Composition for producing self-healing polymer, self-healing polymer and self-healing material

A composition of alginic acid and epoxy compounds with catalysts forms self-healing polymers that address the limitations of cellulose derivatives by enabling efficient bonding and reshaping under heat, offering improved repair and remouldability.

JP2024159092AInactive Publication Date: 2024-11-08TOKYO UNIVERSITY OF SCIENCE

Patent Information

Application Number
JP2023074857
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing self-healing materials using cellulose derivatives have limitations, and there is a need for alternative polysaccharides that are environmentally friendly and cost-effective with improved self-healing properties under external stimuli.

Method used

A composition comprising alginic acid or its derivatives and an epoxy compound with specific structural ratios and catalysts is used to create a self-healing polymer capable of bond exchange reactions under external stimuli, forming ester bonds and hydroxyl groups for repair.

Benefits of technology

The resulting self-healing polymer exhibits enhanced repairability and reduced remouldability temperatures, allowing for efficient bonding and reshaping under heat stimulation, outperforming cellulose-based materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159092000007
    Figure 2024159092000007
  • Figure 2024159092000008
    Figure 2024159092000008
  • Figure 2024159092000009
    Figure 2024159092000009
Patent Text Reader

Abstract

To provide a composition that enables the production of a self-healing polymer that exhibits self-healing properties in response to external stimuli such as heat.SOLUTION: A composition for producing a self-healing polymer includes alginic acid or a derivative thereof, and an epoxy compound with two or more epoxy groups.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to compositions for producing self-healing polymers, self-healing polymers, and self-healing materials. [Background technology]

[0002] Polysaccharides are naturally abundant and inexpensive materials, and therefore are widely used in a wide variety of industrial fields. For example, cellulose is the most abundant raw material in nature, and liquid crystal materials, liquid crystal films, photonic devices, and the like using cellulose derivatives as raw materials have been developed. Liquid crystal materials, etc. using cellulose derivatives are useful from the viewpoints of safety and reducing environmental load, and further utilization of the liquid crystallinity, optical properties, and the like of cellulose derivatives is expected.

[0003] Self-repairing materials using cellulose derivatives are also being investigated. For example, a self-repairing resin body has been proposed that contains an amorphous polymer X having a dangling chain and a crosslinked structure, and an amorphous polymer Y having a glass transition temperature measured by dynamic viscoelasticity measurement that is equal to or higher than room temperature, where the amorphous polymer Y is a cellulose ester (e.g., Patent Document 1). Furthermore, a self-repairing material has been proposed that includes a polymer composite material that includes a cellulose material and a polymer having a host group, which is a monovalent group formed by removing one hydrogen atom or hydroxyl group from cyclodextrin or a cyclodextrin derivative, and a guest group, which is a monovalent group that can pierce the host group in a skewer-like manner (for example, Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-260979 A [Patent Document 2] Patent Publication No. 2021-70768 Summary of the Invention [Problem to be solved by the invention]

[0005] Polysaccharides other than cellulose derivatives are also low-impact materials for the human body and the global environment, and are inexpensive materials. The present inventors attempted to produce self-repairing materials as described in Patent Documents 1 and 2 using polysaccharides other than cellulose derivatives.

[0006] The present disclosure aims to provide a composition capable of producing a self-healing polymer having self-healing properties in response to an external stimulus such as heat, a self-healing polymer having self-healing properties, and a self-healing material containing this polymer. [Means for solving the problem]

[0007] Specific means for solving the problems include the following aspects. <1> A composition for producing a self-repairing polymer, comprising alginic acid or a derivative thereof and an epoxy compound containing two or more epoxy groups. <2> The alginic acid or derivative thereof contains a structural unit M derived from mannuronic acid and a structural unit G derived from guluronic acid, and the ratio of the number of the structural units M to the number of the structural units G (structural unit M / structural unit G) is less than 1.6. <1> The composition described in <3> Further comprising a transesterification catalyst <1> or <2> The composition described in <4> The epoxy compound is a water-soluble epoxy compound. <1> ~ <3> 13. The composition according to any one of claims 1 to 12. <5> The epoxy compound includes at least one selected from the group consisting of ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, and sorbitol polyglycidyl ether. <1> ~ <4> 13. The composition according to any one of claims 1 to 12. <6> <1> ~ <5> A self-healing polymer obtained by curing the composition described in any one of the above. <7> A self-repairing polymer having a skeleton derived from alginic acid or a derivative thereof, and an ester bond derived from a carboxy group contained in the alginic acid or a derivative thereof and capable of a bond exchange reaction. <8> The ester bond capable of the bond exchange reaction includes a bond formed by reacting an epoxy group contained in an epoxy compound containing two or more epoxy groups with a carboxy group contained in the alginic acid or a derivative thereof. <7> The self-healing polymer according to claim 1. <9> <6> ~ <8> A self-healing material comprising the self-healing polymer described in any one of the above. Effect of the Invention

[0008] According to one embodiment of the present invention, there are provided a composition capable of producing a self-healing polymer having self-healing properties in response to an external stimulus such as heat, a self-healing polymer having self-healing properties, and a self-healing material containing this polymer. [Brief description of the drawings]

[0009] [Figure 1] 1 is a graph showing G(t) / G0 at 80° C. to 130° C. for the crosslinked membrane of Example 1. [Diagram 2] 1 is a graph in which relaxation times for the crosslinked membrane of Example 1 are plotted against temperatures from 80° C. to 130° C. [Diagram 3] 1 is a graph showing G(t) / G0 at 70° C. to 120° C. for the crosslinked membrane of Example 2. [Figure 4] 1 is a graph in which relaxation times for the crosslinked membrane of Example 2 are plotted against temperatures from 70° C. to 120° C. [Diagram 5] 1 is a graph showing G(t) / G0 at 80° C. to 120° C. for the crosslinked membrane of Example 3. [Figure 6] 1 is a graph plotting relaxation times for the crosslinked membrane of Example 3 at temperatures ranging from 80° C. to 120° C. [Figure 7] 1 is a graph showing G(t) / G0 at 100° C. to 130° C. for the crosslinked membrane of Example 4. [Figure 8] 1 is a graph plotting relaxation times for the crosslinked membrane of Example 4 at temperatures ranging from 100° C. to 130° C. [Figure 9] 1 is a graph showing G(t) / G0 at 70° C. to 120° C. for the crosslinked membrane of Example 5. [Figure 10] 1 is a graph plotting the relaxation time for the crosslinked membrane of Example 5 at each temperature from 70° C. to 120° C. [Figure 11] 1 is a graph showing G(t) / G0 at 70° C. to 120° C. for the crosslinked membrane of Example 6. [Figure 12] 1 is a graph plotting the relaxation time for the crosslinked membrane of Example 6 at each temperature from 70° C. to 120° C. [Figure 13] 1 is a graph showing G(t) / G0 at 70° C. to 120° C. for the crosslinked membrane of Example 7. [Figure 14] 1 is a graph plotting the relaxation time for the crosslinked membrane of Example 7 at each temperature from 70° C. to 120° C. [Figure 15] 1 is a graph showing G(t) / G0 at 70° C. to 120° C. for the crosslinked membrane of Example 8. [Figure 16] 1 is a graph plotting relaxation times for the crosslinked membrane of Example 8 at temperatures ranging from 70° C. to 120° C. [Figure 17] 1 is a graph showing G(t) / G0 at 80° C. to 120° C. for the crosslinked membrane of Example 9. [Figure 18] 1 is a graph plotting the relaxation time for the crosslinked membrane of Example 9 at each temperature from 80° C. to 120° C. [Figure 19] 1 is a graph showing G(t) / G0 at 80° C. to 120° C. for the crosslinked membrane of Example 10. [Figure 20] 1 is a graph plotting relaxation times for the crosslinked membrane of Example 10 at temperatures ranging from 80° C. to 120° C. [Figure 21]1 is a graph showing G(t) / G0 at 80° C. to 110° C. for the crosslinked membrane of Example 11. [Figure 22] 1 is a graph plotting the relaxation time for the crosslinked membrane of Example 11 at each temperature from 80° C. to 110° C. [Figure 23] 1 is a graph showing G(t) / G0 at 80° C. to 120° C. for the crosslinked membrane of Example 12. [Figure 24] 1 is a graph plotting the relaxation time for the crosslinked membrane of Example 12 at each temperature from 80° C. to 120° C. [Diagram 25] 1 is a graph showing the results of dynamic viscoelasticity measurement for the crosslinked film of Example 5. [Figure 26] 1 is a graph showing the results of dynamic viscoelasticity measurement of the crosslinked membrane of Example 6. [Figure 27] 1 is a graph showing the results of dynamic viscoelasticity measurement of the crosslinked film of Example 7. [Figure 28] 1 is a graph showing the results of dynamic viscoelasticity measurement of the crosslinked membrane of Example 8. [Figure 29] 1 is a graph showing the results of dynamic viscoelasticity measurement of the crosslinked membrane of Example 9. [Diagram 30] 1 is a graph showing the results of dynamic viscoelasticity measurement of the crosslinked membrane of Example 10. [Diagram 31] 1 is a graph showing the results of dynamic viscoelasticity measurement of the crosslinked membrane of Example 11. [Diagram 32] 1 is a graph showing the results of dynamic viscoelasticity measurement of the crosslinked membrane of Example 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In the present disclosure, the use of "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower limit and upper limit. In the present disclosure, in the ranges of numerical values ​​described stepwise, the upper limit or lower limit of one numerical range may be replaced with the upper limit or lower limit of another numerical range of numerical values ​​described stepwise. In addition, in the ranges of numerical values ​​described in the present disclosure, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. In this disclosure, when referring to the amount of each component in a composition, if multiple substances corresponding to each component are present in the composition, the total amount of the multiple components present in the composition is meant, unless otherwise specified. In the present disclosure, compounds that are not specified as being substituted or unsubstituted may have any substituent as long as the effects of the present disclosure are not impaired. In the present disclosure, a combination of preferred aspects is a more preferred aspect. In the present disclosure, two or more preferred aspects may be combined in any combination. In this disclosure, a carboxy group also encompasses salts of the carboxy group (eg, -COONa).

[0011] <Composition for producing self-healing polymer> The composition for producing the self-healing polymer of the present disclosure includes alginic acid or a derivative thereof and an epoxy compound containing two or more epoxy groups. A crosslinked product (self-healing polymer) in which an ester bond and a hydroxyl group are formed by reacting a carboxyl group with an epoxy group by heating or the like is obtained. The ester bond and the hydroxyl group contained in the crosslinked product can undergo a bond exchange reaction by an ester exchange reaction. Therefore, the self-healing polymer obtained using the composition of the present disclosure has self-healing properties due to an external stimulus such as heat. For example, even if the self-healing polymer is physically damaged by cutting or the like, the physically damaged self-healing polymers can be bonded to each other by applying an external stimulus such as heat in a state where the physically damaged self-healing polymers are in contact with each other, and the self-healing polymer can be repaired. In addition, the self-healing polymers can be bonded to each other by applying an external stimulus such as heat in a state where the self-healing polymers are stacked, and molding using the self-healing polymer is possible.

[0012] Furthermore, the self-repairing polymer obtained using the composition of the present disclosure can reduce the repair temperature or remolding temperature and shorten the time required for repair or remolding compared to a self-repairing polymer using carboxymethyl cellulose. As an example, the self-repairing polymer obtained using the composition of the present disclosure can be repaired or remolded at about 100°C in about 10 minutes to 1 hour.

[0013] (Alginic acid or its derivatives) The compositions of the present disclosure include alginic acid or a derivative thereof. Alginic acid is a polymer that contains building blocks M derived from mannuronic acid and G derived from guluronic acid. Examples of the derivatives of alginic acid include metal salts of alginic acid such as sodium salt, potassium salt and calcium salt of alginic acid, ammonium salt of alginic acid, diethanolamine alginate, triethanolamine alginate, triethylamine alginate and propylene glycol alginate.

[0014] Alginic acid or its derivatives are polymers containing a structural unit M derived from mannuronic acid and a structural unit G derived from guluronic acid. The ratio of the number of structural units M to the number of structural units G (structural unit M / structural unit G) is not particularly limited. From the viewpoint of transparency and strength of the crosslinked film, the ratio of the number of structural units M to the number of structural units G (structural unit M / structural unit G, also called M / G ratio) may be less than 1.6, or may be 0.8 or more and less than 1.6, or less than 0.8. In alginic acid or a derivative thereof, the ratio of structural unit M / structural unit G may be 1.6 or more. The ratio of structural unit M to structural unit G varies depending on the type of seaweed used as the raw material for alginic acid or its derivatives, the place of production, etc.

[0015] The viscosity of alginic acid or a derivative thereof at 20° C. may be 10 mPa·s to 1000 mPa·s, 15 mPa·s to 500 mPa·s, or 20 mPa·s to 100 mPa·s. The viscosity of alginic acid or its derivative at 20°C is the value measured when alginic acid or its derivative is dissolved in water to prepare a 1% by mass aqueous solution, and the viscosity of the aqueous solution is measured at 20°C and 30 rpm using a rotational viscometer.

[0016] The weight average molecular weight of alginic acid or its derivatives is 1.0×10 5 ~5.0×10 6 may be 3.0 x 10 5 ~3.0×10 6 may be 5.0 x 10 5 ~2.0×10 6 The weight average molecular weight can be determined by gel permeation chromatography (GPC).

[0017] (Multifunctional epoxy compound) The composition of the present disclosure includes an epoxy compound containing two or more epoxy groups (hereinafter, also referred to as a "polyfunctional epoxy compound"). The polyfunctional epoxy compound is not particularly limited as long as it is an epoxy compound containing two or more epoxy groups, and may be an epoxy compound containing two epoxy groups or an epoxy compound containing three or more epoxy groups. The polyfunctional epoxy compounds may be used alone or in combination of two or more.

[0018] The polyfunctional epoxy compound contained in the composition of the present disclosure is preferably a water-soluble epoxy compound from the viewpoint of compatibility with alginic acid or a derivative thereof in water.

[0019] Examples of polyfunctional epoxy compounds include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitol polyglycidyl ether, etc. Among these, ethylene glycol diglycidyl ether and polyethylene glycol diglycidyl ether are preferred from the viewpoint of low viscosity.

[0020] When the polyfunctional epoxy compound is polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, polyglycerol polyglycidyl ether, or the like, the number of repeating units is not particularly limited and may be, for example, 2 to 20, 3 to 15, or 4 to 10. When the number of repeating units is 4 to 10, a crosslinked film that is stable at room temperature tends to be easily formed.

[0021] (Monofunctional epoxy compound) The composition of the present disclosure may contain an epoxy compound containing one epoxy group (hereinafter also referred to as a "monofunctional epoxy compound"). The monofunctional epoxy compound is preferably a water-soluble epoxy compound. The monofunctional epoxy compounds may be used alone or in combination of two or more.

[0022] Examples of monofunctional epoxy compounds include epoxy group-containing alkanes such as 1,2-epoxypropane and 1,2-epoxybutane, EO (ethylene oxide) adduct glycidyl ethers such as lauryl alcohol EO adduct glycidyl ether and phenol EO adduct glycidyl ether, and the like.

[0023] From the viewpoint of crosslink density when the composition is crosslinked, the content of the monofunctional epoxy compound may be 50 mass % or less, 30 mass % or less, or 10 mass % or less, based on the total amount of the polyfunctional epoxy compound and the monofunctional epoxy compound.

[0024] From the viewpoint of biocompatibility, the composition of the present disclosure preferably does not contain an epoxy compound having a bisphenol skeleton or has a small content thereof. In the composition of the present disclosure, the content of the epoxy compound having a bisphenol skeleton is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 0% by mass, based on the total amount of the epoxy compounds.

[0025] The molar ratio of the carboxy group contained in the alginic acid or a derivative thereof to the epoxy group contained in the epoxy compound (carboxy group:epoxy group) may be 1:0.2-5.0 or 1:0.4-2.5, from the viewpoint of the crosslinking density when the composition is crosslinked. The above-mentioned "carboxy group: epoxy group" may be read as "carboxy group: epoxy group derived from the polyfunctional epoxy compound" when only a polyfunctional epoxy compound is used as the epoxy compound. When a polyfunctional epoxy compound and a monofunctional epoxy compound are used as the epoxy compound, it may be read as "carboxy group: total of epoxy group derived from the polyfunctional epoxy compound and epoxy group derived from the monofunctional epoxy compound."

[0026] (Transesterification catalyst) The composition of the present disclosure preferably further comprises a transesterification catalyst. The transesterification catalyst is not particularly limited as long as it is a catalyst that promotes the transesterification reaction, and examples thereof include zinc acetate (II), zinc (II) acetylacetonate, zinc naphthenate (II), acetylacetonate iron (III), acetylacetonate cobalt (II), aluminum isopropoxide, titanium isopropoxide, methoxide (triphenylphosphine) copper (I) complex, ethoxide (triphenylphosphine) copper (I) complex, propoxide (triphenylphosphine) copper (I) complex, isopropoxide (triphenylphosphine) copper (I) complex, Examples of the catalyst include methoxide bis(triphenylphosphine) copper(II) complex, ethoxide bis(triphenylphosphine) copper(II) complex, propoxide bis(triphenylphosphine) copper(II) complex, isopropoxide bis(triphenylphosphine) copper(II) complex, tris(2,4-pentanedionato) cobalt(III), tin(II) diacetate, tin(II) di(2-ethylhexanoate), N,N-dimethyl-4-aminopyridine, diazabicycloundecene, diazabicyclononene, triazabicyclodecene, triphenylphosphine, etc. From the viewpoint of strong basicity, the transesterification catalyst is preferably triazabicyclodecene.

[0027] When the composition of the present disclosure contains an ester exchange catalyst, the content of the ester exchange catalyst may be 1 mol% to 10 mol%, 2 mol% to 8 mol%, or 4 mol% to 6 mol% relative to the carboxy groups of alginic acid or a derivative thereof. Examples of components that contribute to the transesterification reaction include alginic acid or a derivative thereof, a polyfunctional epoxy compound, and a monofunctional epoxy compound that is used as needed.

[0028] The composition of the present disclosure may contain water, and each of the above-mentioned components may be dissolved or dispersed in water.

[0029] (Other ingredients) The composition of the present disclosure may contain other components within a range that does not significantly impair the effects of the present disclosure. Examples of other components include polymerizable monomers, crosslinking agents, flame retardants, compatibilizers, antioxidants, release agents (peeling agents), light resistance agents, weather resistance agents, modifiers, antistatic agents, hydrolysis inhibitors, and compounds that can form ester bonds capable of bond exchange reaction by reacting with carboxy groups.

[0030] The composition of the present disclosure may contain, as another component, a compound capable of forming an ester bond capable of a bond exchange reaction by reacting with a carboxy group (hereinafter also referred to as "other compound"). Examples of the other compound include a polyol compound having two or more hydroxyl groups.

[0031] Specific examples of the polyol compound include: Alkylene glycols such as ethylene glycol, propylene glycol, 1,3-butylene glycol, and 1,4-butylene glycol; Polyalkylene glycols such as polyethylene glycol, polypropylene glycol, and copolymers of ethylene oxide and propylene oxide; sugar alcohols such as glucose, maltose, fructose, sucrose, xylitol, and sorbitol; Glycerin, polyglycerin, erythritol, etc.

[0032] <Self-healing polymer> (First embodiment) The first embodiment of the self-healing polymer of the present disclosure is obtained by curing the composition of the present disclosure described above. For example, the composition of the present disclosure is heated to volatilize water contained as necessary, and the carboxy group and the epoxy group are reacted to obtain a crosslinked self-healing polymer. The self-healing polymer contains an ester bond and a hydroxy group formed by the reaction of the carboxy group and the epoxy group, and the ester bond and the hydroxy group can undergo a bond exchange reaction by an ester exchange reaction.

[0033] Second embodiment The second embodiment of the self-healing polymer of the present disclosure may have a backbone derived from alginic acid or a derivative thereof, and an ester bond derived from a carboxyl group contained in alginic acid or a derivative thereof and capable of bond exchange reaction. In the self-healing polymer of this embodiment, the preferred structure of alginic acid or a derivative thereof is the same as the preferred structure of alginic acid or a derivative thereof contained in the composition of the present disclosure described above.

[0034] The self-healing polymer of the second embodiment is derived from a carboxy group contained in alginic acid or a derivative thereof, and has an ester bond capable of a bond exchange reaction, so that the ester bond is exchanged by heating, etc. More specifically, the ester bond and the hydroxy group, etc. contained in the self-healing polymer are capable of a bond exchange reaction by an ester exchange reaction.

[0035] The self-repairing polymer of the second embodiment preferably contains an ester bond capable of bond exchange reaction, which is formed by reacting an epoxy group contained in an epoxy compound containing two or more epoxy groups with a carboxy group contained in alginic acid or a derivative thereof. Here, the preferred structure of the epoxy compound containing two or more epoxy groups is the same as that of the polyfunctional epoxy compound described above. An ester bond and a hydroxyl group are formed by reacting an epoxy group with a carboxyl group, and the formed ester bond and hydroxyl group are capable of undergoing a bond exchange reaction by a transesterification reaction.

[0036] <Self-healing materials> The self-healing material of the present disclosure includes the self-healing polymer of the present disclosure. The self-healing material of the present disclosure may include a self-healing polymer, and may further include an ester exchange catalyst, other components, etc. The self-healing material of the present disclosure may be a cured composition of the present disclosure, may be a molded product of a self-healing polymer, or may be a molded product of any shape such as a film, a plate, or a rod. EXAMPLES

[0037] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.

[0038] [Preparation of sodium alginate] Alginates A to C, which are sodium alginates, were prepared as shown below. Alginic acid A (sodium alginate, manufactured by Kimika Co., Ltd., trade name IL-6M, M / G ratio 1.6 or more, molecular weight 9.9 × 10 5 , viscosity 50mPa·s~80mPa·s) Alginic acid B (sodium alginate, manufactured by Kimika Co., Ltd., product name SKAT-ONE, M / G ratio 0.8 to less than 1.6, molecular weight 7.6 × 10 5 , viscosity 20mPa·s~80mPa·s) Alginic acid C (sodium alginate, manufactured by Kimika Co., Ltd., trade name IL-6G, M / G ratio less than 0.8, molecular weight 9.9 × 10 5 , viscosity 50mPa·s~80mPa·s)

[0039] An example of the structural unit M derived from mannuronic acid in sodium alginate is represented by formula (1), and an example of the structural unit G derived from guluronic acid in sodium alginate is represented by formula (2).

[0040] [ka]

[0041] [Preparation of multifunctional epoxy compounds and transesterification catalysts] The following polyfunctional epoxy compound and transesterification catalyst were prepared. Polyethylene glycol diglycidyl ether (PEGDE, m = 2, 4, 8, 9, 13) represented by the following formula (3): 1,5,7-Triazabicyclo[4.4.0]dec-5-ene (TBD)

[0042] [ka]

[0043] [Examples 1 to 12] (Preparation of crosslinked membrane) Using a 100 mL beaker, 1.5 g of alginic acid A was dissolved in 50 mL of ultrapure water. The sodium alginate solution was then transferred to a 50 mL screw tube, and 5.0 g of ion exchange resin (DIAIONTM SMNUPB, manufactured by Mitsubishi Chemical Corporation) was added. The mixture was then desalted by stirring for 24 hours using a mix rotor.

[0044] After desalting, the aqueous solution from which the ion exchange resin had been removed was transferred to a 100 mL recovery flask, and 3.1518 g (2 eq. relative to the carboxyl groups of alginic acid) of PEGDE (m=4) and 0.0585 g (5 mol%) of TBD relative to the carboxyl groups of alginic acid were added. The mixture was stirred at room temperature until homogenous to obtain a solution (composition for producing a self-healing polymer).

[0045] The solution was heated and stirred at 80°C for about 20 hours to remove water. The solution in the flask was transferred to a small Teflon dish and left to stand overnight in a dryer set at 60°C. The solution was then heated on an aluminum bead bath set at 100°C for 4 to 5 hours to react the carboxyl group and the epoxy group, yielding a crosslinked membrane having an ester bond and a hydroxyl group in the crosslinked structure (the crosslinked membrane of Example 6 in Table 1).

[0046] The crosslinked membranes of Examples 1 to 5 and 7 to 12 shown in Table 1 were prepared in the same manner as in the preparation of the crosslinked membrane of Example 6, except that the types and amounts of each raw material used in the preparation of the crosslinked membrane were changed as shown in Table 1.

[0047] [Table 1]

[0048] (FT-IR measurement) The crosslinked film prepared as described above was subjected to Fourier transform infrared spectrophotometer (FT-IR) measurement to confirm whether the crosslinking reaction had progressed. -1A peak derived from an ester bond was confirmed in the vicinity, confirming that the crosslinking reaction was proceeding.

[0049] (Appearance and strength evaluation of cross-linked membrane) The appearance and strength of the crosslinked membranes of Examples 2, 6, and 10, which were prepared using PEGDE (m=4), were confirmed. In Example 2, the crosslinked membrane was opaque and brittle. On the other hand, in Examples 6 and 10, the crosslinked membranes were transparent and strong. It is presumed that the sodium alginate used in Examples 6 and 10 had a relatively low M / G ratio, which resulted in high reactivity of the carboxyl group, and the crosslinking reaction proceeded uniformly, resulting in the production of a transparent and strong crosslinked membrane.

[0050] (Stress relaxation measurement) The crosslinked membrane prepared as described above was given an initial strain γ0, and stress relaxation measurements were performed to measure the rate of decrease in stress σ(t) while maintaining the strain constant. Specifically, the crosslinked membrane was placed on a parallel plate with a diameter of 8 mm using an Anton Paar MCR102 device, and stress relaxation measurements were performed. The relaxation modulus G, which is the value obtained by dividing stress by strain, was plotted as G(t) / G0, which is the ratio of the relaxation modulus (G(t)) at stress at time t to the relaxation modulus (G0) at the initial stress. In addition, the relaxation time τ, which is the time until the stress σ becomes σ0 / e, was calculated. Since a clear stress relaxation was confirmed within the temperature range of 70°C to 130°C, the stress relaxation measurement was performed under the same conditions as above at 70°C, 80°C, 90°C, or 100°C in 10°C increments. Note that the temperature ranges in which stress relaxation was confirmed were different for the crosslinked membranes of Examples 1 to 12. The plots of G(t) / G0 for the crosslinked membranes of Examples 1 to 12 are shown in the figures. As shown in each figure, stress relaxation was confirmed.

[0051] Furthermore, the results of the relaxation time τ are shown in Tables 2 to 4. In addition, "-" in Tables 2 to 4 means that relaxation of the stress could not be confirmed.

[0052] [Table 2]

[0053] [Table 3]

[0054] [Table 4]

[0055] The results in Tables 2 to 4 show that the relaxation time of the crosslinked membrane can be adjusted by the type of alginic acid, the type of polyfunctional epoxy compound, etc. For example, the crosslinked membranes of Examples 2, 6, and 10 prepared using PEGDE (m=4) tended to have shorter relaxation times than the crosslinked membranes of other Examples. This is presumably because the ease with which the bond exchange reaction occurs varies depending on the length of the PEGDE molecular chain, and the bond exchange reaction occurs more easily with m=4 than in other Examples.

[0056] As shown in the figure, the relaxation time (specifically, In τ) is plotted against each temperature (specifically, 1000 / T(K)) shown in Tables 2 to 4, and the Arrhenius equation (In τ=A+RT / E a , R: gas constant, T: absolute temperature, E a A straight line was obtained that follows the curve (E = activation energy). This result is similar to the behavior in a previous study (L. Leibler et al., Science, 2011, 334, 965-968.), so it was speculated that the crosslinked membrane prepared as described above has self-repairing properties.

[0057] (Confirmation of self-repairing properties of cross-linked membrane) It was confirmed that the crosslinked film prepared as described above had self-repairing properties as follows. It was confirmed that the crosslinked films of Example 6 were bonded together by stacking them on top of each other and then performing heat pressing at 100° C. for 10 minutes. As described above, it was confirmed that the crosslinked film had self-repairing properties due to bonding. It was confirmed that the crosslinked films of Example 10 were bonded together by stacking them on top of each other and then performing heat pressing at 110° C. for 10 minutes. As described above, it was confirmed that the crosslinked film had self-repairing properties due to bonding.

[0058] (Dynamic viscoelasticity measurement) Dynamic viscoelasticity measurements were carried out to measure the elastic modulus when strains of frequencies from 100 Hz to 0.01 Hz were applied to the crosslinked membranes of Examples 5 to 12 prepared as described above at room temperature. Specifically, a dynamic viscoelasticity measurement device manufactured by Anton Paar was used to measure the storage modulus (G') and loss modulus (G'') at frequencies from 100 Hz to 0.01 Hz and room temperature by placing the crosslinked membranes on parallel plates of 8 mm in diameter. The results of dynamic viscoelasticity measurement for the crosslinked membrane of each Example are shown in the figure. As shown in Figures 25 to 28, frequency dependence was confirmed in G' and G'' in Example 5, while little frequency dependence was confirmed in G' and G'' in Examples 6 to 8. From these results, it is presumed that the crosslinked membrane flows gently at room temperature in Example 5, while the crosslinked membrane exists stably at room temperature in Examples 6 to 8. As shown in Figures 29 to 32, frequency dependence was confirmed in G' and G'' in Examples 9 and 12, while little frequency dependence was confirmed in G' and G'' in Examples 10 and 11. From these results, it is inferred that the crosslinked membranes flowed gently at room temperature in Examples 9 and 12, while the crosslinked membranes were stable at room temperature in Examples 10 and 11.

Claims

1. A composition for producing a self-repairing polymer, comprising alginic acid or a derivative thereof and an epoxy compound containing two or more epoxy groups.

2. The composition according to claim 1, wherein the alginic acid or derivative thereof comprises a structural unit M derived from mannuronic acid and a structural unit G derived from guluronic acid, and the ratio of the number of structural units M to the number of structural units G (structural unit M / structural unit G) is less than 1.

6.

3. The composition of claim 1 further comprising a transesterification catalyst.

4. The composition according to claim 1 , wherein the epoxy compound is a water-soluble epoxy compound.

5. 2. The composition according to claim 1, wherein the epoxy compound comprises at least one selected from the group consisting of ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, and sorbitol polyglycidyl ether.

6. A self-repairing polymer obtained by curing the composition according to any one of claims 1 to 5.

7. A self-repairing polymer having a skeleton derived from alginic acid or a derivative thereof, and an ester bond derived from a carboxy group contained in the alginic acid or a derivative thereof and capable of a bond exchange reaction.

8. The self-healing polymer according to claim 7, wherein the ester bond capable of the bond exchange reaction includes a bond formed by reaction of an epoxy group contained in an epoxy compound containing two or more epoxy groups with a carboxy group contained in the alginic acid or a derivative thereof.

9. A self-healing material comprising the self-healing polymer of claim 6.

Citation Information

Patent Citations

  • Self-repairing resin body, self-repairing structure, method for producing self-repairing resin body, and material for forming self-repairing resin body

    JP2010260979A

  • Polymer composite material, polymerizable monomer composition and production method of polymer composite material

    JP2021070768A

Cited By

  • Composition for producing self-healing polymer, self-healing polymer, and self-healing material

    JP2023159014A