Method for manufacturing preform

The method of heat-treating resin flakes under reduced pressure and using biopolymer catalysts to decompose surface impurities addresses the quality deterioration in recycled polyester resin preforms, achieving efficient and high-quality preform production.

JP2024159324APending Publication Date: 2024-11-08TOYO SEIKAN KAISHA LTD +1

Patent Information

Application Number
JP2023075250
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing methods for recycling polyester resin molded products, such as PET bottles, face challenges in maintaining the quality of preforms due to deterioration and contamination from organic impurities, which affect the intrinsic viscosity and productivity in the manufacturing process.

Method used

A method involving the preparation of resin flakes from recycled polyester resin molded products, followed by heat treatment under reduced pressure to promote solid-phase polymerization, and subsequent use of a biopolymer catalyst to decompose surface-layer impurities, combined with plasticization using a twin-screw extruder to minimize organic impurities and maintain resin quality.

Benefits of technology

This approach effectively suppresses deterioration and reduces organic impurities, allowing the production of high-quality preforms with controlled residual impurity levels, enhancing the manufacturing process's efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159324000001_ABST
    Figure 2024159324000001_ABST
Patent Text Reader

Abstract

To recover a polyester-based resin molding, recycle the resin molding as a recycled material by mechanical recycling, and suppress quality deterioration of a preform when the preform is manufactured as a recycled product.SOLUTION: A method for manufacturing a preform includes the steps of: preparing a resin flake obtained by crushing a recovered polyester-based resin molding into a flake shape; decomposing an organic impurity of a surface layer part of the resin flake using a biopolymer catalyst, at a temperature equal to or lower than a glass transition point of the polyester-based resin, as a previous step; and then supplying a molten resin obtained by plasticizing the resin flake to an injection molding device 500, and injection molding a preform.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a preform. [Background technology]

[0002] Conventionally, synthetic resin containers, which are made by producing a bottomed cylindrical preform using a polyester resin such as polyethylene terephthalate and then molding this preform into a bottle shape by biaxial stretch blow molding or the like, are used in a wide range of fields as containers for various beverages, seasonings, etc. This type of container is generally known as a PET bottle, and in recent years, in response to social demand, a recycling technology called "bottle-to-bottle" has been considered, in which used PET bottles are collected and reused as recycled material to manufacture PET bottles.

[0003] For example, Patent Document 1 discloses a technology in which recovered polyester resin molded products are crushed into flakes to produce resin flakes, which are then decontaminated, melted to produce resin pellets, which are then subjected to solid-state polymerization and transported to an injection molding device to produce preforms. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2021-98350 Summary of the Invention [Problem to be solved by the invention]

[0005] Means for Solving the Problems The present inventors have considered the above-mentioned background art and have conducted extensive research into how to prevent deterioration in the quality of preforms produced as recycled products by collecting polyester resin molded products, particularly used PET bottles, and reusing them as recycled materials through mechanical recycling. As a result, they have completed the present invention. [Means for solving the problem]

[0006] The method for manufacturing a preform according to the present invention involves preparing resin flakes by crushing recovered polyester resin molded products into flakes, and as a preliminary step, decomposing organic impurities on the surface of the resin flakes using a biopolymer catalyst at a temperature below the glass transition point of the polyester resin.The molten resin obtained by plasticizing the resin flakes is then supplied to an injection molding device to injection mold a preform. Effect of the Invention

[0007] According to the present invention, when polyester resin molded articles are collected and reused as recycled materials by mechanical recycling to produce preforms as recycled products, deterioration in the quality of the preforms can be suppressed. [Brief description of the drawings]

[0008] [Figure 1] 1 is an explanatory diagram conceptually illustrating an entire apparatus in which an embodiment of the present invention is preferably implemented; [Diagram 2] FIG. 2 is an explanatory diagram showing an example of an apparatus for carrying out a step of heat-treating resin flakes under reduced pressure conditions in an embodiment of the present invention. [Diagram 3] FIG. 2 is an explanatory diagram showing an example of an apparatus for carrying out a step of decomposing organic impurities in the surface layer of resin flakes in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Preferred embodiments of the present invention will now be described.

[0010] In this embodiment, polyester resin molded products, particularly used PET bottles, are collected and reused as recycled materials by mechanical recycling. Needless to say, it is preferable to select and remove plastic containers made of different materials such as olefin resins and polystyrene resins that are mixed into used PET bottles, but in recent years, transparent bottles made of aliphatic polyester resins containing plant-derived polylactic acid as a dicarboxylic acid component have been known. Polylactic acid is highly hydrolyzable, and aliphatic polyester resins containing polylactic acid in their segments have inferior performance compared to aromatic polyester resins, so they are preferably removed from recycled materials. For example, a bale of collected PET bottles (a mass of compressed PET bottles) is heat-treated with water vapor, and transparent bottles made of aliphatic polyester resins containing polylactic acid in their segments are weakened by selective hydrolysis, and can be removed by crushing with mechanical stimulation and physically classifying them.

[0011] In order to collect used PET bottles and reuse them as recycled materials by mechanical recycling, first, the collected used PET bottles are crushed into flakes to prepare resin flakes. In preparing such resin flakes, any cleaning means such as alkaline cleaning or hot water cleaning can be used to remove impurities such as residues of the contents remaining on the surface of the resin flakes and foreign matter mixed in. However, for example, in a PET bottle used to contain a milk drink, if organic impurities derived from the contents such as proteins and lipids are sorbed, it is difficult to remove them by cleaning.

[0012] In addition, when used PET bottles (polyester resin molded products) are collected and reused as recycled materials through mechanical recycling to manufacture recycled products, the decrease in intrinsic viscosity due to deterioration of the resin caused by the heat history during the manufacture of the collected products can cause defects in the manufacturing process of the recycled products. Furthermore, if low-molecular-weight organic impurities such as acetaldehyde (AA) generated by thermal decomposition of polyester resins, and oligomers such as bishydroxyethyl terephthalate (BHET), monohydroxyethyl terephthalate (MHET), and cyclic trimer (CT) generated by depolymerization of polyester resins remain in large amounts as impurity components in the recycled materials, they not only affect the quality of the recycled products manufactured, but also cause productivity to decrease by fouling the manufacturing equipment.

[0013] In this embodiment, in order to recover the intrinsic viscosity and efficiently remove impurity components including the organic impurities as described above, it is preferable to heat-treat the resin flakes under reduced pressure conditions. More specifically, the prepared resin flakes are heat-treated in a temperature atmosphere preferably reduced to 1000 Pa or less and preferably at 160 to 240° C., so that the solid-phase polymerization reaction of the polyester resin forming the resin flakes proceeds without melting the resin flakes and the crystallization of the polyester resin is promoted while the resin flakes remain in the flake form.

[0014] By proceeding with the solid-phase polymerization reaction, the end groups of the polyester resin, whose degree of polymerization has decreased due to the cutting of molecular chains caused by deterioration, are recondensed, and as the degree of polymerization is restored, the intrinsic viscosity corresponding to the molecular weight can be restored. Furthermore, by subjecting the resin flakes to heat treatment under reduced pressure conditions, particularly by exposing them to a temperature atmosphere of 160 to 240°C under reduced pressure conditions, it is possible to suppress hydrolysis of the polyester resin, while favorably promoting crystallization by utilizing the melting point drop caused by reduced pressure.

[0015] As a result, the crystalline volume fraction of the polyester resin increases and the free volume between molecular chains of the polyester resin decreases (amorphous phase decreases), so that organic impurities that have been included or sorbed in the free volume of the resin flakes can be selectively migrated to the surface layer of the resin flakes. As a result, most of the organic impurities that have migrated to the surface layer of the resin flakes can be removed by volatilization or evaporation during the heat treatment.

[0016] Among the organic impurities that have migrated to the surface layer of the resin flakes, those that cannot be completely removed during the heat treatment and remain on the surface layer of the resin flakes are decomposed using a biopolymer catalyst at a temperature below the glass transition point of the polyester resin (for example, below 60°C), thereby making it possible to remove a larger amount of organic impurities from the resin flakes. As the biopolymer catalyst, one or more of hydrolases such as lipase, esterase, glucosidase, peptidase, etc., or protein decomposition enzymes such as protease, etc., can be appropriately selected or combined and used.

[0017] In this embodiment, the specific method of subjecting the resin flakes to the heat treatment is not particularly limited. For example, it is preferable to subject the resin flakes to the heat treatment using a treatment device 100 as shown in FIG. 2, which includes at least one preheating chamber 102 and a treatment chamber 103 capable of adjusting the internal atmosphere to a temperature and pressure suitable for the heat treatment.

[0018] Here, the outline of the processing apparatus 100 shown in FIG. 2 will be described. The processing apparatus 100 is preferably 7 to 18 m 3 The system includes a sealed container 101 constructed to have an internal volume of 100 mm. A processing chamber 103 is provided inside the sealed container 101, and two preheating chambers 102 are provided above the sealed container 101. The preheating chambers 102 are connected to the sealed container 101 via an opening / closing mechanism such as a sliding shutter (not shown) so as to be able to communicate with the processing chamber 103 while maintaining airtightness from the outside of the system. In FIG. 2, illustration of incidental equipment such as a heating device for adjusting the internal atmosphere of the processing chamber 103, a pressure reducing device, and associated piping is omitted.

[0019] In order to subject resin flakes to a heat treatment using such a treatment apparatus 100, it is preferable to, prior to the heat treatment, put the resin flakes into the preheating chamber 102, seal the preheating chamber 102, heat the resin flakes to a predetermined temperature, and reduce the pressure inside the preheating chamber 102 to a predetermined pressure. At that time, it is preferable to, for example, provide a nozzle opening on the inner wall surface of the preheating chamber 102 to spray heated gas (e.g., an inert gas such as N2 gas) into the preheating chamber 102, and appropriately adjust the direction and amount of the gas to generate an airflow inside the preheating chamber 102, thereby stirring and heating the resin flakes, and to reduce the pressure inside the preheating chamber 102 so that at least a part of the impurity components contained in the resin flakes is dispersed and removed outside the system.

[0020] In this way, when raising the temperature of the resin flakes, it is preferable to appropriately adjust the final temperature and pressure in the preheating chamber 102 taking into consideration the internal atmosphere of the processing chamber 103. Then, it is preferable to open the opening and closing device and, while maintaining airtightness from the outside of the system, allow the resin flakes in the preheating chamber 102 to fall by their own weight, so that the resin flakes are supplied into the processing chamber 103 without damaging the internal atmosphere of the processing chamber 103, which has been adjusted to a temperature and pressure suitable for the heat treatment.

[0021] In the processing apparatus 100 shown in FIG. 2, the resin flakes are sequentially fed into two preheating chambers 102 so that preheating treatments for raising the temperature of the resin flakes are alternately performed, and the resin flakes are dropped into the processing chamber 103 in the order from the preheating chamber 102 in which the fed resin flakes have been heated to a predetermined temperature, but this is not limited thereto. The number of preheating chambers 102 may be one or three or more depending on the processing capacity of the processing apparatus 100, i.e., the total amount of resin flakes that can be subjected to heat treatment per unit time. In any case, it is preferable to repeat the operation of dropping the resin flakes from the preheating chamber 102 into the processing chamber 103, so that the resin flakes are stacked in layers for each group that is dropped. It is preferable to expose the resin flakes to the internal atmosphere of the processing chamber 103 while the resin flakes are piled up in the processing chamber 103, so that the resin flakes can be subjected to heat treatment.

[0022] The processing time for heat-treating the resin flakes is usually 30 minutes or more, and is preferably adjusted appropriately within the range of 1 to 8 hours in order to proceed with the solid-phase polymerization reaction while suppressing the deterioration of the resin hue. It is preferable to manage the processing time so that the resin flakes deposited in the processing chamber 103 are sequentially removed from the processing chamber 103 in equal amounts to the amount dropped from the preheating chamber 102, starting from the lower layer side of the resin flakes deposited in layers as described above, after the processing time has elapsed. At that time, the time required for the preheating treatment in the preheating chamber 102 depends on the water content and shape of the resin flakes, and there may be variation in the intervals at which the resin flakes are dropped. Therefore, it is preferable to manage the processing time for each group of dropped resin flakes.

[0023] In this way, in order to suitably manage the processing time when heat-treating the resin flakes, the processing apparatus 100 shown in Fig. 2 is provided with an opening / closing mechanism 104 on the bottom side of the sealed container 101. The opening / closing mechanism 104 forms the bottom surface of the processing chamber 103 and is configured to serve as a partition between the processing chamber 103 and the removal section 105 provided at the bottom of the sealed container 101. This allows the resin flakes to spill into the removal section 105 when the opening / closing mechanism 104 is opened, and by appropriately adjusting the timing of opening and closing the opening / closing mechanism 104, it is possible to remove an amount of resin flakes equal to the amount dropped from the preheating chamber 102, and although there will be some mixing, the resin flakes can be removed in groups dropped from the preheating chamber 102.

[0024] As described above, organic impurities can be efficiently removed by performing heat treatment under reduced pressure conditions, but it is not preferable for the volatilized or evaporated organic impurities to remain in the treatment chamber 103. For this reason, the treatment apparatus 100 shown in FIG. 2 is configured to circulate the gas phase components in the treatment chamber 103, and to include a circulation flow path 106 including a catalyst tank 107 for decomposing organic impurities in the circulation flow path 106, and to connect the circulation flow path 106 to the treatment chamber 103. It is preferable to configure the treatment apparatus 100 in this way, for example, by using an inert gas such as N2 gas as a carrier gas, to guide the gas phase components in the treatment chamber 103 to the circulation flow path 106 and circulate them without damaging the internal atmosphere of the treatment chamber 103, thereby reducing the organic impurities remaining in the treatment chamber 103.

[0025] The resin flakes that have been subjected to the heat treatment in this manner can be sent to a processing device 800 such as that shown in FIG. 3, where the organic impurities on the surface of the resin flakes can be decomposed using a biopolymer catalyst at a temperature below the glass transition point of the polyester resin.

[0026] 3 includes a storage tank 810 for stirring and storing a biopolymer catalyst solution adjusted to the optimum pH and temperature (a temperature below the glass transition point of the polyester resin) of the biopolymer catalyst, a first screw feeder 820, a second screw feeder 830, and a third screw feeder 840. Each of the screw feeders 820, 830, and 840 is disposed at an incline such that the upstream side in the conveying direction is located at the lower position and the downstream side in the conveying direction is located at the upper position.

[0027] In the illustrated example, the transport path 821, excluding the discharge port 823 side of the first screw feeder 820, is filled with a biopolymer catalyst solution supplied from a storage tank 810, and the biopolymer catalyst solution supplied from the downstream side is returned from the upstream side to the storage tank 810 and circulated. The transport path 831, excluding the discharge port 833 side of the second screw feeder 830, is filled with washing water W, and the washing water W supplied from the upstream side is discharged from the downstream side. The third screw feeder 840 has a heater 844 provided on the outer periphery of the transport path.

[0028] The operation of such a processing apparatus will be described. The resin flakes taken out of the processing chamber 103 after the heat treatment are fed from an inlet 822 provided on the upstream side of the first screw feeder 820, and are conveyed through a conveying path 821 filled with a biopolymer catalyst solution while being stirred by the rotation of the screw. In this way, during the process of conveying through the conveying path 821, the biopolymer catalyst acts to decompose organic impurities on the surface layer of the resin flakes. At that time, the time during which the biopolymer catalyst acts on the organic impurities can be appropriately adjusted by adjusting the rotation speed of the screw. The concentration of the biopolymer catalyst in the biopolymer catalyst solution can be appropriately adjusted based on the weight of the resin flakes to be treated, and can be prepared to be preferably 0.0001 to 10 wt %, more preferably 0.1 to 1 wt %, based on the weight of the resin flakes to be treated.

[0029] The resin flakes transported through the transport path 821 of the first screw feeder 820 are discharged from a discharge port 823 provided on the downstream side thereof and fed into the second screw feeder 830. The resin flakes fed from an inlet 832 provided on the upstream side of the second screw feeder 830 are transported through the transport path 831 filled with cleaning water while being stirred by the rotation of the screw, are washed in the process of being transported through the transport path 831, and are then discharged from a discharge port 833 provided on the downstream side of the second screw feeder 830. The resin flakes discharged from the second screw feeder 830 are fed into the third screw feeder 840. The resin flakes fed from an inlet 842 provided on the upstream side of the third screw feeder 840 are transported through the transport path 841 by the rotation of the screw. Then, while being transported along the transport path 841, it is dried by a heater 844 provided on the outer periphery of the transport path 841 of the third screw feeder 840, and is discharged from a discharge outlet 843 provided downstream of the third screw feeder 840.

[0030] In this way, by decomposing organic impurities using a biopolymer catalyst whose optimal temperature is below the glass transition point of the polyester resin, it is possible to remove organic impurities from the surface layer of the resin flakes while suppressing thermal decomposition and depolymerization of the polyester resin, but the specific method for doing so is not limited to the example shown in the figure.

[0031] For example, when decomposing organic impurities using a biopolymer catalyst, the treatment may be performed using a batch-type treatment tank, or individual treatment may be performed using separate modular devices that are not connected to each other. When two or more types of biopolymer catalysts are used, the biopolymer catalysts may be treated separately. Furthermore, to dry the resin flakes from which organic impurities have been removed from the surface using a biopolymer catalyst, it is possible to use two jacketed rolls with spiral grooves on the surface to semi-weld and press the surface of the resin flakes using the shear heat generated by the rotation of the rolls, and then further remove the organic impurities and moisture remaining on the surface of the resin flakes using a rotary forward drying device (open roll twin screw extruder), although this is not shown in the figure. In this case, the resin flakes dried using the open roll twin screw extruder can be easily separated and dispersed into flakes by the pressure of the press rolls in the cooling section downstream of the rolls, and can be recovered as resin flakes.

[0032] In this embodiment, the resin flakes are heat-treated under reduced pressure conditions as described above to remove as much organic impurities as possible that have migrated to the surface layer of the resin flakes, and then the resin flakes are plasticized. At that time, the resin flakes may be fed into the extruder 200 and plasticized while being melt-kneaded by the heat from the heating cylinder and the shear heat from the screw, but it is preferable to use a twin-screw extruder for plasticization. The twin-screw extruder has a high kneading effect, can plasticize the resin flakes more uniformly, and can also shorten the time required for plasticization, so it is also preferable in terms of suppressing deterioration, thermal decomposition, and depolymerization of the resin.

[0033] When plasticizing resin flakes using a twin-screw extruder, it is preferable to configure the twin-screw extruder to have a vent port, and for example, to exhaust gas phase components containing low molecular weight organic impurities derived from polyester resins retained in the twin-screw extruder by vacuum suction through a vent port provided through a heating cylinder. This makes it possible to further reduce organic impurities remaining in the plasticized polyester resin. In this case, cyclic oligomers, etc., are particularly generated by an equilibrium reaction during thermal melting, so cyclic oligomers are generated when polyethylene terephthalate is melted. Therefore, it is important to perform the operation of absorbing and removing them under reduced pressure at the vent port of the twin-screw extruder. The optimal conditions (temperature and pressure) for gas-liquid separation of cyclic oligomers are estimated. The melting point of cyclic oligomers is 319°C and they are sublimable. Assuming that the resin melt temperature at the vent port of a twin-screw extruder for polyethylene terephthalate is 300°C, the reduced vacuum pressure at which cyclic oligomers can sublimate (transform into gas) is generally 0.1 KPa (100 Pa) or less, so it is necessary to adjust the pressure to a relatively high vacuum. This increases the possibility of the molten resin venting up at the vent port. To avoid venting up, it is preferable to use a twin-screw extruder with counter-rotating (different) screw rotations rather than the same (same) screw rotation type.

[0034] Furthermore, as described above, the resin flakes from which organic impurities have been removed as much as possible from the surface layer may be directly fed into the extruder 200 for plasticization, or may be stored in a buffer tank 300 and then fed into the extruder 200 for plasticization.

[0035] When installing the buffer tank 300, it is preferable to appropriately adjust the internal volume of the buffer tank 300 so that a larger amount of resin flakes can be stored. By doing so, even if a problem occurs in the process subsequent to the process of plasticizing the resin flakes, causing the subsequent process to be stopped, the heat treatment of the resin flakes can be continued without being stopped, and the amount that cannot be sent to the subsequent process can be stored in the buffer tank 300.

[0036] Also, in anticipation of such trouble occurring or changes in circumstances such as an increase or decrease in the processing speed of the subsequent process, a relief tank 400 can be installed midway along the transport path that transports the resin flakes to the buffer tank 300. It is preferable to transport the resin flakes to the buffer tank 300 while allowing the resin flakes to be evacuated to the relief tank 400 during transport.

[0037] In this way, for example, when the subsequent process is stopped, the resin flakes can be evacuated to the relief tank 400 and the transport to the buffer tank 300 can be limited. When the processing speed of the subsequent process is increased, the resin flakes evacuated to the relief tank 400 can be transported to the buffer tank 300 together. When the processing speed of the subsequent process is decreased, a part of the resin flakes can be evacuated to the relief tank 400 and the amount of the resin flakes transported to the buffer tank 300 can be appropriately adjusted. In this way, when evacuating the resin flakes to the relief tank 400 as necessary, the internal atmosphere of the relief tank 400 is preferably set to 100° C. or higher so that the resin flakes do not become hydrated.

[0038] In this embodiment, after the above-mentioned steps, the molten resin obtained by plasticizing the resin flakes is supplied to the injection molding device 500 while removing foreign matter from the molten resin obtained by plasticizing the resin flakes, and the preform is injection molded. In order to remove foreign matter from the molten resin obtained by plasticizing the resin flakes, for example, a filter 600 for removing foreign matter may be provided on the discharge port side of the extruder 200. Furthermore, the specific configuration of the injection molding device 500 is not particularly limited, and the preform can be injection molded using the injection molding device 500 having at least one injection pot and a preform mold configured to measure the supplied molten resin and then inject a certain amount of the molten resin.

[0039] In addition, when supplying the molten resin obtained by plasticizing the resin flakes to the injection molding apparatus 500, it is undesirable for the resin to deteriorate (especially its hue) during transportation. To this end, in order to shorten the time that the molten resin remains in the transportation path, it is preferable to set the transportation distance until it is supplied to the injection molding apparatus 500 after removing foreign matter, more specifically, the distance from the outlet of the gear pump 700 installed downstream of the filter 600 to the inlet of the injection pot provided in the injection molding apparatus 500, to 1 to 7 m. In this case, the transportation amount of the molten resin is preferably 900 to 1500 kg / h.

[0040] According to the present embodiment as described above, when polyester resin molded products, particularly used PET bottles, are collected and reused as recycled materials by mechanical recycling to manufacture preforms as recycled products, deterioration of the quality of the preforms can be suppressed. In particular, according to the present embodiment, although the preforms are manufactured by recycling the collected polyester resin molded products, the residual amount of acetaldehyde is 1 to 15 ppm, preferably 1 to 10 ppm, more preferably 1 to 5 ppm, the residual amount of bishydroxyethyl terephthalate is 1 to 35 ppm, preferably 1 to 30 ppm, more preferably 1 to 20 ppm, the residual amount of monohydroxyethyl terephthalate is 1 to 35 ppm, preferably 1 to 30 ppm, more preferably 1 to 20 ppm, the residual amount of cyclic trimer is 6000 ppm or less, preferably 4000 ppm or less, more preferably 3000 ppm or less, and preferably, when the mass of the preform is 14 to 50 g, the residual amount of cyclic trimer is 6000 ppm or less, preferably 4000 ppm or less, more preferably 3000 ppm or less. * a * b * L in color space * Value 70-90, b * Preforms having a value of 2 to 18 can be successfully manufactured.

[0041] Here, the remaining amounts of acetaldehyde, bishydroxyethyl terephthalate (BHET), monohydroxyethyl terephthalate (MHET), and cyclic trimer (CT) can be determined, for example, as follows.

[0042] <Residual amount of acetaldehyde> Using the slices cut from the preform as samples, weigh 1.0 g of such a sample into a glass bottle, add 5.0 mL of pure water, and seal it. After heating this suspension in an oven adjusted to 120°C for 60 minutes, cool it in ice water. Collect 1.0 mL of the supernatant of the suspension, add 0.2 mL of a 2,4-dinitrophenylhydrazine·phosphoric acid solution with a concentration of 0.1% thereto, and measure the one left standing for 30 minutes by high performance liquid chromatography. At the same time, measure the standard solution, and calculate the acetaldehyde content based on the obtained calibration curve.

[0043] <Residual amounts of BHET, MHET, and CT> Using the slices cut from the preform as samples, weigh 0.2 g of such a sample, add 1 mL of a mixed solvent of hexafluoroisopropanol and chloroform (weight ratio 1 / 1) thereto, and completely dissolve it. After adding 4 mL of chloroform to the solution, gradually add 5 mL of acetonitrile, and leave it standing for 3 hours to precipitate the PET polymer. Collect 1 mL from this suspension, filter it through a membrane filter with a pore size of 0.45 μm, and measure the filtrate by high performance liquid chromatography. At the same time, measure the standard solution, and calculate the contents of MHET, BHET, and CT in the pellet based on the obtained calibration curve.

[0044] Also, L * a * b * L in the color system * value, b * The values shall be measured using a spectrocolorimeter under the measurement conditions of a D65 light source and a 2° field of view with the body part of the preform as the measurement site.

[0045] As described above, the present invention has been described by showing preferred embodiments. However, it goes without saying that the present invention is not limited only to the above-described embodiments, and various modifications can be made within the scope of the present invention.

[0046] For example, in the above-described embodiment, the resin flakes are plasticized after undergoing a preliminary process of heat-treating the resin flakes under reduced pressure conditions and a process of decomposing organic impurities on the surface of the resin flakes using a biopolymer catalyst, but the process of heat-treating the resin flakes under reduced pressure conditions can be omitted as appropriate. The step of decomposing organic impurities on the surface layer of the resin flakes using a biopolymer catalyst can also be carried out before the step of heat-treating the resin flakes under reduced pressure. That is, the organic impurities on the surface layer of the resin flakes may be sufficiently removed in advance, and then the resin flakes may be subjected to heat treatment. [Explanation of symbols]

[0047] 500 injection molding equipment 820 First Screw Feeder 821 Transport Route 830 Second Screw Feeder 831 Transport Route W Cleaning water

Claims

1. The collected polyester resin molded products are pulverized into flakes to prepare resin flakes; As a pre-process, a process is performed in which organic impurities on the surface layer of the resin flakes are decomposed using a biopolymer catalyst at a temperature equal to or lower than the glass transition point of the polyester resin, and then: A method for producing a preform, comprising the steps of: supplying a molten resin obtained by plasticizing the resin flakes to an injection molding device and injection molding the preform.

2. 2. A method for producing a preform as described in claim 1, wherein the resin flakes that have been subjected to heat treatment are fed into a first screw feeder that is inclined so that the upstream side in the conveying direction is located at the lower position and the downstream side in the conveying direction is located at the upper position, and the organic impurities are decomposed during the process of being transported through the conveying path of the first screw feeder filled with a biopolymer catalyst solution.

3. The method for producing a preform as described in claim 2, wherein the resin flakes discharged from the first screw feeder are fed into a second screw feeder arranged at an angle so that the upstream side in the conveying direction is located at the lower position and the downstream side in the conveying direction is located at the upper position, and the resin flakes are washed while being transported through a conveying path of the second screw feeder filled with cleaning water.

4. The method for producing a preform according to any one of claims 1 to 3, comprising, as the pre-process, a step of heat-treating the resin flakes in an atmosphere at a temperature of 160 to 240 ° C. and a reduced pressure of 1000 Pa or less.

Citation Information

Patent Citations

  • Resin product manufacturing method, resin product manufacturing system, and transfer device

    JP2021098350A

Cited By

  • Method for producing methane

    EP4796521A1