Optical glass and optical element
A balanced glass composition with controlled components achieves high refractive index and low dispersion, addressing volatility and cost issues in existing optical glasses, ensuring stable optical performance and reduced environmental impact.
Patent Information
- Application Number
- JP2024061176
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-05
- Publication Date
- 2024-11-08
AI Technical Summary
Existing optical glasses with high refractive index and low dispersion face challenges in controlling refractive index and dispersion due to volatile fluorine content, requiring specialized equipment, and high costs associated with gadolinium oxide (Gd2O3).
A glass composition with controlled contents of SiO2, B2O3, ZnO, La2O3, Y2O3, Gd2O3, Yb2O3, ZrO2, TiO2, WO3, Bi2O3, Nb2O5, Li2O, Na2O, K2O, MgO, CaO, SrO, and BaO, along with a limited fluorine content, achieves a high refractive index and low dispersion without volatile issues and high costs.
The composition provides optical glasses with stable refractive index and dispersion properties, reducing environmental impact and production costs while maintaining high optical performance.
Smart Images

Figure 2024159541000001 
Figure 2024159541000002 
Figure 2024159541000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical glass and an optical element. [Background technology]
[0002] In recent years, optical glasses having high refractive index and low dispersion have been proposed as materials for optical elements (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] CN102910816A [Patent Document 2] JP 2002-128539 A Summary of the Invention [Problem to be solved by the invention]
[0004] Patent Document 1 (CN102910816A) discloses a glass composition containing a large amount of F (fluorine) as a glass composition that achieves a high refractive index and low dispersion (see the Examples in CN102910816A). However, since F is an easily volatile component, it is not easy to control the refractive index and dispersion (specifically, Abbe number) of glass containing a large amount of F within a desired range due to the volatilization of F. In addition, in order to produce glass containing a large amount of F, special production equipment is required to prevent the volatilized F from affecting the environment.
[0005] On the other hand, Patent Document 2 (JP Patent Publication No. 2002-128539) discloses a glass composition containing a large amount of Gd2O3 as a glass composition that realizes a high refractive index and low dispersion (see the Examples in JP Patent Publication No. 2002-128539). However, since Gd2O3 is an expensive component whose unit price has risen sharply in recent years, a glass with a low Gd2O3 content is desirable in order to reduce the cost of glass.
[0006] In view of the above, an object of one aspect of the present invention is to provide an optical glass having a low F content and low Gd2O3 content, and having a high refractive index and low dispersion. [Means for solving the problem]
[0007] As a result of extensive investigations, the inventors have newly discovered that it is possible to achieve a high refractive index and low dispersion in a glass composition having a low F content and Gd2O3 content by adjusting the contents of various components as follows.
[0008] One aspect of the present invention is as follows. [1] In the glass composition based on oxides expressed in mole percent, SiO2 content is 0.00% or more and 15.00% or less, B2O3 content is between 40.00% and 90.00%. ZnO content is 0.00% or more and 5.00% or less, La2O3 content is 5.00% or more and 40.00% or less, Y2O3 content is 1.00% or more and 20.00% or less, Gd2O3 content is 0.00% or more and 3.00% or less, Yb2O3 content is 0.00% or more and less than 1.00%; ZrO2 content is 0.00% or more and 15.00% or less, TiO2 content is 0.00% or more and 2.00% or less, WO3 content is 0.00% or more and 2.00% or less, Bi2O3 content is 0.00% or more and 2.00% or less, Nb2O5 content is 0.00% or more and 2.00% or less, The total content of Li2O, Na2O and K2O (Li2O + Na2O + K2O) is 0.00% or more and 5.00% or less, The total content of MgO, CaO, SrO and BaO (MgO+CaO+SrO+BaO) is 0.00% or more and 5.00% or less, The molar ratio of B2O3 to Y2O3 content (B2O3 / Y2O3) is 15.00 or less; The molar ratio of the B2O3 content to the total content of ZrO2, ZnO, Nb2O5, TiO2, WO3 and Bi2O3 (B2O3 / (ZrO2+ZnO+Nb2O5+TiO2+WO3+Bi2O3)) is 15.00 or more and 50.00 or less; The molar ratio of the La2O3 content to the total content of ZrO2, ZnO, Nb2O5 and TiO2 (La2O3 / (ZrO2+ZnO+Nb2O5+TiO2)) is 4.00 or more, and An optical glass in which the content of F element expressed as an exclusive percentage by mole percentage relative to the total content of the glass composition based on the above oxides (hereinafter also referred to as "F content") is 0.00% or more and 3.00% or less. [2] The optical glass according to [1], having a ZnO content of 0.00% or more and 2.00% or less. [3] The optical glass according to [1] or [2], having a ZnO content of 0.00% or more and 1.70% or less. [4] The optical glass according to any one of [1] to [3], having an Yb2O3 content of 0.00% or more and 0.20% or less. [5] The optical glass according to any one of [1] to [4], having a refractive index nd of 1.73000 or more and 1.77000 or less. [6] The optical glass according to any one of [1] to [5], having an Abbe number vd of 52.00 or more and 53.00 or less. [7] The refractive index nd and the Abbe number νd are expressed by the following formula 1: nd≧2.20000-0.00871*νd The optical glass according to any one of [1] to [6], which satisfies the above. [8] The optical glass according to any one of [1] to [7], wherein the value (nd-1) / d calculated from the refractive index nd and the specific gravity d is 0.173 or greater. [9] The ZnO content is 0.00% or more and 1.70% or less, The Yb2O3 content is 0.00% or more and 0.20% or less, The refractive index nd is 1.73000 or more and 1.77000 or less, The Abbe number νd is 52.00 or more and 53.00 or less, The refractive index nd and the Abbe number νd are expressed by the following formula 1: nd≧2.20000-0.00871*νd and The optical glass according to any one of [1] to [8], wherein the value (nd-1) / d calculated from the refractive index nd and the specific gravity d is 0.173 or greater.
[10] An optical element comprising the optical glass according to any one of [1] to [9]. Effect of the Invention
[0009] According to one aspect of the present invention, it is possible to provide an optical glass having a low F content and Gd2O3 content and having a high refractive index and low dispersion, and an optical element made of this optical glass. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Optical glass] In the present invention and this specification, the glass composition of optical glass is expressed as a glass composition based on oxides expressed in mole percent. Here, "glass composition based on oxides" refers to a glass composition obtained by converting the glass raw materials into oxides that exist in the glass after being completely decomposed during melting. In the glass composition expressed in mole percent, the glass composition is expressed on a molar basis (mol%, molar ratio). Hereinafter, for glass compositions expressed in mole percent, "mol%" will also be simply referred to as "%".
[0011] In the present invention and this specification, the F content of the optical glass is the content (unit: mol %) expressed as an external ratio of the F element to the total content of the glass composition based on the above oxides, which is 100 mol %.
[0012] In the present invention and this specification, the content of a component is 0%, 0.0% or 0.00%, or is not included or not introduced, means that the component is substantially not included, and the content of the component is equal to or less than the impurity level. The content of the component is equal to or less than the impurity level, for example, less than 0.01%. "0%" can mean, for example, "0.0%" or "0.00%".
[0013] The glass composition of the present invention and this specification can be determined by a method such as ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). For example, quantitative analysis is performed for each element using ICP-AES. The analytical values are then converted into oxide notation. The analytical values obtained by ICP-AES may contain a measurement error of, for example, about ±5% of the analytical value. Therefore, the oxide notation values converted from the analytical values may also contain an error of about ±5%.
[0014] In the present invention and this specification, the refractive index refers to the refractive index nd at the d line of helium (wavelength 587.56 nm).
[0015] In the present invention and this specification, the Abbe number νd is used as a value indicating a property related to dispersion, and is expressed by the following formula. νd=(nd-1) / (nF-nC) In the above formula, nF is the refractive index at the F line of blue hydrogen (wavelength 486.13 nm), and nC is the refractive index at the C line of red hydrogen (656.27 nm).
[0016] The optical glass (sometimes simply referred to as "glass") will be described in more detail below.
[0017] <Glass composition> SiO2 is a glass-forming oxide, and is a component that contributes to increasing the viscosity of glass and reducing the tendency to devitrification. SiO2 is also a component that lowers the refractive index, increases vd, decreases the specific gravity, increases the glass transition temperature Tg, and decreases the degree of coloration. The glass transition temperature Tg and the degree of coloration will be described later. The SiO2 content of the above glass is 0.00% or more, and can be 0.00% or more or more than 0.00%, and is preferably 0.50% or more, and more preferably 1.00 or more, 2.00 or more, 3.00 or more, 4.00 or more, 5.00 or more, 6.00 or more, and 6.50 or more in that order. On the other hand, in order to easily obtain a homogeneous glass, it is preferable to suppress the deterioration of the melting property of the glass. From this viewpoint, the SiO2 content of the above glass is 15.00% or less, preferably 14.00% or less, and more preferably 13.00% or less, 12.00% or less, 11.00% or less, 10.00% or less, 9.00% or less, 8.00% or less, and 7.50% or less in that order.
[0018] The B2O3 content of the above glass is 40.00% or more. B2O3 is a glass-forming oxide like SiO2. B2O3 is also a component that lowers the refractive index, increases vd, lowers the specific gravity, and lowers the glass transition temperature Tg. By making the B2O3 content 40.00% or more, the devitrification resistance of the glass can be improved and low dispersion can be easily obtained. The B2O3 content of the above optical glass is preferably 45.00% or more, and more preferably 50.00% or more, 55.00% or more, 57.00% or more, 59.00% or more, and 61.00% or more in that order. On the other hand, among various glass components, B2O3 is a component that is relatively easy to volatilize. From the viewpoint of suppressing fluctuations in the glass composition, the B2O3 content of the above glass is 90.00% or less, preferably 85.00% or less, and more preferably 80.00% or less, 75.00% or less, 72.00% or less, 70.00% or less, 68.00% or less, 66.00% or less, and 64.00% or less in that order.
[0019] The ZnO content of the glass is 0.00% or more, and can be 0.00% or more. ZnO is a component that can increase the refractive index, decrease vd, increase the specific gravity, and improve chemical durability. ZnO is also a component that has the effect of decreasing the glass melting temperature, liquidus temperature, glass transition temperature Tg, and the like. From the viewpoint of suppressing crystallization of the glass, the ZnO content of the glass is 5.00% or less, preferably 4.50% or less, and more preferably 4.00% or less, 3.50% or less, 3.00% or less, 2.50% or less, 2.00% or less, 1.70% or less, 1.50% or less, 1.00% or less, and 0.50% or less in that order.
[0020] La2O3 is a component that contributes to imparting high refractive index and low dispersion to the glass. The La2O3 content of the above glass is 5.00% or more, preferably 7.50% or more, and more preferably 10.00% or more, 12.50% or more, 15.00% or more, and 17.50% or more in that order. On the other hand, from the viewpoints of suppressing devitrification and reducing the specific gravity of the glass, the La2O3 content of the above glass is 40.00% or less, preferably 37.50% or less, and more preferably 35.00% or less, 32.50% or less, 30.00% or less, 27.50% or less, 25.00% or less, and 22.50% or less, in that order.
[0021] Like La2O3, Y2O3 is a component that contributes to imparting high refractive index and low dispersion to the glass. The Y2O3 content of the above glass is 1.00% or more, preferably 2.00% or more, and more preferably 3.00% or more, 4.00% or more, 5.00% or more, and 6.00% or more in that order. On the other hand, from the viewpoints of suppressing devitrification and reducing the specific gravity of the glass, the Y2O3 content of the above glass is 20.00% or less, preferably 18.00% or less, and more preferably 16.00% or less, 14.00% or less, 12.00% or less, and 10.00% or less in that order.
[0022] The Gd2O3 content of the glass is 0.00% or more, and can be 0.00% or more. Gd2O3 is an optional component that contributes to increasing the refractive index of the glass and also contributes to low dispersion, similar to La2O3. However, since Gd2O3 has a high unit price and is a component that increases the specific gravity, it is preferable to include as little Gd2O3 as possible in the glass when it is contained in the glass. The Gd2O3 content of the glass is 3.00% or less, preferably 2.50% or less, more preferably 2.00% or less, 1.50% or less, 1.00% or less, and 0.50% or less, in that order, and most preferably 0.00%.
[0023] The Yb2O3 content of the glass is 0.00% or more, and can be 0.00% or more. Yb2O3 is an optional component that can contribute to a high refractive index and low dispersion of the glass. Since Yb2O3 is a particularly expensive raw material among rare earth raw materials, it is preferable that the Yb2O3 content is low. The Yb2O3 content of the glass is less than 1.00%, preferably 0.50% or less, more preferably 0.20% or less, even more preferably 0.10% or less, and most preferably 0.00%.
[0024] The molar ratio of B2O3 to the Y2O3 content of the glass (B2O3 / Y2O3) is 15.00 or less, preferably 14.00 or less, and more preferably 13.00 or less, 12.00 or less, 11.00 or less, 10.00 or less, and 9.00 or less, in that order, from the viewpoint of increasing the refractive index and decreasing the dispersion of the glass. The molar ratio (B2O3 / Y2O3) can be, for example, more than 0.00, 1.00 or more, 2.00 or more, 3.00 or more, 4.00 or more, 5.00 or more, or 6.00 or more.
[0025] The ZrO2 content of the glass is 0.00% or more, and can be 0.00% or more. ZrO2 is a component that contributes to improving the chemical durability of the glass and increasing the refractive index. The ZrO2 content of the glass is preferably 0.40% or more, more preferably 0.80% or more, 1.20% or more, 1.60% or more, and 2.00% or more in that order. On the other hand, from the viewpoint of realizing the desired low dispersion and low specific gravity, the ZrO2 content of the above glass is 15.00% or less, preferably 13.00% or less, and more preferably 11.00% or less, 9.00% or less, 7.00% or less, 5.00% or less, and 3.00% or less in that order.
[0026] In the above glass, the content of each of TiO2, WO3 and Bi2O3 is equal to or greater than 0.00%, and can be 0.00% or more than 0.00%. TiO2, WO3 and Bi2O3 are components that contribute to imparting high refractive index and low dispersion to the glass. By making each content 2.00% or less, it is possible to suppress a decrease in the transmittance of the glass for ultraviolet to visible light (particularly wavelengths of 500 nm or less). From this point of view, each content of TiO2, WO3 and Bi2O3 is 2.00% or less, preferably 1.50% or less, more preferably 1.00% or less, even more preferably 0.50% or less, and most preferably 0.00%.
[0027] The Nb2O5 content of the above glass is equal to or greater than 0.00%, and can be 0.00% or more. Nb2O5 is a component that contributes to imparting a high refractive index and low dispersion to the glass. On the other hand, Nb2O5 is a component that is expensive as a raw material, increases the specific gravity of the glass, and affects the transmittance of the glass for ultraviolet to visible light. In consideration of the above, the Nb2O5 content of the above glass is 2.00% or less, preferably 1.50% or less, more preferably 1.00% or less, even more preferably 0.50% or less, and most preferably 0.00%.
[0028] ZrO2, ZnO, Nb2O5, TiO2, WO3 and Bi2O3 are all components that contribute to imparting high refractive index and low dispersion to glass. Adjusting the molar ratio of the B2O3 content to the total content of these components can contribute to realizing high refractive index and low dispersion in a glass composition with low F and Gd2O3 contents. Regarding the molar ratio of the B2O3 content to the total content of ZrO2, ZnO, Nb2O5, TiO2, WO3 and Bi2O3 in the above glass (B2O3 / (ZrO2+ZnO+Nb2O5+TiO2+WO3+Bi2O3)), if the value of this molar ratio is small, the refractive index nd of the glass increases and the Abbe number νd decreases, and if the value of this molar ratio is large, the refractive index nd of the glass decreases and the Abbe number νd increases. From the viewpoint of realizing a high refractive index and low dispersion, the molar ratio of the above glass (B2O3 / (ZrO2+ZnO+Nb2O5+TiO2+WO3+Bi2O3)) is 15.00 or more and 50.00 or less. The molar ratio (B2O3 / (ZrO2+ZnO+Nb2O5+TiO2+WO3+Bi2O3)) is preferably 16.00 or more, and more preferably 17.00 or more, 18.00 or more, 19.00 or more, 20.00 or more, and 21.00 or more in that order. In addition, the molar ratio (B2O3 / (ZrO2+ZnO+Nb2O5+TiO2+WO3+Bi2O3)) is preferably 45.00 or less, and more preferably 40.00 or less, 35.00 or less, 30.00 or less, and 25.00 or less in that order.
[0029] La2O3, ZrO2, ZnO, Nb2O5 and TiO2 are all components that contribute to increasing the refractive index of the glass, but ZrO2, ZnO, Nb2O5 and TiO2 contribute less to decreasing the dispersion of the glass than La2O3. Adjusting the molar ratio of the La2O3 content to the total content of ZrO2, ZnO, Nb2O5 and TiO2 can contribute to achieving high refractive index and low dispersion in a glass composition with a low F content and Gd2O3 content. The molar ratio of the La2O3 content to the total content of ZrO2, ZnO, Nb2O5 and TiO2 of the optical glass (La2O3 / (ZrO2+ZnO+Nb2O5+TiO2)) is 4.00 or more, preferably 4.50 or more, more preferably 5.00 or more, 5.50 or more, 6.00 or more, 6.50 or more, and 7.00 or more in that order. The molar ratio (La2O3 / (ZrO2+ZnO+Nb2O5+TiO2)) can be, for example, 20.00 or less, 19.00 or less, 18.00 or less, 17.00 or less, or 16.00 or less.
[0030] The total content of Li2O, Na2O and K2O (Li2O+Na2O+K2O) in the above glass is 0.00% or more and 5.00% or less. The total content (Li2O+Na2O+K2O) can be 0.00% or more than 0.00%. Regarding alkali metal oxides, Rb2O and Cs2O are expensive components and are not suitable for general-purpose glass compared to Li2O, Na2O and K2O. From the viewpoint of improving the meltability of glass, lowering the glass transition temperature Tg and lowering the specific gravity of glass while maintaining the thermal stability, chemical durability, weather resistance and machinability of glass, the total content of Li2O, Na2O and K2O in the above glass (Li2O+Na2O+K2O) is 0.00% or more and 5.00% or less. The total content (Li2O+Na2O+K2O) is preferably 4.00% or less, more preferably 3.00% or less, 2.00% or less and 1.00% or less in that order.
[0031] The Li2O content is 0.00% or more, and can be 0.00% or more. From the viewpoints of further improving the thermal stability of the glass, suppressing a decrease in the glass transition temperature (thereby improving machinability), and improving chemical durability and weather resistance, the Li2O content is preferably 5.00% or less, and more preferably 4.00% or less, 3.00% or less, and 2.00% or less in that order. The respective contents of Na2O, K2O, Rb2O and Cs2O are 0.00% or more, and can be 0.00% or more than 0.00%. Na2O, K2O, Rb2O and Cs2O all have the function of improving the meltability of glass, but as their contents increase, the thermal stability, chemical durability, weather resistance and machinability of glass tend to decrease. Therefore, the respective contents of Na2O, K2O, Rb2O and Cs2O are preferably 5.00% or less, more preferably 4.00% or less, 3.00% or less and 2.00% or less in that order.
[0032] The total content (MgO+CaO+SrO+BaO) of MgO, CaO, SrO and BaO in the above glass is 0.00% or more, and can be 0.00% or more. The alkaline earth metal oxides are components that contribute to the production of homogeneous glass, since they facilitate the melting of glass raw materials. From the viewpoint of suppressing devitrification of the glass and realizing the desired optical properties, the total content (MgO+CaO+SrO+BaO) in the above glass is 5.00% or less, preferably 4.00% or less, more preferably 3.00% or less, 2.00% or less, and 1.00% or less in that order.
[0033] Each of the contents of MgO, CaO, SrO and BaO is 0.00% or more and can be 0.00% or more than 0.00%. From the viewpoint of suppressing devitrification of the glass and realizing desired optical properties, each of the contents of MgO, CaO, SrO and BaO is preferably 5.00% or less, more preferably 4.00% or less, and further preferably 3.00% or less, 2.00% or less, and 1.00% or less in that order.
[0034] F is a component that makes glass less dispersible, and is also a component that can improve meltability and lower the glass transition temperature Tg by adding a small amount. However, glass containing a large amount of F is not preferable for the reasons described above. Therefore, in the above glass, the content of F element expressed in mole percent relative to the total content of the glass composition based on oxides (F content) is 0.00% or more and 3.00% or less. The F content can be 0.00% or more than 0.00%. The F content is preferably 2.50% or less, more preferably 2.00% or less, 1.50% or less, 1.00% or less, 0.50% or less, and most preferably 0.00%.
[0035] As for other glass components, taking into consideration the environmental impact, the As2O3 content is preferably 0.10% or less, more preferably 0.01% or less, and most preferably 0.00%. Also, taking into consideration the environmental impact, the PbO content is preferably 1.00% or less, more preferably 0.50% or less, and more preferably 0.10% or less, and most preferably 0.00%.
[0036] Ta2O5 is an expensive component. From the viewpoint of reducing the cost of the glass, the Ta2O5 content is preferably 2.00% or less, more preferably 1.50% or less, 1.00% or less, and 0.50% or less in that order, and is most preferably 0.00%.
[0037] Sb2O3 is a component that can be added as a clarifier. Although a small amount of Sb2O3 can suppress the decrease in light transmittance caused by the inclusion of impurities such as Fe, the coloring of the glass tends to increase when the amount of Sb2O3 added is increased. Therefore, the amount of Sb2O3 added is preferably 0.00% or more and 0.10% or less, more preferably 0.00% or more and 0.08% or less, and even more preferably 0.00% or more and 0.05% or less, in terms of the total amount of Sb2O3 added. The Sb2O3 content by the total amount means the Sb2O3 content by mass % when the total amount of glass components other than Sb2O3 is taken as 100 mass %.
[0038] SnO2 can also be added as a clarifier, but if it is added in an amount exceeding 1.00% by weight, the glass will become colored, and when the glass is heated and softened and reshaped by press molding or the like, Sn will become the starting point for crystal nucleation, causing a tendency for devitrification. Therefore, the amount of SnO2 added is preferably 0.00% or more and 1.00% or less by weight, more preferably 0.00% or more and 0.50% or less, and it is particularly preferable to not add any SnO2. The SnO2 content by weight refers to the SnO2 content expressed in mass% when the total content of glass components other than SnO2 is taken as 100 mass%.
[0039] <Glass properties> (Refractive index nd) The glass can be a high refractive index glass by having the above glass composition. From the viewpoint of usefulness as a material for optical elements, the refractive index nd of the glass is preferably 1.73000 or more, more preferably 1.74000 or more, and even more preferably 1.75000 or more. From the viewpoint of usefulness as a material for optical elements, the refractive index nd of the glass can be 1.77000 or less, and preferably 1.76000 or less.
[0040] (Abbe number νd) The above glass can exhibit low dispersion by having the above glass composition. From the viewpoint of usefulness as a material for optical elements, the Abbe number vd of the above glass is preferably 52.00 or more and 53.00 or less.
[0041] The above glass has the above glass composition and is therefore able to satisfy the following formula 1. From the standpoint of usefulness as a material for optical elements, optical glasses whose refractive index nd and Abbe number vd satisfy the following formula 1 are preferred. Formula 1:nd≧2.20000-0.00871*νd
[0042] (specific gravity) The refractive power of the optical elements that make up an optical system is determined by the refractive index of the glass that makes up the optical element and the curvature of the optical functional surface of the optical element (the surface through which the light rays to be controlled enter and exit). If you try to increase the curvature of the optical functional surface, the thickness of the optical element also increases. As a result, the optical element becomes heavier. In contrast, if glass with a high refractive index is used, it is possible to obtain a large refractive power without increasing the curvature of the optical functional surface. From the above, if the refractive index can be increased while suppressing an increase in the specific gravity of the glass, it will be possible to reduce the weight of an optical element having a certain refractive power. From the above viewpoints, the specific gravity of the glass is preferably 4.50 or less, more preferably 4.40 or less, and more preferably 4.30 or less. Since a lower specific gravity is more preferable from the viewpoint of reducing the weight of the optical element, there is no particular lower limit for the specific gravity of the optical glass. In one embodiment, the specific gravity can be 3.50 or more, 3.75 or more, or 4.00 or more. In the present invention and this specification, the "specific gravity" is a value measured by the Archimedes method. From the above viewpoints, the value calculated as (nd-1) / d from the refractive index nd and specific gravity d of the glass is preferably 0.173 or more, more preferably 0.174 or more, 0.175 or more, 0.176 or more, 0.177 or more, and 0.178 or more in that order. The value calculated as (nd-1) / d can be, for example, 0.200 or less or 0.190 or less.
[0043] (Coloring degree λ5, λ 80 ) The light transmittance of the glass, specifically, the suppression of the shift of the light absorption edge on the short wavelength side to longer wavelengths, is the coloring degree λ5 and λ 80 The coloring degree λ5 represents the wavelength at which the spectral transmittance (including surface reflection loss) of a glass with a thickness of 10±0.1 mm is 5% from the ultraviolet region to the visible region. λ 80 represents the wavelength at which the spectral transmittance measured by the method described for λ5 is 80%. 80is a value measured in the wavelength range of 250 to 700 nm. The spectral transmittance T (%) of glass in the present invention and this specification is calculated by dividing the intensity of light incident perpendicularly on one of two optically polished parallel flat surfaces of a glass sample by the intensity of light I in The intensity of the light that passes through the glass sample and exits from the other side is I out When T(%)=I out / I in ×100 It is expressed as: Coloring degree λ5 and λ 80 According to the method, the absorption edge on the short wavelength side of the spectral transmittance can be quantitatively evaluated. For example, when lenses are bonded together with an ultraviolet-curable adhesive to produce a cemented lens, the adhesive is cured by irradiating it with ultraviolet light through an optical element. From the viewpoint of efficiently curing the ultraviolet-curable adhesive, it is preferable that the absorption edge on the short wavelength side of the spectral transmittance is in a short wavelength range. As an index for quantitatively evaluating the absorption edge on the short wavelength side, the coloring degree λ5 and λ 80 One or more of the following may be used. The above glass can preferably exhibit λ5 of 300 nm or less. λ5 is more preferably 295 nm or less, 290 nm or less, and 285 nm or less, in that order. The shorter the wavelength of λ5, the more preferable it is, and there is no particular lower limit. The optical glass has a λ of, for example, 550 nm or less or 500 nm or less. 80 and preferably has a λ value of 400 nm or less. 80 It can be shown that λ 80 is more preferably 395 nm or less, 390 nm or less, 385 nm or less, and 380 nm or less, in that order. 80 The shorter the wavelength, the more preferable it is, and the lower limit is not particularly limited.
[0044] (glass transition temperature Tg) From the viewpoint of reducing the burden on the annealing furnace and the molding die, the glass transition temperature Tg of the above glass is preferably 750° C. or lower, and more preferably 745° C. or lower, 740° C. or lower, 735° C. or lower, 730° C. or lower, and 725° C. or lower in that order. On the other hand, from the viewpoint of machinability (more specifically, from the viewpoint of being less likely to break during mechanical processing of the glass such as cutting, milling, grinding, polishing, etc.), the glass transition temperature Tg of the above glass is preferably 600° C. or higher, more preferably 620° C. or higher, and even more preferably 640° C. or higher. The glass transition temperature Tg is determined by a differential scanning calorimeter at a heating rate of 10° C. / min.
[0045] <Method of manufacturing optical glass> The optical glass can be obtained by weighing, preparing and thoroughly mixing raw materials such as oxides, carbonates, sulfates, nitrates and hydroxides so as to obtain the desired glass composition, heating and melting the mixture in a melting vessel, degassing and stirring the mixture to produce a homogeneous, bubble-free molten glass, and then molding the glass. Specifically, the glass can be produced by using a known melting method.
[0046] [Glass material for press molding, optical element blanks, and their manufacturing methods] Another aspect of the present invention is a glass material for press molding comprising the optical glass; an optical element blank made of the optical glass; Regarding.
[0047] According to another aspect of the present invention, a method for producing a glass material for press molding, comprising a step of molding the optical glass into a glass material for press molding; a method for producing an optical element blank, comprising a step of press-molding the glass material for optical glass press molding using a press mold to produce an optical element blank; A method for producing an optical element blank, comprising the step of forming the optical glass into an optical element blank; will also be provided.
[0048] An optical element blank is an optical element base material that approximates the shape of a target optical element and has polishing margins (surface layers to be removed by polishing) and, if necessary, grinding margins (surface layers to be removed by grinding) added to the shape of the optical element. The optical element is finished by grinding and polishing the surface of the optical element blank. In one embodiment, the optical element blank can be produced by a method (called a direct press method) in which a molten glass obtained by melting an appropriate amount of the above glass is press-molded. In another embodiment, the optical element blank can also be produced by solidifying a molten glass obtained by melting an appropriate amount of the above glass.
[0049] In another embodiment, a glass material for press molding is prepared, and the prepared glass material for press molding is press molded to produce an optical element blank.
[0050] The press molding of the glass material for press molding can be carried out by a known method in which the glass material for press molding in a heated and softened state is pressed in a press mold. Both heating and press molding can be carried out in the atmosphere. By annealing after press molding to reduce distortion inside the glass, a homogeneous optical element blank can be obtained.
[0051] Glass materials for press molding include not only those called glass gobs for press molding, which are used for press molding as they are to produce optical element blanks, but also those that are mechanically processed such as by cutting, grinding, polishing, etc., and are used for press molding via glass gobs for press molding. Cutting methods include a method in which a groove is formed in the portion of the surface of the glass plate to be cut by a method called scribing, and local pressure is applied to the grooved portion from the back side of the surface on which the groove is formed, thereby breaking the glass plate at the grooved portion, and a method in which the glass plate is cut by a cutting blade. Grinding and polishing methods include barrel polishing, etc.
[0052] The glass material for press molding can be produced, for example, by casting molten glass into a mold to form a glass plate, and cutting this glass plate into a plurality of glass pieces. Alternatively, a suitable amount of molten glass can be molded to produce a glass gob for press molding. An optical element blank can also be produced by reheating, softening, and press-molding the glass gob for press molding. The method of producing an optical element blank by reheating, softening, and press-molding glass is called a reheat press method, as opposed to a direct press method.
[0053] [Optical elements and their manufacturing methods] Another aspect of the present invention is An optical element made of the above optical glass Regarding.
[0054] The optical element is produced using the optical glass. In the optical element, the glass surface may be coated with one or more layers of coating, such as a multilayer film including an anti-reflection film.
[0055] According to another aspect of the present invention, A method for producing an optical element, comprising the step of producing an optical element by grinding and / or polishing the optical element blank described above; will also be provided.
[0056] In the manufacturing method of the optical element, the mechanical processing such as grinding and polishing can be performed by applying a known method, and the surface of the optical element after processing can be sufficiently cleaned and dried to obtain an optical element with high internal quality and surface quality. In this way, an optical element made of the optical glass can be obtained. Examples of optical elements include various lenses such as spherical lenses, aspherical lenses, and microlenses, and prisms.
[0057] In addition, the optical element made of the optical glass is also suitable as a lens constituting a cemented optical element. Examples of cemented optical elements include a cemented lens formed by cementing lenses together, and a lens and a prism. For example, a cemented optical element can be produced by precisely processing the cemented surfaces of two optical elements to be cemented (for example, by spherical polishing) so that the shapes are inverted, applying an ultraviolet-curing adhesive used for bonding the cemented lens, bonding them together, and then irradiating ultraviolet light through the lens to cure the adhesive. In order to produce a cemented optical element in this way, the optical glass is preferable. A plurality of optical elements to be cemented are each produced using a plurality of types of glass having different Abbe numbers νd, and cemented together to produce an element suitable for correcting chromatic aberration. EXAMPLES
[0058] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the embodiments shown in the examples.
[0059] [Example 1] <Examples No. 1 to 57> The raw materials for introducing each component were the corresponding nitrates, sulfates, carbonates, hydroxides, oxides, boric acid, etc., and the raw materials were weighed and thoroughly mixed to obtain the glass composition (unit: mol%) shown in the table below. The mixed raw materials were placed in a platinum crucible and heated in a furnace set at 1350°C for 2 hours. The molten glass was stirred to homogenize it, then poured into a preheated mold and allowed to cool to near the glass transition temperature. It was then immediately placed in an annealing furnace and held at about the glass transition temperature for about 30 minutes, then slowly cooled at a rate of -30°C / hour for 4 hours, and then allowed to cool to room temperature in the furnace to obtain the optical glasses No. 1 to 57 shown in the table below. None of these optical glasses contain F. The Sb2O3 content shown in the table below is an exclusive percentage, with the unit of content being % by mass. The physical properties of the optical glass thus obtained are shown in the following table. The physical properties of the optical glasses were measured by the methods described below.
[0060] <Evaluation of physical properties of optical glass> (1) Refractive index nd Abbe number νd The refractive index nd and Abbe number vd of the obtained glass were measured by the refractive index measurement method specified by the Japan Optical Glass Industry Association.
[0061] (2) Glass transition temperature Tg The glass was thoroughly crushed in a mortar and used as a sample. A platinum cell was used as a sample container, and the glass transition temperature Tg was measured at a heating rate of 10°C / min using a Rigaku differential scanning calorimeter (DSC8271).
[0062] (3) Specific gravity Specific gravity was measured by Archimedes' method.
[0063] (4) Coloring degree λ5, λ80 A glass sample having a thickness of 10±0.1 mm and two optically polished flat surfaces facing each other was used to measure the spectral transmittance T (%) using a spectrophotometer. The wavelength (nm) at which T is 5% was defined as λ5, and the wavelength (nm) at which T is 80% was defined as λ80.
[0064] [Table 1-1]
[0065] [Table 1-2]
[0066] [Table 1-3]
[0067] [Table 1-4]
[0068] [Table 1-5]
[0069] [Table 1-6]
[0070] [Table 1-7]
[0071] [Table 1-8]
[0072] [Table 1-9]
[0073] [Table 1-10]
[0074] [Table 1-11]
[0075] [Table 1-12]
[0076] [Example 2] A glass gob for press molding was prepared using the various glasses obtained in Example 1. The glass gob was heated and softened in the atmosphere, and press molded in a press mold to prepare a lens blank (optical element blank). The prepared lens blank was removed from the press mold, annealed, and machined, including polishing, to prepare a spherical lens made of the various glasses prepared in Example 1.
[0077] [Example 3] A desired amount of the molten glass produced in Example 1 was press molded in a press mold to produce a lens blank (optical element blank). The produced lens blank was removed from the press mold, annealed, and subjected to mechanical processing including polishing to produce a spherical lens made of the various glasses produced in Example 1.
[0078] [Example 4] The molten glass produced in Example 1 was solidified to produce a glass lump (optical element blank), which was then annealed and machined, including polishing, to produce spherical lenses made of the various glasses produced in Example 1.
[0079] [Example 5] The spherical lenses produced in Examples 2 to 4 were bonded to spherical lenses made of other types of glass to produce cemented lenses. The cemented surfaces of the spherical lenses produced in Examples 2 to 4 were convex, and the cemented surfaces of the spherical lenses made of other types of glass were concave. The above two cemented surfaces were produced so that the absolute values of the radii of curvature were equal to each other. An ultraviolet-curing adhesive for bonding optical elements was applied to the cemented surfaces, and the two lenses were bonded together with their cemented surfaces facing each other. Thereafter, ultraviolet light was irradiated onto the adhesive applied to the cemented surfaces through the spherical lenses produced in Examples 2 to 4 to solidify the adhesive. A cemented lens was produced in the manner described above. The cemented lens had a sufficiently high bonding strength and exhibited a sufficient level of optical performance.
[0080] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. For example, by subjecting the above-mentioned exemplary glass compositions to compositional adjustments as described in the specification, an optical glass according to one aspect of the present invention can be obtained. Furthermore, it is of course possible to arbitrarily combine two or more of the items described in the specification as examples or preferred ranges.
Claims
1. In the glass composition based on oxides expressed in mole percent, SiO 2 The content is 0.00% or more and 15.00% or less, B 2 O 3 The content is 40.00% or more and 90.00% or less, ZnO content is 0.00% or more and 5.00% or less, La 2 O 3 The content is 5.00% or more and 40.00% or less, Y 2 O 3 The content is 1.00% or more and 20.00% or less, G.D. 2 O 3 The content is 0.00% or more and 3.00% or less, Yb 2 O 3 The content is 0.00% or more and less than 1.00%, ZrO 2 The content is 0.00% or more and 15.00% or less, TiO 2 The content is 0.00% or more and 2.00% or less, WO 3 The content is 0.00% or more and 2.00% or less, Bi 2 O 3 The content is 0.00% or more and 2.00% or less, Nb 2 O 5 The content is 0.00% or more and 2.00% or less, Li 2 O, Na 2 O and K 2 Total content of O (Li 2 O+Na 2 O+K 2 O) is 0.00% or more and 5.00% or less; The total content of MgO, CaO, SrO and BaO (MgO+CaO+SrO+BaO) is 0.00% or more and 5.00% or less, Y 2 O 3 B relative to content 2 O 3 Molar ratio (B 2 O 3 / Y 2 O 3 ) is 15.00 or less, ZrO 2 , ZnO, Nb 2 O 5 , TiO 2 , W.O. 3 and Bi 2 O 3 B relative to the total content of 2 O 3 Molar ratio of content (B 2 O 3 / (ZrO 2 +ZnO+Nb 2 O 5 + TiO 2 +W.O. 3 +Bi 2 O 3 ) is between 15.00 and 50.00, ZrO 2 , ZnO, Nb 2 O 5 and TiO 2 La relative to the total content 2 O 3 Molar ratio of content (La 2 O 3 / (ZrO 2 +ZnO+Nb 2 O 5 + TiO 2 ) is 4.00 or more, and An optical glass in which the content of F element expressed as an external ratio by mole percent relative to the total content of the glass composition based on the oxides (100 mole percent) is 0.00% or more and 3.00% or less.
2. 2. The optical glass according to claim 1, wherein the ZnO content is from 0.00% to 2.00%.
3. 2. The optical glass according to claim 1, wherein the ZnO content is from 0.00% to 1.70%.
4. Yb 2 O 3 2. The optical glass according to claim 1, wherein the content is from 0.00% to 0.20%.
5. 2. The optical glass according to claim 1, having a refractive index nd of 1.73000 or more and 1.77000 or less.
6. 2. The optical glass according to claim 1, having an Abbe number vd of 52.00 or greater and 53.00 or less.
7. The refractive index nd and the Abbe number νd are expressed by the following formula 1: nd≧2.20000-0.00871*νd The optical glass according to claim 1 , which satisfies the above.
8. 2. The optical glass according to claim 1, wherein the value calculated as (nd-1) / d from the refractive index nd and the specific gravity d is 0.173 or greater.
9. The ZnO content is 0.00% or more and 1.70% or less, Yb 2 O 3 The content is 0.00% or more and 0.20% or less, The refractive index nd is 1.73000 or more and 1.77000 or less, The Abbe number νd is 52.0 or more and 53.0 or less, The refractive index nd and the Abbe number νd are expressed by the following formula 1: nd≧2.20000-0.00871*νd and 2. The optical glass according to claim 1, wherein the value calculated as (nd-1) / d from the refractive index nd and the specific gravity d is 0.173 or greater.
10. An optical element comprising the optical glass according to any one of claims 1 to 9.
Citation Information
Patent Citations
Optical glass, preform, and optical element
CN102910816A
Low fluorescent optical glass
JP2002128539A