Photocurable resin composition, dry film, and cured product
The photocurable resin composition balances high transparency and adhesion to base materials by using a specific blend of carboxyl group-containing resin, photopolymerization initiator, and polyfunctional (meth)acrylate, addressing the challenge of achieving both properties in existing technologies.
Patent Information
- Application Number
- JP2023074063
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Existing photocurable resin compositions struggle to balance high transparency with adhesion to base materials, particularly those with less uneven surfaces, making it difficult to achieve both resolution and adhesion simultaneously.
A photocurable resin composition comprising a carboxyl group-containing resin, a photopolymerization initiator, and a polyfunctional (meth)acrylate compound, with specific ratios of residues derived from epoxy group-containing (meth)acrylate and ethylenically unsaturated compounds, ensuring high transparency and adhesion to base materials.
The composition achieves high transparency with a light transmittance of 85% or more in the 450-800 nm range and maintains adhesion to base materials, even on surfaces with minimal irregularities, while ensuring resolution and resistance to external stimuli.
Smart Images

Figure 2024158676000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a photocurable resin composition, a dry film, and a cured product thereof. In particular, the present disclosure relates to a photocurable resin composition, a dry film made from the photocurable resin composition, and a cured product of the photocurable resin composition. [Background technology]
[0002] Patent Document 1 discloses a curable resin composition containing an acid group-containing (meth)acrylate resin and a photopolymerization initiator. It is described that the acid group-containing (meth)acrylate contains, as essential raw materials, a (meth)acrylic copolymer (A), a compound (B) having a polymerizable unsaturated group, and a polybasic acid anhydride (C). The copolymer (A) is a copolymer containing, as essential raw materials, a methacrylate compound (a1) having an aromatic ring, and a compound (a2) having a reactive functional group and a polymerizable unsaturated group other than the compound (a1). The compound (B) has a functional group that can react with the copolymer (A) and the reactive functional group derived from the compound (a2) of the copolymer (A), and has a polymerizable unsaturated group other than the compound (a1) and the compound (a2). A cured product having high reflectivity and excellent heat yellowing resistance is produced from this curable resin composition. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2021 / 220922 Summary of the Invention [Problem to be solved by the invention]
[0004] According to the inventors' own research, it was found that it is difficult to simultaneously ensure the resolution of a resin composition, impart transparency to the cured product, and impart adhesion to a base material with minimal unevenness.
[0005] An object of the present disclosure is to provide a photocurable resin composition, a dry film, and a cured product that can ensure resolution and maintain high transparency of the cured product while having adhesion to an undercoat material. [Means for solving the problem]
[0006] The photocurable resin composition according to one embodiment of the present disclosure contains a carboxyl group-containing resin (A), a photopolymerization initiator (B), and a polyfunctional (meth)acrylate compound (C). The carboxyl group-containing resin (A) is a reaction product of an intermediate reaction product of a copolymer of an epoxy group-containing (meth)acrylate compound (a1) and an ethylenically unsaturated compound (a2) other than the epoxy group-containing (meth)acrylate compound (a1) and a carboxylic acid (a3) having an ethylenically unsaturated group, and a polybasic acid anhydride (a4). The ratio of the residues derived from the epoxy group-containing (meth)acrylate compound (a1) to the total residues constituting the carboxyl group-containing resin (A) is 40 mol% or more and less than 100 mol%, and the ratio of the residues derived from the ethylenically unsaturated compound (a2) is more than 0 mol% and 60 mol% or less. When a cured product having a thickness of 10 μm is produced from the photocurable resin composition, the cured product has a light transmittance of 85% or more in a wavelength range of 450 nm or more and 800 nm or less.
[0007] A dry film according to one embodiment of the present disclosure includes a dried or semi-cured product of the photocurable resin composition.
[0008] A cured product according to one embodiment of the present disclosure is a cured product of the photocurable resin composition. Effect of the Invention
[0009] According to the present disclosure, a photocurable resin composition, a dry film, and a cured product can be obtained that can ensure resolution and maintain high transparency of the cured product while having adhesion to an undercoat material. [Brief description of the drawings]
[0010] [Figure 1]1A to 1C are cross-sectional views showing an outline of a laminate according to one embodiment of the present invention. [Diagram 2] 2A to 2D are cross-sectional views each showing an outline of a laminate according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] 1. Overview The photocurable resin composition of the present embodiment will be outlined below. In this disclosure, including the following description, "(meth)acrylic" means at least one of "acrylic" and "methacrylic". For example, (meth)acrylate means at least one of acrylate and methacrylate.
[0012] The photocurable resin composition according to the present embodiment contains a carboxyl group-containing resin (A), a photopolymerization initiator (B), and a polyfunctional (meth)acrylate compound (C). The carboxyl group-containing resin (A) is a reaction product of an intermediate reaction product of a copolymer of an epoxy group-containing (meth)acrylate compound (a1) and an ethylenically unsaturated compound (a2) other than the compound (a1) and a carboxylic acid (a3) having an ethylenically unsaturated group, and a polybasic acid anhydride (a4). The ratio of the residues derived from the epoxy group-containing (meth)acrylate compound (a1) to the total residues constituting the carboxyl group-containing resin (A) is 40 mol% or more and less than 100 mol%, and the ratio of the residues derived from the ethylenically unsaturated compound (a2) is more than 0 mol% and 60 mol% or less. When a cured product having a thickness dimension of 10 μm is produced from the photocurable resin composition, the light transmittance of the cured product in the wavelength range of 450 nm to 800 nm is 85% or more. As a result, the photocurable resin composition of this embodiment can ensure resolution and provide adhesion to an undercoat while maintaining high transparency of the cured product.
[0013] Specifically, the carboxyl group-containing resin (A) is a product in which a polybasic acid anhydride (a4) is further added to an intermediate reaction product in which a carboxylic acid (a3) having an ethylenically unsaturated group is added to a specific copolymer. Here, the epoxy group-containing (meth)acrylic compound (a1) and the ethylenically unsaturated compound (a2) are blended in a specific ratio, so that the epoxy group-containing (meth)acrylic compound (a1) and the ethylenically unsaturated compound (a2) have a specific molar ratio of residues that are structural units derived from the ethylenically unsaturated compound (a2) relative to the total residues of the carboxyl group-containing resin (A), and therefore the alkali resistance of the photocurable resin composition is particularly easy to increase. As a result, even if the UV-cured portion of the photocurable resin composition is subjected to an alkali development treatment, the surface is not easily roughened and can easily maintain smoothness, so that light scattering is unlikely to occur and good low haze is easily achieved. In this case, the transparency of the cured product of the photocurable resin composition can be improved. Furthermore, the carboxyl group-containing resin (A) is a product of the intermediate reaction product in which a part or all of the carboxylic acid (a3) having an ethylenically unsaturated group is added to a copolymer having structural units derived from a monomer in the above-mentioned specific ratio, and a polybasic acid anhydride (a4) is further added to the intermediate reaction product, and since the intermediate reaction product has a carboxyl group that can be generated by this reaction, it can contribute to improving the resolution of the photocurable resin composition. Furthermore, since the photocurable resin composition of this embodiment contains the above-mentioned specific carboxyl group-containing resin (A), it can have high adhesion. Note that, in this disclosure, adhesion means the degree of adhesion between the object (e.g., base material) to which the photocurable resin composition is applied, and the film or cured product, but in the photocurable resin composition of this embodiment, when a copper sputtered film is used as the base material, adhesion to the copper sputtered film can be particularly increased. The copper sputtered film can be prepared, for example, by the method of the Examples below (see "(4-6) Adhesion 2 (Adhesion to copper sputtered film)"), and is a metallic base material with almost no unevenness on its surface. Normally, it is often difficult for a resin composition or a cured product thereof to improve adhesion to a surface without unevenness compared to a surface with unevenness (for example, a surface roughened after copper plating), but the photocurable resin composition of this embodiment makes it easy to improve adhesion even when the surface is almost free of unevenness.Of course, the photocurable resin composition of this embodiment also exhibits excellent adhesion when a film (such as a polyethylene terephthalate film) is used as a base material.
[0014] Furthermore, in this embodiment, when a cured product having a thickness of 10 μm is produced from the photocurable resin composition, the light transmittance of the cured product in the wavelength range of 450 nm to 800 nm is 85% or more, so that the cured product produced from the photocurable resin composition has high transparency. In particular, the photocurable resin composition of this embodiment has excellent transparency even after treatment with an alkaline solution.
[0015] The photocurable resin composition of this embodiment can be particularly suitably used to prepare a dry film having a thickness of 10 μm or less and transparency, and a cured product having a thickness of 10 μm or less and transparency, for example. However, there is no limitation in that a cured product having a thickness other than 10 μm can be prepared from the photocurable resin composition of this embodiment.
[0016] 2.Details The photocurable resin composition according to this embodiment will be specifically described below.
[0017] [Photocurable resin composition] The photocurable resin composition of this embodiment contains a carboxyl group-containing resin (A), a photopolymerization initiator (B), and a polyfunctional (meth)acrylate compound (C). The carboxyl group-containing resin (A) is a reaction product of an intermediate reaction product of a copolymer of an epoxy group-containing (meth)acrylate compound (a1) and an ethylenically unsaturated compound (a2) other than the epoxy group-containing (meth)acrylate compound (a1) and a carboxylic acid (a3) having an ethylenically unsaturated group, and a polybasic acid anhydride (a4). In the carboxyl group-containing resin (A), the ratio of the residues derived from the epoxy group-containing (meth)acrylate compound (a1) to the total residues constituting the carboxyl group-containing resin (A) is 40 mol% or more and less than 100 mol%, and the ratio of the residues derived from the ethylenically unsaturated compound (a2) is more than 0 mol% and 60 mol% or less. As a result, the carboxyl group-containing resin (A) can impart excellent resolution to the photocurable resin composition, and high transparency and adhesion of the cured product.
[0018] When a cured product having a thickness of 10 μm is produced from the photocurable resin composition, the light transmittance of the cured product in the wavelength range of 450 nm to 800 nm is 85% or more. Therefore, the cured product of the photocurable resin composition has high transparency. Furthermore, according to the photocurable resin composition of this embodiment, the haze of the cured product is also easily reduced. Regarding the transparency of the cured product, when the resin composition is cured, the transparency immediately after curing can often be ensured, but it may be difficult to maintain the transparency due to external stimuli (effects of treatment agents such as resolution liquid and resist liquid, environmental effects such as light and heat, etc.) or deterioration over time. In contrast, according to the photocurable resin composition of this embodiment, the light resistance is excellent and the haze can be suppressed to a low level. Therefore, high transparency can be better maintained even if there are external stimuli, etc.
[0019] Components that may be contained in the photocurable resin composition according to this embodiment will be described in detail.
[0020] <Carboxyl group-containing resin> The carboxyl group-containing resin (A) is a compound having at least one carboxyl group in one molecule, which allows the photocurable resin composition to be developed well with an alkaline solution.
[0021] As described above, the carboxyl group-containing resin (A) of this embodiment is a reaction product of an intermediate reaction product of a copolymer of an epoxy group-containing (meth)acrylate compound (a1) and an ethylenically unsaturated compound (a2) with a carboxylic acid (a3) having an ethylenically unsaturated group, and a polybasic acid anhydride (a4). That is, the carboxyl group-containing resin (A) is synthesized by reacting a copolymer obtained by polymerizing the epoxy group-containing (meth)acrylate compound (a1) and the ethylenically unsaturated compound (a2) with a carboxylic acid (a3) having an ethylenically unsaturated group, and then reacting the intermediate reaction product obtained thereby with a polybasic acid anhydride (a4).
[0022] The carboxyl group-containing resin (A) of this embodiment preferably has at least one ethylenically unsaturated group in one molecule, which can contribute to improving photocurability.
[0023] The synthesis of the carboxyl group-containing resin (A) will be specifically described below. In the following description, the copolymer of the epoxy group-containing (meth)acrylate compound (a1) and the ethylenically unsaturated compound (a2) will be referred to as "copolymer (X)", the intermediate reaction product of the copolymer (copolymer (X)) and the carboxylic acid (a3) having an ethylenically unsaturated group will be referred to as "product (Y)", and the reaction product of the intermediate reaction product (product (Y)) and the polybasic acid anhydride (a4) will be referred to as "product (Z)".
[0024] (copolymer) The copolymer (X) is a polymer obtained by a polymerization reaction between an epoxy group-containing (meth)acrylate compound (a1) and an ethylenically unsaturated compound (a2).
[0025] The epoxy group-containing (meth)acrylate compound (a1) is a compound having at least one epoxy group and at least one (meth)acryloyl group in one molecule. Therefore, the epoxy group-containing (meth)acrylate compound (a1) can be said to be a bifunctional or higher compound. The epoxy group includes, for example, a glycidyl ether group. It is preferable that the epoxy group-containing (meth)acrylate compound (a1) has at least one glycidyl ether group and at least one (meth)acryloyl group in one molecule.
[0026] The epoxy group-containing (meth)acrylate compound (a1) may be, for example, at least one compound selected from the group consisting of glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, 3,4-epoxycyclohexyl (meth)acrylate, vinyl glycidyl ether, and diglycidyl bisphenol A di(meth)acrylate. The epoxy group-containing (meth)acrylate compound (a1) is preferably glycidyl (meth)acrylate. In this case, it is easy to obtain a good copolymer (X), and it is easy to further improve the photocurability of the photocurable resin composition. Therefore, it is easy to realize good light resistance and low haze of the cured product of the photocurable resin composition.
[0027] The ethylenically unsaturated compound (a2) is a compound having at least one ethylenically unsaturated group in one molecule. The ethylenically unsaturated compound (a2) is also a component that can be copolymerized with the epoxy group-containing (meth)acrylic compound (a1). However, the ethylenically unsaturated compound (a2) is a compound having an ethylenically unsaturated group other than the epoxy group-containing (meth)acrylate compound (a1). Therefore, the compound contained in the epoxy group-containing (meth)acrylate compound (a1) is not an ethylenically unsaturated compound (a2).
[0028] Examples of the ethylenically unsaturated compound (a2) include at least one compound (monomer) selected from the group consisting of methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, styrene, α-methylstyrene, o-, m-, and p-methylstyrene, o-, m-, and p-chlorostyrene, vinylnaphthalene, propene, butene, vinylcyclohexane, (meth)acrylonitrile, α-chloro(meth)acrylonitrile, α-ethyl(meth)acrylonitrile, vinylidene cyanide, maleimide, N-alkylmaleimide, and N-phenylmaleimide.
[0029] In copolymerization, the ethylenically unsaturated compound (a2) can be polymerized with the epoxy group-containing (meth)acrylate compound (a1) by using at least one compound (monomer) that can be included in the above. Therefore, the ethylenically unsaturated compound (a2) may be synthesized by polymerizing two or more of the compounds that can be included in the above with the epoxy group-containing (meth)acrylate compound (a1) to synthesize the copolymer (X).
[0030] The copolymer (X) can be obtained, for example, by mixing an epoxy group-containing (meth)acrylate compound (a1) and an ethylenically unsaturated compound (a2) with an appropriate solvent and a polymerization initiator (e.g., a radical polymerization initiator) and heating the mixture. In this embodiment, when synthesizing the copolymer (X), it is preferable to polymerize the epoxy group-containing (meth)acrylate compound (a) at a ratio of 40 mol% or more and less than 100 mol%, and the ethylenically unsaturated compound (a2) at a ratio of more than 0 mol% and 60 mol% or less, based on the total moles of the residues constituting the copolymer (X) obtained. When synthesizing the copolymer (X), the ratio of the epoxy group-containing (meth)acrylate compound (a) to the total moles of the residues constituting the copolymer (X) is more preferably 50 mol% or more, and even more preferably 55 mol% or more. The ratio of the epoxy group-containing (meth)acrylate compound (a) to the total moles of the copolymer (X) is more preferably 90 mol% or less, and even more preferably 80 mol% or less.
[0031] In the polymerization reaction between the epoxy group-containing (meth)acrylate compound (a1) and the ethylenically unsaturated compound (a2), the ethylenically unsaturated bond of the epoxy group-containing (meth)acrylate compound (a1) and the ethylenically unsaturated compound (a2) are linked to generate a copolymer (X). The polymerization reaction between the epoxy group-containing (meth)acrylate compound (a1) and the ethylenically unsaturated compound (a2) proceeds via their respective ethylenically unsaturated bonds, so that the copolymer (X) has a plurality of epoxy groups (at least two or more).
[0032] (Intermediate reaction products) The intermediate reaction product (product (Y)) is a product obtained by reacting the above-mentioned copolymer (X) with a carboxylic acid (a3) having an ethylenically unsaturated group. The product (Y) can be said to be a kind of intermediate in the carboxyl group-containing resin (A). Therefore, the product (Y) has a residue derived from the copolymer (X), that is, a residue derived from the epoxy group-containing (meth)acrylate compound (a1) and a residue derived from the ethylenically unsaturated compound (a2).
[0033] Examples of the carboxylic acid (a3) having an ethylenically unsaturated group include at least one compound selected from the group consisting of (meth)acrylic acid, ω-carboxy-polycaprolactone (n≈2) monoacrylate, crotonic acid, cinnamic acid, 2-acryloyloxyethyl succinic acid, 2-methacryloyloxyethyl succinic acid, 2-acryloyloxyethyl phthalic acid, 2-methacryloyloxyethyl phthalic acid, 2-acryloyloxypropyl phthalic acid, 2-methacryloyloxypropyl phthalic acid, 2-acryloyloxyethyl maleic acid, 2-methacryloyloxyethyl maleic acid, β-carboxyethyl acrylate, 2-acryloyloxyethyl tetrahydrophthalic acid, 2-methacryloyloxyethyl tetrahydrophthalic acid, 2-acryloyloxyethyl hexahydrophthalic acid, and 2-methacryloyloxyethyl hexahydrophthalic acid. Among these, the carboxylic acid (a3) having an ethylenically unsaturated group is preferably (meth)acrylic acid.
[0034] The product (Y) is synthesized, for example, as follows.
[0035] The product (Y) produced by reacting the copolymer (X) with the carboxylic acid (a3) having an ethylenically unsaturated group contains a product (Y1) produced by reacting a carboxyl group in the carboxylic acid (a3) having an ethylenically unsaturated group with each of two epoxy groups among the multiple epoxy groups in the copolymer (X). This product (Y1) has a secondary hydroxyl group generated by the reaction of the epoxy group with the carboxyl group and an ethylenically unsaturated group derived from the carboxylic acid (a3) having an ethylenically unsaturated group. The product (Y) may also contain a product (Y2) produced by reacting a carboxyl group in the carboxylic acid (a3) having an ethylenically unsaturated group with only one of the two epoxy groups in the copolymer (X). The product (Y2) has a secondary hydroxyl group, an ethylenically unsaturated group, and an epoxy group. The product (Y) may also contain unreacted copolymer (X). That is, the product (Y) may contain a component having an epoxy group, and this component may include at least one of the product (Y2) and the copolymer (X).
[0036] When reacting the copolymer (X) with the carboxylic acid (a3) having an ethylenically unsaturated group, an appropriate method can be adopted. For example, the carboxylic acid (a3) having an ethylenically unsaturated group is added to a solution containing the copolymer (X) and a solvent, and a polymerization inhibitor and a catalyst are added as necessary, followed by stirring and mixing to obtain a reactive solution. The reactive solution is reacted by an appropriate method at a temperature of preferably 60°C to 150°C, particularly preferably 80°C to 120°C, to obtain the product (Y). The solvent in this case can contain at least one component selected from the group consisting of ketones such as methyl ethyl ketone and cyclohexanone, aromatic hydrocarbons such as toluene and xylene, acetate esters such as ethyl acetate, butyl acetate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, and propylene glycol monomethyl ether acetate, and dialkyl glycol ethers. The polymerization inhibitor includes at least one hydroquinone-based polymerization inhibitor selected from the group consisting of, for example, hydroquinone, hydroquinone monomethyl ether, methylhydroquinone, methoquinone, etc. The catalyst can contain at least one component selected from the group consisting of, for example, tertiary amines such as benzyldimethylamine and triethylamine, quaternary ammonium salts such as trimethylbenzylammonium chloride and methyltriethylammonium chloride, triphenylphosphine, and triphenylstibine.
[0037] The catalyst preferably contains triphenylphosphine. That is, it is preferable to react the copolymer (X) with the (meth)acrylic acid (a3) in the presence of triphenylphosphine. In this case, the ring-opening addition reaction between the epoxy group in the copolymer (X) and the carboxylic acid (a3) having an ethylenically unsaturated group is particularly likely to be promoted, and a reaction rate (conversion rate) of 95% or more, 97% or more, or nearly 100% can be achieved.
[0038] When reacting the copolymer (X) with the carboxylic acid (a3) having an ethylenically unsaturated group, the carboxylic acid equivalent of the carboxylic acid (a3) having an ethylenically unsaturated group to 1 mole of the epoxy group of the copolymer (X) is preferably 0.7 equivalents or more and 1.2 equivalents or less. When reacted at this equivalent ratio, the carboxyl group-containing resin (A) can impart excellent photosensitivity and storage stability to the photocurable resin composition. The carboxylic acid equivalent of the carboxylic acid (a3) having an ethylenically unsaturated group to 1 mole of the epoxy group of the copolymer (X) is more preferably 0.9 equivalents or more. In addition, the carboxylic acid equivalent of the carboxylic acid (a3) having an ethylenically unsaturated group to 1 mole of the epoxy group of the copolymer (X) is more preferably 1.1 equivalents or less.
[0039] The product (Y) thus obtained may have a hydroxyl group produced by the reaction between the epoxy group of the copolymer (X) and the carboxyl group of the carboxylic acid (a3) having an ethylenically unsaturated group.
[0040] (Reaction Products) The reaction product (product (Z)) is a product obtained by reacting the above product (Y) with the polybasic acid anhydride (a4). Therefore, the product (Z) has a residue derived from the product (Y), i.e., a residue derived from the copolymer (X), in other words, a residue derived from the epoxy group-containing (meth)acrylate compound (a1) and a residue derived from the ethylenically unsaturated compound (a2).
[0041] The polybasic acid anhydride (a4) contains at least one of an acid monoanhydride (a41) and an acid dianhydride (a42).
[0042] The acid monoanhydride (a41) is a compound having one acid anhydride group. The acid monoanhydride (a41) may contain, for example, an anhydride of a dicarboxylic acid. The acid monoanhydride (a41) may contain, for example, at least one compound selected from the group consisting of phthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, succinic anhydride, methylsuccinic anhydride, maleic anhydride, citraconic anhydride, glutaric anhydride, cyclohexane-1,2,4-tricarboxylic-1,2-anhydride, and itaconic anhydride. The polybasic acid anhydride (a4) preferably has a cyclohexane skeleton. In this case, it is easy to improve the transparency of the cured product of the photocurable resin composition, and in particular, it is easy to improve the light resistance of the cured product. In the present disclosure, light resistance particularly refers to the degree of resistance to light, and can be evaluated by the method described in the Examples below.
[0043] The acid monoanhydride (a41) preferably contains either one or both of hexahydrophthalic anhydride and cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride. By checking the residue of the polybasic acid anhydride (a4) in the carboxyl group-containing resin (A), it can be confirmed whether the acid monoanhydride (a41) has a cyclohexane skeleton. The residue of the polybasic acid anhydride (a4) in the carboxyl group-containing resin (A) can be quantitatively confirmed by performing a composite component analysis using nuclear magnetic resonance, gas chromatography mass spectrometry, infrared absorption spectroscopy, etc.
[0044] The acid dianhydride (a42) is a compound having two acid anhydride groups. The acid dianhydride (a42) may contain, for example, an anhydride of a tetracarboxylic acid. The acid dianhydride (a42) may contain at least one compound selected from the group consisting of, for example, 1,2,4,5-benzenetetracarboxylic dianhydride, benzophenone tetracarboxylic dianhydride, methylcyclohexene tetracarboxylic dianhydride, naphthalene-1,4,5,8-tetracarboxylic dianhydride, ethylene tetracarboxylic dianhydride, 9,9'-bis(3,4-dicarboxyphenyl)fluorene dianhydride, glycerin bisanhydrotrimellitate monoacetate, ethylene glycol bisanhydrotrimellitate, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-c]furan-1,3-dione, 1,2,3,4-butane tetracarboxylic dianhydride, and 3,3',4,4'-biphenyl tetracarboxylic dianhydride. In the case where the acid dianhydride (a42) has a cyclohexane skeleton, it is possible to confirm whether or not the acid dianhydride (a41) has a cyclohexane skeleton by checking the residue of the polybasic acid anhydride (a4) in the carboxyl group-containing resin (A), in the same manner as in the case of the above-mentioned acid monoanhydride (a41).
[0045] The product (Z) can be synthesized, for example, as follows.
[0046] When reacting the product (Y) with the polybasic acid anhydride (a4), an appropriate method can be adopted. For example, the polybasic acid anhydride (a4) is added to a solvent solution of the product (Y), and a polymerization inhibitor and a catalyst are added as necessary, followed by stirring and mixing to obtain a reactive solution. The reactive solution is reacted by a conventional method at a temperature preferably from 60°C to 150°C, particularly preferably from 70°C to 120°C, to obtain the product (Z). As the solvent, catalyst, and polymerization inhibitor, appropriate ones can be used, and the solvent, catalyst, and polymerization inhibitor used in the synthesis of the product (Y) can also be used as they are.
[0047] The catalyst preferably contains triphenylphosphine. That is, it is preferable to react the product (Y) with the polybasic acid anhydride (a4) in the presence of triphenylphosphine. In this case, the reaction between the secondary hydroxyl group in the product (Y) and the polybasic acid anhydride (a4) is particularly promoted, and a reaction rate (conversion rate) of 90% or more, 95% or more, 97% or more, or nearly 100% can be achieved.
[0048] When the polybasic acid anhydride (a4) contains an acid dianhydride (a42), the reaction product (Z) produced by the reaction of the product (Y) with the polybasic acid anhydride (a4) may contain a component (Z1) produced by the reaction of the product (Y) with the acid dianhydride (a42). The component (Z1) may have a carboxyl group derived from the acid dianhydride (a42). In addition, since a crosslinking reaction may occur due to the acid dianhydride (a42), the component (Z1) is likely to have a molecular weight distribution.
[0049] When the polybasic acid anhydride (a4) contains an acid monoanhydride (a41), the reaction product (Z) produced by reacting the product (Y) with the polybasic acid anhydride (a4) may contain a component (Z2) produced by reacting the product (Y) with the acid monoanhydride (a41). The component (Z2) has a carboxyl group derived from the acid monoanhydride (a41).
[0050] In addition, when the polybasic acid anhydride (a4) contains an acid dianhydride (a42) and an acid monoanhydride (a41), it may contain a component (Z1) generated by the reaction of the product (Y) with the acid dianhydride (a42), and a component (Z2) generated by the reaction of the product (Y) with the acid monoanhydride (a41). Specifically, a part of the secondary hydroxyl groups in the product (Y) is reacted with the acid dianhydride (a42), and another part of the secondary hydroxyl groups in the product (Y) is reacted with the acid monoanhydride (a41). As a result, the product (Z) may contain a component (Z1) having a structure having a residue of a carboxylic acid (a3) having an ethylenically unsaturated group, a residue of the acid dianhydride (a42), and a carboxyl group, and a component (Z2) having a structure having a residue of a carboxylic acid (a3) having an ethylenically unsaturated group, a residue of the acid monoanhydride (a41), and a carboxyl group.
[0051] The product (Z) may contain a component (Z3) having a structure obtained by reacting only one of the two acid anhydride groups in the acid dianhydride (a42) with a secondary hydroxyl group in the product (Y). The component (Z3) may contain a residue of a carboxylic acid (a3) having an ethylenically unsaturated group and a residue of the acid dianhydride (a42).
[0052] Furthermore, the product (Z) may also contain unreacted product (Y), and therefore the product (Z) may have an epoxy group.
[0053] As described above, when the acid dianhydride (a42) is contained, the molecular weight of the product (Z) depends on the number of crosslinks by the acid dianhydride (a42), so the product (Z) can have an appropriate molecular weight distribution by optimizing the reaction conditions during synthesis. The reaction conditions include controlling the amount of the acid monoanhydride (a41) and the acid dianhydride (a42), and the amount of the acid monoanhydride (a41) relative to the acid dianhydride (a42). This makes it easy to obtain the product (Z) having the desired molecular weight and polydispersity, i.e., the carboxyl group-containing resin (A).
[0054] When the polybasic acid anhydride (a4) contains an acid dianhydride (a42), the amount of the acid dianhydride (a42) is preferably 0.01 mol or more and 0.24 mol or less per 1 mol of the epoxy group of the copolymer (X). In this case, a carboxyl group-containing resin (A) with an appropriately adjusted acid value and molecular weight can be easily obtained. The amount of the acid dianhydride (a42) is more preferably 0.04 mol or more and 0.22 mol or less.
[0055] When the polybasic acid anhydride (a4) contains an acid monoanhydride (a41), the amount of the acid monoanhydride (a41) is preferably 0.05 mol or more and 0.8 mol or less per mol of the epoxy group of the copolymer (X). In this case, a carboxyl group-containing resin (A) having an appropriately adjusted acid value and molecular weight can be easily obtained.
[0056] It is also preferred to react the product (Y) with the polybasic acid anhydride (a4) under air bubbling, which can particularly improve the developability of the photocurable resin composition with an alkaline aqueous solution by suppressing excessive increase in the molecular weight of the resulting carboxyl group-containing resin (A).
[0057] The carboxyl group-containing resin (A) has photoreactivity due to the ethylenically unsaturated group derived from the (meth)acrylic acid (a3). Therefore, the carboxyl group-containing resin (A) can impart photosensitivity (specifically, UV curability) to the photocurable resin composition. In addition, the carboxyl group-containing resin (A) has a carboxyl group derived from the polybasic acid anhydride (a4), and can impart developability with an alkaline aqueous solution containing at least one of an alkali metal salt and an alkali metal hydroxide to the photocurable resin composition. Furthermore, when the polybasic acid anhydride (a4) contains an acid dianhydride (a42), the molecular weight of the carboxyl group-containing resin (A) can depend on the number of crosslinks by the acid dianhydride (a42). Therefore, the acid value and molecular weight of the carboxyl group-containing resin (A) can be appropriately adjusted. When the polybasic acid anhydride (a4) contains an acid dianhydride (a42), a carboxyl group-containing resin (A) having a desired molecular weight and acid value can be easily obtained by controlling the amount of the acid dianhydride (a42).
[0058] The product (Z) thus obtained, i.e., the carboxyl group-containing resin (A), has a ratio of the residues derived from the epoxy group-containing (meth)acrylate compound (a1) to the total residues constituting the carboxyl group-containing resin (A) of 40 mol% or more and less than 100 mol%, and the ratio of the residues derived from the ethylenically unsaturated compound (a2) is more than 0 mol% and 60 mol% or less. In the present disclosure, the ratio of the residues derived from the epoxy group-containing (meth)acrylate compound (a1) and the ratio of the residues derived from the ethylenically unsaturated compound (a2) to the total residues constituting the carboxyl group-containing resin (A) can be confirmed, for example, by quantifying the respective ratios of the structural units derived from the epoxy group-containing (meth)acrylate compound (a1) and the structural units derived from the ethylenically unsaturated compound (a2) based on the mass spectrometry (e.g., GC-MS method) of the carboxyl group-containing resin (A) to calculate the molar ratio to the total amount of the carboxyl group-containing resin (A).
[0059] The weight average molecular weight of the carboxyl group-containing resin (A) is preferably 4000 or more and 50000 or less. In this case, the developability of the photocurable resin composition with an alkaline aqueous solution is easily improved. The weight average molecular weight is more preferably 5000 or more, and even more preferably 6000 or more. The weight average molecular weight is more preferably 35000 or less, and even more preferably 20000 or less.
[0060] The weight average molecular weight of the carboxyl group-containing resin (A) is calculated from the results of molecular weight measurement by gel permeation chromatography. The molecular weight measurement by gel permeation chromatography can be carried out, for example, under the following conditions. GPC equipment: Showa Denko SHODEX SYSTEM 11, Column: SHODEX KF-800P, KF-005, KF-003, KF-001, 4 columns in series, Mobile phase: THF, Flow rate: 1mL / min, Column temperature: 45°C, Detector: RI, Conversion: Polystyrene.
[0061] The acid value of the carboxyl group-containing resin (A) is preferably 40 mgKOH / g or more and 140 mgKOH / g or less. In this case, the resolution of the cured product produced from the photocurable resin composition is particularly improved. The acid value of the carboxyl group-containing resin (A) is more preferably 45 mgKOH / g or more, even more preferably 55 mgKOH / g or more, and particularly preferably 65 mgKOH / g or more. The acid value of the carboxyl group-containing resin (A) is more preferably 130 mgKOH / g or less, even more preferably 120 mgKOH / g or less, and particularly preferably 110 mgKOH / g or less.
[0062] As long as the above is satisfied, the carboxyl group-containing resin (A) may have a bisphenolfluorene skeleton. When the carboxyl group-containing resin (A) has a bisphenolfluorene skeleton, the resolution of the photocurable resin composition is easily improved. In addition, when the carboxyl group-containing resin (A) has a bisphenolfluorene skeleton, the physical properties of the cured product produced from the photocurable resin composition are easily improved.
[0063] <Photopolymerization initiator> The photopolymerization initiator (B) is a component that can improve the photosensitivity of the photocurable resin composition. The photopolymerization initiator (B) may contain at least one selected from the group consisting of, for example, an acylphosphine oxide-based photopolymerization initiator (B1), an oxime ester-based photopolymerization initiator (B2), and an α-aminoalkylphenone-based photopolymerization initiator (B3). In this case, when the photocurable resin composition is exposed to light such as ultraviolet light, high photosensitivity can be imparted to the photocurable resin composition. The photopolymerization initiator (B) preferably contains either one or both of an acylphosphine oxide-based photopolymerization initiator (B1) and an oxime ester-based photopolymerization initiator (B2). In this case, high photosensitivity can be imparted to the photocurable resin composition, the degree of coloring of the cured product can be reduced, and the high transparency of the cured product of the curable resin composition can be more easily maintained. In addition, when the photopolymerization initiator (B) contains an acylphosphine oxide-based photopolymerization initiator (B1), the photopolymerization initiator (B) is likely to increase the deep curing property of the photocurable resin composition, so that the cured product of the photocurable resin composition is likely to be cured well. It is more preferable that the photopolymerization initiator (B) contains both an acylphosphine oxide-based photopolymerization initiator (B1) and an oxime ester-based photopolymerization initiator (B2). In this case, the photocurable resin composition can be given higher photosensitivity, the degree of coloring of the cured product can be reduced, and the high transparency of the cured product of the photocurable resin composition can be more easily maintained. In addition, when the photopolymerization initiator (B) contains an oxime ester-based photopolymerization initiator (B2), the adhesion and light resistance of the cured product of the photocurable resin composition can be well balanced and well maintained.
[0064] Examples of the acylphosphine oxide photopolymerization initiator (B1) include monoacylphosphine oxide photopolymerization initiators such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and 2,4,6-trimethylbenzoyl-ethyl-phenyl-phosphinate, as well as bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, and bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide. The photopolymerization initiator may contain at least one component selected from the group consisting of bisacylphosphine oxide-based photopolymerization initiators such as sphingoside oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and (2,5,6-trimethylbenzoyl)-2,4,4-trimethylpentylphosphine oxide.
[0065] The oxime ester photopolymerization initiator (B2) may contain at least one component selected from the group consisting of, for example, 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], and ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime). Specific examples of commercially available oxime ester photopolymerization initiators include, for example, Irgacure OXE01, OXE02, OXE03, and OXE04 manufactured by BASF Japan Ltd., and ADEKA Arcreuse N-1919T, NCI-831E, NCI-930, and NCI-730 manufactured by ADEKA Corporation.
[0066] The α-aminoalkylphenone photopolymerization initiator (B3) may contain at least one component selected from the group consisting of, for example, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone.
[0067] The photopolymerization initiator (B) may contain a photopolymerization initiator other than those mentioned above.
[0068] The photocurable resin composition may further contain an appropriate photopolymerization accelerator, a sensitizer, etc. For example, the photocurable resin composition may contain hydroxyketones such as 1-hydroxy-cyclohexyl-phenyl-ketone, phenylglyoxylic acid methyl ester, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, and 2-hydroxy-2-methyl-1-phenyl-propan-1-one; benzoin and its alkyl ethers; acetophenones such as acetophenone and benzyl dimethyl ketal; anthraquinones such as 2-methylanthraquinone; 2,4-dimethyl The photocurable resin composition may contain at least one component selected from the group consisting of thioxanthones such as thioxanthone, 2,4-diethylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, and 2,4-diisopropylthioxanthone; benzophenone, 4-benzoyl-4'-methyldiphenylsulfide, and bis(diethylamino)benzophenone; xanthones such as 2,4-diisopropylxanthone; and α-hydroxyketones such as 2-hydroxy-2-methyl-1-phenyl-propan-1-one; and compounds containing nitrogen atoms such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone. The photocurable resin composition may contain, together with the photopolymerization initiator (B), appropriate photopolymerization accelerators and sensitizers such as tertiary amines such as p-dimethylbenzoic acid ethyl ester, p-dimethylaminobenzoic acid isoamyl ester, and 2-dimethylaminoethyl benzoate. The photocurable resin composition may contain at least one of a photopolymerization initiator for visible light exposure and a photopolymerization initiator for near-infrared light exposure, if necessary. The photosensitive adhesive composition may contain, together with the photopolymerization initiator (B), a coumarin derivative such as 7-diethylamino-4-methylcoumarin, which is a sensitizer for laser exposure, a carbocyanine dye, a xanthene dye, or the like.
[0069] The content of the photopolymerization initiator (B) relative to 100 parts by mass of the carboxyl group-containing resin (A) is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1.0 parts by mass or more. When it is within the above range, it is possible to ensure higher curability of the photocurable resin composition and maintain the transparency of the cured product. The preferred upper limit of the content is 40 parts by mass or less.
[0070] When the photopolymerization initiator (B) contains an acylphosphine oxide-based photopolymerization initiator (B1), the mass ratio of the acylphosphine oxide-based photopolymerization initiator (B1) to the total amount of the photopolymerization initiator (B) is preferably 10 mass % or more and 100 mass % or less.
[0071] When the photopolymerization initiator (B) contains an oxime ester photopolymerization initiator (B2), the mass ratio of the oxime ester photopolymerization initiator (B2) to the total amount of the photopolymerization initiator (B) is preferably 1 mass % or more and 50 mass % or less.
[0072] <Polyfunctional (meth)acrylate compound> The polyfunctional (meth)acrylate compound (C) is a compound having two or more (meth)acryloyl groups in one molecule. In this case, the resolution is particularly improved when a film (dried film, dry film) made from the photocurable resin composition is exposed to light and developed, and the developability of the photocurable resin composition with an alkaline aqueous solution is particularly improved. The polyfunctional (meth)acrylate compound (C) may overlap with the epoxy group-containing (meth)acrylate compound (a1) or the ethylenically unsaturated compound (a2) described in the above-mentioned carboxyl group-containing resin (A).
[0073] The polyfunctional (meth)acrylate compound (C) can impart photocurability to the photocurable resin composition in the presence of the photopolymerization initiator (B). If the polyfunctional (meth)acrylate compound (C) has two or more (meth)acryloyl groups in one molecule, it is preferable that the polyfunctional (meth)acrylate compound (C) contains at least one selected from the group consisting of photopolymerizable monomers and photopolymerizable prepolymers. The photopolymerizable monomer may contain at least one compound selected from the group consisting of, for example, diethylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ε-caprolactone-modified pentaerythritol hexaacrylate, tricyclodecane dimethanol di(meth)acrylate, and 1,9-nonanediol di(meth)acrylate.
[0074] The photopolymerizable prepolymer may contain at least one compound selected from the group consisting of prepolymers obtained by polymerizing a monomer having an ethylenically unsaturated bond and then adding an ethylenically unsaturated group, and oligo(meth)acrylate prepolymers.
[0075] The polyfunctional (meth)acrylate compound (C) preferably contains a bifunctional (meth)acrylate compound (C1). The bifunctional (meth)acrylate compound (C1) is a compound having two (meth)acryloyl groups in one molecule. In this case, it is easy to achieve low haze while maintaining good resolution and adhesion of the cured product of the photocurable resin composition. The polyfunctional (meth)acrylate compound (C) may contain a trifunctional or higher (meth)acrylate compound.
[0076] The amount of the polyfunctional (meth)acrylate compound (C) per 100 parts by mass of the carboxyl group-containing resin (A) is preferably 1 part by mass or more and 60 parts by mass or less. The amount of the polyfunctional (meth)acrylate compound (C) per 100 parts by mass of the carboxyl group-containing resin (A) is more preferably 5 parts by mass or more, and even more preferably 15 parts by mass or more. The amount of the polyfunctional (meth)acrylate compound (C) per 100 parts by mass of the carboxyl group-containing resin (A) is more preferably 55 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 40 parts by mass or less.
[0077] <Carboxyl group-containing epoxy (meth)acrylate compound> The photocurable resin composition of the present embodiment preferably further contains a carboxyl group-containing epoxy (meth)acrylate compound (D). In the present disclosure, the carboxyl group-containing epoxy (meth)acrylate compound (D) is a compound having an aromatic ring and not having a novolac skeleton. More specifically, the carboxyl group-containing epoxy (meth)acrylate compound (D) has at least one carboxyl group, one epoxy group, one (meth)acryloyl group, and one aromatic ring in one molecule, but does not have a novolac skeleton. When the photocurable resin composition contains the carboxyl group-containing epoxy (meth)acrylate compound (D) in addition to the carboxyl group-containing resin (A), the cured product of the photocurable resin composition can achieve excellent physical properties such as high heat resistance and insulation reliability. As described above, the carboxyl group-containing epoxy (meth)acrylate compound (D) can be said to be a carboxyl group-containing resin, but is a carboxyl group-containing resin that is not included in the above-mentioned carboxyl group-containing resin (A).
[0078] The carboxyl group-containing epoxy (meth)acrylate compound (D) can be obtained, for example, as follows.
[0079] The carboxyl group-containing epoxy (meth)acrylate compound (D) contains, for example, a resin that is a reaction product between a polymer of an ethylenically unsaturated monomer containing an ethylenically unsaturated compound having a carboxyl group and an ethylenically unsaturated compound having an epoxy group. This ethylenically unsaturated compound may further contain an ethylenically unsaturated compound that does not have a carboxyl group. The carboxyl group-containing epoxy (meth)acrylate compound (D) is obtained by reacting an ethylenically unsaturated compound having an epoxy group with a part of the carboxyl group in the polymer. The ethylenically unsaturated compound having a carboxyl group contains, for example, compounds such as (meth)acrylic acid, ω-carboxy-polycaprolactone (n≒2) monoacrylate, pentaerythritol triacrylate, and pentaerythritol trimethacrylate. Examples of the ethylenically unsaturated compound having no carboxyl group include 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, linear or branched aliphatic or alicyclic (which may have some unsaturated bonds in the ring) (meth)acrylic acid esters, etc. The ethylenically unsaturated compound having a carboxyl group may overlap with the carboxylic acid (a3) having an ethylenically unsaturated group described above.
[0080] The carboxyl group-containing epoxy (meth)acrylate compound (D) preferably has a bisphenolfluorene skeleton. In this case, the carboxyl group-containing epoxy (meth)acrylate compound (D) is likely to absorb light in the wavelength range of 300 to 330 nm, so the resolution of the cured product produced from the photocurable resin composition can be further improved. In addition, when the carboxyl group-containing epoxy (meth)acrylate compound (D) has a bisphenolfluorene skeleton, it has a bulky structure, so that the diffusion of the generated radical species in the photocurable resin composition can be prevented, and even when exposed to light not having a wavelength range of 300 to 330 nm, the resolution of the cured product produced from the photocurable resin composition can be improved.
[0081] The carboxyl group-containing epoxy (meth)acrylate compound (D) is, for example, a reaction product of a polybasic acid anhydride and a product generated by reacting an epoxy compound having a bisphenol fluorene skeleton represented by the following formula (1) with a carboxylic acid having an ethylenically unsaturated group. That is, the carboxyl group-containing epoxy (meth)acrylate compound (D) is synthesized by reacting an epoxy compound having a bisphenol fluorene skeleton represented by the following formula (1) with a carboxylic acid having an ethylenically unsaturated group, and then reacting the product obtained by the reaction with a polybasic acid anhydride.
[0082] [ka]
[0083] Each of R1 to R8 in formula (1) may be hydrogen, an alkyl group having 1 to 5 carbon atoms, or a halogen. This is because even if hydrogen in the aromatic ring is replaced with a low-molecular-weight alkyl group or a halogen, there is no adverse effect on the physical properties of the carboxyl group-containing epoxy (meth)acrylate compound (D), and rather, the heat resistance or flame retardancy of the cured product of the photocurable resin composition containing the carboxyl group-containing epoxy (meth)acrylate compound (D) may be improved.
[0084] The ethylenically unsaturated compound having an epoxy group used to obtain the carboxyl group-containing epoxy (meth)acrylate compound (D) having a bisphenolfluorene skeleton may have a structure shown in the following formula (2), for example. In formula (2), n is, for example, an integer in the range of 0 to 20. In order to appropriately control the molecular weight of the carboxyl group-containing epoxy (meth)acrylate compound (D), it is particularly preferable that the average of n is in the range of 0 to 1. If the average of n is in the range of 0 to 1, even when the acid anhydride (a3) contains an acid dianhydride, excessive increase in molecular weight is easily suppressed. In addition, in formula (2), R1 to R8 are each independently hydrogen, an alkyl group having 1 to 5 carbon atoms, or a halogen.
[0085] [ka]
[0086] When the photocurable resin composition contains a carboxyl group-containing epoxy (meth)acrylate compound (D), the amount of the carboxyl group-containing epoxy (meth)acrylate compound (D) relative to the total amount of the carboxyl group-containing resin (A) and the carboxyl group-containing epoxy (meth)acrylate compound (D) is preferably 20 mass % or more and 80 mass % or less.
[0087] The photocurable resin composition may further contain a resin having a carboxyl group other than the above-mentioned carboxyl group-containing resin (A) and carboxyl group-containing epoxy (meth)acrylate compound (D). Examples of the resin having a carboxyl group other than the carboxyl group-containing resin (A) and carboxyl group-containing epoxy (meth)acrylate compound (D) include compounds having a novolac skeleton that are not included in the carboxyl group-containing resin (A).
[0088] (Other Ingredients) In this embodiment, the photocurable resin composition may contain a colorant, but preferably does not contain a colorant. Usually, when preparing a thin film from a resin composition, a colorant may be blended into the resin composition to compensate for the decrease in resolution, but in this case, the transparency may decrease due to the influence of the colorant. Conversely, if the colorant is not included, the transparency is expected to be improved, but in the case of a thin film, the resolution may be insufficient. In contrast, in this embodiment, even if a colorant is not blended, even when a thin film is prepared from the photocurable resin composition, the cured product can have particularly high transparency without impairing the resolution.
[0089] The colorant includes color pigments and dyes. The colorant may include coloring components of colors such as white colorants and colorants other than white (e.g., black, blue, red, green, yellow, etc.). An example of a white colorant is titanium oxide. When the colorant is a white colorant, the ratio of the white colorant to the total solid content of the photocurable resin composition is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1% by mass or less, and particularly preferably 0.5% by mass or less. When the colorant is other than a white colorant, the ratio of the colorant other than the white colorant to the total solid content of the photocurable resin composition is preferably 0.3% by mass or less, more preferably 0.1% by mass or less, even more preferably 0.05% by mass or less, and particularly preferably 0.01% by mass or less. In the present disclosure, the term "total solid content of the photocurable resin composition" refers to the total amount of components obtained by excluding the amount of volatile components from the total components that may be included in the photocurable resin composition. Volatile components are components that volatilize during the process of heating the photocurable resin composition to produce a dried product, or during the process of irradiating the composition with light to produce a cured product, and do not constitute the dried product, semi-cured product, or cured product, such as solvents.
[0090] The photocurable resin composition may contain an inorganic filler, but preferably does not contain an inorganic filler. When the photocurable resin composition does not contain an inorganic filler, the photocurable resin composition, as well as the dry film and cured product produced from the photocurable resin composition, can achieve higher transparency. When the photocurable resin composition contains an inorganic filler, the ratio of the inorganic filler to the total solid content of the photocurable resin composition is preferably 15% by mass or less. If the ratio of the inorganic filler to the total solid content of the photocurable resin composition is 15% by mass or less, good transparency of the photocurable resin composition and the cured product produced from the photocurable resin composition can be ensured. In addition, in this case, excessive increase in haze of the cured product of the photocurable resin composition can be prevented. The ratio of the inorganic filler to the total solid content of the photocurable resin composition is more preferably 10% by mass or less, even more preferably 5% by mass or less, and particularly preferably 1% by mass or less. Examples of the inorganic filler include at least one inorganic component selected from the group consisting of crystalline silica, finely powdered silica, nanosilica, carbon nanotubes, talc, bentonite, aluminum hydroxide, magnesium hydroxide, magnesium oxide, calcium carbonate, hydrotalcite, clay, calcium silicate, mica, barium sulfate, potassium titanate, barium titanate, aluminum nitride, boron nitride, zinc borate, aluminum borate, montmorillonite, and sepiolite.
[0091] The photocurable resin composition may contain a solvent. The solvent may contain at least one compound selected from the group consisting of water, ethanol, isobutanol, 1-butanol, isopropanol, hexanol, ethylene glycol, 3-methyl-3-methoxybutanol, and other linear, branched, secondary, or polyhydric alcohols; ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene and xylene; petroleum-based aromatic mixed solvents such as the Swasol series (manufactured by Maruzen Petrochemical Co., Ltd.) and the Solvesso series (manufactured by Exxon Chemical Co., Ltd.); cellosolves such as cellosolve and butyl cellosolve; carbitols such as carbitol and butyl carbitol; alkylene glycol alkyl ethers such as ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, and propylene glycol methyl ether; polypropylene glycol alkyl ethers such as dipropylene glycol methyl ether; acetate esters such as ethyl acetate, butyl acetate, cellosolve acetate, and carbitol acetate; and dialkyl glycol ethers. The solvent may contain at least one alcohol-based solvent selected from the group consisting of propylene glycol monomethyl ether, ethanol, isobutanol, 1-butanol, isopropanol, hexanol, ethylene glycol, 3-methyl-3-methoxybutanol, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, propylene glycol methyl ether, and polypropylene glycol alkyl ether such as dipropylene glycol methyl ether. That is, the photocurable resin composition may contain an alcohol-based solvent. In this case, when preparing the photocurable resin composition, the coatability and uniformity of the photocurable resin composition can be further improved. In addition, even when a thermoplastic film is used as the substrate, the substrate is less likely to be dissolved, and the substrate is less likely to be damaged. It is more preferable that the solvent contains propylene glycol monomethyl ether. In this case, the coatability and uniformity of the photocurable resin composition can be further improved, and good drying properties can also be obtained. It is more preferable that propylene glycol monomethyl ether is contained in a ratio of 50% by mass or more with respect to the entire solvent.
[0092] The amounts of the components in the photocurable resin composition are appropriately adjusted so that the photocurable resin composition has photocurability and is developable with an alkaline solution.
[0093] Specifically, the amount of the carboxyl group-containing resin (A) relative to the total solid content of the photocurable resin composition is preferably 55% by mass or more, more preferably 60% by mass or more, and even more preferably 65% by mass or more. The amount of the carboxyl group-containing resin (A) relative to the total solid content of the photocurable resin composition is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less.
[0094] The amount of the photopolymerization initiator (B) relative to the total amount of solids in the photocurable resin composition is preferably 0.1 mass % or more, which can further enhance the curability of the photocurable resin composition.
[0095] The amount of the photopolymerization initiator (B) relative to the total solid content of the photocurable resin composition is preferably 0.5% by mass or more, and more preferably 1% by mass or more. The upper limit of the amount of the photopolymerization initiator (B) relative to the total solid content of the photocurable resin composition is not particularly limited, but is preferably 25% by mass or less.
[0096] When the photocurable resin composition contains a solvent, the proportion of the solvent is preferably 15% by mass or more and 95% by mass or less based on the total mass of the photocurable resin composition, which can improve the coatability of the photocurable resin composition when the photocurable resin composition is applied.
[0097] The photocurable resin composition may further contain components other than the components described above, so long as the effects of this embodiment are not impaired.
[0098] The photocurable resin composition may contain at least one component selected from the group consisting of adhesion imparting agents, rheology control agents, surface modifiers, curing accelerators; copolymers of silicone, acrylate, and the like; leveling agents; thixotropic agents; polymerization inhibitors; antihalation agents; flame retardants; antifoaming agents; antioxidants; surfactants; and polymer dispersants.
[0099] The photocurable resin composition of the present embodiment may be prepared by an appropriate method. For example, the photocurable resin composition can be prepared by mixing and stirring the raw materials of the photocurable resin composition. The photocurable resin composition may also be prepared by kneading using an appropriate kneading method using, for example, a three-roll mill, a ball mill, a sand mill, or the like. When the raw materials contain liquid components, low-viscosity components, etc., the raw materials may be kneaded first to prepare a mixture, and then the liquid components, low-viscosity components, etc. may be added to the obtained mixture and mixed to prepare the photocurable resin composition. When the photocurable resin composition contains a solvent, first, a part or all of the solvent may be mixed among the raw materials, and then mixed with the remaining raw materials.
[0100] As described above, when a cured product having a thickness dimension of 10 μm is produced from the photocurable resin composition of this embodiment, the light transmittance of the cured product in the wavelength range of 450 nm to 800 nm is 85% or more. As a result, a highly transparent cured film (transparent cured film) can be obtained from the photocurable resin composition, and the transparent cured film can be particularly suitably used for optical applications. The absorption spectrum of the cured product produced from the photocurable resin composition is measured by a spectroscopic analyzer such as a spectrophotometer. A specific measurement method can be performed in the same manner as in the evaluation test (4-1) of the examples described later. The light transmittance can be obtained by measuring the absorption spectrum of the cured product produced from the photocurable resin composition. When a cured product having a thickness dimension of 10 μm is produced from the photocurable resin composition, the light transmittance in the wavelength range of 450 nm to 800 nm is preferably 90% or more, and more preferably 95% or more. In addition, when the photocurable resin composition of this embodiment is used to prepare a cured product having a thickness of 10 μm, the cured product has a light transmittance of 85% or more in the wavelength range of 450 nm or more and 800 nm or less. Therefore, a cured product having a thickness thinner than 10 μm (i.e., 10 μm or less) naturally has a light transmittance of 85% or more in the above wavelength range.
[0101] The photocurable resin composition of the present embodiment can be suitably used to prepare a protective layer, particularly a transparent protective layer, for protecting the surface of a substrate and electronic components such as a semiconductor element. However, the photocurable resin composition has high transparency, and therefore may be used to prepare an electrically insulating layer for optical applications. Examples of the electrically insulating layer include a solder resist layer, an interlayer insulating layer, and a plating resist layer.
[0102] The photocurable resin composition preferably has such a property that even a film having a thickness of 25 μm can be developed with an aqueous sodium carbonate solution. In this case, since a sufficiently thick electrically insulating layer can be produced from the photocurable resin composition by photolithography, the photocurable resin composition can be widely applied to produce an interlayer insulating layer, a solder resist layer, etc. in a printed wiring board. Of course, as described above, it is also possible to produce a protective layer and an electrically insulating layer having a thickness less than 25 μm, particularly 10 μm or less, from the photocurable resin composition.
[0103] Whether or not a 25 μm-thick film can be developed with an aqueous sodium carbonate solution can be confirmed by the following method. A wet coating film is prepared by applying a photocurable resin composition onto a suitable substrate, and this wet coating film is heated at 80° C. for 40 minutes to form a 25 μm-thick film. A negative mask having an exposed area that transmits ultraviolet light and a non-exposed area that blocks ultraviolet light is directly applied to this film, and 500 mJ / cm2 is applied to the film. 2 The film is exposed to ultraviolet light under the following conditions. After the exposure, a 1% by mass Na2CO3 aqueous solution at 30°C is sprayed onto the film at a spray pressure of 0.2 MPa for 90 seconds, and then pure water is sprayed onto the film at a spray pressure of 0.2 MPa for 90 seconds. When the film is observed after this treatment and the portions of the film corresponding to the non-exposed portions are removed and no residue is found, it can be determined that the 25 μm thick film can be developed with an aqueous sodium carbonate solution. It is also possible to similarly check whether films of other thicknesses (e.g., 30 μm) can be developed with an aqueous sodium carbonate solution.
[0104] [Dry film and cured product] The dry film and the cured product produced from the photocurable resin composition of this embodiment will be specifically described with reference to FIGS. 1A to 1C, with the "dry film" and the "cured product" being designated by reference numerals.
[0105] The dry film 1 of this embodiment is obtained by drying or semi-curing the above-mentioned photocurable resin composition. That is, the dry film 1 is a dried or semi-cured product of the photocurable resin composition. The semi-cured product of the photocurable resin composition refers to a state in which some of the components in the photocurable resin composition are cured but not completely cured.
[0106] The dry film 1 can be produced, for example, as follows.
[0107] First, a supporting substrate (eg, substrate 2) for supporting the photocurable resin composition and the photocurable resin composition are prepared, and the photocurable resin composition is applied onto the substrate 2.
[0108] The substrate 2 may be, for example, a suitable substrate such as glass, plastic, or ceramic. More specifically, the substrate 2 may include a film made of a thermoplastic resin such as polyethylene terephthalate, cycloolefin polymer, liquid crystal polymer, or polycarbonate. The substrate 2 includes a core material 21, which will be described later. That is, the substrate 2 may be a substrate including an insulating layer, and a conductive layer such as a conductor, a conductor wiring, or the like, such as a printed wiring board.
[0109] The coated photocurable resin composition is then dried by heating to form a dry film. Methods for forming a dry film from the photocurable resin composition include, for example, a coating method and a dry film method.
[0110] In the coating method, for example, a photocurable resin composition is coated on a substrate 2 to form a wet coating film. The method for coating the photocurable resin composition is selected from the group consisting of an appropriate method, for example, a dipping method, a spray method, a spin coating method, a roll coating method, a curtain coating method, and a screen printing method. Then, in order to volatilize the organic solvent in the photocurable resin composition, the wet coating film is dried at a temperature in the range of, for example, 60°C to 130°C for an appropriate time, for example, 1 to 80 minutes, thereby obtaining a dry film.
[0111] In the dry film method, a photocurable resin composition is first applied onto a suitable support made of polyester or the like, and then dried to form a dry film 1, which is a dried product of the photocurable resin composition, on the support. This results in a dry film with a support (see laminate 10 shown in FIG. 1A) that includes the dry film 1 and a support that supports the dry film 1. The laminate 10 may be a laminate 101 in which a covering layer (e.g., a cover film 4) is provided on the surface of the dry film 1 opposite to the substrate 2 (see FIG. 1B). The cover film 4 includes at least one selected from the group consisting of, for example, polyethylene terephthalate (PET), biaxially oriented polypropylene (OPP: Oriented Polypropylene), and polyethylene. A release-treated film may be used as the covering layer.
[0112] The semi-cured product of the photocurable resin composition is obtained by partially curing the dried film formed on the substrate 2.
[0113] In this way, the dry film 1 can be produced from the photocurable resin composition. Moreover, according to the above method, a laminate 10 (sometimes referred to as "first laminate 10" to distinguish it from the second laminate described later) including the substrate 2 and the dry film 1 can also be obtained. The first laminate 10 is not limited to the configuration shown in FIG. 1A, and may include, for example, a layer different from the substrate 2 and the dry film 1 between the substrate 2 and the dry film 1. As described above, the semi-cured product of the photocurable resin composition is not limited to being produced on the substrate 2, and can be produced by applying it to an appropriate object, etc.
[0114] The cured product 11 of this embodiment can be produced by curing the above-mentioned photocurable resin composition. The cured product 11 may also be produced by curing the above-mentioned dry film 1. The method of photocuring the photocurable resin composition or the dry film 1 will be described in detail later.
[0115] By such a method, a laminate 20 (sometimes called "second laminate 20" to distinguish it from the first laminate 10 described above) including a substrate 2 and a cured product 11 overlapping the substrate 2 can be produced. The first laminate 10 may be irradiated with light to cure the dry film 1 to form a cured product 11, thereby producing a second laminate 2 (see FIG. 1C). The second laminate 20 includes a cured product 11 derived from a photocurable resin composition, and therefore can be suitably used for optical applications. Therefore, the cured product 11 of the photocurable resin composition of this embodiment can also be called a transparent cured film. The second laminate 10 is not limited to the configuration shown in FIG. 1C, and may further include a layer different from the substrate 2 and the cured product 11 between the substrate 2 and the cured product 11, for example.
[0116] The dry film 1 and the cured product 11 of this embodiment may be produced by methods other than those described above. Specifically, the dry film 1 may be used, for example, as follows to produce a cured product. However, the methods of using the dry film and the cured product are not limited to these.
[0117] To produce a coating (dry film 1) of a photocurable resin composition on a substrate 2, first, a core material 21 is prepared as the substrate 2, as shown in FIG. 2A. The core material 21 includes, for example, at least one insulating layer 200 and at least one conductive layer 3. The conductive layer 3 may be a conductor wiring. The conductive layer 3 provided on one surface of the core material 21 is hereinafter referred to as a first conductor wiring 31.
[0118] 2B, a coating film made of a photocurable resin composition is formed on the surface of the core material 21 on which the first conductor wiring 31 is provided. The dry film 1 can be formed from the photocurable resin composition by, for example, the same method as the above-mentioned coating method and dry film method.
[0119] In the coating method, a photocurable resin composition is coated on a substrate 2 such as a core material 21 to form a wet coating film. The method for coating the photocurable resin composition is selected from the group consisting of, for example, a dipping method, a spray method, a spin coating method, a roll coating method, a curtain coating method, and a screen printing method. Next, when the photocurable resin composition contains an organic solvent, the wet coating film is dried at a temperature in the range of, for example, 60 to 120°C to volatilize the organic solvent, thereby obtaining a dry film 1 (dried coating film).
[0120] In the dry film method, a photocurable resin composition is first applied onto a suitable support (substrate 2) such as polyester, and then dried to form a dry film 1 containing the photocurable resin composition on the support. This results in a dry film with a support that includes the dry film 1 and the support (substrate 2) that supports the dry film 1. The dry film with a support (e.g., laminate 10) may be provided with a covering layer (e.g., cover film 4) that overlaps the surface of the dry film 1 opposite to the substrate 2 (see FIG. 1B).
[0121] The dry film 1 in this dry film with support is overlapped on the core material 21, pressure is applied to the dry film 1 and the core material 21, and then the substrate 2, which is the support, is peeled off from the dry film 1, thereby transferring the dry film 1 from the support onto the core material 21 (see Figures 2C and 2D).
[0122] As a result, the dry film 1 is produced on the core material 21. When the dry film with support includes the cover film 4, the cover film 4 is peeled off from the dry film 1 before the dry film 1 is superimposed on the core material 21, and then the dry film 1 is superimposed on the core material 21, and the dry film 1 is produced in the same manner as described above.
[0123] In this manner, the dry film 1 made of the photocurable resin composition is disposed on the substrate 2 such as the core material 21, and the dry film 1 can be formed on the core material 21 (substrate 2).
[0124] The film made from the photocurable resin composition is exposed to light to cure the film entirely or partially. The film may be a dry film 1 since it contains a dried product of the photocurable resin composition. In this case, when partially exposing the film, for example, a negative mask may be placed on the film and then the film may be irradiated with ultraviolet light. The negative mask has an exposed portion that transmits ultraviolet light and a non-exposed portion that blocks ultraviolet light, and the non-exposed portion is provided at a position where appropriate curing is not required. The negative mask is, for example, a photo tool such as a mask film or a dry plate. The light source of the ultraviolet light is, for example, a chemical lamp, a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a xenon lamp, a metal halide lamp, an LED, a YAG, a g-line (436 nm), an h-line (405 nm), an i-line (365 nm), and a combination of two or more of g-line, h-line, and i-line. The ultraviolet light source is not limited to these, and any light source that can irradiate ultraviolet light capable of curing the photocurable resin composition may be used.
[0125] The exposure method may be a method other than the method using a negative mask. For example, the film may be exposed by a direct writing method in which ultraviolet light emitted from a light source is irradiated only to the portion of the film to be exposed. The light source applied to the direct writing method is selected from the group consisting of, for example, a chemical lamp, a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an extra-high pressure mercury lamp, a xenon lamp, a metal halide lamp, an LED, a YAG, g-line (436 nm), h-line (405 nm), i-line (365 nm), and a combination of two or more of g-line, h-line, and i-line. The light source of the ultraviolet light is not limited to these, and may be any light source that can irradiate ultraviolet light capable of curing the photocurable resin composition.
[0126] In the dry film method, the dry film 1 in the dry film with a support (substrate 2) may be superimposed on another substrate 2 or core material 21, and then the coating made of the dry film 1 may be exposed to ultraviolet light through the support without peeling off the support, and then the support may be peeled off from the dry film 1 before development. In this case, oxygen inhibition during exposure can be more effectively prevented, and curability is improved.
[0127] The film may be subjected to a development treatment to remove the unexposed portions of the film. In the development treatment, an appropriate developer may be used according to the composition of the photocurable resin composition. The developer may be, for example, an alkaline aqueous solution containing at least one of an alkali metal salt and an alkali metal hydroxide, or a solution containing an organic amine. More specifically, the alkaline aqueous solution contains at least one component selected from the group consisting of sodium carbonate, potassium carbonate, ammonium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, sodium hydroxide, potassium hydroxide, ammonium hydroxide, tetramethylammonium hydroxide, and lithium hydroxide. The solvent in the alkaline aqueous solution may be water alone or a mixture of water and a hydrophilic organic solvent such as a lower alcohol. The organic amine contains at least one component selected from the group consisting of monoethanolamine, diethanolamine, triethanolamine, monoisopropanolamine, diisopropanolamine, and triisopropanolamine.
[0128] The developer is preferably an alkaline aqueous solution containing at least one of an alkali metal salt and an alkali metal hydroxide, and is particularly preferably an aqueous sodium carbonate solution, which can improve the working environment and reduce the burden of waste disposal.
[0129] After the development treatment, the coating may be further subjected to either or both of UV irradiation and heat treatment.
[0130] This results in a second laminate 20 having a cured product 11 of the photocurable resin composition on the substrate 2. As described above, the laminate 20 having a cured product 11 of the photocurable resin composition on the core material 21 may be produced.
[0131] In this way, by partially exposing the dry film 1 in the first laminate 10 and then developing it with an alkaline developer to form a pattern, it is possible to produce a cured product 11 (also called a transparent cured film) that overlaps the substrate 2 and has a pattern.
[0132] The thickness of the cured product 11 can be adjusted as appropriate, but can be, for example, 10 μm or less. In this embodiment, the cured product 11 made from the photocurable resin composition has high transparency as described above. And, even if the film made from the photocurable resin composition is made relatively thin (thinned) to, for example, 10 μm or less, the high resolution of the cured product can be realized. Also, if the thickness of the cured product is 10 μm or less, it can be suitably used as, for example, a protective layer. In addition, the photocurable resin composition of this embodiment has a light transmittance of 85% or more in the wavelength range of 450 nm to 800 nm when a cured product having a thickness dimension of 10 μm is made, so that a cured product having a thickness dimension thinner than 10 μm naturally has a light transmittance of 85% or more in the above range.
[0133] In the photocurable resin composition of this embodiment, electrically insulating layers such as plating resist layers, solder resist layers, and interlayer insulating layers can be particularly well formed from the dried product, that is, a dry film, or from a coating of the photocurable resin composition. EXAMPLES
[0134] Specific examples of the present disclosure will be presented below, but the present disclosure is not limited to the examples.
[0135] (1) Synthesis of resin containing carboxyl groups In the following Synthesis Examples A-1 to E-2, resins having carboxyl groups are synthesized, and therefore the resins obtained in each Synthesis Example are referred to as "carboxyl group-containing resins" for convenience. In this disclosure, unless otherwise specified, "parts" and "%" mean "parts by mass" and "% by mass".
[0136] (1-1) Synthesis Example A-1 (Carboxyl Group-Containing Resin A-1) Into a four-neck flask equipped with a reflux condenser, a thermometer, a glass tube for nitrogen replacement, and a stirrer, 60 parts of glycidyl methacrylate, 40 parts of methyl methacrylate, 100 parts of propylene glycol monomethyl ether acetate, and 8 parts of azobisisobutyronitrile were added, and the mixture was heated under a nitrogen stream and polymerized at 95°C for 5 hours to obtain a 50% copolymer solution.
[0137] To the above 50% copolymer solution, 0.1 parts of methoquinone (p-Methoxyphenol), 30.24 parts of acrylic acid, and 1 part of triphenylphosphine were added, and an addition reaction was carried out at 110°C for 24 hours. Subsequently, 31.92 parts of tetrahydrophthalic anhydride and 62.16 parts of propylene glycol monomethyl ether acetate were added, and the mixture was reacted at 80°C for 3 hours while stirring under air bubbling, to obtain a 50% solution of carboxyl group-containing resin A-1 (Mw: 7200, acid value 73 mgKOH / g) having an ethylenically unsaturated group.
[0138] (1-2) Synthesis Example A-2 (Carboxyl Group-Containing Resin A-2) Into a four-neck flask equipped with a reflux condenser, a thermometer, a glass tube for nitrogen replacement, and a stirrer, 60 parts of glycidyl methacrylate, 20 parts of benzyl methacrylate, 20 parts of methyl methacrylate, 100 parts of propylene glycol monomethyl ether acetate, and 8 parts of azobisisobutyronitrile were added, and the mixture was heated under a nitrogen stream and polymerized at 95°C for 5 hours to obtain a 50% copolymer solution.
[0139] To the above 50% copolymer solution, 0.1 parts of methoquinone (p-Methoxyphenol), 30.24 parts of acrylic acid, and 1 part of triphenylphosphine were added, and an addition reaction was carried out at 110°C for 24 hours. Subsequently, 31.92 parts of tetrahydrophthalic anhydride and 62.16 parts of propylene glycol monomethyl ether acetate were added, and the mixture was reacted at 80°C for 3 hours while stirring under air bubbling, to obtain a 50% solution of carboxyl group-containing resin A-2 (Mw: 7400, acid value 73 mgKOH / g) having an ethylenically unsaturated group.
[0140] (1-3) Synthesis Example A-3 (Carboxyl Group-Containing Resin A-3) Into a four-neck flask equipped with a reflux condenser, a thermometer, a glass tube for nitrogen replacement, and a stirrer, 60 parts of glycidyl methacrylate, 20 parts of styrene, 20 parts of methyl methacrylate, 100 parts of propylene glycol monomethyl ether acetate, and 8 parts of azobisisobutyronitrile were added, and the mixture was heated under a nitrogen stream and polymerized at 95°C for 5 hours to obtain a 50% copolymer solution.
[0141] To the above 50% copolymer solution, 0.1 parts of methoquinone (p-Methoxyphenol), 30.24 parts of acrylic acid, and 1 part of triphenylphosphine were added, and an addition reaction was carried out at 110°C for 24 hours. Subsequently, 31.92 parts of tetrahydrophthalic anhydride and 62.16 parts of propylene glycol monomethyl ether acetate were added, and the mixture was reacted at 80°C for 3 hours while stirring under air bubbling, to obtain a 50% solution of carboxyl group-containing resin A-3 (Mw: 7500, acid value 73mgKOH / g) having an ethylenically unsaturated group.
[0142] (1-4) Synthesis Example A-4 (Carboxyl Group-Containing Resin A-4) Into a four-neck flask equipped with a reflux condenser, a thermometer, a glass tube for nitrogen replacement, and a stirrer, 60 parts of glycidyl methacrylate, 20 parts of N-phenylmaleimide, 20 parts of methyl methacrylate, 100 parts of propylene glycol monomethyl ether acetate, and 8 parts of azobisisobutyronitrile were added, and the mixture was heated under a nitrogen stream and polymerized at 95°C for 5 hours to obtain a 50% copolymer solution.
[0143] To the above 50% copolymer solution, 0.1 parts of methoquinone (p-Methoxyphenol), 30.24 parts of acrylic acid, and 1 part of triphenylphosphine were added, and the mixture was subjected to an addition reaction at 110°C for 24 hours. Subsequently, 31.92 parts of tetrahydrophthalic anhydride and 62.16 parts of propylene glycol monomethyl ether acetate were added, and the mixture was reacted at 80°C for 3 hours while stirring under air bubbling, to obtain a 50% solution of carboxyl group-containing resin A-4 (Mw: 7400, acid value 73 mgKOH / g) having an ethylenically unsaturated group.
[0144] (1-5) Synthesis Example A-5 (Carboxyl Group-Containing Resin A-5) Into a four-neck flask equipped with a reflux condenser, a thermometer, a glass tube for nitrogen replacement, and a stirrer, 60 parts of glycidyl methacrylate, 10 parts of N-phenylmaleimide, 20 parts of benzyl methacrylate, 10 parts of methyl methacrylate, 100 parts of propylene glycol monomethyl ether acetate, and 8 parts of azobisisobutyronitrile were added, and the mixture was heated under a nitrogen stream and polymerized at 95°C for 5 hours to obtain a 50% copolymer solution.
[0145] To the above 50% copolymer solution, 0.1 parts of methoquinone (p-Methoxyphenol), 30.24 parts of acrylic acid, and 1 part of triphenylphosphine were added, and an addition reaction was carried out at 110°C for 24 hours. Subsequently, 31.92 parts of tetrahydrophthalic anhydride and 62.16 parts of propylene glycol monomethyl ether acetate were added, and the mixture was reacted at 80°C for 3 hours while stirring under air bubbling, to obtain a 50% solution of carboxyl group-containing resin A-5 (Mw: 7800, acid value 73 mgKOH / g) having an ethylenically unsaturated group.
[0146] (1-6) Synthesis Example A-6 (Carboxyl Group-Containing Resin A-6) Into a four-neck flask equipped with a reflux condenser, a thermometer, a glass tube for nitrogen replacement, and a stirrer, 60 parts of glycidyl methacrylate, 10 parts of N-phenylmaleimide, 20 parts of benzyl methacrylate, 10 parts of methyl methacrylate, 100 parts of propylene glycol monomethyl ether acetate, and 8 parts of azobisisobutyronitrile were added, and the mixture was heated under a nitrogen stream and polymerized at 95°C for 5 hours to obtain a 50% copolymer solution.
[0147] To the above 50% copolymer solution, 0.1 parts of methoquinone (p-Methoxyphenol), 30.24 parts of acrylic acid, and 1 part of triphenylphosphine were added, and the addition reaction was carried out at 110°C for 24 hours. Subsequently, 32.34 parts of hexahydrophthalic anhydride and 62.58 parts of propylene glycol monomethyl ether acetate were added, and the reaction was carried out at 80°C for 3 hours while stirring under air bubbling, to obtain a 50% solution of carboxyl group-containing resin A-6 (Mw: 8000, acid value 73 mgKOH / g) having an ethylenically unsaturated group.
[0148] (1-7) Synthesis Example A-7 (Carboxyl Group-Containing Resin A-7) Into a four-neck flask equipped with a reflux condenser, a thermometer, a glass tube for nitrogen replacement, and a stirrer, 60 parts of glycidyl methacrylate, 10 parts of N-phenylmaleimide, 20 parts of benzyl methacrylate, 10 parts of methyl methacrylate, 100 parts of propylene glycol monomethyl ether acetate, and 8 parts of azobisisobutyronitrile were added, and the mixture was heated under a nitrogen stream and polymerized at 95°C for 5 hours to obtain a 50% copolymer solution.
[0149] To the above 50% copolymer solution, 0.1 parts of methoquinone (p-Methoxyphenol), 30.24 parts of acrylic acid, and 1 part of triphenylphosphine were added, and an addition reaction was carried out at 110°C for 24 hours. Subsequently, 31.11 parts of phthalic anhydride and 61.35 parts of propylene glycol monomethyl ether acetate were added, and the mixture was reacted at 80°C for 3 hours while stirring under air bubbling, to obtain a 50% solution of carboxyl group-containing resin A-7 (Mw: 8200, acid value 73mgKOH / g) having an ethylenically unsaturated group.
[0150] (1-8) Synthesis Example A-8 (Carboxyl Group-Containing Resin A-8) Into a four-neck flask equipped with a reflux condenser, a thermometer, a glass tube for nitrogen replacement, and a stirrer, 60 parts of glycidyl methacrylate, 10 parts of N-phenylmaleimide, 20 parts of benzyl methacrylate, 10 parts of methyl methacrylate, 100 parts of propylene glycol monomethyl ether acetate, and 8 parts of azobisisobutyronitrile were added, and the mixture was heated under a nitrogen stream and polymerized at 95°C for 5 hours to obtain a 50% copolymer solution.
[0151] To the above 50% copolymer solution, 0.1 parts of methoquinone (p-Methoxyphenol), 30.24 parts of acrylic acid, and 1 part of triphenylphosphine were added, and the addition reaction was carried out at 110°C for 24 hours. Subsequently, 20.79 parts of cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride and 51.03 parts of propylene glycol monomethyl ether acetate were added, and the mixture was reacted at 80°C for 3 hours while stirring under air bubbling, to obtain a 50% solution of carboxyl group-containing resin A-8 (Mw: 8400, acid value 78mgKOH / g) having an ethylenically unsaturated group.
[0152] (1-9) Synthesis Example A-9 (Carboxyl Group-Containing Resin A-9) Into a four-neck flask equipped with a reflux condenser, a thermometer, a glass tube for nitrogen replacement, and a stirrer, 60 parts of glycidyl methacrylate, 10 parts of N-phenylmaleimide, 20 parts of benzyl methacrylate, 10 parts of methyl methacrylate, 100 parts of propylene glycol monomethyl ether acetate, and 8 parts of azobisisobutyronitrile were added, and the mixture was heated under a nitrogen stream and polymerized at 95°C for 5 hours to obtain a 50% copolymer solution.
[0153] To the above 50% copolymer solution, 0.1 parts of methoquinone (p-Methoxyphenol), 30.24 parts of acrylic acid, and 1 part of triphenylphosphine were added, and the addition reaction was carried out at 110°C for 24 hours. Subsequently, 20.18 parts of trimellitic anhydride and 50.42 parts of propylene glycol monomethyl ether acetate were added, and the mixture was reacted at 80°C for 3 hours while stirring under air bubbling, to obtain a 50% solution of carboxyl group-containing resin A-9 (Mw: 8500, acid value 78mgKOH / g) having an ethylenically unsaturated group.
[0154] (1-10) Synthesis Example A-10 (Carboxyl Group-Containing Resin A-10) Into a four-neck flask equipped with a reflux condenser, a thermometer, a glass tube for nitrogen replacement, and a stirrer, 45 parts of glycidyl methacrylate, 10 parts of N-phenylmaleimide, 20 parts of benzyl methacrylate, 25 parts of methyl methacrylate, 100 parts of propylene glycol monomethyl ether acetate, and 8 parts of azobisisobutyronitrile were added, and the mixture was heated under a nitrogen stream and polymerized at 95°C for 5 hours to obtain a 50% copolymer solution.
[0155] To the above 50% copolymer solution, 0.1 parts of methoquinone (p-Methoxyphenol), 23.04 parts of acrylic acid, and 1 part of triphenylphosphine were added, and the mixture was subjected to an addition reaction at 110°C for 24 hours. Subsequently, 24.64 parts of hexahydrophthalic anhydride and 47.68 parts of propylene glycol monomethyl ether acetate were added, and the mixture was reacted at 80°C for 3 hours while stirring under air bubbling, to obtain a 50% solution of carboxyl group-containing resin A-10 (Mw: 7600, acid value 61 mgKOH / g) having an ethylenically unsaturated group.
[0156] (1-11) Synthesis Example B-1 (Carboxyl Group-Containing Resin B-1) Into a four-neck flask equipped with a reflux condenser, a thermometer, a glass tube for nitrogen replacement, and a stirrer, 35 parts of glycidyl methacrylate, 10 parts of N-phenylmaleimide, 20 parts of benzyl methacrylate, 35 parts of methyl methacrylate, 100 parts of propylene glycol monomethyl ether acetate, and 8 parts of azobisisobutyronitrile were added, and the mixture was heated under a nitrogen stream and polymerized at 95°C for 5 hours to obtain a 50% copolymer solution.
[0157] To the above 50% copolymer solution, 0.1 parts of methoquinone (p-Methoxyphenol), 18 parts of acrylic acid, and 1 part of triphenylphosphine were added and subjected to an addition reaction at 110°C for 24 hours. Subsequently, 19.25 parts of hexahydrophthalic anhydride and 37.25 parts of propylene glycol monomethyl ether acetate were added and reacted at 80°C for 3 hours while stirring under air bubbling, to obtain a 50% solution of carboxyl group-containing resin B-1 (Mw: 7100, acid value 51 mgKOH / g) having an ethylenically unsaturated group.
[0158] (1-12) Synthesis Example C-1 (Carboxyl Group-Containing Resin C-1) In a four-neck flask equipped with a reflux condenser, a thermometer, an air inlet tube and a stirrer, 40 parts by mass of methacrylic acid, 47.5 parts by mass of methyl methacrylate, 12.5 parts by mass of styrene, 40 parts by mass of dipropylene glycol monomethyl ether acetate, 215 parts by mass of dipropylene glycol monomethyl ether and 1.75 parts by mass of azobisisobutyronitrile were added. The mixture in the four-neck flask was heated at a heating temperature of 75°C for 5 hours while stirring under a nitrogen stream to allow the polymerization reaction to proceed. As a result, a copolymer solution with a concentration of 32% was obtained.
[0159] Next, 0.05 parts by mass of methoquinone (p-Methoxyphenol), 32 parts by mass of glycidyl methacrylate, and 0.4 parts by mass of dimethylbenzylamine were added to this copolymer solution. These were heated at 80°C for 24 hours while stirring under air bubbling to allow the addition reaction to proceed. As a result, a 38% by mass solution of carboxyl group-containing resin C-1 (Mw: 22400, acid value 104 mgKOH / g) having an ethylenically unsaturated group was obtained.
[0160] (1-13) Synthesis Example D-1 (Carboxyl Group-Containing Resin D-1) Into a four-neck flask equipped with a reflux condenser, a thermometer, an air inlet tube, and a stirrer, 252 parts by mass of a bisphenol fluorene type epoxy compound (an epoxy compound represented by the following formula (2), in which R1 to R8 in formula (2) are all hydrogen and have an epoxy equivalent of 252 g / eq), 72 parts by mass of acrylic acid, 1.5 parts by mass of triphenylphosphine, 0.2 parts by mass of 4-methoxyphenol, and 200 parts by mass of propylene glycol monomethyl ether acetate were added. These were stirred under air bubbling to prepare a mixture. This mixture was heated in the flask under stirring under air bubbling at a heating temperature of 115°C for a heating time of 12 hours. In this way, an intermediate solution was prepared.
[0161] Next, 73.55 parts by mass of 3,3',4,4'-biphenyltetracarboxylic dianhydride and 15 parts by mass of propylene glycol monomethyl ether acetate were added to the intermediate solution in the flask. These were heated at a heating temperature of 115°C and a heating time of 6 hours while being stirred under air bubbling. As a result, a 65% by mass solution of carboxyl group-containing resin D-1 (Mw: 3400, acid value 69 mgKOH / g) having an ethylenically unsaturated group was obtained.
[0162] [ka]
[0163] (1-14) Synthesis Example D-2 (Carboxyl Group-Containing Resin D-2) Into a four-neck flask equipped with a reflux condenser, a thermometer, an air inlet tube, and a stirrer, 252 parts by mass of a bisphenol fluorene type epoxy compound (an epoxy compound having an epoxy equivalent of 252 g / eq, represented by the above formula (2), in which R1 to R8 in formula (2) are all hydrogen), 72 parts by mass of acrylic acid, 1.5 parts by mass of triphenylphosphine, 0.2 parts by mass of 4-methoxyphenol, and 200 parts by mass of propylene glycol monomethyl ether acetate were added. These were stirred under air bubbling to prepare a mixture. This mixture was heated in the flask under stirring under air bubbling at a heating temperature of 115°C for a heating time of 12 hours. In this way, an intermediate solution was prepared.
[0164] Next, 60.8 parts by mass of 1,2,3,6-tetrahydrophthalic anhydride, 58.8 parts by mass of 3,3',4,4'-biphenyltetracarboxylic dianhydride, and 40 parts by mass of propylene glycol monomethyl ether acetate were added to the intermediate solution in the flask. These were heated under air bubbling with stirring at a heating temperature of 115°C for 6 hours, and further heated under air bubbling with stirring at a heating temperature of 60°C for 6 hours. This resulted in a 65% by mass solution of carboxyl group-containing resin D-2 (Mw: 2900, acid value 104 mgKOH / g) having an ethylenically unsaturated group.
[0165] (1-15) Synthesis Example E-1 (Carboxyl Group-Containing Resin E-2) A mixture was prepared by placing 188 parts by mass of phenol novolac epoxy resin (manufactured by DIC Corporation, product number EPICLON N-770, epoxy equivalent 188), 103 parts by mass of diethylene glycol monoethyl ether acetate, 0.2 parts by mass of methylhydroquinone, 72 parts by mass of acrylic acid, and 1.5 parts by mass of triphenylphosphine in a four-neck flask equipped with a reflux condenser, a thermometer, an air blowing tube, and a stirrer. The mixture was heated at a heating temperature of 115°C for a heating time of 12 hours while blowing air into the four-neck flask, to allow the addition reaction to proceed.
[0166] Next, 76 parts by mass of tetrahydrophthalic anhydride and 78.8 parts by mass of diethylene glycol monoethyl ether acetate were added to the mixture, and the mixture was further heated at 90° C. for 3 hours. This produced a 65% by mass solution of carboxyl group-containing resin E-1 (Mw: 7700, acid value 84 mgKOH / g) having an ethylenically unsaturated group.
[0167] (1-16) Synthesis Example E-2 (Carboxyl Group-Containing Resin E-2) A mixture was prepared by adding 203 parts by mass of cresol novolac epoxy resin (manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., product number YDCN-700-5, epoxy equivalent 203), 103 parts by mass of diethylene glycol monoethyl ether acetate, 0.2 parts by mass of methyl hydroquinone, 72 parts by mass of acrylic acid, and 1.5 parts by mass of triphenylphosphine into a four-neck flask equipped with a reflux condenser, a thermometer, an air blowing tube, and a stirrer. The mixture was heated at a heating temperature of 115°C and a heating time of 12 hours while blowing air into the four-neck flask, to allow the addition reaction to proceed. Next, 60.8 parts by mass of tetrahydrophthalic anhydride and 78.9 parts by mass of diethylene glycol monoethyl ether acetate were added to the mixture, and the mixture was further heated at a heating temperature of 90°C and a heating time of 3 hours while stirring under air bubbling. This gave a 65% by mass solution of carboxyl group-containing resin E-2 (Mw: 6200, acid value 67 mgKOH / g) having an ethylenically unsaturated group.
[0168] The components (raw materials, etc.) used in the above Synthesis Examples A-1 to E-2 are listed in Table 1 below. Note that in Synthesis Example C-1, "GMA" is used to obtain a carboxyl group-containing resin in a manner different from that in Synthesis Examples A-1 to A-10, and therefore is indicated differently (marked with *, ●, etc.). In Table 1, the "first reaction" refers to the reaction between the copolymer and (meth)acrylic acid, and the "second reaction" refers to the reaction between the intermediate reaction product and a polybasic acid anhydride. As mentioned above, the details of the "raw materials" shown in Table 1 are as follows: GMA: Glycidyl methacrylate MMA; Methyl methacrylate ·BZMA: Benzyl methacrylate ST: Styrene PM: Phenylmaleimide ·BPFE: Bisphenol fluorene type epoxy compound PNE: Phenol novolac type epoxy resin ·CNE: Cresol novolac epoxy resin Aa: Acrylic acid ·THPA: Tetrahydrophthalic anhydride HHPA: Hexahydrophthalic anhydride (cyclohexane-1,2-dicarboxylic anhydride) ·PA: Phthalic anhydride H-TMA: Cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride TMA: Trimellitic anhydride BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride
[0169] [Table 1]
[0170] (2) Preparation of resin composition [Examples and Comparative Examples] The components shown in the table below were added to a flask and mixed by stirring at a temperature of 35° C. to obtain a resin composition. Details of the components shown in the table are as follows. The values in the table are parts by mass, and for carboxyl group-containing resins, they are parts by mass converted into solid content. -Photopolymerization initiator Photopolymerization initiator A: 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (manufactured by IGM Resins BV, product number Omnirad TPO H). Photopolymerization initiator B: 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (manufactured by IGM Resins BV, product number Omnirad 907). Photopolymerization initiator C: Oxime ester photoinitiator (1,2-octadienone, 1-[4-(phenylthio)phenyl]-, 2-(o-benzoyloxime) (product name Irgacure OXE01 manufactured by BASF Japan Ltd.)). Photopolymerization initiator D: Oxime ester photoinitiator, product name Irgacure OXE04 manufactured by BASF Japan Ltd. -Multifunctional (meth)acrylate compounds Polymerizable compound A: 1,9-nonanediol diacrylate. ·Polymerizable compound B: Dimethylol-tricyclodecane diacrylate. ·Polymerizable compound C: Trimethylolpropane triacrylate. -Other ingredients - Antioxidant: Hindered phenol-based antioxidant (manufactured by BASF Japan Ltd., product number Irganox 1010). Surface modifier: DIC Corporation, product number Megafac F-563) Solvent: propylene glycol monomethyl ether. The solvent is mixed in such a way that the solid content of the components in the resin composition is 30% by mass.
[0171] (3) Preparation of dry film A dry film was produced from the resin composition prepared in (2) above as follows.
[0172] First, a film (base film) made of polyethylene terephthalate (PET) with a thickness of 16 μm was prepared. On this film, the compositions of each Example and Comparative Example were applied with a spin coater to form a wet coating film. This coating film was thermally dried at 110° C. for 5 minutes to form a film with a thickness of 10 μm on the PET, thereby producing a dry film.
[0173] (4) Evaluation The following evaluations (4-1) to (4-8) were carried out for each of the Examples and Comparative Examples. The evaluation results are shown in Table 2-4 below.
[0174] (4-1) Transmittance (transmittance curve 450nm~800nm) (3) The entire surface of the dry film of each of the Examples and Comparative Examples was irradiated with 200 mJ / cm 2 by an ultra-high pressure mercury lamp. 2 The film was irradiated with ultraviolet light under the conditions of 1.0 and then developed after exposure. In the development, a 1% by mass Na2CO3 aqueous solution at 30°C was sprayed onto the film at a pressure of 0.05 MPa for 30 seconds. Then, pure water was sprayed onto the film at a pressure of 0.05 MPa for 30 seconds.
[0175] This produced a cured product of the photocurable resin composition on a PET film (base film). The cured product was set in an ultraviolet-visible-near infrared spectrophotometer (Shimadzu Corporation, product number UV-3100PC) to measure the transmittance of the cured product from 450 nm to 800 nm, and a transmittance curve was obtained. A PET film, which was the substrate (base film), was used as a reference. Based on the obtained transmittance curve, the transmittance was evaluated according to the following criteria. ◯: In the wavelength range of 450 nm to 800 nm, the transmittance was 85% or more. ×: Within the wavelength range of 450 nm to 800 nm, there was a wavelength range in which the transmittance was less than 85%.
[0176] (4-2) Hayes The haze value of the cured products of each of the Examples and Comparative Examples prepared in (4-1) was measured in accordance with JIS K7105 using a haze meter (product number NDH7000, manufactured by Nippon Denshoku Industries Co., Ltd.) and evaluated according to the following criteria. A: The haze value is less than 0.8%. B: The haze value is 0.8 or more and less than 1.0%. C: The haze value is 1.0% or more and less than 1.5%. D: The haze value is 1.5% or more.
[0177] (4-3) Light resistance (3) The entire surface of the dry film of each of the Examples and Comparative Examples was irradiated with 200 mJ / cm 2 by an ultra-high pressure mercury lamp. 2The film was then exposed to ultraviolet light under the conditions of:
[0178] In the development process, a 1% by mass Na2CO3 aqueous solution at 30° C. was sprayed onto the film at a spray pressure of 0.05 MPa for 30 seconds, followed by spraying pure water onto the film at a spray pressure of 0.05 MPa for 30 seconds.
[0179] In this way, a cured product of the photocurable resin composition was produced on the PET film (base film).
[0180] The cured product was exposed to a metal halide light source at 2000 mJ / cm 2 After irradiation with ultraviolet light under the above conditions, the sample was visually observed and evaluated according to the following criteria. A: No yellowing is observed in the cured product. B: Very slight yellowing is observed in the cured product. C: The cured product shows some yellowing. D: Significant yellowing is observed in the cured product.
[0181] (4-4) Sensitivity A glass epoxy copper-clad laminate (FR-4 type) with a copper foil having a thickness of 17.5 μm was prepared. The dry film of each of the examples and comparative examples prepared in (3) was heat-laminated on one entire surface of the copper-clad laminate using a vacuum laminator. The heat lamination conditions were 0.5 MPa, 80° C., and 1 minute. As a result, a coating of 10 μm thick made of the dry film was formed on the copper-clad laminate.
[0182] With the PET film (base film) still attached to the coating, a photo tool "Stouffer step tablet 21 steps" was placed on the PET film and brought into close contact under reduced pressure, after which it was exposed to 200 mJ / cm 2 light from an ultra-high pressure mercury lamp. 2The film was irradiated with ultraviolet rays under the following conditions. The PET film (base film) was peeled off from the exposed film, and the film was subjected to a development process. In the development process, a 1% by mass Na2CO3 aqueous solution at 30°C was sprayed onto the film at a spray pressure of 0.05 MPa for 30 seconds. Then, pure water was sprayed onto the film at a spray pressure of 0.05 MPa for 30 seconds. The number of remaining steps (remaining step stages) in the cured film after development was determined.
[0183] (4-5) Resolution A glass epoxy copper-clad laminate (FR-4 type) with a copper foil having a thickness of 17.5 μm was prepared. The dry film of each of the examples and comparative examples prepared in (3) was heat-laminated on one entire surface of the copper-clad laminate using a vacuum laminator. The heat lamination conditions were 0.5 MPa, 80° C., and 1 minute. As a result, a coating of 10 μm thick made of the dry film was formed on the copper-clad laminate.
[0184] With the PET film (base film) still attached to the coating, a negative mask with a pattern including lines / spaces of 80 μm, 90 μm, and 100 μm in width was placed on the coating, and after bonding under reduced pressure, it was irradiated with 200 mJ / cm 2 from an ultra-high pressure mercury lamp. 2 The film was irradiated with ultraviolet light under the following conditions: After exposure, the PET film (base film) was peeled off from the film, and the film was subjected to a development process.
[0185] In the development process, a 1% by mass Na2CO3 aqueous solution at 30°C was sprayed onto the film at a spray pressure of 0.05 MPa for 30 seconds. Then, pure water was sprayed onto the film at a spray pressure of 0.05 MPa for 30 seconds. This removed the unexposed parts of the film, forming a line-free pattern on the film. The test pieces were observed and evaluated according to the following criteria. A: Lines / spaces of 80 μm width can be resolved. B: Lines / spaces with a width of 90 μm can be resolved, but lines / spaces with a width of 80 μm cannot be resolved. C: Lines / spaces with a width of 100 μm can be resolved, but lines / spaces with a width of 90 μm cannot be resolved. D: Lines / spaces of 100 μm width cannot be resolved.
[0186] (4-6) Adhesion 1 (adhesion to PET film) The dry film of each of the Examples and Comparative Examples prepared in (3) was heat-laminated on the entire surface of the PET film using a vacuum laminator. The heat lamination conditions were 0.5 MPa, 80°C, and 1 minute. As a result, a coating of 10 μm thick made of the dry film was formed on the PET film.
[0187] With the PET film (base film) still attached to the film, the entire surface of the film was irradiated with 200mJ / cm 2 by an ultra-high pressure mercury lamp. 2 The specimen was irradiated with ultraviolet light under the following conditions.
[0188] The PET film (base film) was peeled off from the exposed film, and the film was subjected to a development process. In the development process, a 1% by mass Na2CO3 aqueous solution at 30°C was sprayed onto the film at a spray pressure of 0.05 MPa for 30 seconds. After that, the entire surface of the film was exposed to 200 mJ / cm2 of a metal halide lamp. 2 A test piece was prepared by irradiating ultraviolet rays under the above conditions.
[0189] In accordance with JIS D0202, cross-cuts (10 lines x 10 lines, 1 mm intervals) were made in a grid pattern on the test pieces of each Example and Comparative Example, and cellophane adhesive tape was attached to the cuts to perform a peeling test. After the peeling test, the state of peeling on the test pieces was visually observed and evaluated according to the following criteria. The following criteria are based on "Section 6: Adhesion (Cross-cut Method)" of JIS K5600-5-6. A: The edges of the cut are completely smooth and there is no peeling on any of the grids. B: There is minor peeling of the coating at the intersections of the cuts, and the cross-cut area affected is not significantly greater than 5%. C: The coating has delaminated along the edges of the cuts and / or at the intersections. Clearly more than 5% but not more than 15% of the cross-cut area is affected. D: The coating has partially or completely peeled off significantly along the edges of the cuts and / or partially or completely peeled off in various areas of the mesh. The cross-cut areas are clearly more than 15% affected.
[0190] (4-7) Adhesion 2 (adhesion to copper sputtered film) A substrate was prepared by forming a copper sputtered film on a PET film. The dry films of each of the examples and comparative examples prepared in (3) were heat-laminated on the entire surface of the substrate using a vacuum laminator. The heat lamination conditions were 0.5 MPa, 80°C, and 1 minute. As a result, a coating of 10 μm thick made of the dry film was formed on the PET film.
[0191] With the PET film (base film) still attached to the film, the entire surface of the film was irradiated with 200mJ / cm 2 by an ultra-high pressure mercury lamp. 2 The specimen was irradiated with ultraviolet light under the following conditions.
[0192] The PET film (base film) was peeled off from the exposed film, and the film was subjected to a development process in which a 1% by mass Na2CO3 aqueous solution at 30°C was sprayed onto the film at a spray pressure of 0.05 MPa for 30 seconds.
[0193] After that, the entire film was irradiated with 200mJ / cm 2 using a metal halide lamp. 2 A test piece was prepared by irradiating ultraviolet rays under the above conditions.
[0194] In accordance with JIS D0202, cross-cuts (10 lines x 10 lines, 1 mm intervals) were made in a grid pattern on the test pieces of each Example and Comparative Example, and a peeling test was performed by attaching cellophane adhesive tape to the cuts. After the peeling test, the state of peeling on the test pieces was visually observed and evaluated according to the following criteria. A: The edges of the cut are completely smooth and there are no peeling marks on any of the grids. B: There is minor peeling of the coating at the intersections of the cuts, and the cross-cut area affected is not significantly greater than 5%. C: The coating has delaminated along the edges of the cuts and / or at the intersections. Clearly more than 5% but not more than 15% of the cross-cut area is affected. D: The coating has partially or completely peeled off significantly along the edges of the cuts and / or partially or completely peeled off in various areas of the mesh. The cross-cut areas are clearly more than 15% affected.
[0195] (4-8) Pencil hardness The pencil hardness of the cured test pieces of each of the Examples and Comparative Examples prepared in (4-6) above was measured in accordance with JIS K5400 using a Mitsubishi Hi-Uni pencil (manufactured by Mitsubishi Pencil Co., Ltd.).
[0196] [Table 2]
[0197] [Table 3]
[0198] [Table 4]
[0199] 3. Summary As is apparent from the above embodiments and examples, the present disclosure includes the following aspects.
[0200] The photocurable resin composition of the first embodiment contains a carboxyl group-containing resin (A), a photopolymerization initiator (B), and a polyfunctional (meth)acrylate compound (C). The carboxyl group-containing resin (A) is a reaction product of an intermediate reaction product of a copolymer of an epoxy group-containing (meth)acrylate compound (a1) and an ethylenically unsaturated compound (a2) other than the epoxy group-containing (meth)acrylate compound (a1) with a carboxylic acid (a3) having an ethylenically unsaturated group, and a polybasic acid anhydride (a4). The proportion of the residues derived from the epoxy group-containing (meth)acrylate compound (a1) to the total residues constituting the carboxyl group-containing resin (A) is 40 mol% or more and less than 100 mol%, and the proportion of the residues derived from the ethylenically unsaturated compound (a2) is more than 0 mol% and 60 mol% or less. When a cured product having a thickness of 10 μm is produced from the photocurable resin composition, the cured product has a light transmittance of 85% or more in a wavelength range of 450 nm or more and 800 nm or less.
[0201] According to this embodiment, the resolution of the photocurable resin composition can be ensured, and the cured product can have adhesion to a base material while maintaining high transparency.
[0202] In the photocurable resin composition of the second embodiment, in the first embodiment, the polybasic acid anhydride (a4) has a cyclohexane skeleton.
[0203] According to this embodiment, it is easy to improve the transparency of the cured product of the photocurable resin composition, and in particular, it is easy to improve the light resistance of the cured product.
[0204] The photocurable resin composition of the third embodiment is the first or second embodiment, further comprising a carboxyl group-containing epoxy (meth)acrylate compound (D) having an aromatic ring and no novolac skeleton.
[0205] According to this embodiment, the cured product of the photocurable resin composition can achieve excellent physical properties such as high heat resistance and insulation reliability.
[0206] A fourth aspect of the photocurable resin composition is any one of the first to third aspects, in which the acid value of the carboxyl group-containing resin (A) is 40 mgKOH / g or more and 140 mgKOH / g or less.
[0207] According to this embodiment, the resolution of the cured product produced from the photocurable resin composition can be particularly improved.
[0208] A fifth aspect of the photocurable resin composition is any one of the first to fourth aspects, in which the photopolymerization initiator (B) contains an acylphosphine oxide-based photopolymerization initiator (B1).
[0209] According to this embodiment, higher photosensitivity can be imparted to the photocurable resin composition, the degree of coloration of the cured product can be reduced, and the high transparency of the cured product of the photocurable resin composition can be more easily maintained.
[0210] A sixth aspect of the photocurable resin composition is any one of the first to fifth aspects, in which the photopolymerization initiator (B) contains an oxime ester-based photopolymerization initiator (B2).
[0211] According to this embodiment, it is easy to maintain a good balance between adhesion and light resistance in the cured product of the photocurable resin composition.
[0212] A seventh aspect of the photocurable resin composition is any one of the first to sixth aspects, in which the polyfunctional (meth)acrylate compound (C) contains a difunctional (meth)acrylate compound (C1).
[0213] According to this embodiment, the resolution is particularly improved when a film (dried film, dry film) made from the photocurable resin composition is exposed to light and developed, and the developability of the photocurable resin composition with an alkaline aqueous solution is particularly improved.
[0214] The dry film of the eighth embodiment includes a dried or semi-cured product of the photocurable resin composition of any one of the first to seventh embodiments.
[0215] According to this embodiment, the resolution of the dry film can be ensured, and the cured product can have high adhesion to the base material while maintaining high transparency.
[0216] The cured product of the ninth embodiment is a cured product of the photocurable resin composition of any one of the first to eighth embodiments.
[0217] According to this embodiment, the cured product has high transparency and excellent adhesion to the base material. [Explanation of symbols]
[0218] 1 Dry film 11 Cured product
Claims
1. A photocurable resin composition comprising a carboxyl group-containing resin (A), a photopolymerization initiator (B), and a polyfunctional (meth)acrylate compound (C), the carboxyl group-containing resin (A) is a reaction product of an intermediate reaction product of a copolymer of an epoxy group-containing (meth)acrylate compound (a1) and an ethylenically unsaturated compound (a2) other than the epoxy group-containing (meth)acrylate compound (a1), and a carboxylic acid (a3) having an ethylenically unsaturated group, and a polybasic acid anhydride (a4); a ratio of residues derived from the epoxy group-containing (meth)acrylate compound (a1) to all residues constituting the carboxyl group-containing resin (A) is 40 mol % or more and less than 100 mol %, and a ratio of residues derived from the ethylenically unsaturated compound (a2) is more than 0 mol % and 60 mol % or less, When a cured product having a thickness of 10 μm is produced from the photocurable resin composition, the light transmittance of the cured product in a wavelength range of 450 nm or more and 800 nm or less is 85% or more. Photocurable resin composition.
2. The polybasic acid anhydride (a4) has a cyclohexane skeleton. The photocurable resin composition according to claim 1.
3. Further containing a carboxyl group-containing epoxy (meth)acrylate compound (D) having an aromatic ring and no novolak skeleton, The photocurable resin composition according to claim 1 or 2.
4. The acid value of the carboxyl group-containing resin (A) is 40 mgKOH / g or more and 140 mgKOH / g or less. The photocurable resin composition according to claim 1 or 2.
5. The photopolymerization initiator (B) contains an acylphosphine oxide-based photopolymerization initiator (B1). The photocurable resin composition according to claim 1 or 2.
6. The photopolymerization initiator (B) contains an oxime ester-based photopolymerization initiator (B2). The photocurable resin composition according to claim 1 or 2.
7. The polyfunctional (meth)acrylate compound (C) contains a bifunctional (meth)acrylate compound (C1), The photocurable resin composition according to claim 1 or 2.
8. The photocurable resin composition according to claim 1 or 2, comprising a dried product or a semi-cured product thereof. Dry film.
9. A cured product of the photocurable resin composition according to claim 1 or 2.
Citation Information
Patent Citations
Acid group-containing (METH)acrylate resin, curable resin composition, insulating material, resin material for solder resist, and resist member
WO2021220922A1