wherein the first ready-mixed concrete sludge water and the second ready-mixed concrete sludge water are supplied from a single ready-mixed concrete sludge water supply facility.

8. 3. The method for manufacturing a roadbed material according to claim 1 or 2, wherein the first fresh concrete sludge water and the second fresh concrete sludge water are supernatant water obtained by removing solids from the fresh concrete sludge or sludge water containing the solids.

9. The method for manufacturing a roadbed material according to claim 8, wherein the first fresh concrete sludge water and the second fresh concrete sludge water are the supernatant water.

10. The method for producing a roadbed material according to claim 1 or 2, wherein the temperature of the carbon dioxide-containing gas in the second contact step is 10°C or higher and 90°C or lower.

11. 1 m of the carbon dioxide-containing gas in the third contact step 3 3. The method for manufacturing a roadbed material according to claim 1 or 2, wherein the supply amount of the fresh concrete sludge water 2 per hour is 0.5 kg / h or more and 600 kg / h or less.

12. The method for producing a roadbed material according to claim 1 or 2, wherein the roadbed material is a base material having a surface coated with the calcium carbonate.

13. A contacting device for contacting the fresh concrete sludge water 1 with a base material to obtain a content containing the fresh concrete sludge water 1 and the base material; A reaction vessel for obtaining a roadbed material containing the base material and calcium carbonate by contacting the content with a carbon dioxide-containing gas; a flue through which the carbon dioxide-containing gas discharged from the reaction vessel passes; A spray nozzle for supplying fresh concrete sludge water 2 to the flue; and a dust collector for recovering a reaction product containing calcium carbonate obtained by contacting the carbon dioxide-containing gas in the flue with the fresh concrete sludge water 2; A roadbed material manufacturing device comprising:

14. A first contact step of obtaining a content containing the fresh concrete sludge water 1 and the base material by contacting the fresh concrete sludge water 1 with the base material; a second contact step of contacting the mixture with a carbon dioxide-containing gas to react carbon dioxide contained in the carbon dioxide-containing gas to obtain a reaction product containing calcium carbonate; A third contact step in which the carbon dioxide contained in the carbon dioxide-containing gas is reacted with the carbon dioxide-containing gas to obtain a reaction product containing calcium carbonate by contacting the carbon dioxide-containing gas with the fresh concrete sludge water 2; and a recovery step of recovering the reaction product containing calcium carbonate obtained in the third contact step with a dust collector; A method for capturing carbon dioxide, comprising: