Polycarbonate resin composition

The polycarbonate resin composition with a specific ethylene resin ratio addresses melt flowability and recyclability issues, ensuring improved heat resistance, impact resistance, and reduced warping in molded products.

JP2024158654APending Publication Date: 2024-11-08TOSOH CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023074018
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Polycarbonate resin compositions face issues with melt flowability during molding, leading to deformation and appearance deterioration in thin-walled or complex shapes, and lack recyclability due to high heat resistance and low melt fluidity, with existing additives compromising impact resistance or introducing hygroscopic materials that affect processing.

Method used

A polycarbonate resin composition containing a specific ratio of ethylene resin, which provides sufficient melt fluidity, heat resistance, and impact resistance, while reducing warping and improving recyclability by using ethylene polymers that are non-polar and less susceptible to oxidative deterioration.

Benefits of technology

The composition achieves improved melt fluidity, heat resistance, and impact resistance, reducing appearance defects and enhancing recyclability, making it suitable for injection molding and material recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158654000001
    Figure 2024158654000001
  • Figure 2024158654000002
    Figure 2024158654000002
Patent Text Reader

Abstract

To provide a polycarbonate resin composition comprising a specific polycarbonate resin combined with a specific ethylene resin at a specific ratio, ensuring sufficient melting fluidity during injection molding and producing a molded product excellent in heat resistance, impact resistance, material recyclability, and appearance quality.SOLUTION: A polycarbonate resin composition comprises 100 pts.mass of a polycarbonate resin (A) in combination with 1-10 pts.mass of an ethylene resin (B). The polycarbonate resin (A) has a melt volume flow rate of 5-14 cm3 / g as measured in accordance with JIS K 7210 and at 300°C and 1.2 kg load. The ethylenic polymer (B) has a melt mass flow rate of 50-10000 g / 10 min as measured in accordance with JIS K6924-1 and at 190°C and 2160 g load.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polycarbonate resin composition and an injection-molded article thereof. [Background technology]

[0002] Polycarbonate resin is a plastic with excellent heat resistance, impact resistance, and transparency, and is widely used in various fields such as electrical and electronic equipment, automobiles, office equipment, and home appliances. In these fields, polycarbonate resin is used not only for transparent parts but also for colored parts because it has better heat resistance and impact resistance than ABS (acrylonitrile-butadiene-styrene terpolymer) and PMMA (polymethyl methacrylate).

[0003] However, polycarbonate resins have poor melt fluidity during molding due to their high heat resistance, and therefore, when they are used to manufacture thin-walled parts or parts with complex shapes, problems such as deformation of the molded product or deterioration of its appearance can occur.

[0004] Therefore, molded products are provided by adopting special molding methods such as injection compression molding, but these special molding methods have the problem of lowering cost performance. Also, there have been attempts to lower the viscosity and improve melt flowability by increasing the molding temperature in injection molding or by decreasing the molecular weight of the polycarbonate resin, but the former is not only insufficient in terms of modifying properties, but also causes thermal degradation, and the latter has the problem of lowering heat resistance and mechanical properties.

[0005] Furthermore, in recent years, from the viewpoint of effective resource utilization, there has been a demand for the promotion of material recycling, in which product waste is reused as raw materials, and there is a strong demand for material recycling of polycarbonate resin due to its wide range of product fields. However, in material recycling of polycarbonate resin, the low melt fluidity is an issue, just like virgin resin, and much research and development is being carried out to bring it to a usable level.

[0006] In this context, the addition of lubricants has been investigated to improve the melt fluidity of polycarbonate resins and the like. For example, a polycarbonate resin composition in which pentaerythritol, linear saturated fatty acid, adipic acid, and fatty acid complex ester wax are added to polycarbonate resin to improve melt fluidity and heat resistance (see, for example, Patent Document 1), a polycarbonate resin composition in which an oxidized acid-modified polyethylene wax is added to polycarbonate resin to improve melt fluidity without deteriorating heat resistance (see, for example, Patent Document 2), and a polycarbonate resin composition in which a polyorganosiloxane containing a nitrogen-containing organic group is added to a resin mixture consisting of a specific ratio of polycarbonate resin and polylactic acid, and which has excellent melt fluidity and impact resistance, and furthermore, the moisture resistance of polycarbonate is improved by the addition of polylactic acid, and durability is improved, resulting in excellent material recyclability (see, for example, Patent Document 3). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent Publication No. 2021-195453 [Patent Document 2] Patent No. 6682534 [Patent Document 3] JP 2008-37965 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, the polycarbonate resin compositions proposed in Patent Documents 1 and 2 have problems in that no consideration has been given to maintaining or improving impact resistance. Also, the polycarbonate resin composition proposed in Patent Document 3 contains highly hygroscopic polylactic acid, and has a problem in handleability in that the absorbed moisture significantly affects processing during injection molding of polycarbonate resin, which requires very high processing temperatures. Furthermore, these polycarbonate resin compositions have not been considered at all as injection molding materials with fluidity or recyclability.

[0009] Therefore, the present invention aims to solve these problems by providing a polycarbonate resin composition containing a specific ethylene-based resin, which imparts sufficient melt fluidity during injection molding, and provides molded articles with excellent heat resistance, impact resistance, and material recyclability, while reducing warpage, which is a defect in the appearance of the molded articles. [Means for solving the problem]

[0010] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems and have found that a resin composition comprising a specific polycarbonate resin and a specific ethylene-based resin in a specific ratio imparts sufficient melt fluidity during injection molding, and provides molded articles with excellent heat resistance, impact resistance, and material recyclability, while reducing warpage, which is a defect in the appearance of the molded articles, and have thus completed the present invention.

[0011] That is, the respective aspects of the present invention are as follows [1] to

[13] . [1] A resin composition comprising 100 parts by mass of a polycarbonate resin (A) and 1 to 10 parts by mass of an ethylene-based resin (B), wherein the polycarbonate resin (A) has a melt volume flow rate of 5 to 14 cm3 measured at 300°C under a load of 1.2 kg in accordance with JIS K 7210. 3 / g polycarbonate resin, and the ethylene polymer (B) is an ethylene polymer having a melt mass flow rate of 50 to 10,000 g / 10 min measured at 190°C under a load of 2,160 g in accordance with JIS K6924-1. [2] The polycarbonate resin composition according to [1], wherein the polycarbonate resin (A) is a recycled polycarbonate resin. [3] The polycarbonate resin composition according to [1] or [2], which is for injection molding. [4] An injection molding comprising the polycarbonate resin composition according to [1] or [2]. Effect of the Invention

[0012] The polycarbonate resin composition of the present invention is excellent in the effect of imparting sufficient melt fluidity during injection molding and the effect of reducing defects in the appearance of the obtained molded product while ensuring the heat resistance and impact resistance, which are the advantages of polycarbonate. Furthermore, it is also excellent in material recyclability due to the improved durability. Therefore, it is useful for producing injection molded products of polycarbonate resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below.

[0014] The polycarbonate resin composition according to one embodiment of the present invention has a melt volume flow rate of 5 to 14 cm3 measured at 300°C under a load of 1.2 kg in accordance with JIS K 7210. 3 The composition contains 1 to 10 parts by mass of an ethylene polymer (B) having a melt mass flow rate of 50 to 10,000 g / 10 min, measured at 190°C under a load of 2,160 g in accordance with JIS K6924-1, per 100 parts by mass of polycarbonate resin (A) of 100% by mass or less and a viscosity of 100 / g. The composition imparts sufficient melt fluidity during injection molding, and the molded article is excellent in heat resistance, impact resistance, and material recyclability, while reducing warpage, which is a defect in the appearance of the molded article.

[0015] The polycarbonate resin (A) is generally a polymer in which dihydroxy compound residues are linked by carbonate bonds, and typically includes a polymer obtained by reacting a dihydroxy component with a carbonate precursor by interfacial polymerization or melt polymerization.

[0016] The dihydroxy compounds in this case include 2,2-bis(4-hydroxyphenyl)propane (sometimes called bisphenol A), 2,2-bis((4-hydroxy-3-methyl)phenyl)propane (sometimes called bisphenol C), bis(4-hydroxyphenyl)methane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)-3-methylbutane, 2,2-bis(4-hydroxyphenyl)-3,3-dimethylbutane, 2,2- Examples include bis(4-hydroxyphenyl)-4-methylpentane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 9,9-bis((4-hydroxy-3-methyl)phenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, α,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene, isosorbide, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, etc. These may be used alone or in combination to form a polycarbonate resin, and it is preferable to use one containing 2,2-bis(4-hydroxyphenyl)propane, since this is a polycarbonate resin that has an excellent balance between heat resistance and impact resistance.

[0017] Examples of carbonate precursors include carbonyl halides, carbonyl esters, and haloformates, and specific examples thereof include phosgene, diphenyl carbonate, dihaloformates of dihydric phenols, diphenyl carbonate, dimethyl carbonate, and diethyl carbonate.

[0018] Furthermore, the polycarbonate resin (A) may have a branched structure, and examples of the branching agent include 1,1,1-tris(4-hydroxyphenyl)ethane, α,α',α''-tris(4-hydroxyphenyl)-1,3,5-triisopropylbenzene, phloroglycine, trimellitic acid, and isatin bis(o-cresol).

[0019] The polycarbonate resin (A) has a melt volume flow rate of 5 to 14 cm3 measured at 300°C under a load of 1.2 kg in accordance with JIS K 7210. 3 / g, and any commercially available product that falls within this category may be used, for example, (trade name) Toughlon #2000 (manufactured by Idemitsu Kosan Co., Ltd.), (trade name) Toughlon #2200 (manufactured by Idemitsu Kosan Co., Ltd.), (trade name) Panlite L-1250Y (manufactured by TEIJIN Co., Ltd.), (trade name) Panlite L-1225Y (manufactured by TEIJIN Co., Ltd.), etc. 3 If the viscosity is less than 14 cm / g, the resulting composition will have a high viscosity and will be poor in melt flowability and moldability, and will also be prone to deterioration due to the excessive heat history required for recycling, resulting in poor recyclability. 3 If the molecular weight exceeds 1 / g, not only will the molecular weight be low and the impact resistance will be poor, but the polymer will also be susceptible to thermal degradation during recycling.

[0020] The polycarbonate resin (A) may be an unused virgin resin or a recycled resin obtained by recovering used molded bodies. That is, the polycarbonate resin (A) may be an unused virgin resin, at least one of the one or more resins may be a recycled resin, or all of the one or more resins may be a recycled resin.

[0021] When using recycled resin, polycarbonate resin (A) may contain multiple types of resin. In this case, it may contain organic impurities such as wax, adhesives, plasticizers, and antioxidants. On the other hand, it may contain inorganic impurities such as fillers.

[0022] The ethylene resin (B) does not contain any polar functional group, and examples thereof include an ethylene polymer or a polyethylene wax. As a result, the highly polar polycarbonate resin and the non-polar ethylene resin are incompatible, and when injection molding is performed, the interface between the polycarbonate resin and the ethylene resin slides, resulting in improved melt flowability of the polycarbonate resin composition. In addition, the ethylene resin is a resin that is less prone to oxidative degradation and decomposition even in high-temperature molding above the melting temperature of the polycarbonate resin, and has durability. As a result, even when the ethylene resin is blended during material recycling using waste polycarbonate resin as a raw material, the polycarbonate resin composition is less prone to oxidative degradation and decomposition and has excellent material recyclability.

[0023] Examples of the ethylene polymer include high-pressure low-density polyethylene, high-density polyethylene, and linear low-density polyethylene.

[0024] The high-pressure low-density polyethylene may be a commercially available product. Here, the high-pressure method refers to a method of radically polymerizing ethylene under high temperature and high pressure. It is generally known that the high-pressure radical polymerization of ethylene results in low-density polyethylene with a dendritic structure (a structure having both long-chain branches and short-chain branches), which has a different structure from linear low-density polyethylene (a structure having only short-chain branches), such as linear low-density polyethylene.

[0025] The high density polyethylene may be a commercially available product. The high density polyethylene may be produced by the following method. For example, it may be produced by a slurry method, a solution method, a gas phase method, or the like. When producing the high density polyethylene, a Ziegler catalyst consisting of a solid catalyst component containing magnesium and titanium and an organoaluminum compound, a metallocene catalyst consisting of an organotransition metal compound containing a cyclopentadienyl derivative and a compound and / or an organometallic compound that reacts with the cyclopentadienyl derivative to form an ionic complex, a vanadium catalyst, or the like may be used, and the high density polyethylene may be produced by homopolymerizing ethylene or copolymerizing ethylene and an α-olefin using the catalyst. The α-olefin may be one generally called an α-olefin, and is preferably an α-olefin having 3 to 12 carbon atoms, such as propylene, butene-1, hexene-1, octene-1, or 4-methyl-1-pentene. Examples of the copolymer of ethylene and an α-olefin include an ethylene-hexene-1 copolymer, an ethylene-butene-1 copolymer, and an ethylene-octene-1 copolymer.

[0026] The linear low-density polyethylene may be a commercially available product. The linear low-density polyethylene may be produced by the following method. For example, it may be produced by a high-pressure method, a solution method, a gas-phase method, or the like. When producing the linear low-density polyethylene, a Ziegler catalyst consisting of a solid catalyst component containing magnesium and titanium and an organoaluminum compound, a metallocene catalyst consisting of an organic transition metal compound containing a cyclopentadienyl derivative and a compound and / or an organic metal compound that reacts with the compound to form an ionic complex, a vanadium catalyst, or the like may be used, and the linear low-density polyethylene may be produced by copolymerizing ethylene and an α-olefin with the catalyst. The α-olefin may be one generally called an α-olefin, and is preferably an α-olefin having 3 to 12 carbon atoms, such as propylene, butene-1, hexene-1, octene-1, or 4-methyl-1-pentene. Examples of the copolymer of ethylene and an α-olefin include an ethylene-hexene-1 copolymer, an ethylene-butene-1 copolymer, and an ethylene-octene-1 copolymer.

[0027] The polyethylene wax may be a commercially available product. The polyethylene wax may be produced by the following methods. For example, it may be produced by pyrolysis of an ethylene polymer or by direct polymerization of ethylene. Suitable production methods include a free radical process in which ethylene is reacted under high pressure and high temperature to form a wax having some branching, and a metallocene catalyst comprising an organometallic compound and a Ziegler catalyst comprising a solid catalyst component containing magnesium and titanium and an organoaluminum compound to polymerize ethylene and / or a higher 1-olefin into a branched or branched wax.

[0028] The ethylene resin (B) has a melt mass flow rate (hereinafter sometimes referred to as MFR) of 50 to 10,000 g / 10 min, measured at 190° C. and a load of 2,160 g according to JIS K 6924-1, and preferably 100 to 10,000 g / 10 min, since it is particularly excellent in balance of impact resistance, moldability, and recyclability. If the MFR is less than 50 g / 10 min, the effect of improving the melt fluidity is insufficient. On the other hand, if it exceeds 10,000 g / 10 min, the mechanical properties such as impact resistance and heat resistance of the resulting molded article will be significantly deteriorated.

[0029] The polycarbonate resin composition contains 1 to 10 parts by mass of ethylene-based resin (B) per 100 parts by mass of polycarbonate resin (A), and preferably contains 1 part by mass or more and 5 parts by mass or less, since it has an excellent balance of impact resistance, moldability, and recyclability. Here, if the ethylene-based resin (B) is less than 1 part by mass, the effect of improving the flowability and the appearance of the molded product becomes insufficient. On the other hand, if it exceeds 10 parts by mass, the impact resistance and heat resistance become deteriorated.

[0030] The polycarbonate resin composition can be molded into various molded articles by injection molding, injection compression molding, extrusion molding, blow molding, press molding, vacuum molding, foam molding, or the like.

[0031] Preferably, the polycarbonate resin composition is used to produce a pellet-shaped molding material by the melt kneading molding method, and then the pellets are used to produce an injection molded product in injection molding or injection compression molding, where melt flowability, heat resistance, impact resistance, and molded appearance are the most important. The molding temperature is usually appropriately selected within the range of 240 to 320°C according to the melting point of the polycarbonate resin.

[0032] The polycarbonate resin composition is useful as a molding material for molded articles that become parts for electric / electronic devices, precision machinery-related devices, office equipment, home appliances, optical materials, and the like.

[0033] The injection-molded article, which is one embodiment of the present invention, can be obtained by injecting the above-mentioned polycarbonate resin composition. Examples of the injection-molded article include office automation equipment such as copiers, fax machines, televisions, radios, tape recorders, video decks, personal computers, printers, telephones, information terminals, refrigerators, and microwave ovens, home appliances, housings and various parts of electric and electronic devices, and optical lenses used in cameras, etc. EXAMPLES

[0034] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these. (1) Preparation of test specimens Using an injection molding machine MD100Xi2.7 (manufactured by Ube Industries Machinery Co., Ltd.), the following test pieces were molded using a JIS family mold at a resin temperature of 280°C, a mold temperature of 80°C, an injection speed of 40 mm / s, and a holding pressure of 20 MPa. (2) Injection pressure (unit: MPa) Ten test pieces were molded under the above conditions, and the average injection pressure was recorded as an index of melt fluidity. (3) Izod impact strength (unit: kJ / m 2 ) Measurements were performed using notched rectangular test pieces measuring 64 mm x 12.7 mm x 4 mm in accordance with JIS K7110-1984 "Izod impact test method for hard plastics." The measurement temperature was 23°C. (4) Deflection temperature under load Using a rectangular test piece of 120 mm x 12.7 mm x 4 mm, measurements were performed at a test load of 0.45 MPa in accordance with JIS K7207-1995 "Test method for deflection temperature under load of rigid plastics." (5) Amount of warping The test pieces obtained using the family mold were evaluated for the amount of warpage. The amount of warpage here means the linear distance between the sprue lock at the end of the sprue and the plane when the four gate vertices of the family mold are fixed on a plane.

[0035] Example 1 Polycarbonate resin (A) with a melt volume flow rate of 12 cm 3 A polycarbonate resin (A-1) (manufactured by Idemitsu Kosan Co., Ltd., product name Toughlon A2200) having a melt mass flow rate of 8990 g / 10 min (temperature 300° C., load 1.2 kg) was dried at 100° C. for 5 hours, and then 100 parts by mass of a low-density polyethylene wax (B-1) (manufactured by Sanyo Chemical Industries, Ltd., product name Sunwax 161P) having a melt mass flow rate of 8990 g / 10 min (temperature 190° C., load 2.16 kg) was blended with the ethylene-based resin (B) as 100 parts by mass. The mixture was pre-blended in a tumbler mixer, and then melt-kneaded at 250° C. using a single-screw extruder to obtain pellets of a polycarbonate resin composition.

[0036] The obtained polycarbonate resin composition pellets were dried at 100° C. for 5 hours, and then an injection-molded article was obtained by the above-mentioned method for preparing a test piece. The results of evaluation using the injection-molded article are shown in Table 1.

[0037] Example 2 Except for using 5.0 parts by mass of low-density polyethylene wax (B-1) per 100 parts by mass of polycarbonate resin (A-1) instead of 1 part by mass of low-density polyethylene wax (B-1) per 100 parts by mass of polycarbonate resin (A-1), pellets of the polycarbonate resin composition and its injection-molded product were obtained in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0038] Example 3 A pellet of a polycarbonate resin composition and an injection-molded product thereof were obtained in the same manner as in Example 2, except that a low-density polyethylene (B-2) (manufactured by Tosoh Corporation, product name Petrothene 353) having a melt mass-flow rate of 145 g / 10 min (temperature 190° C., load 2.16 kg) was used as the ethylene-based resin (B) instead of the low-density polyethylene wax (B-1). The evaluation results are shown in Table 1.

[0039] Example 4 As the polycarbonate resin (A), recycled resin (A-2) obtained by the following procedure, which is a crushed product of a polycarbonate molded body, was used, and as the ethylene-based resin (B), 2.0 parts by mass of low-density polyethylene wax (B-1) and 3.0 parts by mass of low-density polyethylene (B-2) were used instead of 1.0 part by mass of low-density polyethylene wax (B-1). Except for this, pellets of the polycarbonate resin composition and its injection-molded product were obtained in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0040] Polycarbonate resin (A-1) was dried at 100°C for 5 hours, and then an injection molded article was obtained by the method described in the preparation of the test piece above. The obtained injection molded article was left in a room with an average temperature of 20°C for one year, and then crushed with a rotary cutter to obtain recycled resin (A-2) of polycarbonate resin (A-1).

[0041] Example 5 A pellet of a polycarbonate resin composition and an injection-molded product thereof were obtained in the same manner as in Example 2, except that a high-density polyethylene wax (B-3) (manufactured by Mitsui Chemicals, Inc., trade name: Sanwax 161P) having a melt mass-flow rate of 9000 g / 10 min (temperature: 190° C., load: 2.16 kg) was used as the ethylene-based resin (B) instead of the low-density polyethylene wax (B-1). The evaluation results are shown in Table 1.

[0042] Example 6 Except for using the recycled resin (A-2) as the polycarbonate resin (A), pellets of a polycarbonate resin composition and an injection-molded article thereof were obtained in the same manner as in Example 2. The evaluation results are shown in Table 1.

[0043] Polycarbonate resin (A-1) was dried at 100°C for 5 hours, and then an injection molded article was obtained by the method described in the preparation of the test piece above. The obtained injection molded article was left in a room with an average temperature of 20°C for one year, and then crushed with a rotary cutter to obtain recycled resin (A-2) of polycarbonate resin (A-1).

[0044] Example 7 Except for using high density polyethylene wax (B-3) instead of low density polyethylene wax (B-1) as the ethylene resin (B), pellets of a polycarbonate resin composition and an injection molded article thereof were obtained in the same manner as in Example 6. The evaluation results are shown in Table 1.

[0045] [Table 1]

[0046] Comparative Example 1 Except for not using the ethylene-based resin (B), pellets and an injection-molded article were obtained in the same manner as in Example 1. The evaluation results are shown in Table 2.

[0047] Comparative Example 2 Except for using 20.0 parts by mass of low-density polyethylene wax (B-1) instead of 1.0 part by mass of low-density polyethylene wax (B-1) as the ethylene-based resin (B), pellets of a polycarbonate resin composition and an injection-molded article thereof were obtained in the same manner as in Example 1. The evaluation results are shown in Table 2.

[0048] Comparative Example 3 Except for using 0.5 parts by mass of low-density polyethylene wax (B-1) instead of 1.0 part by mass of low-density polyethylene wax (B-1) as the ethylene-based resin (B), pellets of a polycarbonate resin composition and an injection-molded product thereof were obtained in the same manner as in Example 1. The evaluation results are shown in Table 2.

[0049] Comparative Example 4 Except for using 5.0 parts by mass of low-density polyethylene wax (B-4) (manufactured by Sanyo Chemical Industries, Ltd., product name: Sanwax 171P) having a melt mass-flow rate exceeding 10,000 g / 10 min (temperature 190° C., load 2.16 kg) instead of 1.0 part by mass of low-density polyethylene wax (B-1) as the ethylene-based resin (B), pellets of a polycarbonate resin composition and an injection-molded product thereof were obtained in the same manner as in Example 1. The evaluation results are shown in Table 2.

[0050] Comparative Example 5 As the polycarbonate resin (A), recycled resin (A-2) was used, and as the ethylene-based resin (B), 5.0 parts by mass of low-density polyethylene (B-5) (manufactured by Tosoh Corporation, product name Petrothene 212) having a melt mass flow rate of 13 g / 10 min (temperature 190 ° C., load 2.16 kg) was used instead of 1.0 part by mass of low-density polyethylene wax (B-1). Except for this, pellets of the polycarbonate resin composition and its injection molded product were obtained in the same manner as in Example 1. The evaluation results are shown in Table 2.

[0051] Comparative Example 6 A polycarbonate resin composition pellet and its injection molded product were obtained in the same manner as in Example 1, except that recycled resin (A-2) was used as polycarbonate resin (A) and 5.0 parts by mass of high-density polyethylene (B-6) (manufactured by Tosoh Corporation, product name Nipolonhard 1200) having a melt mass flow rate of 20 g / 10 min (temperature 190 ° C., load 2.16 kg) was used as ethylene-based resin (B) instead of 1.0 part by mass of low-density polyethylene wax (B-1). The evaluation results are shown in Table 2.

[0052] Comparative Example 7 Instead of ethylene resin (B), it has excellent compatibility with polycarbonate (A) and has a melt volume flow rate of 150 cm 3 Polycarbonate resin pellets and injection-molded articles thereof were obtained in the same manner as in Example 1, except that 5.0 mass of polycarbonate (A-3) (trade name: Toughlon LC1202PURE, manufactured by Idemitsu Kosan Co., Ltd.) was used, which was 0.15 g / 10 min (temperature 300° C., load 1.2 kg). The evaluation results are shown in Table 2.

[0053] Comparative Example 8 Except for using recycled resin (A-2) as polycarbonate resin (A) without using ethylene-based resin (B), polycarbonate resin pellets and its injection-molded product were obtained in the same manner as in Example 1. The evaluation results are shown in Table 2.

[0054] [Table 2] [Industrial Applicability]

[0055] The polycarbonate resin composition of the present invention is excellent in the effect of imparting sufficient melt fluidity during injection molding processing while maintaining the heat resistance and impact resistance that are characteristic of polycarbonate, reducing the appearance defects of the obtained molded product, and further, has excellent material recyclability due to improved durability. Therefore, it is useful as a molding material for molded products that become parts for electric / electronic related devices, precision machinery related devices, office equipment, home appliances, optical materials, etc.

Claims

1. The resin composition contains 100 parts by mass of a polycarbonate resin (A) and 1 to 10 parts by mass of an ethylene-based resin (B), and the polycarbonate resin (A) has a melt volume flow rate of 5 to 14 cm3 measured at 300°C under a load of 1.2 kg in accordance with JIS K 7210. 3 / g polycarbonate resin, and the ethylene polymer (B) is an ethylene polymer having a melt mass flow rate of 50 to 10,000 g / 10 min, measured at 190°C under a load of 2,160 g in accordance with JIS K6924-1.

2. 2. The polycarbonate resin composition according to claim 1, wherein the polycarbonate resin (A) is a recycled polycarbonate resin.

3. The polycarbonate resin composition according to claim 1 or 2, which is for injection molding.

4. An injection-molded article comprising the polycarbonate resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Polycarbonate resin composition and molded product

    JP2008037965A

  • Polycarbonate resin composition for molding

    JP2021195453A

  • PE wax-containing copolycarbonate compositions with improved processability.

    JP6682534B2