External part for watches or jewelry comprising coating of saturated intrinsic color and method for manufacturing said external part

A tantalum-based metal nitride or oxynitride coating on watch and jewelry parts addresses the challenge of achieving bright, durable, and angle-independent red colors, maintaining structural integrity.

JP2024159499AActive Publication Date: 2024-11-08THE SWATCH GRP RES & DEVELONMENT LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024026455
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-02-26
Publication Date
2024-11-08
Estimated Expiration
2044-02-26

AI Technical Summary

Technical Problem

Existing deposition methods for watch and jewelry exterior parts fail to produce bright, saturated red colors that maintain their appearance and structure under mechanical stress without deterioration, and are angle-dependent.

Method used

A substrate coated with a tantalum-based metal nitride or oxynitride layer, 300 nm to 10 μm thick, is applied to achieve a bright red color with specific CIE L*a*b* coordinates, using PVD and nitriding processes.

Benefits of technology

The method provides a durable, angle-independent, and mechanically stable bright red coating that preserves the substrate's structure and appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159499000001_ABST
    Figure 2024159499000001_ABST
Patent Text Reader

Abstract

To provide: an external part with a bright and saturated color, for example red, obtained by one or more thin layers to preserve the structure of the substrate, the appearance of which does not vary with a user's viewing angle, and which is adapted to be subjected to mechanical stress without degrading; and a method for manufacturing said external part.SOLUTION: A watch or jewelry external part (10), in which the external part (10) includes a substrate (11) on a surface of which extends a coating (12) including a tantalum (Ta)-based nitride or oxynitride having a thickness ranging from 300 nm to 10 μm and an intrinsic and saturated color.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of watchmaking or jewellery, and more particularly to an external part of a watch or jewellery provided with an inherently coloured coating, and to a method for manufacturing said external part.

[0002] In this specification, the term "exterior part" refers to any ornament in the field of watchmaking or jewellery, consisting for example of a case, dial, dial applique, hands, bezel, crown, bracelet links, etc., that are intended to be visible to the user.

[0003] Preferably, the invention relates to an exterior piece of a watch or piece of jewellery provided with a coating whose intrinsic colour is a red shade. [Background technology]

[0004] In the field of watchmaking or jewellery, and more generally in the field of decorative articles, deposition methods by painting, varnishing or enameling are not always suitable.

[0005] Indeed, on the one hand, the layer of material applied to the surface of the article to be decorated is too thick to reveal the surface structure, such as a brushed, sunray brushed, sandblasted or laser structured surface, and on the other hand, the lifespan of this layer and the resulting color are not always satisfactory.

[0006] Therefore, thin layer vacuum deposition techniques such as physical vapor deposition (PVD), chemical vapor deposition (CVD) and atomic layer deposition (ALD) are preferred. Indeed, these thin layer vacuum deposition techniques allow the deposition of thin and resistant layers, which are generally suitable for coating small and abrasion-sensitive parts, for example with fine surface structures.

[0007] However, despite the fact that coatings of many unique colors can be obtained by these deposition techniques, certain unique colors, such as shades of red, especially bright and vivid red colors, cannot be obtained on an industrial scale by implementing these methods.

[0008] It is also known to deposit a stack of thin layers to form an interference optical system to produce a given color. However, the perception of the color is likely to depend on the viewing angle. Moreover, stacking of thin layers has significant manufacturing constraints insofar as the color produced is highly dependent on the thickness of the thin layers. Summary of the Invention [Problem to be solved by the invention]

[0009] There is therefore a need to obtain exterior parts having a bright, saturated colour, for example red, which are obtained by one or more thin layers to preserve the structure of the substrate, whose appearance does not vary depending on the user's viewing angle and which are adapted to be subjected to mechanical stresses without deterioration. [Means for solving the problem]

[0010] To this end, the invention relates to an external part for a watch or piece of jewellery, comprising a substrate, on whose surface is spread a coating comprising a metal nitride or oxynitride of the tantalum Ta series, the thickness of which is between 300 nm and 10 μm, so as to have a predetermined colour.

[0011] In particular embodiments, the invention may further include one or more of the following features, taken alone or in any technically possible combination:

[0012] In a particular embodiment, the coating has a thickness of 1 μm to 3 μm, preferably 2 μm.

[0013] In a particular embodiment, the red coating is made of tantalum nitride Ta having a stoichiometric composition substantially close to or equal to Ta3N5 so as to have a bright red color.

[0014] In a particular embodiment, the coating is produced with an oxygen addition in the range of 0-5 atomic %.

[0015] In a particular embodiment the coating has a red colour which is characterised in the CieLAB colour space in transmission mode for standard illuminant D65, with a 10° observer and measurement geometry d:0°, by coordinates a* and b* greater than 20, preferably by coordinates a* and b* greater than 50, more preferably by coordinates L*=[30;50], a*=[50;70] and b*=[60;80], in particular by L*=42, a*=58 and b*=72.

[0016] In a particular embodiment, the coating forms a composition of the type AB(O,N) where B is tantalum Ta and A is the metallic element.

[0017] In certain embodiments, the metal element A is preferably selected from Ba, Ca, Nd, La, Sr, Eu and Yb, and the coating comprises a composition substantially close to or equal to BaTaO2N, CaTaO2N, NdTaO2N, LaTaO2N, SrTaO2N, EuTaO2N or Yb2Ta2O5N2, respectively.

[0018] According to another object, the invention relates to a method for manufacturing an external part of a watch or piece of jewellery, such as that described above, comprising the steps: depositing a thin layer of tantalum (Ta)-based metal oxide having a thickness of 300 nm to 10 μm on the substrate; nitriding the thin layer to form a coating comprising at least one metal nitride or oxynitride; The present invention relates to a method comprising the steps of:

[0019] In certain implementations, the step of nitriding the deposited layer is incomplete to produce an oxynitride of the coating material.

[0020] In a particular implementation, during the deposition step, the deposited thin layer is TaO xand the nitriding step is carried out so as to produce a coating of tantalum nitride Ta, the stoichiometric composition of which is substantially close to or equal to the orthorhombic Ta3N5 system, so that the coating has a red colour.

[0021] In a particular implementation, during the deposition step, the deposited thin layer is TaO x and is combined with at least one metallic element selected from Ba, Ca, Nd, La, Sr, Eu or Yb.

[0022] In a particular implementation, the nitriding step is carried out in a suitable atmosphere at a temperature between 600° C. and 1200° C. for a period of 10 to 60 hours, preferably between 700° C. and 1000° C. for a period of 20 to 50 hours.

[0023] In a particular implementation, the nitridation step is carried out at a temperature of 900° C. for 40 hours in a suitable atmosphere. [Brief description of the drawings]

[0024] Other characteristics and advantages of the invention will become apparent from the following detailed description, given by way of non-limiting example with reference to the attached FIG. [Figure 1] 1 shows a schematic cross-sectional view of an exterior part according to a preferred embodiment of the present invention;

[0025] Please note that the figures are not necessarily drawn to scale for clarity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The present invention relates to an exterior watch or jewellery part 10, as shown diagrammatically in Figure 1, comprising a substrate 11, on whose visible surface extends a coating 12 comprising a metal nitride or oxynitride, the coating 12 having a predetermined colour depending on the metal of which it is composed, as will be described later in this specification.

[0027] The coating 12 is thick enough to be saturated in color, but at the same time thin enough so as not to obliterate the structure of the surface of the substrate 11 and not to affect the compatibility of the exterior part 10. To this end, the thickness of the coating 12 is between 300 nm and 10 μm, preferably between 1 μm and 3 μm. More preferably, the thickness of the coating 12 is 2 μm.

[0028] The material constituting the substrate 11 is advantageously chosen so as to be able to withstand the conditions of deposition of the metal oxide layer and of the nitridation of said layer, as will be explained in more detail below.

[0029] For example, the substrate 11 may be made of a ceramic material such as zirconia or sapphire, or a metal alloy such as stainless steel, or it may be made of silicon.

[0030] Advantageously, the exterior part 10 may include a bonding layer 13 made of Ti, Cr or other suitable metal known to those skilled in the art, interposed between the substrate 11 and the coating 12. The bonding layer 13 has a thickness of 20 nm to 500 nm, preferably 100 nm.

[0031] In a preferred exemplary embodiment of the invention, coating 12 is made of tantalum nitride, which is chemically and structurally substantially close to or equivalent to orthorhombic Ta3N5. This metal nitride has a bright red, i.e. saturated color, defined by the following coordinates in the CieLAB color space in the reflective mode of standard illuminant D65, with (SCI, measurement geometry di: 8°) and without (SCE, measurement geometry de: 8°) specular reflection at an observer angle of 10°: [Table 1]

[0032] In the case where the material constituting the substrate 11 is sapphire, the coating 12 can be observed either directly, i.e. the coating 12 is placed between the observer and the substrate 11, or indirectly, i.e. the substrate 11 is placed between the observer and the coating 12, so that the latter is observed through the substrate 11. It should be noted that in the case of applications of the invention where the coating 12 is observed indirectly, the exterior part 10 does not include a bonding layer 13 so as not to reduce the perception of the color of the coating 12.

[0033] The top table shows the color coordinates of coating 12 under direct observation, and the bottom table shows the color coordinates of coating 12 under indirect observation. [Table 2]

[0034] The bright red colour of the coating 12 deposited on the sapphire substrate 11 can be characterised by the values ​​L*=42, a*=58 and b*=72 obtained during a colourimetric measurement in transmission mode with standard illuminant D65, observer at 10° and measurement geometry d:0°. It is preferable to obtain red colours with coordinates a* and b* greater than 20, preferably greater than 50. More particularly, it is preferable to obtain red colours with coordinates L*=[30;50], a*=[50;70] and b*=[60;80].

[0035] In another exemplary embodiment of the present invention, the coating 12 can be formed of a composition of the type AB(O,N) where A is a metal element and B is tantalum Ta. This feature allows for the selection of different colored metal oxynitrides so that the coating 12 can have a wide variety of colors.

[0036] In an embodiment, metallic element A is selected from Ba, Ca, Nd, La, Sr, Eu, and Yb. Thus, coating 12 can be formed to have a composition substantially close to or equal to BaTaO2N having a dark red or brown color, CaTaO2N having a green or yellow color, NdTaO2N having a red or brown color, SrTaO2N having an orange color, LaTaO2N having a red or orange color, EuTaO2N having a brown color, or Yb2Ta2O5N2 having a green color.

[0037] The invention also relates to a method for manufacturing an external part 10 for a watch or an article of jewellery, for example as described above.

[0038] The method comprises the step of depositing a thin layer comprising a metal oxide on a substrate 11, such that the thin layer has a thickness selected between 300 nm and 10 μm. This deposition step is followed by a step of nitriding the thin layer to form a coating 12 of a metal nitride or oxynitride.

[0039] Preferably, the deposited thin layer is TaO x In particular, in this preferred embodiment, the deposition step is carried out by carrying out a PVD deposition method using a tantalum Ta target and a reactive gas consisting of O2. In particular, the thin layer can be deposited by cathodic sputtering, by gas phase electron beam evaporation, by arc or by pulsed laser beam ablation.

[0040] Therefore, at the end of the deposition step, the deposited thin layer is TaO x and a nitriding step is performed such that the coating 12 is made of red Ta3N5.

[0041] In detail, the nitriding step consists of exposing the thin layer to a suitable atmosphere, for example resulting from the thermal decomposition of ammonia, for several hours in a furnace enclosure heated to several hundred °C. More specifically, the nitriding step is carried out at a temperature between 600 °C and 1200 °C for a period of 10 to 60 hours, preferably at a temperature between 700 °C and 1000 °C for a period of 20 to 50 hours. In the most preferred embodiment, the nitriding step is carried out at a temperature of 900 °C for a period of 40 hours. By way of example, the flow rate of ammonia decomposed in the furnace enclosure during the nitriding step is 200 ml / min.

[0042] In one variation of the method, the nitridation of the deposited layer is not complete to produce an oxynitride of the coating material 12 .

[0043] It is also possible that during the thin layer deposition step, the thin layer is deposited from several different metal or alloy metal sources so that at the end of the nitridation step, the coating 12 comprises a composition of the AB(O,N) type, where A is the metallic element and B is tantalum Ta.

[0044] The manufacturing method can advantageously include a step of depositing a bonding layer 13 as described above, for example by CVD, ALD or PVD deposition, before carrying out a step of depositing the coating 12. Advantageously, the steps of depositing the bonding layer 13 and the coating 12 can be carried out successively in the same deposition enclosure, the pressure in said enclosure being maintained between the two depositions. These deposition steps require at least two different material sources, one of which is intended to be used to form the bonding layer 13 on the substrate 11 and one of which is intended to be used to form the coating 12 on the bonding layer 13.

[0045] More generally, it should be noted that the above implementations and embodiments are described as non-limiting examples, and therefore other variations are possible.

[0046] In particular, it is possible to carry out a step of selectively structuring the thin layer over its entire thickness before or after the nitriding step in order to form specific decorations, such a step can be carried out by means of photolithographic methods, laser ablation, etc.

[0047] For the same purpose, a preliminary step of structuring the surface of the substrate 11 may also be carried out.

Claims

1. An exterior part (10) for a watch or piece of jewellery, characterized in that it comprises a substrate (11) on whose surface a coating (12) comprising a tantalum Ta-based nitride or oxynitride having a thickness of between 300 nm and 10 μm is spread so as to have a predetermined colour.

2. The exterior part (10) of claim 1, wherein the coating (12) has a thickness of 1 μm to 3 μm.

3. 3. The exterior part (10) according to claim 2, wherein said coating (12) has a thickness equal to 2 μm.

4. The coating (12) has a stoichiometric composition substantially of orthorhombic Ta. 3 N 5 2. The exterior part (10) of claim 1, made of tantalum nitride having a thickness close to or equal to 1.0 mm.

5. The exterior component (10) of claim 1, wherein the coating is produced with an oxygen addition in the range of 0 to 5 atomic %.

6. 2. The exterior part (10) according to claim 1, wherein the coating (12) has a red colour characterized by coordinates a* and b* greater than 20, preferably greater than 50, in the CieLAB colour space in transmission mode for standard illuminant D65, with an observer at 10° and measurement geometry d:0°.

7. 7. The exterior part (10) according to claim 6, wherein the coating (12) has a red colour characterized in CieLAB colour space in transmission mode for standard illuminant D65 by coordinates L*=[30; 50], a*=[50; 70] and b*=[60; 80] with an observer angle of 10° and measurement geometry d:0°.

8. 8. The exterior part (10) according to claim 7, wherein the coating (12) has a red colour characterized by the coordinates L*=42, a*=58 and b*=72 in the CieLAB colour space in transmission mode for standard illuminant D65, with an observer at 10° and measurement geometry d:0°.

9. 2. The exterior part (10) according to claim 1, wherein the coating (12) forms a composition of the AB(O,N) type, where B is tantalum (Ta) and A is a metallic element selected from Ba, Ca, Nd, La, Sr, Eu and Yb.

10. The coating (12) is BaTaO 2 N, CaTaO 2 N, NdTaO 2 N, LaTaO 2 N, SrTaO 2 N, EuTaO 2 N or Yb 2 T 2 O 5 N 2 The exterior part (10) according to claim 9, made of

11. A method for manufacturing an external part (10) of a watch or piece of jewellery, comprising the steps of: Depositing a thin layer of tantalum (Ta)-based metal oxide having a thickness of 300 nm to 10 μm on the substrate (11); - nitriding said thin layer to form a coating (12) comprising at least one metal nitride or oxynitride; The method includes:

12. During the deposition step, the deposited thin layer is TaO x The nitriding step is carried out on a stoichiometric composition of substantially orthorhombic Ta. 3 N 5 The method of claim 11, wherein the coating (12) is made of tantalum nitride equal to

13. During the deposition step, the deposited thin layer is TaO x and in combination with at least one metallic element selected from Ba, Sr, Ca, Nd, La, Eu or Yb.

14. A method according to claim 11, wherein the nitriding step is carried out at a temperature between 600°C and 1200°C for a period of 10 to 60 hours, preferably between 700°C and 1000°C for a period of 20 to 50 hours.

15. The method of claim 14, wherein the nitriding step is performed at a temperature of 900° C. for 40 hours.

Citation Information

Patent Citations

  • External parts for watch

    JP1983104177A

  • Comfortable clock and its manufacturing method

    JP2004093134A

  • Photocatalyst, method for producing thin film-like photocatalyst and visible light responsive photocatalyst device

    JP2017000971A

  • Pearl base substrate coated with yellow layer

    JP2018104814A

  • mobile watch