Silicon single crystal manufacturing method, and silicon single crystal manufacturing device

The silicon single crystal manufacturing method and apparatus stabilize the convection mode using a heater with uneven heat distribution and support electrodes, ensuring consistent oxygen concentration and improved yield and efficiency.

JP2024158935AActive Publication Date: 2024-11-08SUMCO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023074578
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

Existing methods for controlling the convection mode in silicon single crystal manufacturing using the MCZ method are prone to variations due to workmanship issues and require special equipment configurations, making it difficult to achieve a stable oxygen concentration in the silicon single crystal.

Method used

A silicon single crystal manufacturing method and apparatus that utilizes a heater configuration with uneven heat generation and heat removal distribution, combined with a specific arrangement of support electrodes and a heat insulating material, to stabilize the convection mode of the silicon melt, allowing for consistent oxygen concentration.

Benefits of technology

The method and apparatus enable the production of silicon single crystals with stable oxygen concentration, improving yield, energy efficiency, and reducing waste without significant modifications to conventional equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158935000001_ABST
    Figure 2024158935000001_ABST
Patent Text Reader

Abstract

To provide a silicon single crystal manufacturing method capable of manufacturing a silicon single crystal with a stable oxygen concentration without significantly changing a conventional device configuration.SOLUTION: A silicon single crystal manufacturing device comprises: a cylindrical heater surrounding a crucible; and first to fourth support electrodes supporting the heater. The heater comprises first to fourth heat generating parts. The first support electrode connects the first and second heat generating parts to a positive electrode of a power source, and the second support electrode connects the second and third heat generating parts to a negative electrode of the power source. The third support electrode connects the third and fourth heat generating parts to a positive electrode, and the fourth support electrode connects the fourth and first heat generating parts to a negative electrode. At least one of the first to fourth support electrodes is constituted of a diameter-reduced support electrode whose thickness is at least partially thinner than that of remaining support electrodes. The rotating crucible is heated in a state where heat distribution of the heater is uneven to create a silico melt, stars applying a horizontal magnetic field to the silicon melt, and grows the silicon single crystal.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a silicon single crystal and an apparatus for producing a silicon single crystal. [Background technology]

[0002] As a method for producing silicon single crystals, the MCZ (magnetically coupled Czochralski) method, in which a horizontal magnetic field is applied to a silicon melt, is sometimes used. When a horizontal magnetic field is applied to a silicon melt using the MCZ method, the direction of convection in a virtual plane perpendicular to the direction of application of the horizontal magnetic field in the silicon melt may be clockwise (hereinafter, sometimes referred to as "right vortex mode") or counterclockwise (hereinafter, sometimes referred to as "left vortex mode").

[0003] Whether the convection mode is the right vortex mode or the left vortex mode is random, and the concentration of oxygen taken into the silicon single crystal varies depending on the convection mode and the environment inside the furnace. In order to obtain a silicon single crystal with a stable oxygen concentration, it is important to control the convection mode of the silicon melt during pulling. For this reason, various methods for controlling the convection mode of the silicon melt in the crucible have been studied (for example, see Patent Document 1).

[0004] Patent Document 1 discloses a method of fixing the convection mode to one of the right vortex mode and the left vortex mode by making the thermal environment in the furnace of the manufacturing apparatus asymmetrical with respect to the central axis of the crucible, thereby eliminating the variation in oxygen concentration caused by the convection mode.As a specific method, Patent Document 1 discloses a method of using a heating unit in which the heat generation amount of a first heating region on one side in the left-right direction in a virtual plane perpendicular to the application direction of a horizontal magnetic field in the silicon melt and the heat generation amount of a second heating region on the other side are set to different values.

[0005] Patent document 1 discloses a method for making the heat generation amounts of the first heating area and the second heating area different by making the contact resistance values ​​of the power supply units that supply power to the heat generating elements of each of the first and second heating areas different. The methods disclosed for varying the contact resistance values ​​include varying the total number of electrical resistance adjustment members interposed between the terminals and electrodes connected to the heat generating parts of the first and second heating areas, varying the fastening force of the fastening means fastening the terminals and electrodes connected to the heat generating parts of the first and second heating areas, and varying the material or thickness of the adhesive layer joining the terminals and electrodes connected to the heat generating parts of the first and second heating areas.

[0006] Patent document 1 also discloses another method of making the heat generation amounts of the first heating area and the second heating area different, which is to make at least one of the length and total number of slits provided in the first and second heating areas different. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent Publication No. 2022-102247 Summary of the Invention [Problem to be solved by the invention]

[0008] However, in the method of varying the contact resistance value disclosed in Patent Document 1, when the contact resistance value is set to a desired value, the convection mode of the silicon melt may change from the desired state due to the influence of work variations, deterioration of components, etc. In addition, the method of varying at least one of the length and the total number of slits disclosed in Patent Document 1 requires a heating unit with a special shape.

[0009] An object of the present invention is to provide a silicon single crystal manufacturing method and a silicon single crystal manufacturing apparatus that are capable of manufacturing silicon single crystals with a stable oxygen concentration without significantly modifying the conventional apparatus configuration. [Means for solving the problem]

[0010] The method for producing a silicon single crystal of the present invention is a method for producing a silicon single crystal by using a silicon single crystal production apparatus to pull up a silicon single crystal while applying a horizontal magnetic field to a silicon melt, the silicon single crystal production apparatus comprising: a crucible for accommodating the silicon melt; a heater formed in a cylindrical shape surrounding the crucible and arranged so that a central axis of the cylinder is coaxial with a central axis of the crucible; and a first supporting electrode, a second supporting electrode, a third supporting electrode and a fourth supporting electrode formed in a rod shape from a conductive material and supporting the heater, the heater comprising a first heating portion, a second heating portion, a third supporting electrode and a fourth supporting electrode which have the same heating characteristics as each other and are arranged in a circumferential direction of the crucible, the first supporting electrode connecting the first heating portion and the second heating portion to a positive electrode of a power source, the second supporting electrode connecting the second heating portion and the third heating portion to a negative electrode of the power source or a ground, The electrodes connect the third heating portion and the fourth heating portion to the positive electrode, and the fourth supporting electrode connects the fourth heating portion and the first heating portion to the negative electrode or the earth, and at least one of the first supporting electrode, the second supporting electrode, the third supporting electrode and the fourth supporting electrode is configured as a thin-diameter supporting electrode having at least a portion thinner than the remaining supporting electrodes. The method for producing a silicon single crystal includes a silicon melt generating step of heating the silicon raw material in the rotating crucible in a state where the heat distribution of the heater is non-uniform to generate the silicon melt, a magnetic field application step of starting to apply the horizontal magnetic field to the silicon melt, and a growing step of growing the silicon single crystal by pulling up a seed crystal immersed in the silicon melt when the direction of convection of the silicon melt in a virtual plane perpendicular to the central magnetic field line of the horizontal magnetic field is fixed in one direction.

[0011] In the silicon single crystal manufacturing method of the present invention, it is preferable that the silicon single crystal manufacturing apparatus is provided with a thermal insulator formed in a cylindrical shape surrounding the heater and configured so that the heat extraction distribution to the heater is non-uniform.

[0012] In the method for producing a silicon single crystal of the present invention, it is preferable that the insulating material is configured so as to have a uniform thermal conductivity throughout, and is arranged so that the central axis of the insulating material is not coaxial with the central axis of the crucible.

[0013] In the method for producing a silicon single crystal of the present invention, it is preferable that the insulation material is configured so that the thermal conductivity of one portion is different from the thermal conductivity of the other portion, and that the central axis of the insulation material is positioned coaxially with the central axis of the crucible.

[0014] In the method for producing a silicon single crystal of the present invention, the first support electrode, the second support electrode, the third support electrode, the fourth support electrode and the heat insulating material are preferably configured such that, when the rotation speed of the crucible when the horizontal magnetic field is applied to the silicon melt is R (rpm) and the time from the start of application of the horizontal magnetic field to the horizontal magnetic field acting on the silicon melt at a magnetic field strength at which the direction of convection is fixed is T (minutes), a maximum heating temperature position at which the heating temperature for the crucible is the highest in a planar view is located on the opposite side of the rotation direction of the crucible with respect to a first horizontal imaginary line that is perpendicular to the central magnetic field and includes the central axis of the crucible, and an angle θ (°) between a second horizontal imaginary line connecting the central axis of the crucible and the maximum heating temperature position and the first horizontal imaginary line satisfies the following formula (1): θ=360×R×T … (1)

[0015] The silicon single crystal manufacturing apparatus of the present invention is a silicon single crystal manufacturing apparatus that pulls up a silicon single crystal while applying a horizontal magnetic field to a silicon melt, and includes a crucible that contains the silicon melt, a heater that is formed in a cylindrical shape surrounding the crucible and is arranged so that the central axis of the cylinder is located coaxially with the central axis of the crucible, and a first supporting electrode, a second supporting electrode, a third supporting electrode and a fourth supporting electrode that are formed in a rod shape from a conductive material and support the heater, the heater having the same heat generating characteristics as each other and a first heating portion, a second heating portion, a third heating portion and a fourth heating portion that are arranged in a circumferential direction of the crucible. The first support electrode connects the first heating portion and the second heating portion to the positive electrode of a power source, the second support electrode connects the second heating portion and the third heating portion to the negative electrode of the power source or earth, the third support electrode connects the third heating portion and the fourth heating portion to the positive electrode, and the fourth support electrode connects the fourth heating portion and the first heating portion to the negative electrode or earth, and at least one of the first support electrode, the second support electrode, the third support electrode and the fourth support electrode is composed of a thin-diameter support electrode having at least a portion thinner than the remaining support electrodes.

[0016] In the silicon single crystal manufacturing apparatus of the present invention, it is preferable to further include a thermal insulator formed in a cylindrical shape surrounding the heater and configured so that the heat extraction distribution to the heater is non-uniform.

[0017] In the silicon single crystal manufacturing apparatus of the present invention, it is preferable that the insulation material is configured so as to have a uniform thermal conductivity throughout, and is arranged so that the central axis of the insulation material is not coaxial with the central axis of the crucible.

[0018] In the silicon single crystal manufacturing apparatus of the present invention, it is preferable that the insulation material is configured so that the thermal conductivity of one portion is different from the thermal conductivity of the other portion, and that the central axis of the insulation material is positioned coaxially with the central axis of the crucible.

[0019] In the silicon single crystal manufacturing apparatus of the present invention, the first support electrode, the second support electrode, the third support electrode, the fourth support electrode and the heat insulating material are preferably configured such that, when the rotation speed of the crucible when the horizontal magnetic field is applied to the silicon melt is R (rpm) and the time from when the application of the horizontal magnetic field is started to when the horizontal magnetic field, having a magnetic field strength at which the direction of the convection is fixed, acts on the silicon melt is T (minutes), the maximum heating temperature position at which the heating temperature for the crucible is the highest in a planar view is located on the opposite side of the rotation direction of the crucible with respect to a first horizontal virtual line that is perpendicular to the central magnetic field line of the horizontal magnetic field and includes the central axis of the crucible, and the angle θ (°) between a second horizontal virtual line connecting the central axis of the crucible and the maximum heating temperature position and the first horizontal virtual line satisfies the following formula (2). θ=360×R×T … (2) [Brief description of the drawings]

[0020] [Figure 1] 1 is a vertical cross-sectional view showing a schematic configuration of a silicon single crystal manufacturing apparatus according to an embodiment. [Diagram 2] FIG. 2 is a schematic plan view showing a heater, a heat insulating material, and a magnetic field application unit according to the embodiment. [Diagram 3] FIG. 2 is a perspective view of a heater according to the embodiment. [Figure 4] FIG. 2 is a side view showing a low resistance support electrode and a high resistance support electrode according to the embodiment. [Diagram 5] FIG. 4 is an equivalent circuit diagram of a heater and a power supply unit according to the embodiment. [Figure 6] 1A and 1B are explanatory diagrams of preferred configurations of first to fourth support electrodes and thermal insulators according to an embodiment, in which (A) is a plan view showing the position of the maximum heating temperature, and (B) is a graph showing the relationship between the elapsed time from the start of application of a horizontal magnetic field and the magnetic field strength. [Figure 7] 1 is a block diagram of a main part of a silicon single crystal manufacturing apparatus according to an embodiment. FIG. [Figure 8] 1 is a flowchart showing a method for producing a silicon single crystal according to an embodiment. [Figure 9]FIG. 4 is a plan view showing the position of a high melt temperature region in the embodiment. [Figure 10] 5 is a graph showing the incidence rate of each convection mode in the examples, where (A) shows the incidence rate of each convection mode in the comparative example and examples 1 to 8, and (B) shows the incidence rate of each convection mode in the comparative example and examples 9 to 16. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] [Embodiment] [Configuration of silicon single crystal manufacturing equipment] First, the configuration of a silicon single crystal manufacturing apparatus according to an embodiment of the present invention will be described. FIG. 1 is a vertical cross-sectional view showing a schematic configuration of a silicon single crystal manufacturing apparatus. FIG. 2 is a plan view schematic showing a heater, a heat insulating material, and a magnetic field application unit. FIG. 3 is a perspective view of the heater. FIG. 4 is a side view showing a low resistance support electrode and a high resistance support electrode. FIG. 5 is an equivalent circuit diagram of a heater and a power supply unit. FIG. 6 is an explanatory diagram of a preferred configuration of the first to fourth support electrodes and the heat insulating material, where (A) is a plan view showing the maximum heating temperature position, and (B) is a graph showing the relationship between the elapsed time from the start of application of a horizontal magnetic field and the magnetic field strength. FIG. 7 is a block diagram of the main parts of the silicon single crystal manufacturing apparatus.

[0022] 1 is an apparatus for producing a silicon single crystal SM by the MCZ method, and pulls up a silicon single crystal SM having a neck portion SM1, a shoulder portion SM2, a straight body portion SM3, and a tail portion (not shown) while applying a horizontal magnetic field to a silicon melt M. The silicon single crystal production apparatus 1 includes a chamber 2 forming an outer shell, a crucible 3 arranged in the center of the chamber 2, a heater 4 arranged around the inside of the crucible 3, and a temperature measurement unit 15.

[0023] The crucible 3 has a double structure consisting of an outer graphite crucible 3A and an inner quartz crucible 3B, and the quartz crucible 3B contains silicon melt M. The graphite crucible 3A and the quartz crucible 3B are cylindrical containers with bottoms, and are circular in plan view when viewed vertically from above. The crucible 3 is fixed to the upper end of a support shaft 5 that can rotate and move up and down.

[0024] The heater 4 is a graphite heater formed in a substantially cylindrical shape and disposed around the crucible 3. A cylindrical heat insulating material 6 is provided on the outside of the heater 4 along the inner surface of the chamber 2. The heat insulating material 6 is configured so as to have a uniform thermal conductivity throughout.

[0025] A pulling shaft 7 is disposed above the crucible 3 and coaxially with the support shaft 5. The pulling shaft 7 is formed of a wire, etc. A seed crystal SC is attached to the lower end of the pulling shaft 7.

[0026] In the chamber 2, a cylindrical heat shield 8 is disposed above the silicon melt M in the crucible 3 to surround the silicon single crystal SM being grown. The thermal shield 8 blocks radiant heat from the silicon melt M, the side wall of the crucible 3, and the heater to the silicon single crystal SM during growth, thereby suppressing a temperature rise of the silicon single crystal SM.

[0027] A gas inlet 2A is provided at the top of the chamber 2 to introduce an inert gas such as argon gas into the chamber 2. A gas exhaust port 2B is provided at the bottom of the chamber 2 to suck and exhaust gas from within the chamber 2 by driving a vacuum pump (not shown).

[0028] The temperature measuring unit 15 measures the temperatures of the first measurement point P1 and the second measurement point P2. The radial positions of the first measurement point P1 and the second measurement point P2 are between the outer peripheral surface of the silicon single crystal SM to be grown and the inner peripheral surface of the opening of the thermal shield 8. As described later, the convection mode of the silicon melt M can be confirmed by measuring the temperatures of the first measurement point P1 and the second measurement point P2. For example, when the convection direction of the silicon melt M is fixed to the right in FIG. 1 by heating the silicon melt M by the heater 4, that is, when the convection mode of the silicon melt M becomes the right vortex mode, the measured temperature of the first measurement point P1 is higher than the measured temperature of the second measurement point P2. Also, when the convection direction of the silicon melt M is fixed to the left by heating the silicon melt M by the heater 4, that is, when the convection mode becomes the left vortex mode, the measured temperature of the first measurement point P1 is lower than the measured temperature of the second measurement point P2.

[0029] The temperature measuring unit 15 includes a pair of reflecting units 15A and a pair of radiation thermometers 15B. The reflecting section 15A is installed inside the chamber 2. The reflecting section 15A is preferably installed such that the angle between the reflecting surface 15C and the horizontal plane is equal to or greater than 40° and equal to or less than 50°. The radiation thermometer 15B is installed outside the chamber 2. The radiation thermometer 15B receives radiant light L incident through a quartz window 2C (see FIG. 1) provided in the chamber 2, and measures the temperatures of the first measurement point P1 and the second measurement point P2 in a non-contact manner.

[0030] As shown in FIG. 2, the silicon single crystal manufacturing apparatus 1 further includes a magnetic field application unit 16. The magnetic field applying unit 16 includes a first magnetic body 16A and a second magnetic body 16B, each of which is formed of an electromagnetic coil. The first magnetic body 16A and the second magnetic body 16B are provided outside the chamber 2 so as to face each other across the crucible 3. The magnetic field applying unit 16 applies a horizontal magnetic field such that, in a plan view, a central magnetic field line 16C passing through the coil central axis intersects with a central axis 3C of the crucible 3 (hereinafter, may be referred to as the "crucible central axis 3C") and is in a direction from the second magnetic body 16B to the first magnetic body 16A (the upward direction indicated by the arrow indicating the central magnetic field line 16C in FIG. 2, and the direction from the front to the back of the paper in FIG. 1).

[0031] The heater 4 is arranged so that its central axis 4C (hereinafter, sometimes referred to as the "heater central axis 4C") is located on the same axis as the crucible central axis 3C. On the other hand, the heat insulating material 6 is arranged so that its central axis 6C (hereinafter, sometimes referred to as the "heater central axis 6C") is not located on the same axis as the crucible central axis 3C and the heater central axis 4C. In other words, the heater 4 is arranged so that the gap between the heater 4 and the crucible 3 is uniform in the circumferential direction of the crucible 3. The heat insulating material 6 is also arranged so that the gap between the heater 4 and the heat insulating material 6 is non-uniform in the circumferential direction of the heater 4. Due to such an arrangement of the heater 4 and the heat insulating material 6, the heat extraction distribution from the heater 4 by the heat insulating material 6 becomes non-uniform in the circumferential direction of the crucible 3.

[0032] As shown in Figs. 2 and 3, the heater 4 includes a heat generating portion 40, which is a cylindrical graphite heater. The heat generating portion 40 is formed with a uniform thickness over the entire circumference. In the heat generating portion 40, a plurality of upper slits 41 extending downward from the upper end and a plurality of lower slits 42 extending upward from the lower end are formed so as to be alternately arranged in the circumference. The upper slits 41 and the lower slits 42 have the same width dimension and the same cutting depth in the up-down direction. The interval between the upper slits 41 and the lower slits 42 is also the same over the entire circumference of the heater 4.

[0033] The heating section 40 is divided into four parts by a first vertical imaginary plane VF1 and a second vertical imaginary plane VF2 that are orthogonal to each other and include the heater central axis 4C, and includes a first heating section 40A, a second heating section 40B, a third heating section 40C, and a fourth heating section 40D that have the same heating characteristics. The same heating characteristics means that the same parts generate heat at the same temperature when the same amount of power is supplied. The first heat generating portion 40A to the fourth heat generating portion 40D have the same total number of upper slits 41 and lower slits 42. In this embodiment, two upper slits 41 and three lower slits 42 are formed in each of the first heat generating portion 40A to the fourth heat generating portion 40D, and the total number of the upper slits 41 and lower slits 42 is five each. In this manner, the first heat generating portion 40A to the fourth heat generating portion 40D having the same shape have the same resistance value. The heater 4 is disposed so that the heater central axis 4C is coaxial with the crucible central axis 3C and the central magnetic field line 16C overlaps with the first vertical imaginary plane VF1 in a plan view. The heater 4 may be disposed so that the central magnetic field line 16C does not overlap with the first vertical imaginary plane VF1 in a plan view.

[0034] The silicon single crystal manufacturing apparatus 1 includes a power supply unit 9 that supplies power to the heat generating unit 40. The power supply unit 9 includes a first terminal 91A, a second terminal 91B, a third terminal 91C, and a fourth terminal 91D, a first support electrode 92A, a second support electrode 92B, a third support electrode 92C, and a fourth support electrode 92D, and four nuts 93A, 93B, 93C, and 93D. The first terminal 91A to the fourth terminal 91D are arranged at 90° intervals along the circumferential direction of the heat generating unit 40. The first terminal 91A to the fourth terminal 91D extend downward from the lower end of the portion of the heat generating portion 40 defined by the two lower slits 42, and are formed integrally with the heat generating portion 40. The first terminal 91A to the fourth terminal 91D also include connection portions 911A to 911D bent at a right angle inward from the lower end, and through holes 912A to 912D are formed in the connection portions 911A to 911D. That is, the heater 4 is configured using a graphite heater in which the cylindrical heat generating portion 40, which is a heater element, and the first terminal 91A to the fourth terminal 91D, which are heater legs, are integrally molded.

[0035] As shown in Fig. 3, the first support electrode 92A to the fourth support electrode 92D are rod-shaped electrodes made of conductive carbon. Among the first support electrode 92A to the fourth support electrode 92D, one to three support electrodes are configured as low-resistance support electrodes 92L shown in the upper diagram of Fig. 4, and the remaining support electrodes are configured as high-resistance support electrodes 92H as small-diameter support electrodes shown in the lower diagram of Fig. 4. The low resistance support electrode 92L includes an electrode body 921L, a clamping portion 922, a male screw portion 923, and a power supply connection portion 924. The electrode body 921L is formed in a cylindrical shape. The clamping portion 922 is formed in a cylindrical shape with a larger diameter and a smaller height than the electrode body 921L, and is provided at one axial end of the electrode body 921L. The male screw portion 923 is provided so as to extend from the clamping portion 922 to the opposite side to the electrode body 921L. The power supply connection portion 924 is provided at the other axial end of the electrode body 921L. The high resistance supporting electrode 92H has a configuration including a small diameter electrode body 921H instead of the electrode body 921L. The small diameter electrode body 921H is formed in a substantially cylindrical shape with at least a part of the diameter smaller than the diameter of the electrode body 921L, and is configured so that the resistance value of the high resistance supporting electrode 92H is higher than the resistance value of the low resistance supporting electrode 92L. From the viewpoint of supporting the heater 4, the diameter of the thinnest part of the small diameter electrode body 921H is preferably 50 mm or more. As is well known, the resistance values ​​of the low resistance supporting electrode 92L and the high resistance supporting electrode 92H can be set to desired values ​​by adjusting the diameter or length of the electrode main body 921L and the small diameter electrode main body 921H. The first support electrode 92A to the fourth support electrode 92D, which are constituted by the high resistance support electrode 92H or the low resistance support electrode 92L, have carbon nuts 93A to 93D screwed into male threaded portions 923 inserted into the through holes 912A to 912D of the terminals 91A to 91D, and the terminals 91A to 91D are clamped between the nuts 93A to 93D and the clamping portions 922, thereby electrically connecting the terminals 91A to 91D and supporting the heater 4.

[0036] As shown in FIG. 5, the power supply unit 9 further includes a power source 94, a first anode wiring 95A, a first cathode wiring 95B, a second anode wiring 95C, and a second cathode wiring 95D. One end of the first and second anode wirings 95A, 95C is connected to the power supply connection parts 924 of the first and third support electrodes 92A, 92C, for example, via a connector not shown, and the other end is connected to the anode of the power supply 94. One end of the first and second cathode wirings 95B, 95D is connected to the power supply connection parts 924 of the second and fourth support electrodes 92B, 92D, for example, via a connector not shown, and the other end is connected to the cathode of the power supply 94. The other ends of the first and second cathode wirings 95B, 95D may be connected to earth.

[0037] 5, if the fourth support electrode 92D is configured as a high resistance support electrode 92H and the first support electrode 92A to the third support electrode 92C are configured as low resistance support electrodes 92L, the current flowing from the power source 94 to the fourth support electrode 92D will be smaller than the current flowing from the power source 94 to the second support electrode 92B. As a result, the first and second heating portions 40A and 40B generate heat at a higher temperature than the third and fourth heating portions 40C and 40D, and the heat distribution will be non-uniform in the circumferential direction of the crucible 3. In this manner, by configuring one to three of the first support electrode 92A to the fourth support electrode 92D as the high-resistance support electrode 92H, the position at which the heating temperature of the crucible 3 is highest in a planar view (hereinafter sometimes referred to as the "maximum heating temperature position") can be set to a desired position. Furthermore, as described above, the insulation material 6 is arranged so that the insulation material central axis 6C is not located on the same axis as the crucible central axis 3C and the heater central axis 4C, and is configured so that the heat extraction distribution from the heater 4 is non-uniform in the circumferential direction of the crucible 3. Therefore, by adjusting the position of the high resistance support electrode 92H relative to the crucible 3 and the position where the gap between the insulation material 6 and the heater 4 is smallest, the maximum heating temperature of the crucible 3 and the maximum heating temperature position can be adjusted more precisely. In the following, the state in which the crucible 3 is heated so that a maximum heating temperature position exists by adjusting the heat generation distribution of the heater 4 and the heat extraction distribution from the heater 4 by the heat insulating material 6 may be referred to as a "non-uniform heating state." On the other hand, the state in which the crucible 3 is heated so that a maximum heating temperature position does not exist, that is, the state in which the crucible 3 is heated so that the heating distribution of the crucible 3 is uniform in the circumferential direction of the crucible 3, may be referred to as a "uniform heating state."

[0038] Here, since the thermal conductivity of the crucible 3 is high and the thickness of the entire crucible 3 is uniform, the temperature of the crucible 3 heated in a non-uniform heating state by the heater 4 changes continuously. Therefore, the region heated to the highest temperature at the maximum heating temperature position in the silicon melt M (hereinafter, may be referred to as the "high-temperature melt region") and the region heated to the lowest temperature (hereinafter, may be referred to as the "low-temperature melt region") face each other across the center of the silicon melt M. The positions of the high-resistance support electrode 92H and the heat insulator 6 relative to the crucible 3 are preferably set so that the melt temperature difference, obtained by subtracting the temperature of the low-temperature melt region from the temperature of the high-temperature melt region, is 3° C. or more, and more preferably 5° C. or more. By setting the melt temperature difference to 3° C. or more, it becomes easier to fix the convection mode to one mode regardless of the timing of application of the horizontal magnetic field, and by setting it to 5° C. or more, it becomes easier to fix the convection mode to one mode regardless of the timing of application of the horizontal magnetic field.

[0039] It is preferable that the first support electrode 92A to the fourth support electrode 92D and the insulating material 6 are configured so that the heating amounts of the first portion 31A and the second portion 31B of the crucible 3, which are located on either side of the first vertical imaginary plane VF1 shown in Figures 1 and 2, are different from each other. As shown in FIG. 6(A), the first support electrode 92A to the fourth support electrode 92D and the insulating material 6 are preferably configured such that the maximum heating temperature position 3MA, where the heating temperature for the crucible 3 is the highest in a planar view, is located on the right side of the crucible central axis 3C and is located in the opposite direction of the rotation direction D1 of the crucible 3 with respect to a first horizontal imaginary line VL1 that is perpendicular to the central magnetic line 16C and includes the crucible central axis 3C, and the angle θ (°) between the first horizontal imaginary line VL1 and a second horizontal imaginary line VL2 connecting the crucible central axis 3C and the maximum heating temperature position 3MA satisfies the following formula (3). Alternatively, it is more preferable that the first support electrode 92A to the fourth support electrode 92D and the insulating material 6 are configured so that the maximum heating temperature position 3MB, where the heating temperature for the crucible 3 is the highest in a planar view, is located on the left side of the crucible central axis 3C and is located in the opposite direction of the rotational direction D1 with respect to the first horizontal imaginary line VL1, and that the angle θ (°) between the first horizontal imaginary line VL1 and a second horizontal imaginary line VL3 connecting the crucible central axis 3C and the maximum heating temperature position 3MB satisfies the following formula (3). θ=360×R×T … (3) In addition, in formula (3), R is the rotation speed (rpm) of the crucible 3 when the horizontal magnetic field is applied to the silicon melt M. T is the time (minutes) from the start of application of the horizontal magnetic field until the horizontal magnetic field with a magnetic field strength at which the convection direction is fixed (hereinafter, sometimes referred to as "convection direction fixed magnetic field strength K1") acts on the silicon melt M. The convection direction fixed magnetic field strength K1 is 0.05 Tesla (500 Gauss) or more and 0.15 Tesla (1500 Gauss) or less.

[0040] Here, the reason why first support electrode 92A to fourth support electrode 92D and heat insulating material 6 are configured so that maximum heating temperature positions 3MA, 3MB are located at the positions shown in FIG. 6(A) will be described. If the crucible 3 is heated in a uniform heating state, the silicon melt M in the crucible 3 is heated uniformly over the entire area in the circumferential direction of the crucible 3 . In this case, convection occurs in the silicon melt M, which rises near the side of the crucible 3 and falls near the center. In a state in which no horizontal magnetic field is applied to the silicon melt M, the position of the downward flow changes randomly and may deviate from the center of the crucible 3 due to instability of the convection. When application of a horizontal magnetic field is started to the silicon melt M in this state so that the magnetic field strength reaches a predetermined magnetic field strength K2, the magnitude of the magnetic field acting on the silicon melt M increases in proportion to the elapsed time from the start of application, as shown in Fig. 6(B). Then, when a horizontal magnetic field with a convection direction fixed magnetic field strength K1 acts on the silicon melt M, the rotation of the downward flow in the rotation direction D1 is restricted, and the direction of convection in an imaginary plane perpendicular to the application direction of the horizontal magnetic field is fixed. When the crucible 3 is heated in this uniform heating state, the horizontal magnetic field is applied while the position of the downward flow is changing randomly, so that the convection mode becomes either a right vortex mode or a left vortex mode depending on the timing of application of the magnetic field.

[0041] On the other hand, when the crucible 3 is heated in a non-uniform heating state, even when no horizontal magnetic field is applied to the silicon melt M, an upward flow of the silicon melt M occurs stably on the right side of the crucible 3 and a downward flow occurs stably on the left side of the crucible 3, or an upward flow occurs stably on the left side of the crucible 3 and a downward flow occurs stably on the right side of the crucible 3, and the position of the downward flow does not change randomly as in the case where the crucible 3 is heated in a uniform heating state. Furthermore, the high-temperature melt region rotates in a rotation direction D1 with the rotation of the crucible 3 at a rotation speed R (rpm). That is, the region in which an upward flow is generated in the silicon melt M moves from the vicinity of the maximum heating temperature positions 3MA, 3MB in the rotation direction D1 at the rotation speed R (rpm). As described above, the maximum heating temperature position 3MA is set to satisfy the above formula (3), so that when the horizontal magnetic field with the fixed magnetic field strength in the convection direction K1 acts on the silicon melt M after T minutes from the start of the application of the horizontal magnetic field, regardless of the timing of the application of the horizontal magnetic field, the rotation of the upward flow in the rotation direction D1 is restricted in a state where the melt high temperature region overlaps with the first horizontal virtual line VL1 in a plan view, and eventually the convection is fixed to the left and the left vortex mode is established. Also, the maximum heating temperature position 3MB is set to satisfy the above formula (3), so that when the horizontal magnetic field with the fixed magnetic field strength in the convection direction K1 acts on the silicon melt M after T minutes from the start of the application of the horizontal magnetic field, regardless of the timing of the application of the horizontal magnetic field, the rotation of the upward flow in the rotation direction D1 is restricted in a state where the melt high temperature region overlaps with the first horizontal virtual line VL1 in a plan view, and eventually the convection is fixed to the right and the right vortex mode is established. In this way, by applying a horizontal magnetic field of convection direction fixed magnetic field strength K1 to the silicon melt M when the melt high temperature region overlaps with the first horizontal virtual line VL1, a left vortex mode or a right vortex mode can be generated more stably than when a horizontal magnetic field of convection direction fixed magnetic field strength K1 is applied to the silicon melt M when the melt high temperature region does not overlap with the first horizontal virtual line VL1.

[0042] 7, the silicon single crystal manufacturing apparatus 1 further includes a raw material supply unit 18, a crucible rotation drive unit 19, a pull-up drive unit 20, an input unit 21, a memory unit 22, and a control unit 23. A power supply 94, a radiation thermometer 15B, a magnetic field application unit 16, the raw material supply unit 18, the crucible rotation drive unit 19, the pull-up drive unit 20, the input unit 21, and the memory unit 22 are connected to the control unit 23 so as to be able to transmit and receive various information.

[0043] The power supply 94 supplies power to the heat generating unit 40 via the power supply unit 9 under the control of the control unit 23 . The radiation thermometer 15B outputs a signal corresponding to the measurement result to the control unit . The magnetic field application unit 16 applies a horizontal magnetic field of a predetermined strength to the silicon melt M based on the control of the control unit 23. The raw material supply unit 18 charges the silicon raw material into the crucible 3 under the control of the control unit 23 . Under the control of the control unit 23, the crucible rotation drive unit 19 rotates the crucible 3 at a predetermined speed in a predetermined direction. The lifting drive unit 20 raises and lowers the lifting shaft 7 based on the control of the control unit 23. In addition, the lifting drive unit 20 rotates the lifting shaft 7 at a predetermined speed in the opposite direction to or in the same direction as the rotation direction of the support shaft 5 based on the control of the control unit 23.

[0044] The input unit 21 is configured with, for example, a touch panel or physical buttons. The input unit 21 is used for inputting various settings, and outputs a signal corresponding to the input operation to the control unit 23.

[0045] The storage unit 22 is configured with a well-known storage device such as a HDD (Hard Disk Drive), etc. The storage unit 22 stores various information necessary for controlling the pulling of the silicon single crystal SM.

[0046] The control unit 23 includes a CPU (Central Processing Unit). The control unit 23 controls the pulling of the silicon single crystal SM by the CPU executing a program stored in the storage unit 22.

[0047] [Method for producing silicon single crystal] Next, a method for manufacturing a silicon single crystal SM using the silicon single crystal manufacturing apparatus 1 will be described. Fig. 8 is a flow chart showing the method for manufacturing a silicon single crystal. Note that in this embodiment, a case will be described in which the first support electrode 92A to the fourth support electrode 92D and the heat insulator 6 are configured so that the maximum heating temperature position is the maximum heating temperature position 3MA shown in Fig. 6(A).

[0048] First, the operator operates the input unit 21 to input the pulling conditions for the silicon single crystal SM to be produced. As shown in FIG. 8, the control unit 23 acquires the inputted raising condition (step S1). Thereafter, the control unit 23 performs the manufacturing process of the silicon single crystal SM based on the acquired pulling conditions. Specifically, while maintaining an inert gas atmosphere under reduced pressure within chamber 2, turning off heater 4 (not supplying power to heater 4), and not applying a horizontal magnetic field, control unit 23 controls raw material supply unit 18 to load silicon raw material into crucible 3, and then controls crucible rotation drive unit 19 to rotate crucible 3 in rotation direction D1 at rotation speed R (step S2).

[0049] Next, the control unit 23 controls the power source 94 to heat the crucible 3 in a non-uniform heating state using the heat generating unit 40 of the heater 4, thereby melting the silicon raw material and generating a silicon melt M (step S3: silicon melt generating step). When all the silicon raw material is melted in step S3, the region in which an upward flow is generated in the silicon melt M moves in the rotation direction D1 at a rotation speed R (rpm) from a position near the maximum heating temperature position 3MA.

[0050] Thereafter, the control unit 23 controls the magnetic field application unit 16 to start application of a horizontal magnetic field to the silicon melt M so that the magnetic field strength becomes a predetermined magnetic field strength K2 (e.g., 0.3 Tesla) (step S4: magnetic field application step). When a horizontal magnetic field with a convection direction fixed magnetic field strength K1 (e.g., 0.1 Tesla) acts on the silicon melt M by the process of step S4, the convection of the silicon melt M is fixed counterclockwise and becomes a left vortex mode.

[0051] Next, the control unit 23 determines whether or not the convection mode of the silicon melt M has been fixed to the left vortex mode based on a signal corresponding to the measurement result from the radiation thermometer 15B (step S5: convection direction confirmation step). When the control unit 23 determines that the convection mode is not fixed to the left vortex mode (step S5: NO), the control unit 23 performs the process of step S5 again after a predetermined time has elapsed. On the other hand, when the control unit 23 determines that the convection mode is fixed to the left vortex mode (step S6: YES), it controls the pull-up drive unit 20 to grow a silicon single crystal SM while continuing to apply the horizontal magnetic field (step S6: growth step). In step S6, under the control of the control unit 23, the pull-up drive unit 20 raises and lowers the pull-up shaft 7 so as to place the seed crystal SC in the silicon melt M and then pull up the seed crystal SC, thereby growing the silicon single crystal SM.

[0052] [Effects of the embodiment] In the silicon single crystal manufacturing apparatus 1, the first heat generating portion 40A to the fourth heat generating portion 40D of the heater 4 are electrically connected to a power source 94, and at least one of the first support electrode 92A to the fourth support electrode 92D that support the heater 4 is composed of a high-resistance support electrode 92H. By configuring the first support electrode 92A to the fourth support electrode 92D in this manner, the current flowing through the high resistance support electrode 92H can be made smaller than the current flowing through the low resistance support electrode 92L, and the heat generation temperatures of the first heat generating portion 40A to the fourth heat generating portion 40D can be made non-uniform. Therefore, the crucible 3 can be heated in a non-uniform heating state, and the downward flow of the silicon melt M can be generated at a stable position. Therefore, by applying a horizontal magnetic field to the silicon melt M in which the downward flow is generated at a stable position, the convection mode of the silicon melt M can be fixed to a desired state, and a silicon single crystal SM with a stable oxygen concentration can be manufactured. In addition, since a silicon single crystal SM with a stable oxygen concentration can be manufactured, the yield of the silicon single crystal SM is improved, and it is possible to realize improved energy efficiency, improved production efficiency, and reduced waste. Furthermore, since a non-uniform heating state can be achieved simply by using the high resistance support electrode 92H as at least one of the first support electrode 92A to the fourth support electrode 92D, a conventional heater 4 can be used and there is no need to significantly modify the conventional device configuration. Furthermore, the resistance value of the high resistance support electrode 92H can be adjusted to a large value by a simple method of simply adjusting the diameter of the small diameter electrode main body 921H, and a desired non-uniform heating state can be easily achieved.

[0053] [Variations] Although an embodiment of the present invention has been described in detail above with reference to the drawings, the specific configuration is not limited to this embodiment, and various improvements and design changes that do not deviate from the gist of the present invention are also included in the present invention.

[0054] When a plurality of the first to fourth support electrodes 92A to 92D are constituted by high resistance support electrodes 92H, the resistance value of at least one of the high resistance support electrodes 92H may be higher than the resistance values ​​of the other high resistance support electrodes 92H.

[0055] The heat insulating material 6 may be arranged so that the heat insulating material central axis 6C is positioned on the same axis as the crucible central axis 3C and the heater central axis 4C, so that the heat extraction distribution to the crucible 3 is uniform. Although an example has been given of a configuration using an insulating material 6 with a uniform thermal conductivity overall, a cylindrical insulating material configured so that the thermal conductivity of one part is different from that of the other parts may also be arranged so that the central axis of the insulating material is positioned on the same axis as the crucible central axis 3C and the heater central axis 4C, thereby configuring the heat extraction distribution to the crucible 3 to be non-uniform.In this case, the thermal conductivity of the insulating material may be set to satisfy the above formula (3), or may not be set to satisfy it. EXAMPLES

[0056] Next, examples of the present invention will be described, but the present invention is not limited to the examples.

[0057] [Experimental conditions] [Definition of the position of the high-temperature region of the melt] Positions A to H, which represent the positions of the melt high temperature region in a plan view, are defined as shown in Fig. 9. Position A is a position where the angle between a reference line extending forward in the application direction of the central magnetic field line 16C from the center of the silicon melt M in a plan view and a level line extending from the center of the silicon melt M to position A is 0°. Positions B, C, D, E, F, G, and H are positions rotated by 45°, 90°, 135°, 180°, 225°, 270°, and 315° clockwise from position A.

[0058] Comparative Example First, the silicon single crystal manufacturing apparatus 1 of the above embodiment was prepared. Then, the first support electrode 92A to the fourth support electrode 92D were all made to have the same thickness, and the heat insulator 6 was arranged so that the heat insulator central axis 6C was positioned coaxially with the crucible central axis 3C and the heater central axis 4C. In the comparative example, the crucible 3 is heated in a uniform heating state, so that no high-temperature melt region or low-temperature melt region is generated in the silicon melt M. In other words, under the conditions of the comparative example, the melt temperature difference is 0°C. Then, by carrying out the processes of steps S1 to S6 in the manufacturing method of the silicon single crystal SM, a silicon single crystal SM having a straight body portion SM3 with a diameter of 300 mm and a length of 2000 mm was grown. The rotation direction D1 of the crucible 3 is the counterclockwise direction in FIG.

[0059] [Examples 1 to 16] In Examples 1 to 8, the insulator 6 was arranged so that the insulator central axis 6C was coaxial with the crucible central axis 3C and the heater central axis 4C. Then, the thicknesses of the first support electrode 92A to the fourth support electrode 92D were adjusted so that the melt high temperature regions were located at positions A, B, C, D, E, F, G, and H, respectively, and the melt temperature difference was 3° C., and a silicon single crystal SM was grown under the same conditions as in the comparative example. In Examples 9 to 16, silicon single crystals SM were grown under the same conditions as in Examples 1 to 8, except that the position of the insulation material 6 relative to the crucible 3 and heater 4 was adjusted so that the high melt temperature regions were located at positions A, B, C, D, E, F, G, and H, respectively, and the melt temperature differences were each 5°C.

[0060] [evaluation] Before starting the growth of silicon single crystal SM in the comparative example and examples 1 to 16, a horizontal magnetic field was applied at random timing after the generation of silicon melt M to observe the convection modes, and the occurrence rate of each convection mode and the stability of the generated vortexes were evaluated. The occurrence rate of each convection mode is shown in Table 1 below and Figures 10(A) and (B), and the evaluation results of the vortex stability are shown in Table 1.

[0061] [Table 1]

[0062] In the comparative example, the occurrence rate of the right vortex mode was almost the same as that of the left vortex mode, as shown in Table 1 and Figures 9(A) and (B). In addition, in the comparative example, the direction of the vortex once fixed reversed with a probability of 10% or more. The reason for this result is believed to be that crucible 3 was heated in a uniform heating state, and the position of the downward flow changed randomly, resulting in a right-vortex mode or a left-vortex mode depending on the timing of application of the horizontal magnetic field.

[0063] On the other hand, in Examples 1 to 8, as shown in Table 1 and Figure 9 (A), the difference between the occurrence rate of the right vortex mode and the occurrence rate of the left vortex mode was 10% or more, and it was confirmed that, compared to the comparative example, it was easier to fix the convection mode to one mode regardless of the timing of application of the horizontal magnetic field. The reason for this result is believed to be that crucible 3 was heated in a non-uniform manner, which fixed the position of the downward flow, increasing the probability that the convection mode would be fixed to one mode regardless of the timing of application of the horizontal magnetic field.

[0064] In particular, in Examples 3, 4, 6, and 7, the difference between the occurrence rate of the right vortex mode and the occurrence rate of the left vortex mode was 30% or more, and it was confirmed that it was easier to fix one convection mode regardless of the application timing of the horizontal magnetic field compared to Examples 1, 2, 5, and 8. Furthermore, in Examples 1, 2, and 5, the direction of the vortex once fixed reversed with a probability of 10% or more, but in Examples 3, 4, 6 to 8, the probability that the direction of the vortex once fixed reversed was less than 10%.

[0065] From a comparison between the comparative example and Examples 1 to 8, it was confirmed that by adjusting at least the thicknesses of the first support electrode 92A to the fourth support electrode 92D and the arrangement position of the insulating material 6, so that the melt temperature difference is 3°C or more, it is possible to easily fix the convection mode to one mode, and that it is possible to produce silicon single crystals with a stable oxygen concentration without significantly modifying the conventional apparatus configuration.

[0066] 9(B), in Examples 9 to 16, the difference between the occurrence rate of the right vortex mode and the occurrence rate of the left vortex mode was 40% or more, and it was confirmed that the direction of the convection was more easily fixed in one direction regardless of the application timing of the horizontal magnetic field compared to the comparative example and Examples 1 to 8. Furthermore, in Examples 9 to 16, the probability that the direction of the vortex once fixed would be reversed was less than 10%. The reason for these results is believed to be that the melt temperature difference was larger than in Examples 1 to 8, resulting in a stronger downward flow than in Examples 1 to 8, and the position of the downward flow was fixed, thereby increasing the probability that the convection direction would be fixed in one direction regardless of the timing of application of the horizontal magnetic field.

[0067] In particular, in Examples 10 to 12 and 14 to 16, the difference between the occurrence rate of the right vortex mode and the occurrence rate of the left vortex mode was 70% or more, and it was confirmed that, compared to Examples 9 and 13, it was easier to fix the direction of convection in one direction regardless of the timing of application of the horizontal magnetic field. The reason for these results is believed to be that in Examples 9 and 13, the high-temperature melt region is located on the central magnetic field line 16C in a planar view, and therefore the downward flow generated on the opposite side of the melt cooling region from the center of the silicon melt M occurs near the central magnetic field line 16C, whereas in Examples 10 to 12 and 14 to 16, the high-temperature melt region is located to the right or left of the central magnetic field line 16C in a planar view, and therefore the downward flow occurs in a region away from the central magnetic field line 16C, and therefore, compared to Examples 9 and 13, the probability that the convection direction is fixed in one direction is further increased.

[0068] Furthermore, in Examples 11, 12, 15, and 16, the difference between the occurrence rate of the right vortex mode and the occurrence rate of the left vortex mode was 100%, confirming that, compared to Examples 10 and 14, it was easier to fix the direction of convection in one direction regardless of the timing of application of the horizontal magnetic field. The reason why such a result was obtained is considered as follows. As described above, the high-temperature melt region rotates in the rotation direction D1 with the rotation of the crucible 3. The high-temperature melt region of Example 10 is located forward of the rotation direction D1 with respect to the high-temperature melt region of Examples 11 and 12, and the high-temperature melt region of Example 14 is located forward of the rotation direction D1 with respect to the high-temperature melt region of Examples 15 and 16. For this reason, the position of the high-temperature melt region when a horizontal magnetic field of 0.1 Tesla, which is the convection direction fixed magnetic field strength K1, acts in Examples 11, 12, 15, and 16 is closer to the first horizontal virtual line VL1 than in Examples 10 and 14, which is considered to be because the probability of the convection direction being fixed in one direction is further increased regardless of the application timing of the horizontal magnetic field.

[0069] Furthermore, in Examples 12 and 16, once the vortex direction is fixed, it does not reverse, and it has been confirmed that, compared to Examples 11 and 15, it is easier to stably generate a right vortex mode or a left vortex mode regardless of the timing of application of the horizontal magnetic field. The reason for these results is believed to be that the high melting point region in Example 11 is located forward in the rotation direction D1 relative to the high melting point region in Example 12, and the high melting point region in Example 15 is located forward in the rotation direction D1 relative to the high melting point region in Example 16. Therefore, the position of the high melting point region when a horizontal magnetic field of 0.1 Tesla is applied in Examples 12 and 16 is closer to the first horizontal virtual line VL1 than in Examples 11 and 15, making it easier to stably generate a right vortex mode or a left vortex mode regardless of the timing of application of the horizontal magnetic field.

[0070] From a comparison between Examples 1 to 8 and Examples 9 to 16, it was confirmed that by adjusting the thicknesses of the first support electrode 92A to the fourth support electrode 92D and the positions of the insulating material 6 so that the melt temperature difference is 5°C or more, it is possible to more easily fix the convection mode to one mode, and that it is possible to produce silicon single crystals with a more stable oxygen concentration without significantly modifying the conventional apparatus configuration. It is believed that similar results to those of this embodiment can be obtained by using a cylindrical insulating material in which the thermal conductivity of one part is different from that of the other part instead of the insulating material 6 having a uniform thermal conductivity overall. [Industrial Applicability]

[0071] The silicon single crystal manufacturing method and silicon single crystal manufacturing apparatus of the present invention can manufacture silicon single crystals with a stable oxygen concentration without making significant changes to the configuration of conventional equipment, thereby improving the yield of silicon single crystals, improving energy efficiency, improving production efficiency, and reducing waste. [Explanation of symbols]

[0072] 1...silicon single crystal manufacturing apparatus, 3...crucible, 3C...crucible central axis, 3MA, 3MB...maximum heating temperature position, 4...heater, 40A...first heating section, 40B...second heating section, 40C...third heating section, 40D...fourth heating section, 4C...heater central axis, 6...insulating material, 6C...insulating material central axis, 92A...first supporting electrode, 92B...second supporting electrode, 92C...third supporting electrode, 92D...fourth supporting electrode, 92H...high resistance supporting electrode (thin diameter supporting electrode), 94...power source, M...silicon melt, SM...silicon single crystal, VL1...first horizontal virtual line, VL2, VL3...second horizontal virtual line.

Claims

1. A method for producing a silicon single crystal, comprising the steps of: applying a horizontal magnetic field to a silicon melt while pulling up the silicon single crystal using a silicon single crystal production apparatus, The silicon single crystal manufacturing apparatus comprises: a crucible for containing the silicon melt; a heater formed in a cylindrical shape surrounding the crucible, the central axis of the cylindrical heater being positioned coaxially with the central axis of the crucible; a first supporting electrode, a second supporting electrode, a third supporting electrode and a fourth supporting electrode each formed in a rod shape from a conductive material and supporting the heater; the heater includes a first heating portion, a second heating portion, a third heating portion, and a fourth heating portion that have the same heating characteristics and are arranged in a circumferential direction of the crucible, the first support electrode connects the first heat generating portion and the second heat generating portion to a positive electrode of a power source; the second support electrode connects the second heat generating portion and the third heat generating portion to a negative electrode of the power source or a ground; the third support electrode connects the third heat generating portion and the fourth heat generating portion to the positive electrode, the fourth support electrode connects the fourth heat generating portion and the first heat generating portion to the negative electrode or the earth; at least one of the first support electrode, the second support electrode, the third support electrode, and the fourth support electrode is configured as a small-diameter support electrode having at least a portion thinner than the remaining support electrodes; The method for producing a silicon single crystal comprises: a silicon melt generating step of heating the silicon raw material in the rotating crucible in a state where the heat distribution of the heater is non-uniform to generate the silicon melt; a magnetic field application step of starting application of the horizontal magnetic field to the silicon melt; a growing step of growing the silicon single crystal by pulling up a seed crystal immersed in the silicon melt when the direction of convection of the silicon melt in a virtual plane perpendicular to a central magnetic field line of the horizontal magnetic field is fixed in one direction.

2. The method for producing a silicon single crystal according to claim 1, The silicon single crystal manufacturing apparatus includes a heat insulating material formed in a cylindrical shape surrounding the heater and configured to provide a non-uniform heat extraction distribution to the heater.

3. The method for producing a silicon single crystal according to claim 2, A method for producing a silicon single crystal, wherein the insulating material is configured so that the thermal conductivity is uniform throughout, and the central axis of the insulating material is not positioned on the same axis as the central axis of the crucible.

4. The method for producing a silicon single crystal according to claim 2, A method for producing a silicon single crystal, wherein the insulation material is configured so that the thermal conductivity of one portion is different from the thermal conductivity of the other portion, and the central axis of the insulation material is positioned coaxially with the central axis of the crucible.

5. The method for producing a silicon single crystal according to any one of claims 2 to 4, The first support electrode, the second support electrode, the third support electrode, the fourth support electrode, and the thermal insulating material are The rotation speed of the crucible when the horizontal magnetic field is applied to the silicon melt is R (rpm), When the time from when the application of the horizontal magnetic field is started until the horizontal magnetic field having a magnetic field strength at which the direction of the convection is fixed acts on the silicon melt is T (minutes), a maximum heating temperature position where the heating temperature for the crucible is the highest in a planar view is located on the opposite side of the rotation direction of the crucible with respect to a first horizontal imaginary line that is perpendicular to the central magnetic field line and includes the central axis of the crucible, and an angle θ (°) formed between a second horizontal imaginary line connecting the central axis of the crucible and the maximum heating temperature position and the first horizontal imaginary line satisfies the following formula (1): θ=360×R×T… (1)

6. A silicon single crystal manufacturing apparatus that pulls up a silicon single crystal while applying a horizontal magnetic field to a silicon melt, a crucible for containing the silicon melt; a heater formed in a cylindrical shape surrounding the crucible, the central axis of the cylindrical heater being positioned coaxially with the central axis of the crucible; a first supporting electrode, a second supporting electrode, a third supporting electrode and a fourth supporting electrode each formed in a rod shape from a conductive material and supporting the heater; the heater includes a first heating portion, a second heating portion, a third heating portion, and a fourth heating portion that have the same heating characteristics and are arranged in a circumferential direction of the crucible, the first support electrode connects the first heat generating portion and the second heat generating portion to a positive electrode of a power source; the second support electrode connects the second heat generating portion and the third heat generating portion to a negative electrode of the power source or a ground; the third support electrode connects the third heat generating portion and the fourth heat generating portion to the positive electrode, the fourth support electrode connects the fourth heat generating portion and the first heat generating portion to the negative electrode or the earth; At least one of the first support electrode, the second support electrode, the third support electrode, and the fourth support electrode is composed of a thin-diameter support electrode, at least a portion of which is thinner than the remaining support electrodes.

7. 7. The silicon single crystal manufacturing apparatus according to claim 6, A silicon single crystal manufacturing apparatus comprising: a heat insulating material formed in a cylindrical shape surrounding the heater and configured so that heat extraction distribution to the heater is non-uniform.

8. The silicon single crystal manufacturing apparatus according to claim 7, A silicon single crystal manufacturing apparatus, wherein the insulating material is configured to have a uniform thermal conductivity throughout, and is positioned so that the central axis of the insulating material is not coaxial with the central axis of the crucible.

9. The silicon single crystal manufacturing apparatus according to claim 7, A silicon single crystal manufacturing apparatus, wherein the insulation material is configured so that the thermal conductivity of one portion is different from the thermal conductivity of the other portion, and the central axis of the insulation material is positioned coaxially with the central axis of the crucible.

10. The silicon single crystal manufacturing apparatus according to any one of claims 7 to 9, The first support electrode, the second support electrode, the third support electrode, the fourth support electrode, and the thermal insulating material are The rotation speed of the crucible when the horizontal magnetic field is applied to the silicon melt is R (rpm), When the time from when the application of the horizontal magnetic field is started until the horizontal magnetic field having a magnetic field strength at which the direction of the convection is fixed acts on the silicon melt is T (minutes), A silicon single crystal manufacturing apparatus configured such that a maximum heating temperature position where the heating temperature for the crucible is the highest in a planar view is located on the opposite side of the rotation direction of the crucible with respect to a first horizontal imaginary line that is perpendicular to the central magnetic field line of the horizontal magnetic field and includes the central axis of the crucible, and an angle θ (°) between a second horizontal imaginary line connecting the central axis of the crucible and the maximum heating temperature position and the first horizontal imaginary line satisfies the following formula (2): θ=360×R×T… (2)

Citation Information

Patent Citations

  • Special-shaped graphite electrode column capable of reducing power consumption

    CN217307913U

  • Graphite heater for manufacturing single crystal, single crystal manufacturing unit, and manufacturing method of single crystal

    JP2004315292A

  • Silicon single crystal production apparatus, and silicon single crystal production method using the same

    JP2014189468A

  • Production method for silicon monocrystal and production method for silicon wafer

    JP2023040824A

  • Heating part of manufacturing apparatus of silicon single crystal, convection pattern control method of silicon melt, manufacturing method of silicon single crystal, manufacturing method of silicon wafer, manufacturing apparatus of silicon single crystal, and convection pattern control system of silicon melt

    JP2022102247A