Toner, toner storage unit, developer, and image forming apparatus

A toner with controlled binder resin and release agent ratios addresses stress resistance and low-temperature fixability issues by minimizing surface exposure and additive embedding, ensuring high-quality image formation.

JP2024158832APending Publication Date: 2024-11-08RICOH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023074392
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing toners fail to achieve both excellent stress resistance and low-temperature fixability, particularly when subjected to low printing rates, due to issues with toner deformation, cracking, and exposure of release agents, which affect chargeability and image quality.

Method used

A toner formulation with specific ratios of binder resin and release agent determined by DSC and FTIR-ATR methods, ensuring a peak intensity ratio of 0.28 to 0.45, using styrene acrylic resin and polyethylene wax, with controlled release agent content, to minimize surface exposure and additive embedding.

Benefits of technology

The toner maintains chargeability and forms high-quality images over time with excellent low-temperature fixability, resisting stress and reducing abnormal images.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158832000003
    Figure 2024158832000003
  • Figure 2024158832000004
    Figure 2024158832000004
  • Figure 2024158832000005
    Figure 2024158832000005
Patent Text Reader

Abstract

To provide a toner that achieves both stress resistance and low temperature fixability.SOLUTION: A toner contains toner base particles including at least a binder resin, a mold release agent, and a coloring agent, and an external additive, wherein an endothermic quantity derived from the mold release agent in a differential scanning calorimetry (DSC) method is 7.0 [J / g] or more and 15.0 [J / g] or less, and when the peak intensity of a peak derived from the mold release agent is defined as Wabs, and the peak strength of a peak derived from the binder resin as Rabs, which are obtained by a total reflection absorption infrared spectroscopy (FTIR-ATR) method, the Wabs and the Rabs satisfy the following relational expression (1). (1) 0.28≤Wabs / Rabs≤0.45.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner, a toner storage unit, a developer, and an image forming apparatus. [Background technology]

[0002] In an electrophotographic image forming method, an electrostatic image (latent image) is formed on a photoconductor, and the resulting latent image is developed with toner to form a toner image.

[0003] In order to form a good image, it is preferable that the chargeability of the toner is less affected by external factors. An example of an external factor is the effect of stress within the machine, which causes deformation, cracking, chipping, and embedding of external additives in the surface of the toner particles due to the toner being held in the developing section for a long period of time. This causes changes in the particle size distribution, shape, adhesive force, and fluidity of the toner, which affect the chargeability of the toner, and is particularly noticeable when printing at a low printing rate.

[0004] On the other hand, from the viewpoint of energy saving and miniaturization of devices such as copiers, there is a demand for toners with low cold offset occurrence temperature and excellent low-temperature fixing properties. This is common to monochrome / full-color printers and full-color copiers. Accordingly, there is a trend to design the melting points of the raw materials used in toners and the toner itself to be lower, and there are more cases where low-molecular-weight materials are used than in the past.

[0005] To date, for example, in order to achieve both low-temperature fixability and heat-resistant storage stability and further improve stress resistance, a toner has been reported in which a release agent and / or a crystalline resin is encapsulated in an amorphous resin, thereby improving the heat-resistant storage stability of the toner and preventing the release agent / crystalline resin from seeping out to the toner particle surface even when subjected to physical stress (see, for example, Patent Document 1).

[0006] In addition, an electrophotographic toner has been proposed that is excellent in pressurized storage stability while satisfying excellent low-temperature fixability by incorporating at least two kinds of crystalline polyester resins having different molecular weights, namely, crystalline polyester A having a storage modulus at 160°C of 120 Pa to 100,000 Pa and crystalline polyester B having a storage modulus at 160°C of 0.01 Pa to 500 Pa, into a binder resin to obtain a binder resin with high crystallinity, thereby increasing the crystal growth rate during melt kneading (see, for example, Patent Document 2).

[0007] In addition, a toner binder containing two or more types of crystalline resins, in which a set of endothermic peak temperatures consisting of the total of the endothermic peak temperatures of each of the two or more types of crystalline resins has two or more different endothermic peak temperatures, is used to increase the viscosity of the toner layer fixed on paper when continuously printed, and toner binders have excellent low-temperature fixing properties, heat-resistant storage stability, and hot offset resistance, as well as excellent blocking resistance of paper when continuously printed (see, for example, Patent Document 3).

[0008] In addition, a toner has been proposed that significantly improves high-temperature offset resistance without impairing low-temperature fixability by adding an ester wax that quickly exudes during fixing and a polyolefin wax that has high compatibility with binder resins and slowly exudes during fixing to a crosslinking reaction type styrene acrylic resin that contains a carboxyl group-containing styrene acrylic resin and a glycidyl group-containing styrene acrylic resin (for example, see Patent Document 4). Summary of the Invention [Problem to be solved by the invention]

[0009] The above-mentioned conventional techniques can achieve a certain level of effect, but from the viewpoint of the high level of toners required in recent years, that is, toners having both excellent stress resistance and low-temperature fixing properties, it cannot be said that a fully satisfactory toner has been obtained, and there is room for further research. An object of the present invention is to provide a toner which has both high stress resistance and low-temperature fixability.

[0010] As a result of intensive research, the present inventors have found that the above problems can be solved by the present invention having the following configuration. A toner containing toner base particles containing at least a binder resin, a release agent, and a colorant, and an external additive, wherein the amount of heat absorbed by the release agent as determined by a DSC (differential scanning calorimeter) method is 7.0 [J / g] or more and 15.0 [J / g] or less, and when the peak intensity of the peak as determined by a FTIR-ATR (attenuated total reflection infrared spectroscopy) method is Wabs and the peak intensity of the peak as determined by a FTIR-ATR (attenuated total reflection infrared spectroscopy) method is Rabs, the Wabs and the Rabs satisfy the following relationship (1). 0.28≦Wabs / Rabs≦0.45 (1) Effect of the Invention

[0011] According to the present invention, it is possible to provide a toner that has both high stress resistance and low-temperature fixability. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic diagram showing an example of a tandem type image forming apparatus of the present invention. [Diagram 2] FIG. 2 is a partially enlarged view of FIG. [Diagram 3] FIG. 3 is a diagram showing an example of a process cartridge as a toner storage unit of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention relates to the following (1), but also includes the following (2) to (8). (1) A toner comprising toner base particles including at least a binder resin, a release agent, and a colorant, and an external additive, The endothermic heat amount derived from the release agent as determined by a DSC (differential scanning calorimeter) method is 7.0 [J / g] or more and 15.0 [J / g] or less, When the peak intensity of the peak derived from the release agent determined by FTIR-ATR (attenuated total reflection infrared spectroscopy) is designated as Wabs and the peak intensity of the peak derived from the binder resin is designated as Rabs, Wabs and Rabs satisfy the following relational formula (1): A toner characterized by: 0.28≦Wabs / Rabs≦0.45 (1) (2) The toner according to the above (1), wherein the binder resin is a styrene-acrylic resin, and the release agent is a polyethylene wax. (3) The toner according to (1) or (2) above, wherein the amount of heat absorption originating from the release agent is at least 8.0 [J / g] to 11.0 [J / g]. (4) The toner according to any one of (1) to (3) above, wherein the toner base particles contain metal oxide particles therein. (5) The toner according to any one of the above (1) to (4), wherein the toner base particles are obtained by a pulverization method. (6) A toner storage unit, characterized in that it stores the toner according to any one of (1) to (5) above. (7) A developer comprising the toner according to any one of (1) to (5) above and a carrier. (8) an electrostatic latent image carrier; and an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image carrier; a developing unit having a toner for developing the electrostatic latent image formed on the electrostatic latent image carrier to form a visible image, 13. An image forming apparatus, comprising the toner according to claim 12, wherein the toner is a toner according to any one of (1) to (5).

[0014] The toner of the present invention will now be described in detail. According to the investigations of the present inventors, when an attempt is made to achieve low temperature fixability by increasing the formulation amount of the release agent, a large amount of the release agent is exposed on the toner surface, and the external additives become embedded, which leads to a decrease in the toner chargeability and the occurrence of abnormal images, particularly when printing at a low printing rate. However, if the amount of release agent prescribed for the entire toner is reduced in order to reduce the exposure of the release agent to the surface, it is difficult to obtain a toner having excellent low-temperature fixability.

[0015] In order to solve the problems of the conventional techniques, the present inventors have conducted intensive research and have found that a toner containing toner base particles containing at least a binder resin, a release agent, and a colorant and an external additive, in which the amount of heat absorbed by the release agent as determined by a DSC (differential scanning calorimeter) method is 7.0 [J / g] to 15.0 [J / g], and when the peak intensity of the peak derived from the release agent as determined by a FTIR-ATR (attenuated total reflection infrared spectroscopy) method is Wabs and the peak intensity of the peak derived from the binder resin is Rabs, Wabs and Rabs satisfy the relationship of 0.28≦Wabs / Rabs≦0.45, thereby making it possible to suppress exposure of the release agent to the toner surface even under stress in the development process, suppress embedding of the external additive, and maintain the chargeability of the toner, thereby providing a toner that is resistant to stress, has excellent low-temperature fixing properties, and is capable of forming high-quality images over a long period of time, thereby completing the present invention.

[0016] <Toner base particles> The toner base particles (hereinafter sometimes referred to as "toner base") contain a binder resin and a release agent, and preferably contain a colorant and a charge control agent, and more preferably contain metal oxide particles. The toner base particles are preferably obtained by a pulverization method.

[0017] <<Binding resin>> As the binder resin, it is preferable to use a styrene-acrylic resin from the viewpoint of high affinity with the release agent.

[0018] The styrene-acrylic resin is not particularly limited and can be appropriately selected from known copolymers of monomers containing a styrene monomer and an acrylic monomer depending on the purpose, and the monomers may contain other monomers, crosslinking agents, etc. Examples of the styrene monomer include o-methylstyrene, m-methylstyrene, p-methylstyrene, p-methoxystyrene, p-phenylstyrene, p-chlorostyrene, 3,4-dichlorostyrene, p-ethylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, and pn-dodecylstyrene. These may be used alone or in combination of two or more.

[0019] Examples of the acrylic monomer include acrylic acid and methacrylic acid; acrylic acid ester monomers or methacrylic acid ester monomers such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, butyl acrylate, butyl methacrylate, octyl acrylate, octyl methacrylate, dodecyl acrylate, dodecyl methacrylate, stearyl acrylate, stearyl methacrylate, behenyl acrylate, behenyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, diethylaminoethyl acrylate, and diethylaminoethyl methacrylate. These may be used alone or in combination of two or more.

[0020] A crosslinking agent may be used to increase the mechanical strength of the toner particles and to control the molecular weight of the styrene acrylic resin.

[0021] The crosslinking agent is not particularly limited, and any known crosslinking agent can be appropriately selected depending on the purpose. Examples of the crosslinking agent include bifunctional crosslinking agents and trifunctional or higher crosslinking agents. These may be used alone or in combination of two or more.

[0022] Examples of the bifunctional crosslinking agent include divinylbenzene, bis(4-acryloxypolyethoxyphenyl)propane, ethylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butanediol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol #200, #400, and #600 diacrylates, dipropylene glycol diacrylate, polypropylene glycol diacrylate, and the above diacrylates replaced with dimethacrylates.

[0023] Examples of the trifunctional or higher crosslinking agent include pentaerythritol triacrylate, trimethylolethane triacrylate, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, oligoester acrylates and those in which the acrylates are replaced with methacrylates, 2,2-bis(4-methacryloxypolyethoxyphenyl)propane, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and triallyl trimellitate.

[0024] <<Release agent>> The release agent (wax) is not particularly limited and can be appropriately selected from known agents depending on the purpose, but preferably contains polyethylene wax. These may be used alone or in combination of two or more.

[0025] The polyethylene wax is preferably one having a melting point of 80° C. to 115° C. in order to achieve both heat resistance and offset resistance. If the melting point is lower than 80° C., the heat resistance of the toner is significantly deteriorated, and if the melting point is higher than 115° C., the wax is prevented from seeping out onto the toner surface during heat, compression and fixing, which can cause degradation of image quality such as offset.

[0026] The polyethylene wax is a polyethylene oligomer obtained industrially by a medium-pressure or low-pressure polyethylene polymerization method using a Ziegler catalyst or a metallocene catalyst, and can be obtained by purifying the polyethylene oligomer by removing oil, oligomers, etc. from the polyethylene oligomer by a vacuum distillation method or the like, and then removing low molecular weight components appropriately from the distillate residue obtained therefrom at high temperature and high reduced pressure as necessary.

[0027] Examples of the polyethylene wax include Neowax (melting point 110° C., manufactured by Yasuhara Chemical Co., Ltd.) and Polywax 500 (melting point 88° C., manufactured by Toyochem Co., Ltd.), which is a fully saturated ethylene homopolymer.

[0028] The content of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 part by mass to 20 parts by mass, more preferably 2 parts by mass to 8 parts by mass, relative to 100 parts by mass of the toner. When the content is 1 part by mass or more, problems such as poor high-temperature offset resistance and poor low-temperature fixability during fixing can be prevented, and when the content is 20 parts by mass or less, problems such as poor heat-resistant storage stability and image fogging can be easily caused can be prevented.

[0029] <<Charge control agent>> The toner of the present invention may be positively or negatively chargeable. The chargeability can be controlled by a charge control agent.

[0030] The charge control agent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charge control agent include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus simple substances or compounds, tungsten simple substances or compounds, fluorine-based activators, salicylic acid metal salts, metal salts of salicylic acid derivatives, oxynaphthoic acid metal salts, phenol-based condensates, azo-based pigments, boron complexes, and polymeric compounds having functional groups (e.g., sulfonic acid groups, carboxyl groups, or quaternary ammonium salts). These may be used alone or in combination of two or more.

[0031] Specific examples of the charge control agent include the nigrosine dye Bontron 03, the quaternary ammonium salt Bontron P-51, the metal-containing azo dye Bontron S-34, the oxynaphthoic acid metal complex E-82, the salicylic acid metal complex E-84, and the phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), the quaternary ammonium salt molybdenum complexes TP-302 and TP-415 (both manufactured by Hodogaya Chemical Co., Ltd.), the quaternary ammonium salt Copy Charge PSY VP2038, the triphenylmethane derivative Copy Blue PR, the quaternary ammonium salt Copy Charge NEG VP2036, and Copy Charge NX VP434 (all manufactured by Hoechst), LRA-901, and the boron complex LR-147 (all manufactured by Nippon Carlit Co., Ltd.), as well as copper phthalocyanine, perylene, quinacridone, and azo pigments.

[0032] The content of the charge control agent is not particularly limited and may be appropriately selected depending on the purpose. It is sufficient that the charge control agent is used in an amount that allows the agent to exhibit its performance and does not impair fixability or the like. The content of the charge control agent is preferably from 0.5% by mass to 5% by mass, and more preferably from 0.8% by mass to 3% by mass, based on the total mass of the toner base particles.

[0033] The charge control agent may be premixed with a resin, wax and pigment and kneaded and melted when the toner base particles are produced, or may be made into a master batch and kneaded and dispersed; there is no particular limitation on the type of the charge control agent.

[0034] <<Coloring agent>> The colorant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the colorant include carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ocher, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, and anthrazan yellow B. GL, Isoindolinone Yellow, Bengala, Red Lead, Cinnabar, Cadmium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Carmine BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Red F5R, Brilliant Rhianth Carmine 6B, Pogment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkaline Blue - Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake,Examples include malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, and lithopone. These may be used alone or in combination of two or more.

[0035] By using the above colorant, the toner of the present invention can be used as both a black toner and a full-color toner. The content of the colorant is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 part by mass or more and 35 parts by mass or less, and more preferably 3 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the toner.

[0036] <<Metal oxide particles>> The toner base particles preferably contain metal oxide particles, which improves the dispersibility of the release agent and allows the amount of the release agent exposed on the surface to be adjusted to an appropriate range.

[0037] Examples of the metal oxide particles include silicon dioxide, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, iron oxide, copper oxide, zinc oxide, tin oxide, chromium oxide, cerium oxide, pengalla, antimony trioxide, magnesium oxide, zirconium oxide, hydrophobic silica, etc. The content of the metal oxide particles is, for example, preferably 0.1 part by mass or more and 1.0 part by mass or less, and more preferably 0.2 part by mass or more and 0.5 part by mass or less, relative to 100 parts by mass of the toner.

[0038] <External additives> Examples of the external additives include abrasives such as silica, Teflon (registered trademark) resin powder, polyvinylidene fluoride powder, cerium oxide powder, silicon carbide powder, and strontium titanate powder; flowability-imparting agents and anti-aggregation agents such as titanium oxide powder and aluminum oxide powder; and conductivity-imparting agents such as zinc oxide powder, antimony oxide powder, and tin oxide powder. In addition, white fine particles and black fine particles of opposite polarity can also be used as a developability improver. These may be used alone or in combination of two or more, and are selected so as to have resistance to development stress such as idle spin.

[0039] <Characteristics of toner> The endothermic heat of the wax determined by DSC (differential scanning calorimetry) is preferably 7.0 [J / g] or more and 15.0 [J / g] or less, and more preferably 8.0 [J / g] or more and 11.0 [J / g] or less. The total amount of the release agent in the toner particles can be obtained by a DSC (differential scanning calorimeter) method.

[0040] The toner sample was measured using the following measuring device and conditions to obtain the endothermic heat of the wax. Measurement equipment: DSC equipment (DSC60; Shimadzu Corporation) Sample size: Approx. 5 mg Temperature rise: 10℃ / min Measurement range: Room temperature to 150℃ Measurement environment: Nitrogen gas atmosphere

[0041] The ratio of the amount of wax on the toner surface to the amount of wax in the toner is preferably in the range of 0.28 to 0.45, more preferably in the range of 0.30 to 0.40. If the amount of surface wax in the initial toner exceeds 0.45, there is no margin for storage stability. It is considered that the surface wax is likely to bleed out and form toner aggregates when stored at high temperatures. In addition, it is considered that the external additives are buried starting from the exposed parts of the wax, resulting in a deterioration of stress resistance. Furthermore, if the wax amount is less than 0.28, the amount of wax near the surface is insufficient, and sufficient releasability cannot be obtained, causing abnormal images due to offset.

[0042] The amount of wax near the surface of the toner particles can be obtained by FTIR-ATR (attenuated total reflection infrared spectroscopy) method. Based on the measurement principle, the analysis depth is about 0.3 μm, and this analysis makes it possible to determine the relative amount of wax in a region 0.3 μm deep from the surface of the toner particle.

[0043] The measurement method is as follows. First, as a sample, 3 g of the toner was pressed for 1 minute under a load of 6 t in an automatic pellet molding machine (Type M No. 50 BRP-E; manufactured by MAEKAWA TESTING MACHINE CO.) to prepare a 40 mmφ (approximately 2 mm thick) pellet. The surface of the toner pellets was measured by the FTIR-ATR method. The micro-FTIR device used was a PERKIN ELMER Spectrum One equipped with a MultiScope FTIR unit, and measurements were taken with a micro-ATR of a germanium (Ge) crystal with a diameter of 100 μm. Infrared incident angle 41.5°, resolution 4cm -1 The measurements were made 20 times in total.

[0044] The peak Wabs (2850 cm) derived from the wax obtained -1 ) and the peak Rabs (styrene acrylic resin 1729 cm ) derived from the binder resin -1 The intensity ratio (Wabs / Rabs) was taken as the relative amount of wax near the toner particle surface. The value was the average value obtained by measuring four times at different measurement locations.

[0045] [Toner manufacturing method] The toner can be produced by a known method including a melt-kneading process of melting and kneading toner materials, a pulverizing process of pulverizing the resulting molten and kneaded material, a classification process of classifying the pulverized material obtained by the pulverization, and an external addition process of externally adding an external additive to the resulting toner base particles.

[0046] In the melt-kneading step, the toner materials are mixed, and the mixture obtained is charged into a melt-kneader and melt-kneaded. As the melt-kneader, for example, a single-screw or twin-screw continuous kneader or a batch-type kneader using a roll mill can be used, and for example, a KTK twin-screw extruder manufactured by Kobe Steel, Ltd., a TEM extruder manufactured by Toshiba Machine Co., Ltd., a twin-screw extruder manufactured by KCK Corporation, a PCM twin-screw extruder manufactured by Ikegai Corporation, a co-kneader manufactured by Buss Co., Ltd., etc. are preferably used. The melt-kneading is preferably carried out under appropriate conditions so as not to cut the molecular chains of the binder resin. Specifically, the melt-kneading temperature is preferably set with reference to the softening point of the binder resin. If the temperature is too high above the softening point, severe cutting may occur, and if the temperature is too low, dispersion may not proceed.

[0047] In the pulverization step, the kneaded product obtained in the melt-kneading step is pulverized. In this pulverization, it is preferable to first coarsely pulverize the kneaded product and then finely pulverize it. Suitable examples of the pulverization method include a method of pulverizing the product by colliding it with a collision plate in a jet stream, a method of pulverizing the product by colliding particles with each other in a jet stream, and a method of pulverizing the product in a narrow gap between a mechanically rotating rotor and a stator.

[0048] In the classification step, the pulverized material obtained in the pulverization step is classified to adjust the particles to a predetermined particle size. Examples of the classification method include a method of removing fine particles using a cyclone, a decanter, a centrifuge, etc. After the pulverization step and the classification step are completed, the pulverized material is classified in an air stream by centrifugal force, etc., to produce toner base particles of a predetermined particle size.

[0049] In the external addition step, an external additive is added to the toner base particles obtained in the classification step. The toner base particles and the external additive are mixed and stirred using a mixer, so that the external additive is coated on the surfaces of the toner base particles while being crushed. By mixing and stirring and applying a mechanical impact force, the external additive can be attached to the toner base particles.

[0050] Methods for applying a mechanical impact force include, for example, a method in which an impact force is applied to particles using a blade rotating at high speed, and a method in which particles are introduced into a high-speed air stream and accelerated, and then the particles collide with each other or the composite particles with an appropriate collision plate to apply an impact force. Examples of devices that apply mechanical impact force include an Angmill (manufactured by Hosokawa Micron Corporation), a modified I-type mill (manufactured by Japan Pneumatic Co., Ltd.) with reduced grinding air pressure, a Hybridization System (manufactured by Nara Machinery Works), a Cryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), and an automatic mortar.

[0051] (Developer) The developer of the present invention contains at least the toner, and further contains other components such as a carrier, which are appropriately selected as necessary.

[0052] When the toner of the present invention is used as a developer, it may be used as a one-component developer composed of only the toner, or may be mixed with a carrier to be used as a two-component developer, and is not particularly limited. However, the toner of the present invention is preferred because it is resistant to stress even in the one-component developer, which is a more severe condition that is easily subjected to stress in an image forming device, has excellent low-temperature fixing properties, and can form high-quality images for a long period of time. In addition, when used in a high-speed printer or the like that corresponds to the recent improvement in information processing speed, a two-component developer is preferred from the viewpoint of improving life.

[0053] When the developer is a two-component developer containing the toner of the present invention and a carrier, the carrier may be a magnetic carrier or a non-magnetic carrier depending on the two-component development method. Examples of the magnetic carrier include magnetite, spinel ferrites such as gamma iron oxide, spinel ferrites containing one or more metals other than iron (Mn, Ni, Zn, Mg, Cu, etc.), magnetoplumbite-type ferrites such as barium ferrite, and particles of iron or alloys having an oxide layer on the surface.

[0054] The shape of the magnetic carrier may be any of granular, spherical and needle-like. Among these, when particularly high magnetization is required, it is preferable to use ferromagnetic fine particles such as iron, and from the standpoint of chemical stability, magnetite, spinel ferrite containing gamma iron oxide, and magnetoplumbite-type ferrite such as barium ferrite are preferred. Specific preferred examples of the magnetoplumbite ferrite include MFL-35S and MFL-35HS (manufactured by Powder Tech Co., Ltd.); DFC-400M, DFC-410M, and SM-350NV (manufactured by DOWA IP Creation Co., Ltd.).

[0055] As the magnetic carrier, a resin carrier containing magnetic fine particles such as ferromagnetic fine particles and having a desired magnetization by selecting the type and content of the fine particles can also be used. The magnetic properties of the resin carrier are preferably 30 emu / g to 150 emu / g in terms of magnetization strength at 1,000 oersted.

[0056] Examples of the method for producing the resin carrier include a method for producing the resin carrier by spraying a molten mixture of magnetic fine particles and an insulating binder resin with a spray dryer; a method for producing a resin carrier in which magnetic fine particles are dispersed in a condensation type binder resin by reacting and curing a monomer or prepolymer in an aqueous medium in the presence of magnetic fine particles; and a method for producing a resin carrier by fixing positively or negatively charged fine particles or conductive fine particles to the surface of the magnetic carrier, coating the surface of the magnetic carrier with a resin, or coating the surface of the magnetic carrier with a resin containing positively or negatively charged fine particles or conductive fine particles. By these methods, the chargeability can be appropriately controlled.

[0057] Examples of the resin for coating include silicone resin, acrylic resin, epoxy resin, fluorine-based resin, etc. Among these, silicone resin and acrylic resin are preferable.

[0058] The carrier content in the two-component developer is preferably 85% by mass or more and less than 98% by mass. When the content is 85% by mass or more, the occurrence of defective images due to the tendency of toner scattering from the developing device can be suppressed. When the content is less than 98% by mass, the charge amount of the electrophotographic toner can be suppressed from increasing excessively and the supply amount of the electrophotographic toner can be suppressed from being insufficient, and a decrease in image density and the occurrence of defective images can be effectively prevented.

[0059] (Toner storage unit) The toner storage unit in the present invention refers to a unit having a function of storing toner, which stores the above-mentioned toner of the present invention. Examples of the toner storage unit include a toner storage container, a developing device, and a process cartridge. The toner storage container refers to a container that stores the toner. The developing device has a means for containing the toner and performing development. The process cartridge is a cartridge which integrates at least an image carrier and a developing unit, contains the toner, and is detachably mountable to an image forming apparatus. The process cartridge may further include at least one selected from a charging unit, an exposure unit, and a cleaning unit.

[0060] The toner storage unit of the present invention stores the toner of the present invention. By mounting the toner storage unit of the present invention on an image forming apparatus and forming an image, the toner of the present invention, which is resistant to stress and has excellent low-temperature fixing property, is used to form an image, so that high-quality images can be formed for a long period of time.

[0061] (Image forming apparatus and image forming method) The image forming apparatus of the present invention has at least an electrostatic latent image carrier, an electrostatic latent image forming means, a developing means, a transfer means, and a fixing means, and further has other means appropriately selected as necessary, such as a discharging means, a cleaning means, a recycling means, a control means, etc.

[0062] The image forming method of the present invention includes at least an electrostatic latent image forming step, a developing step, a transferring step, and a fixing step, and further includes other steps appropriately selected as necessary, such as a discharging step, a cleaning step, a recycling step, and a control step. The image forming method of the present invention can be suitably carried out by the image forming apparatus of the present invention, and the electrostatic latent image forming step can be performed by the electrostatic latent image forming means, the developing step can be performed by the developing means, the transfer step can be performed by the transfer means, the fixing step can be performed by the fixing means, and the other steps can be performed by the other means.

[0063] <Electrostatic latent image forming process and electrostatic latent image forming means> The electrostatic latent image forming step is a step of forming an electrostatic latent image on an electrostatic latent image bearing member. The electrostatic latent image forming unit is a unit for forming an electrostatic latent image on an electrostatic latent image carrier. The electrostatic latent image carrier (sometimes referred to as a "photoconductive insulator" or "photoreceptor") is not particularly limited in terms of its material, shape, structure, size, etc., and may be appropriately selected from known ones. A preferred shape is a drum shape, and examples of its material include inorganic photoreceptors such as amorphous silicon and selenium, and organic photoreceptors such as polysilane and phthalopolymethine.

[0064] Examples of the organic photoreceptor include a laminated type photoreceptor having a laminated structure in which a layer (charge generation layer) in which a charge generation material such as metal-free phthalocyanine or titanyl phthalocyanine is dispersed in a binder resin and a layer (charge transport layer) in which a charge transport material is dispersed in a binder resin are stacked on a support such as an aluminum drum, and a single-layer type photoreceptor having a single-layered photosensitive layer in which both a charge generation material and a charge transport material are dispersed in a binder resin on a support. In the single-layer type photoreceptor, a hole transport material and an electron transport material can also be added to the photosensitive layer as charge transport materials. An undercoat layer may be provided between the support and the multi-layer charge generating layer or the single-layer photosensitive layer.

[0065] The electrostatic latent image can be formed, for example, by uniformly charging the surface of the electrostatic latent image bearing member and then exposing it imagewise, and can be formed by the electrostatic latent image forming unit. The electrostatic latent image forming unit includes, for example, at least a charger that uniformly charges the surface of the electrostatic latent image carrier, and an exposure device that imagewise exposes the surface of the electrostatic latent image carrier. The charging can be carried out, for example, by applying a voltage to the surface of the electrostatic latent image bearing member using the charger.

[0066] The charger is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charger include a contact charger known per se having a conductive or semiconductive roller, brush, film, rubber blade, or the like, and a non-contact charger utilizing corona discharge such as a corotron or scorotron.

[0067] The charger is preferably disposed in contact or non-contact with the electrostatic latent image carrier, and charges the surface of the electrostatic latent image carrier by applying a superimposed DC voltage and an AC voltage to the charger. The charger is preferably a charging roller disposed in close proximity to the photoconductor in a non-contact manner via a gap tape, and charges the surface of the photoconductor by applying a superimposed DC voltage and an AC voltage to the charging roller.

[0068] The exposure can be carried out, for example, by exposing the surface of the electrostatic latent image bearing member imagewise using the exposure unit. The exposure device is not particularly limited as long as it can perform image-wise exposure on the surface of the photoconductor charged by the charger, and can be appropriately selected depending on the purpose, and examples thereof include a copying optical system, a rod lens array system, a laser optical system, a liquid crystal shutter optical system, etc. Note that a light back system in which image-wise exposure is performed from the back side of the photoconductor may be adopted.

[0069] <Developing step and developing means> The developing step is a step of developing the electrostatic latent image with the toner or developer of the present invention to form a visible image. The developing means is a means for developing the electrostatic latent image with the toner or the developer of the present invention to form a visible image. The visible image can be formed, for example, by developing the electrostatic latent image with the toner or the developer of the present invention, and can be formed by the developing unit.

[0070] The developing means is not particularly limited as long as it can develop using the toner or the developer of the present invention, and can be appropriately selected from known ones. For example, a developing means that contains the toner or the developer of the present invention and has at least a developing unit that can apply the toner or the developer to the electrostatic latent image in a contact or non-contact manner is preferable, and a developing unit that is detachably provided with the toner container of the present invention is more preferable.

[0071] The developing device may be of a dry developing type or a wet developing type, and may be a single-color developing device or a multi-color developing device. For example, a suitable example is one having an agitator that frictionally agitates the toner or developer to charge it, and a rotatable magnetic roller.

[0072] In the developing device, for example, the toner and the carrier are mixed and stirred, and the toner is charged by friction during this process and held in a bristled state on the surface of a rotating magnet roller to form a magnetic brush. Since the magnet roller is disposed in the vicinity of the electrostatic latent image carrier, a part of the toner constituting the magnetic brush formed on the surface of the magnet roller moves to the surface of the electrostatic latent image carrier by electrical attraction. As a result, the electrostatic latent image is developed by the toner, and a visible image made of the toner is formed on the surface of the electrostatic latent image carrier. It is preferable to apply an alternating electric field when moving the toner to the surface of the electrostatic latent image carrier.

[0073] <Transfer process and transfer means> The transfer step is a step of transferring the visible image onto a recording medium. The transfer means is a means for transferring the visible image onto a recording medium. The transfer step preferably uses an intermediate transfer body, and after a visible image is primarily transferred onto the intermediate transfer body, the visible image is secondarily transferred onto the recording medium. It is more preferable that the toner used is a toner of two or more colors, preferably a full-color toner, and includes a primary transfer step of transferring the visible image onto the intermediate transfer body to form a composite transfer image, and a secondary transfer step of transferring the composite transfer image onto the recording medium.

[0074] The transfer of the visible image can be performed, for example, by charging the electrostatic latent image carrier using a transfer charger, and can be performed by the transfer means. The transfer means preferably has a first transfer means for transferring the visible image onto an intermediate transfer body to form a composite transfer image, and a second transfer means for transferring the composite transfer image onto a recording medium.

[0075] The transfer means (primary transfer means, secondary transfer means) preferably has at least a transfer device that peels and charges the visible image formed on the electrostatic latent image carrier to the transferee side. The number of transfer devices may be one or more. Examples of the transfer device include a corona transfer device that uses corona discharge, a transfer belt, a transfer roller, a pressure transfer roller, and an adhesive transfer device.

[0076] The intermediate transfer body is not particularly limited and can be appropriately selected from known transfer bodies depending on the purpose. Suitable examples include a transfer belt. The transfer medium is not particularly limited and can be appropriately selected from known recording media (recording paper).

[0077] <Fixing process and fixing means> The fixing step is a step of fixing the visible image transferred onto the recording medium. The fixing means is a means for fixing the visible image transferred onto the recording medium. The fixing step may be carried out for each color toner each time it is transferred onto the recording medium, or may be carried out simultaneously for each color toner in a laminated state.

[0078] The fixing means is not particularly limited and can be appropriately selected according to the purpose, but known heating and pressurizing means are suitable. Examples of the fixing means include a combination of a heating roller and a pressure roller; a combination of a heating roller, a pressure roller and an endless belt; a means having a heating body with a heating element, a film in contact with the heating body, and a pressure member in pressure contact with the heating body through the film, and passing a transfer body on which an unfixed image has been formed between the film and the pressure member to heat and pressurize the image; and the like. The heating temperature in the fixing means is usually preferably 80°C to 200°C. In the present invention, depending on the purpose, for example, a known optical fixing device may be used together with or instead of the fixing step and fixing means.

[0079] <Other steps and other means> The charge removing step is a step of removing electricity by applying a charge removing bias to the electrostatic latent image bearing member, and can be suitably performed by a charge removing unit. The charge removing means is not particularly limited as long as it can apply a charge removing bias to the electrostatic latent image bearing member, and can be appropriately selected from known charge removers. For example, a charge removing lamp is preferably used.

[0080] The cleaning step is a step of removing the toner remaining on the electrostatic latent image bearing member, and can be suitably performed by a cleaning unit. The cleaning means is not particularly limited as long as it can remove the toner remaining on the electrostatic latent image carrier, and can be appropriately selected from among known cleaners. Suitable examples of the cleaning means include magnetic brush cleaners, electrostatic brush cleaners, magnetic roller cleaners, blade cleaners, brush cleaners, and web cleaners.

[0081] The recycling step is a step of recycling the toner removed in the cleaning step to the developing means, and can be suitably carried out by a recycling means. The recycling means is not particularly limited, and examples thereof include known transport means. The control step is a step of controlling each of the steps, and can be suitably performed by a control means. The control means is not particularly limited as long as it can control the movement of each of the means, and can be appropriately selected depending on the purpose. For example, the control means includes devices such as a sequencer and a computer.

[0082] Next, another embodiment of the image forming method of the present invention will be described with reference to FIG. 1 is a tandem type color image forming apparatus, which includes a copying machine main body 150, a paper feed table 200, a scanner 300, and an automatic document feeder (ADF) 400.

[0083] An endless belt-like intermediate transfer body 50 is provided in the center of the copying machine main body 150. The intermediate transfer body 50 is stretched around support rollers 14, 15, and 16, and can rotate clockwise in FIG. 2. An intermediate transfer body cleaning device 17 for removing residual toner on the intermediate transfer body 50 is provided near the support roller 15. An image forming unit 120 is provided on the intermediate transfer body 50 stretched around the support rollers 14 and 15 along the conveying direction of the intermediate transfer body 50, in which four image forming means 18 for yellow, cyan, magenta, and black are arranged in a row facing each other. An exposure device 21 is provided near the image forming unit 120. A secondary transfer device 22 is provided on the side of the intermediate transfer body 50 opposite the side where the image forming unit 120 is provided. In the secondary transfer device 22, a secondary transfer belt 24, which is an endless belt, is stretched around a pair of rollers 23, and the transfer paper conveyed on the secondary transfer belt 24 and the intermediate transfer body 50 can come into contact with each other. A fixing device 25 is disposed near the secondary transfer device 22. The fixing device 25 includes a fixing belt 26, which is an endless belt, and a pressure roller 27 disposed so as to be pressed against the fixing belt 26.

[0084] In the tandem image forming apparatus, a sheet inverting device 28 is disposed near the secondary transfer device 22 and the fixing device 25 for inverting the transfer paper so that images can be formed on both sides of the transfer paper.

[0085] Next, a description will be given of the formation of a full-color image (color copy) using the image forming unit 120. That is, first, an original is set on the original table 130 of the automatic document feeder (ADF) 400, or the automatic document feeder 400 is opened and an original is set on the contact glass 32 of the scanner 300, and the automatic document feeder 400 is closed.

[0086] When a start switch (not shown) is pressed, after the document is transported and moved onto the contact glass 32 when the document is set on the automatic document feeder 400, the scanner 300 is driven and the first travelling body 33 and the second travelling body 34 travel, while immediately after the document is set on the contact glass 32. At this time, light from a light source is irradiated by the first travelling body 33, and the reflected light from the document surface is reflected by a mirror in the second travelling body 34, and is received by the reading sensor 36 through the imaging lens 35 to read the color document (color image), which is converted into image information of black, yellow, magenta and cyan. Next, each image information is transmitted to each image forming means 18 in the image forming unit 120, and a visible image of each color of black, yellow, magenta and cyan is formed.

[0087] Then, the black, yellow, magenta, and cyan image information is transmitted to each image forming means 18 (black image forming means, yellow image forming means, magenta image forming means, and cyan image forming means) in the tandem image forming unit 120, and black, yellow, magenta, and cyan toner images are formed in each image forming means.

[0088] That is, as shown in FIG. 2, each of the image forming means 18 of each color (image forming means for black, image forming means for yellow, image forming means for magenta, and image forming means for cyan) in the image forming unit 120 includes an electrostatic latent image carrier 10, a charging device 160 for uniformly charging the electrostatic latent image carrier 10, an exposure device for exposing the electrostatic latent image carrier to light (L in FIG. 2) in the form of an image corresponding to each color image based on each color image information, and forming an electrostatic latent image corresponding to each color image on the electrostatic latent image carrier, a developing device 61 for developing the electrostatic latent image with each color toner (black toner, yellow toner, magenta toner, and cyan toner) to form a toner image with each color toner, a transfer charger 62 for transferring the toner image onto the intermediate transfer body 50, a cleaning device 63, and a static eliminator 64, and each monochrome image (black image, yellow image, magenta image, and cyan image) can be formed based on the image information of each color. The black image formed on the black electrostatic latent image carrier 10K, the yellow image formed on the yellow electrostatic latent image carrier 10Y, the magenta image formed on the magenta electrostatic latent image carrier 10M, and the cyan image formed on the cyan electrostatic latent image carrier 10C are sequentially transferred (primary transfer) onto the intermediate transfer body 50 which is rotated by the support rollers 14, 15, and 16. Then, the black image, the yellow image, the magenta image, and the cyan image formed on the cyan electrostatic latent image carrier 10C are superimposed on the intermediate transfer body 50 to form a composite color image (color transfer image).

[0089] On the other hand, in the paper feed table 200, one of the paper feed rollers 142 is selectively rotated to feed a sheet (recording paper) from one of the paper feed cassettes 144 provided in multiple stages in the paper bank 143, and the sheet is separated one by one by the separation roller 145 and sent to the paper feed path 146, and is conveyed by the conveyance roller 147 to be guided to the paper feed path 148 in the copying machine main body 150, and is stopped by hitting the registration roller 49. Alternatively, the paper feed roller 142 is rotated to feed a sheet (recording paper) on the manual feed tray 54, and the sheet is separated one by one by the separation roller 145 and placed in the manual feed path 53, and is also stopped by hitting the registration roller 49. The registration roller 49 is generally used while being grounded, but may be used with a bias applied to remove paper dust from the sheet.

[0090] Then, the registration rollers 49 are rotated in synchronization with the composite color image (color transfer image) composited on the intermediate transfer body 50, a sheet (recording paper) is sent between the intermediate transfer body 50 and the secondary transfer device 22, and the composite color image (color transfer image) is transferred (secondary transfer) onto the sheet (recording paper) by the secondary transfer device 22, thereby transferring and forming a color image onto the sheet (recording paper). Note that residual toner on the intermediate transfer body 50 after the image transfer is cleaned by the intermediate transfer body cleaning device 17.

[0091] The sheet (recording paper) on which the color image has been transferred and formed is transported by the secondary transfer device 22 and sent to the fixing device 25, where the composite color image (color transfer image) is fixed onto the sheet (recording paper) by heat and pressure. Thereafter, the sheet (recording paper) is switched by the switching claw 55 and discharged by the discharge rollers 56 and stacked on the paper discharge tray 57, or is switched by the switching claw 55 and inverted by the sheet inverting device 28 and guided to the transfer position again, an image is recorded on the back side as well, and then the sheet is discharged by the discharge rollers 56 and stacked on the paper discharge tray 57.

[0092] Next, one embodiment of the process cartridge is shown in Fig. 3. As shown in Fig. 3, the process cartridge 110 of this embodiment has an electrostatic latent image carrier 10 built-in, includes a charger 58 as a charging means, a developing device 40 as a developing means, and a cleaning device 90 as a cleaning means, and further includes other means as necessary. In Fig. 3, the symbol L indicates exposure from an exposure means (not shown), and the symbol 95 indicates recording paper. The electrostatic latent image carrier 10 may be the same as the electrostatic latent image carrier in the image forming apparatus. The charger 58 may be any charging member.

[0093] In the image forming process using the process cartridge shown in FIG. 3, while the electrostatic latent image carrier 10 rotates in the direction of the arrow, an electrostatic latent image corresponding to the exposed image is formed on its surface by charging the electrostatic charger 58 and exposing the electrostatic latent image carrier 10 to light L by the exposing means. This electrostatic latent image is developed with toner by the developing device 40, and the toner development is transferred to recording paper 95 by the transfer roller 80 and printed out. Next, the surface of the electrostatic latent image carrier 10 after the image transfer is cleaned by the cleaning device 90, and further discharged by a discharging means (not shown), and the above operations are repeated again. According to the image forming apparatus and image forming method of the present invention, the toner of the present invention, which is resistant to stress and has excellent low-temperature fixing property, is used, so that high-quality images can be provided for a long period of time. EXAMPLES

[0094] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. In the following description, "parts" means "parts by mass" and "%" means "% by mass" unless otherwise specified.

[0095] <Method of manufacturing styrene acrylic resin> [Production example of styrene acrylic resin 1] 100 parts of xylene, 95.0 parts of styrene, and 5.0 parts of acrylic acid were charged into a reaction vessel, mixed, and the resulting mixture was heated to 70°C. Under a nitrogen atmosphere, a solution of 3.0 parts of tert-butyl hydroperoxide, a radical polymerization initiator, dissolved in 10.0 parts of xylene was dropped into the mixture. The mixture was then kept at that temperature for 7.5 hours to terminate the radical polymerization reaction. The mixture was then heated and decompressed to remove 60.0 parts of xylene, yielding a reaction solution. Meanwhile, 500.0 parts of methanol was charged into a vessel equipped with a stirring blade and stirred. The above reaction solution was added dropwise thereto over 1 hour, and the resulting precipitate was filtered, washed, and then dried to obtain [styrene acrylic resin 1].

[0096] [Production example of styrene acrylic resin 2] The styrene acrylic resin 1 obtained by the above method and a crosslinking agent were mixed in a Henschel mixer or the like, and then melt-kneaded and reacted in the range of 150°C to 220°C using a twin-screw kneader to obtain [styrene acrylic resin 2].

[0097] <Polyethylene wax 1, 2, monoester wax 1> Polywax 500 (melting point 88°C, manufactured by Toyochem Co., Ltd.) was used as [polyethylene wax 1], Neowax (melting point 110°C, manufactured by Yasuhara Chemical Co., Ltd.) was used as [polyethylene wax 2], and LW-13 (melting point 70.5°C, manufactured by Sanyo Chemical Co., Ltd.) was used as [monoester wax 1].

[0098] Example 1 <Production of toner base 1> The toner raw materials having the following composition were premixed for 10 minutes using a Henschel mixer (FM20B, manufactured by Nippon Coke & Engineering Co., Ltd.), and then melted and kneaded at a temperature of 100°C to 130°C using a single-shaft kneader (Ko-Kneader, manufactured by Buss). The kneaded product obtained was cooled to room temperature, and then coarsely pulverized to 200μm to 300μm using a Rotoplex. Next, the mixture was finely pulverized using a counter jet mill (100AFG, manufactured by Hosokawa Micron Corporation) while appropriately adjusting the pulverization air pressure so that the weight average particle size was 5.4±0.3μm, and then classified using an air classifier (EJ-LABO, manufactured by Matsubo Corporation) while appropriately adjusting the louver opening so that the weight average particle size was 5.8±0.4μm and the ratio of weight average particle size / number average particle size was 1.25 or less, to obtain [toner base 1].

[0099] -composition- Styrene acrylic resin 2 87.8 parts 15.0 parts polyethylene wax Carbon black (C-44, manufactured by Mitsubishi Chemical Corporation) 6.0 parts Salicylic acid derivative zirconium salt 1.0 parts (TN-105, Hodogaya Chemical Co., Ltd.) Hydrophobic silica (RY200, Nippon Aerosil Co., Ltd.) 0.2 parts

[0100] <Toner manufacturing> To 100 parts of [Toner Base 1], 1.5 parts of hydrophobic silica (NY50L, manufactured by Nippon Aerosil Co., Ltd., oil-treated silica having an average particle size of 30 nm) was added, and the mixture was stirred and mixed in a Henschel mixer to obtain [Toner 1] of Example 1.

[0101] (Examples 2 to 3) [Toner 2] and [Toner 3] of Examples 2 and 3 were obtained in the same manner as in Example 1, except that the compositions in Example 1 were changed to those shown in Table 1.

[0102] Example 4 Toner 4 of Example 4 was obtained in the same manner as in Example 1, except that the premixing time using a Henschel mixer (FM20B, manufactured by Nippon Coke and Engineering Co., Ltd.) was changed to 5 minutes.

[0103] (Examples 5 to 7) [Toner 5] to [Toner 7] of Examples 5 to 7 were obtained in the same manner as in Example 1, except that the compositions in Example 1 were changed to those shown in Table 1.

[0104] Example 8 Toner 8 of Example 8 was obtained in the same manner as in Example 1, except that the composition in Example 1 was changed to that shown in Table 1.

[0105] Comparative Example 1 [Toner 9] of Comparative Example 1 was obtained in the same manner as in Example 1, except that the composition in Example 1 was changed to that shown in Table 1 and the pre-mixing time using a Henschel mixer (FM20B, manufactured by Nippon Coke and Engineering Co., Ltd.) was changed to 5 minutes.

[0106] (Comparative Examples 2 to 3) [Toner 10] and [Toner 11] of Comparative Examples 2 and 3 were obtained in the same manner as in Example 1, except that the compositions in Example 1 were changed to those shown in Table 1.

[0107] (Toner characteristics) The amount of heat absorbed by the wax (J / g) and the amount of wax on the toner surface (Wabs / Rabs) were measured by DSC (differential scanning calorimetry) for the obtained toners of Examples 1 to 8 and Comparative Examples 1 to 3. The results are shown in Table 1.

[0108] (evaluation) The following evaluations were carried out on the obtained toners of Examples 1 to 8 and Comparative Examples 1 to 3. The evaluation results are shown in Table 2.

[0109] <Low temperature fixability> A fixing tester consisting of a fixing section of an electrophotographic device (RICOH P500; manufactured by Ricoh Co., Ltd.) was used to evaluate cold offset and smear properties using plain paper ("TYPE 6000<70W>Y"; manufactured by Ricoh Co., Ltd.) and copying paper (TYPE 6200; manufactured by Ricoh Co., Ltd.) according to the following evaluation criteria. [Evaluation Criteria] ◎: Fixing temperature is 140°C or less ○: Fixing temperature is more than 140° C. and not more than 145° C. △: Fixing temperature is more than 145°C and 150°C or less. ×: Fixing temperature is more than 150° C.

[0110] <<Cold Offset>> The cold offset was evaluated by adjusting the amount of toner to develop a solid image on plain paper at 0.85±0.2 mg / cm 2 , changing the fixing roller temperature by 2° C. each time, and then evaluating whether or not cold offset occurred. [Evaluation Criteria] ◎: Fixing temperature is 140°C or less ○: Fixing temperature is more than 140° C. and not more than 145° C. △: Fixing temperature is more than 145°C and 150°C or less. ×: Fixing temperature is more than 150° C.

[0111] <<Smearing>> The smear property was evaluated based on the fixing temperature at which the density value (smear ID) of the image adhered after rubbing with a smear tester (rubbing tester type I, JIS L0823) was 0.4 or less, as measured with a spectrometer (X-Rite eXact, manufactured by X-Rite Corporation). [Evaluation Criteria] ◎: Fixing temperature is 140°C or less ○: Fixing temperature is more than 140° C. and not more than 145° C. △: Fixing temperature is more than 145°C and 150°C or less. ×: Fixing temperature is more than 150° C.

[0112] <Stress resistance> The stress resistance of the toner was evaluated using an electrophotographic device (RICOH P500, manufactured by Ricoh Co., Ltd.) and A4T My Paper (manufactured by Ricoh Co., Ltd.). Specifically, after printing 2,000 blank sheets continuously, the toner charge amount was measured and a full solid image was printed, and the charging characteristics (the rate of change in the toner charge amount before and after continuous printing) and image quality (whether or not abnormal images occurred) were evaluated.

[0113] <<Charge characteristics>> As the charging characteristics, the rate of change in the amount of toner charge before and after continuous printing was measured and evaluated according to the following evaluation criteria. [Evaluation Criteria] ◎: The rate of change in toner charge is 10% or less ○: The rate of change in toner charge is more than 10% and 15% or less. △: The rate of change in toner charge is more than 15% and 20% or less. ×: The rate of change in toner charge is more than 20%.

[0114] <<Image quality>> As for image quality, the occurrence of abnormal images such as white or black streaks or fading of images was visually observed in all solid images and blank images printed after continuous printing, and evaluated according to the following evaluation criteria. ◎: No abnormal images are generated ○: Abnormal images occur at a level that is not noticeable to the user. ×: Clearly abnormal images occur

[0115] [Table 1]

[0116] [Table 2] [Explanation of symbols]

[0117] (Fig. 1, Fig. 2) 10, 10K, 10Y, 10M, 10C Electrostatic latent image carrier 14, 15, 16 Support rollers 17 Intermediate transfer body cleaning device 18 Image forming means 21 Exposure equipment 22 Secondary transfer device 23 Support roller 24 Secondary transfer belt 25 Fixing device 26 Fixing belt 27 Pressure roller 28 Sheet reversing device 32 Contact Glass 33 First Running Body 34 Second Running Body 35 Imaging Lens 36 Reading sensor 40 Developer 49 Registration roller 50 Intermediate transfer body 52 Separation roller 53 Manual feed path 54 Manual feed tray 55 Switching claw 56 Discharge roller 57 Output tray 61 Developing device 62 Transfer charger 63 Cleaning Equipment 64 Static eliminator 80 Transfer roller 120 Image forming unit 130 Manuscript stand 142 Paper feed roller 143 Paper Bank 144 Paper feed cassette 145 Separation roller 146 Paper feed path 147 Transport roller 148 Paper feed path 150 Copying device body 160 Charging device 200 Paper feed table 300 Scanner 400 Automatic Document Feeder (ADF) L exposure

[0118] (Figure 3) 10 Electrostatic latent image carrier 40 Developer 58 Charger 80 Transfer roller 90 Cleaning Equipment 95 Recording Paper 110 Process cartridge L exposure [Prior art documents] [Patent documents]

[0119] [Patent Document 1] JP 2014-85566 A [Patent Document 2] JP 2010-151996 A [Patent Document 3] JP 2014-199422 A [Patent Document 4] JP 2010-191219 A

Claims

1. A toner containing toner base particles including at least a binder resin, a release agent, and a colorant, and an external additive, the amount of heat absorbed by the release agent as determined by a DSC (differential scanning calorimeter) method is 7.0 [J / g] or more and 15.0 [J / g] or less; When the peak intensity of the peak derived from the release agent determined by FTIR-ATR (attenuated total reflection infrared spectroscopy) is defined as Wabs and the peak intensity of the peak derived from the binder resin is defined as Rabs, the Wabs and the Rabs satisfy the following relational expression (1): A toner characterized by: 0.28≦W / R≦0.45 (1)

2. 2. The toner according to claim 1, wherein the binder resin is a styrene-acrylic resin, and the release agent is a polyethylene wax.

3. 3. The toner according to claim 1, wherein the amount of heat absorption attributable to the release agent is at least 8.0 [J / g] to 11.0 [J / g].

4. The toner according to claim 1 or 2, wherein the toner base particles contain metal oxide particles therein.

5. 3. The toner according to claim 1, wherein the toner base particles are obtained by a pulverization method.

6. A toner storage unit, comprising the toner according to claim 1 or 2 stored therein.

7. A developer comprising the toner according to claim 1 or 2 and a carrier.

8. an electrostatic latent image carrier; and an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image carrier; a developing unit having a toner for developing the electrostatic latent image formed on the electrostatic latent image carrier to form a visible image, 3. An image forming apparatus, comprising the toner according to claim 1 or 2.

Citation Information

Patent Citations

  • Toner for electrophotography

    JP2010151996A

  • toner

    JP2010191219A

  • Toner, manufacturing method of toner, and process cartridge

    JP2014085566A

  • Toner binder and resin particle

    JP2014199422A