Epoxy resin composition, prepreg and fiber-reinforced composite material
The epoxy resin composition with monofunctional phenols and curing agents addresses the imbalance in elastic modulus, improving compressive and tensile strength of fiber-reinforced composites under severe conditions.
Patent Information
- Application Number
- JP2024065099
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-15
- Publication Date
- 2024-11-08
AI Technical Summary
Existing epoxy resin compositions for fiber-reinforced composites fail to achieve a balance between high temperature/humid elastic modulus and low rubber state elastic modulus, leading to insufficient tensile strength utilization and compressive strength under severe conditions.
An epoxy resin composition comprising specific components: [A] (epoxy resin with 4 or more epoxy groups), [B] (monofunctional phenols), [C] (curing agent), and [D] (curing accelerator), with [B] filling free volume to reduce crosslinking density and [C] ensuring heat resistance, resulting in a cured resin with improved properties.
The composition achieves both high elastic modulus under high temperature/humid conditions and low rubber state elastic modulus, enhancing compressive and tensile strength of fiber-reinforced composites.
Smart Images

Figure 2024159567000001 
Figure 2024159567000002 
Figure 2024159567000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an epoxy resin composition which provides a fiber-reinforced composite material having excellent mechanical properties, and to a prepreg and a fiber-reinforced composite material which use the epoxy resin composition. [Background technology]
[0002] Traditionally, fiber-reinforced composite materials made of reinforcing fibers such as carbon fibers and glass fibers and thermosetting resins such as epoxy resins and phenolic resins have been applied to many fields such as aerospace, automobiles, railway vehicles, ships, civil engineering and construction, and sporting goods because they are lightweight and have excellent mechanical properties such as strength and rigidity, heat resistance, and corrosion resistance. In particular, fiber-reinforced composite materials using continuous reinforcing fibers are used in applications that require high performance, and carbon fibers with excellent specific strength and specific elastic modulus are used as the reinforcing fibers, and thermosetting resins, especially epoxy resins that have adhesion to carbon fibers, heat resistance, elastic modulus, and chemical resistance, and have minimal cure shrinkage, are often used as the matrix resin. In recent years, as the use of fiber-reinforced composite materials has increased, the required properties have become stricter. In particular, when applied to aerospace applications and structural materials such as vehicles, it is required to fully maintain different physical properties such as tensile strength and compressive strength even under severe conditions. In order to meet these physical property requirements, the matrix resin has been improved. It is known that increasing the elastic modulus of the cured matrix resin is effective in improving the compressive strength of reinforced fiber composite materials under high temperature / humid conditions in order to suppress buckling of the reinforcing fibers under compressive load. On the other hand, it is necessary to increase the tensile strength utilization rate of the reinforcing fibers in order to improve the tensile strength, and it is known that decreasing the elastic modulus of the cured matrix resin in its rubber state improves the tensile strength utilization rate. It is also known that decreasing the elastic modulus of the cured matrix resin in its rubber state is effective in decreasing the density of crosslinking points (hereinafter sometimes referred to as crosslink density) of the cured matrix resin.
[0003] Patent Document 1 proposes an epoxy resin composition using a multifunctional epoxy resin and naphthol glycidyl ethers. Patent Document 2 proposes an epoxy resin composition using a pendant type epoxy resin. Patent Document 3 proposes an epoxy resin composition using a specified amount of a phenol compound having a specific functional group. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2020 / 058766 [Patent Document 2] International Publication No. 2010 / 109929 [Patent Document 3] International Publication No. 2018 / 159574 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the cured product of the epoxy resin composition described in Patent Document 1 exhibits a high elastic modulus under high temperature / humid conditions, but has a high crosslinking density structure, so that the elastic modulus in the rubber state is also high, and as a result, the tensile strength utilization rate has not been significantly improved. On the other hand, the cured product of the epoxy resin composition described in Patent Document 2 exhibits a high high-temperature / humid elastic modulus superior to epoxy resin compositions using conventional epoxy resins, and can also exhibit a lower rubber-state elastic modulus, but this is still insufficient. In addition, the cured product of the epoxy resin composition described in Patent Document 3 also has insufficient high-temperature / humid elastic modulus and rubber-state elastic modulus.
[0006] Therefore, the present invention provides an epoxy resin composition which can exhibit superior properties compared to conventional techniques in terms of the high temperature / wet elastic modulus and rubbery state elastic modulus of the cured product, a fiber-reinforced composite material using the epoxy resin composition, and a prepreg obtained by impregnating a fiber substrate with the resin composition. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention provides an epoxy resin composition having the following components: 1. An epoxy resin composition comprising at least the following components [A] to [D]: The component [A] is contained in an amount of 60 to 100 parts by mass relative to 100 parts by mass of the total epoxy resin, An epoxy resin composition comprising 13 parts by mass or more and 45 parts by mass or less of component [B]. [A]: Epoxy resin having four or more epoxy groups in one molecule [B]: Monofunctional phenols [C]: Hardener [D]: Curing accelerator 2. The epoxy resin composition according to 1 above, wherein the component [A] is represented by the general formula (I) described below. 3. The epoxy resin composition according to 1 or 2 above, wherein the component [B] is a hydroxyphenyl compound, a naphthol compound or a hydroxybiphenyl compound. 4. The epoxy resin composition according to any one of 1 to 3 above, wherein the component [B] is represented by the general formula (II), general formula (III), general formula (IV) or general formula (V) described below. 5. The epoxy resin composition according to any one of 1 to 4 above, wherein the component [C] is an aromatic polyamine. 6. The epoxy resin composition according to any one of 1 to 5 above, wherein the epoxy equivalent of component [A] is 90 g / eq or more and 300 g / eq or less, and the active hydrogen equivalent derived from the phenolic hydroxyl group of component [B] is 100 g / eq or more and 400 g / eq or less. The prepreg according to the present invention is obtained by impregnating reinforcing fibers with the epoxy resin composition according to any one of 1 to 6 above.
[0008] Furthermore, a fiber-reinforced composite material according to the present invention comprises a cured epoxy resin obtained by curing the epoxy resin composition according to any one of 1 to 6 above, and reinforcing fibers. Effect of the Invention
[0009] According to the present invention, it is possible to provide an epoxy resin composition that provides an epoxy resin cured product with both excellent elastic modulus and low rubber-state elastic modulus under high temperature / humid conditions. Fiber-reinforced composite materials and prepregs that use the epoxy resin composition of the present invention together with a fiber substrate exhibit excellent compressive strength and excellent tensile properties under high temperature / humid conditions due to the excellent properties of the epoxy resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Each of the components in the epoxy resin composition of the present invention will be described in detail below. In the present invention, the term "aromatic" refers to a compound containing an aromatic hydrocarbon or a conjugated unsaturated heterocyclic compound in its chemical structure.
[0011] The component [A] used in the present invention is an epoxy resin having four or more epoxy groups in one molecule. Specific examples of epoxy resins include diaminodiphenylmethane type, diaminodiphenylsulfone type, metaxylenediamine type, phenol novolac type, tetraphenylolethane type, naphthalene type, biphenyl type, and isocyanurate type epoxy resins and their halogen atom-substituted, alkyl-substituted, and hydrogenated products. In the present invention, one or two of the four or more epoxy groups contained in one molecule of the component [A] contain a molecular structure in which they have reacted with a phenolic hydroxyl group of a monofunctional phenol (component [B]) described below, and thus, in the cured product of the epoxy resin composition (hereinafter, sometimes referred to as a resin cured product), the structure has a low density of crosslinking points (i.e., a structure that can have a low rubber-state elastic modulus), but exhibits a high elastic modulus under high temperature / humid conditions. The high temperature / humid conditions refer to high temperature and humid conditions. In the case of resin compositions according to the conventional technology, a low crosslink density usually means that a large free volume is generated in the resin cured product, and therefore the elastic modulus is low under the above conditions. However, in the case of the epoxy resin composition of the present invention, although the crosslink density is low in the cured product, the free volume that is thought to be generated in the above conventional technology is filled by using the residue of monofunctional phenols derived from the component [B]. Therefore, the resin cured product does not have a low elastic modulus under high temperature / humid conditions. That is, in at least a part of the component [A], one or two of the four or more epoxy groups do not function as crosslinking points, but play a role of filling the free volume in the resin cured product, and the remaining epoxy groups react with the component [C] curing agent to function as crosslinking points and ensure heat resistance. From the viewpoint of suppressing the decrease in heat resistance due to such a reaction and forming a crosslinked structure with sufficient strength, it is important that the component [A] is an epoxy resin having four or more epoxy groups in one molecule. It is preferable that the number of epoxy groups in one molecule of the component [A] is six or less, because the density of crosslinking points in the resin cured product is not too high, and a structure with a low rubber-state elastic modulus is obtained.
[0012] In the present invention, from the viewpoint of the heat resistance and elastic modulus of the cured resin, the epoxy equivalent of the component [A] is preferably 90 g / eq or more and 300 g / eq or less, and more preferably 100 g / eq or more and 200 g / eq or less. When the epoxy equivalent is 300 g / eq or less, the crosslink density of the cured resin is not too low, and the heat resistance and elastic modulus are excellent, which is preferable. In addition, when the epoxy equivalent is 90 g / eq or more, the crosslink density of the cured resin is not too high, and the rubber-state elastic modulus is low, which is preferable. When multiple epoxy resins are used in combination as the component [A], each epoxy resin is preferably a component [A]. i ], then the value calculated by (Equation 1) is the epoxy equivalent of component [A].
[0013]
number
[0014] The specific chemical structure of the component [A] is preferably a compound represented by the following general formula (I): 2 The - or -O- group is preferable from the viewpoint of handling since the epoxy resin has a low viscosity.
[0015] [ka]
[0016] (In the above general formula (I), R 1 , R 2 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 1 , m 2 are integers from 0 to 4. 1 or m 2 If is 2 or more, multiple R 1 , R 2may be the same or different. X is -O-, -S-, -CO-, -C(=O)O-, -SO 2 -, -CH 2 -, -CH(CH 3 )-, -C(CH 3 ) 2 -, -N=N-, or -N=N-.) Examples of the epoxy resin represented by the above general formula (I) include tetraglycidyl-4,4'-diaminodiphenylmethane, tetraglycidyl-3,4'-diaminodiphenylmethane, tetraglycidyl-3,3'-diaminodiphenylmethane, tetraglycidyl-4,4'-diaminodiphenyl ether, tetraglycidyl-3,4'-diaminodiphenyl ether, tetraglycidyl-3,3'-diaminodiphenyl ether, tetraglycidyl-4,4'-diaminodiphenyl sulfone, tetraglycidyl-3,4'-diaminodiphenyl sulfone, tetraglycidyl-3,3'-diaminodiphenyl sulfone, etc. For example, the following commercially available products can be used as tetraglycidyl-4,4'-diaminodiphenylmethane. Examples of such epoxy resins include "Sumiepoxy" (registered trademark) ELM-434 (manufactured by Sumitomo Chemical Co., Ltd.), "jER" (registered trademark) 604 (manufactured by Mitsubishi Chemical Corporation), and "Araldite" (registered trademark) MY721 (manufactured by Huntsman Advanced Materials, Inc.).
[0017] In the present invention, from the viewpoint of heat resistance of the resin cured product, suppression of curing failure, and formation of a crosslinked structure with sufficient strength, the component [A] must be contained in an amount of 60 to 100 parts by mass relative to 100 parts by mass of the total epoxy resin, more preferably 80 to 100 parts by mass, even more preferably 90 to 100 parts by mass, and particularly preferably 100 parts by mass. By containing the component [A] in such a ratio relative to the total epoxy resin, a resin cured product exhibiting higher heat resistance is easily obtained. In addition, in the present invention, an epoxy resin other than the component [A] may be contained within a range that does not impede the effects of the invention.
[0018] The component [B] used in the present invention is a monofunctional phenol. Here, the monofunctional phenol is a compound that is a phenol and does not have a functional group capable of addition reaction with the epoxy group in the component [A] other than one phenolic hydroxyl group bonded to an aromatic ring in the molecule. By not having two or more functional groups that undergo addition reaction with the epoxy group of the component [A] in one molecule, the residue of the monofunctional phenol that has reacted with the epoxy group does not function as a crosslinking point, and the free volume is filled in the cured product, so that a high elastic modulus is expressed under high temperature / humid conditions. If two or more functional groups that can undergo addition reaction with the functional group of the component [A] containing an epoxy group are contained in one molecule together with the phenolic hydroxyl group, they react with the component [A] in the resin cured product and function as crosslinking points, so that the function for filling the free volume in the cured product is very small, and the high elastic modulus under high temperature / humid conditions shown in the present invention is not generally expressed.
[0019] In addition, the reaction between the phenolic hydroxyl group and the epoxy group usually starts at a relatively low temperature of about 100°C under the condition of the curing accelerator [D] described later, and the monofunctional phenols can be incorporated into the composition as an epoxy resin by reacting with the epoxy group of the component [A] before volatilization, so that the volatile content (mass%) in the process of curing the epoxy resin composition of the present invention is kept low compared to epoxy resin compositions using epoxy resins of the conventional technology such as pendant type epoxy resins. If the volatile content is high in the curing process, voids will be generated in the cured product, and these will become the starting point of destruction, causing a decrease in resin strength, so it is preferable that the volatile content is as low as possible. As a guideline for the volatile content, when the epoxy resin composition is left to stand in a hot air oven at 160°C for 30 minutes, it is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0.2% by mass or less.
[0020] As described above, from the viewpoint of filling the free volume in the cured product and improving the elastic modulus under high temperature / humid heat conditions, and from the viewpoint of reducing the volatile content in the process of curing the epoxy resin composition, the active hydrogen equivalent (hereinafter sometimes referred to as P-OH equivalent) derived from the phenolic hydroxyl group in the component [B] is preferably 100 g / eq or more and 400 g / eq or less, more preferably 120 g / eq or more and 300 g / eq or less, and even more preferably 130 g / eq or more and 260 g / eq or less. When multiple monofunctional phenols are used in combination as the component [B], each monofunctional phenol is preferably used as the component [B]. i ], then the value calculated using (Equation 2) is the active hydrogen equivalent derived from the phenolic hydroxyl group of the above component [B].
[0021]
number
[0022] The number of aromatic rings contained in one molecule of the monofunctional phenols is not limited, but may be two or more, and among them, those having two aromatic rings are preferably used. However, the number of aromatic rings contained in one molecule may be one. Examples include hydroxyphenyl compounds, naphthol compounds, and hydroxybiphenyl compounds. Specific examples include 4-hydroxybiphenyl, 3-hydroxybiphenyl, 2-hydroxybiphenyl, α-naphthol, β-naphthol, p-cumylphenol, m-cumylphenol, o-cumylphenol, 4-phenoxyphenol, 3-phenoxyphenol, 4-benzylphenol, 3-benzylphenol, styrenated phenol, tribenzylphenol, 2,6-di-tert-butyl-4-methylphenol, 3-methyl-6-tert-butylphenol, and 2,3,6-trimethylphenol.
[0023] The hydroxyphenyl compound is preferably a compound represented by the following general formula (II) or (V), the naphthol compound is preferably a compound represented by the following general formula (III), and the hydroxybiphenyl compound is preferably a compound represented by the following general formula (IV). In particular, hydroxyphenyl compounds and naphthol compounds are preferred from the viewpoint of ease of reaction due to their excellent solubility in epoxy resins and general-purpose organic solvents. In particular, the naphthol compound represented by general formula (III) is preferred from the viewpoint of excellent room temperature elastic modulus in the dry state of the resin cured product.
[0024] In the following general formulas (II), (III), and (IV), m 3 +m 4 , m 5 , m 6 +m 7 Each of m is preferably 2 or less, 3 ~m 7 At least one or all of the following are preferably 1 or less, and more preferably 0. In the following general formula (V), from the viewpoints of reducing the volatile content and heat resistance, m 8 is preferably 1 or more and 4 or less, and more preferably 2 or more and 3 or less.
[0025] [ka]
[0026] (In the above general formula (II), R 3 , R 4 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 3 is an integer from 0 to 4, and m 4 is an integer from 0 to 5. 3 or m 4 If is 2 or more, multiple R 3 , R4 may be the same or different. A is -O-, -S-, -CO-, -C(=O)O-, -SO 2 -, -CH 2 -,-CH(CH 3 )-, -C(CH 3 ) 2 -, -N=N-, or -N=N-.)
[0027] [ka]
[0028] (In the above general formula (III), R 5 represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 5 is an integer from 0 to 7. 5 If is 2 or more, multiple R 5 may be the same or different.)
[0029] [ka]
[0030] (In the above general formula (IV), R 6 , R 7 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 6 is an integer from 0 to 4, and m 7 is an integer from 0 to 5. 6 or m 7 If is 2 or more, multiple R 6 , R 7 may be the same or different.)
[0031] [ka]
[0032] (In the above general formula (V), R 8 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 8 is an integer from 0 to 5. 8 If is 2 or more, multiple R 8 may be the same or different.) In the epoxy resin composition according to the present invention, the amount of the component [B] relative to 100 parts by mass of the total epoxy resin is 13 parts by mass or more and 45 parts by mass or less, preferably 15 parts by mass or more and 40 parts by mass or less, and more preferably 17 parts by mass or more and 35 parts by mass or less. If the amount of the component [B] is within this range, the effect of reducing the rubber-state elastic modulus (reducing the density of crosslinking points) and expressing a high elastic modulus under high temperature / humid conditions can be obtained while suppressing the deterioration of heat resistance. In addition, the ratio of the P-OH equivalent of the component [B] to the epoxy group equivalent of the component [A] is preferably 1.00 to 3.00, more preferably 1.05 to 2.30, and even more preferably 1.10 to 2.00. If it is within this range, the above effect can be obtained more effectively.
[0033] The epoxy resin composition of the present invention must be used with the component [C] curing agent. The curing agent described here is a curing agent for the epoxy resin contained in the epoxy resin composition of the present invention, and is a compound having at least two or more active groups in one molecule that can react with epoxy groups. Specific examples of the curing agent include dicyandiamide, aromatic polyamines, and various acid anhydrides. By using an aromatic polyamine as a curing agent, an epoxy resin cured product with good heat resistance can be obtained. In particular, among aromatic polyamines, various isomers of diaminodiphenylsulfone have a rigid chemical structure, so that an epoxy resin cured product with good heat resistance and elastic modulus can be obtained. In addition, since they have an electron-withdrawing functional group, the nucleophilicity of the amine is appropriately suppressed, and a good pot life can be obtained in the resin preparation process and the intermediate substrate manufacturing process such as prepreg. Therefore, they are suitable curing agents. Among aromatic polyamines, compounds in which an alkyl group is substituted on the diaminodiphenylmethane skeleton are suitable curing agents from the viewpoint that the cured resin has a low water absorption rate due to the effect of the substituted alkyl group, and therefore has an excellent elastic modulus under high temperature / humid conditions.
[0034] Commercially available aromatic polyamine curing agents include Seika-Cure-S (manufactured by Wakayama Seika Kogyo Co., Ltd.), "JER Cure" (registered trademark) W (manufactured by Japan Epoxy Resins Co., Ltd.), and 3,3'-DAS (manufactured by Mitsui Chemicals, Inc.), "Prima Cure'' (registered trademark) M-DEA (manufactured by Arcsada Japan Co., Ltd.), "Prima Cure'' (registered trademark) M-DIPA (manufactured by Arcsada Japan Co., Ltd.), "Prima Cure'' (registered trademark) M-MIPA (manufactured by Arcsada Japan Co., Ltd.), and "Prima Cure'' (registered trademark) DETDA (manufactured by Arcsada Japan Co., Ltd.). These aromatic polyamines may be used alone or in a suitable mixture of two or more types. When mixed with other components, they may be in either a solid (powder) or liquid form, or both may be mixed and used.
[0035] The preferred amount of component [C] is an amount in which the ratio of the total number of moles of active hydrogen, including the number of moles of active hydrogen in component [B] and component [C], to the number of moles of epoxy groups derived from all epoxy resins contained in the epoxy resin composition is 0.6 to 1.4 times, which is preferable from the viewpoint of obtaining an epoxy resin cured product exhibiting good mechanical properties. If the molar ratio is 0.8 to 1.2 times, it is more preferable because the heat resistance is excellent. If the molar ratio is 1.1 to 1.5 times, it is preferable because the fast curing property is excellent.
[0036] In addition, in the preparation process of the epoxy resin composition, the component [C] is preferably kneaded in a state where the temperature of the epoxy resin composition containing the component [A] is less than 100°C, and the above temperature is more preferably 90°C or less, and further preferably 80°C or less. If the temperature at which the component [C] is kneaded is less than 100°C, the reactivity between the component [A] and the component [C] is suppressed, so that the increase in viscosity of the epoxy resin composition during kneading can be reduced. In addition, the lower limit of the temperature at which the component [C] is kneaded is preferably 50°C or more. In general, if the temperature is 50°C or more, the viscosity of the resin composition is not excessively high, and the component [C] can be sufficiently dispersed in the epoxy resin composition by kneading.
[0037] It is essential that the epoxy resin composition of the present invention contains a curing accelerator as component [D]. Specifically, component [D] can act as an accelerator for the addition reaction between the epoxy resin and monofunctional phenols, and promotes the reaction between component [A] and component [B]. On the other hand, it may promote the reaction between component [A] and component [C], which is preferable. As the curing accelerator, it is preferable to use at least one curing accelerator selected from the group consisting of aromatic urea compounds, imidazole derivatives, and phosphorus compounds, from the viewpoint of achieving both storage stability and reactivity of the epoxy resin composition.
[0038] Examples of the aromatic urea compound include 3-phenyl-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, toluenebisdimethylurea, etc. Commercially available aromatic urea compounds include DCMU-99 (manufactured by Hodogaya Chemical Co., Ltd.), "Omicure" (registered trademark) 24 (manufactured by PTI Japan, Inc.), etc.
[0039] Examples of the imidazole derivatives include 1-benzyl-2-methylimidazole, 1-benzyl-2-ethylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, etc. Commercially available imidazole derivatives include "Cureduct" (registered trademark) P-0505, 1B2MZ, 1B2PZ, 2MZ-CN, 2E4MZ-CN, 2PZ-CN (all manufactured by Shikoku Chemical Industry Co., Ltd.), etc.
[0040] Examples of the phosphorus compound include triphenylphosphine, tri-0-tolylphosphine, tris(p-methoxyphenyl)phosphine, triphenylphosphine, triphenylborane, tetraphenylphosphonium tetraphenylborate, etc. Commercially available phosphorus compounds include "Hokuko-TPP" (registered trademark), "TOTP" (registered trademark), "TPP-K" (registered trademark), "TPP-MK" (registered trademark), etc. (all manufactured by Hokko Chemical Industry Co., Ltd.).
[0041] The content of the curing accelerator, which is the component [D], is preferably 0.1 to 8.0 parts by mass, more preferably 0.5 to 5.0 parts by mass, based on 100 parts by mass of the total epoxy resin contained in the resin composition. By containing the curing accelerator in this range, an epoxy resin composition that has an excellent balance between storage stability and reaction rate and gives a resin cured product with good physical properties can be obtained.
[0042] In the epoxy resin composition of the present invention, it is also preferable to contain, as the component [E], a thermoplastic resin that dissolves in any of the epoxy resins constituting the composition at room temperature by dissolving it in the epoxy resin as described above, within the scope of not losing the effects of the present invention. Such a thermoplastic resin can be contained in order to control the tackiness of the obtained prepreg, control the fluidity of the matrix resin when the prepreg is heat-cured, and impart toughness without impairing the heat resistance and elastic modulus of the obtained fiber-reinforced composite material. As such a thermoplastic resin, a thermoplastic resin composed of a polyaryl ether skeleton is preferable, and examples thereof include polysulfone, polyphenylsulfone, polyethersulfone, polyetherimide, polyphenylene ether, polyetheretherketone, and polyetherethersulfone. These thermoplastic resins composed of a polyaryl ether skeleton may be used alone or in combination as appropriate. Among them, polyethersulfone and polyetherimide can be preferably used because they can impart toughness without reducing the heat resistance and mechanical properties of the obtained fiber-reinforced composite material.
[0043] The thermoplastic resin as the component [E] may be a commercially available product. For example, "Sumikaexcel" (registered trademark) 5003P, 5003PS, 5900P, 5400P, 5200P, 4800P, 4100P, 3600P, 2603MP (manufactured by Sumitomo Chemical Co., Ltd.), PET, PBT (manufactured by KDA Co., Ltd.), "J-POVAL" (registered trademark) JC-25, JM-17, JP-03 (manufactured by Nippon Vinyl Acetate Poval Co., Ltd.), "S-LEC" (registered trademark) BX-L, KS-1, KS-10 (manufactured by Sekisui Chemical Co., Ltd.), "Ultrathene" (registered trademark) 515, 530 (manufactured by Tosoh Corporation), "JPH-3800" (manufactured by Johoku Chemical Co., Ltd.), "YS Polystar UH130" (manufactured by Yasuhara Chemical Co., Ltd.), etc. may be mentioned.
[0044] The blending amount of the thermoplastic resin is preferably 1 to 50 parts by mass, based on 100 parts by mass of the total epoxy resin, from the viewpoints of ease of forming a resin film and tackiness of a prepreg produced by impregnating a fiber substrate with the resin film, and more preferably 2 to 20 parts by mass.
[0045] In the present invention, it is also preferable to contain particles mainly composed of a thermoplastic resin (hereinafter, sometimes referred to as thermoplastic resin particles). Such thermoplastic resin particles do not dissolve in other components such as epoxy resin in the prepreg of the present invention, and maintain their particulate form. Furthermore, even when heated at a temperature (e.g., 180°C) that is usually used to prepare a fiber-reinforced composite material, they do not dissolve in the fiber-reinforced composite material and maintain their particulate form. By containing such thermoplastic resin particles, when the prepreg of the present invention is laminated to prepare a fiber-reinforced composite material, the toughness of the resin layer formed between adjacent layers of reinforcing fibers is improved, and thus the impact resistance is improved.
[0046] The resin type of the thermoplastic resin particles can be any type that can be mixed with the epoxy resin composition. Among them, polyamide is most preferable, and among polyamides, polyamide 12, polyamide 6, polyamide 11, polyamide 6 / 12 copolymer, and polyamides (semi-IPN polyamides) that have been semi-IPN (polymer interpenetrating network structure) with epoxy compounds described in Examples 1 to 7 of JP 2009-221460 A provide particularly good adhesive strength with epoxy resins.
[0047] The shape and form of the thermoplastic resin particles may be spherical or non-spherical, and porous particles may also be used. Spherical particles are preferred in terms of shape, as they are excellent in viscoelasticity since they do not reduce the flow characteristics of the resin, and also have no starting point for stress concentration, providing high impact resistance.
[0048] Commercially available polyamide particles include SP-500, SP-10, TR-1, TR-2, 842P-48, and 842P-80 (manufactured by Toray Industries, Inc.), and Orgasol (registered trademark) 1002D, 2001UD, 2001EXD, 2002D, 3202D, 3501D, and 3502D (manufactured by Arkema Co., Ltd.). These polyamide particles may be used alone or in combination.
[0049] The epoxy resin composition of the present invention may contain a coupling agent, thermosetting resin particles, or inorganic fillers such as silica gel, carbon black, clay, carbon nanotubes, graphene, carbon particles, and metal powder, as long as the effects of the present invention are not impaired.
[0050] The prepreg of the present invention is obtained by impregnating the epoxy resin composition of the present invention into reinforcing fibers. That is, the prepreg of the present invention is obtained by using the above-mentioned epoxy resin composition as a matrix resin and compounding the epoxy resin composition with reinforcing fibers. As the reinforcing fibers, carbon fibers, graphite fibers, aramid fibers, glass fibers, etc. can be preferably mentioned. Among them, carbon fibers are particularly preferable. The tensile modulus of the carbon fibers is preferably in the range of 200 to 440 GPa. This range is preferable because the rigidity and strength of the carbon fiber reinforced composite material are all well-balanced at a high level. The tensile elongation of the carbon fibers is preferably in the range of 0.8 to 3.0%. Here, the tensile modulus and tensile elongation are values measured according to JIS R7601-2006.
[0051] Commercially available carbon fibers include "TORAYCA" (registered trademark) T800G-24K, "TORAYCA" (registered trademark) T800S-24K, "TORAYCA" (registered trademark) T700G-24K, "TORAYCA" (registered trademark) T300-3K, and "TORAYCA" (registered trademark) T700S-12K (all manufactured by Toray Industries, Inc.).
[0052] The form and arrangement of the carbon fibers can be appropriately selected from long fibers aligned in one direction, woven fabrics, and the like. In order to obtain a carbon fiber reinforced composite material that is lightweight and has a higher level of durability, it is preferable that the carbon fibers are in the form of continuous fibers such as long fibers aligned in one direction (fiber bundles) or woven fabrics. The prepreg of the present invention can be manufactured by various known methods. For example, the prepreg can be manufactured by a wet method in which the matrix resin is dissolved in an organic solvent to reduce the viscosity and impregnated into the reinforcing fibers, or a hot melt method in which the matrix resin is heated to reduce the viscosity without using an organic solvent and impregnated into the reinforcing fibers. In the wet method, the reinforcing fibers are immersed in a liquid containing the matrix resin, then pulled out, and the organic solvent is evaporated using an oven or the like to obtain a prepreg.
[0053] In addition, in the hot melt method, a method in which the matrix resin whose viscosity has been reduced by heating is directly impregnated into the reinforcing fibers can be used, or a method in which the matrix resin is first coated onto release paper or the like to produce a release paper sheet with a resin film, and then a resin film is placed on the reinforcing fiber side from both sides or one side of the reinforcing fibers, and the matrix resin is impregnated into the reinforcing fibers by heating and pressurizing can be used.
[0054] As a method for producing the prepreg of the present invention, a hot melt method in which the matrix resin is impregnated into the reinforcing fibers without using an organic solvent is preferred, since this method results in substantially no organic solvent remaining in the prepreg.
[0055] The prepreg of the present invention has a reinforcing fiber amount per unit area of 30 to 2,000 g / m 2 It is preferable that the amount of reinforcing fibers is 30 g / m 2 When the amount of reinforcing fibers is 2,000 g / m or more, the number of layers required to obtain a desired thickness during molding of the fiber-reinforced composite material can be reduced, and the work is likely to be simplified. 2 When it is equal to or less than this, the drape property of the prepreg is likely to be improved.
[0056] The fiber mass content of the prepreg of the present invention is preferably 30 to 90% by mass, more preferably 35 to 85% by mass, and even more preferably 40 to 80% by mass. When the fiber mass content is 30% by mass or more, the amount of resin is not too large, and the advantages of a fiber-reinforced composite material having excellent specific strength and specific elastic modulus are easily obtained, and when molding the fiber-reinforced composite material, the amount of heat generated during curing is unlikely to be too high. When the fiber mass content is 90% by mass or less, impregnation failure of the resin is unlikely to occur, and the voids in the obtained fiber-reinforced composite material are likely to be reduced.
[0057] A first embodiment of the fiber-reinforced composite material of the present invention is obtained by curing the prepreg of the present invention. The fiber-reinforced composite material of this embodiment can be produced, for example, by laminating the above-mentioned prepregs of the present invention in a predetermined form and curing the resin by applying pressure and heat. Here, the method of applying heat and pressure may be, for example, a press molding method, an autoclave molding method, a bagging molding method, a wrapping tape method, or an internal pressure molding method.
[0058] A second embodiment of the fiber-reinforced composite material of the present invention comprises a cured epoxy resin obtained by curing the epoxy resin composition of the present invention, and reinforcing fibers. The fiber-reinforced composite material of this embodiment can be produced by impregnating the reinforcing fibers directly with the epoxy resin composition of the present invention without going through a prepreg stage, and then heat curing the impregnated fibers, for example, by a molding method such as a hand lay-up method, a filament winding method, a pultrusion method, a resin injection molding method, or a resin transfer molding method.
[0059] The upper and lower limits of the numerical ranges described above can be combined in any manner. EXAMPLES
[0060] The present invention will be described in detail below with reference to examples. However, the scope of the present invention is not limited to these examples. The unit "parts" in the composition ratio means parts by mass unless otherwise noted. Furthermore, the measurements of various characteristics (physical properties) were performed in an environment with a temperature of 23°C and a relative humidity of 50% unless otherwise noted.
[0061] <Raw materials used in the examples and comparative examples> (1) Component [A] "Sumiepoxy" (registered trademark) ELM434 (tetraglycidyl-4,4'-diaminodiphenylmethane, manufactured by Sumitomo Chemical Co., Ltd.), epoxy equivalent: 122 g / eq, epoxy resin having 4 epoxy groups in one molecule 3,4'-TGDDE (Tetraglycidyl-3,4'-diaminodiphenyl ether, Toray Fine Chemical Co., Ltd.), epoxy equivalent: 106g / eq, epoxy resin with 4 epoxy groups in one molecule 4,4'-TGDDE (Tetraglycidyl-4,4'-diaminodiphenyl ether, manufactured by Toray Fine Chemicals Co., Ltd.), epoxy equivalent: 106g / eq, epoxy resin with 4 epoxy groups in one molecule (2) Epoxy resin other than component [A] "EPICLON" (registered trademark) 830 (bisphenol F type epoxy resin, manufactured by DIC Corporation), epoxy equivalent: 170 g / eq, epoxy resin having two epoxy groups in one molecule "TOREP" (registered trademark) A-204E (N,N-diglycidyl-p-phenoxyaniline, manufactured by Toray Fine Chemicals Co., Ltd.) Epoxy resin having two epoxy groups in one molecule, epoxy equivalent: 162g / eq, epoxy resin having two epoxy groups in one molecule "EPICLON" (registered trademark) HP4770 (bisnaphthalene type epoxy resin, manufactured by DIC Corporation), epoxy equivalent: 205 g / eq, epoxy resin having two epoxy groups in one molecule "Denacol" (registered trademark) EX-142 (o-phenylphenol glycidyl ether, manufactured by Nagase ChemteX Corporation), epoxy equivalent: 240 g / eq, monofunctional epoxy resin having one epoxy group per molecule (3) Component [B] p-Cumylphenol (Mitsui Fine Chemicals Co., Ltd.), P-OH equivalent: 212g / eq, hydroxyphenyl compound β-Naphthol (Mitsui Fine Chemicals Co., Ltd.), P-OH equivalent: 144g / eq, naphthol compound ANTAGE SP (styrenated phenol, Kawaguchi Chemical Industry Co., Ltd.), P-OH equivalent: 308g / eq, hydroxyphenyl compound TBP (tribenzylphenol, Kawaguchi Chemical Industry Co., Ltd.), P-OH equivalent: 348g / eq, hydroxyphenyl compound 2,3,6-TMP (2,3,6-trimethylphenol, Honshu Chemical Industry Co., Ltd.), P-OH equivalent: 136g / eq, hydroxyphenyl compound 3M6B (3-methyl-6-tert-butylphenol, Honshu Chemical Industry Co., Ltd.), P-OH equivalent: 164g / eq, hydroxyphenyl compound (4) Phenols other than component [B] Bisphenol F (Tokyo Chemical Industry Co., Ltd.), active hydrogen equivalent derived from phenolic hydroxyl groups: 100 g / eq, a phenolic compound with two phenolic hydroxyl groups in one molecule (5) Component [C] Seikacure-S (4,4'-diaminodiphenyl sulfone, melting point 178°C, manufactured by Wakayama Seika Co., Ltd.), active hydrogen equivalent derived from amino group: 62g / eq (6) Component [D] TPP-MK (Tetraphenylphosphonium tetra-p-tolylborate, manufactured by Hokko Chemical Industry Co., Ltd.) "Hokuko-TPP" (registered trademark) (triphenylphosphine, manufactured by Hokko Chemical Industry Co., Ltd.) <Various manufacturing and evaluation methods> (7) Preparation of Epoxy Resin Compositions (Examples 1 to 27 and Comparative Examples 1 to 19) The components other than the components [C] and [D] were added in the prescribed amounts in the compounding ratios shown in Tables 1 to 4 (units in the tables: parts by mass), and the mixture was heated to 130°C while kneading, and kneaded for 30 minutes at 130°C to obtain a viscous liquid. Next, the mixture was cooled to 70°C while kneading, and then the prescribed amounts of the components [C] and [D] were added, and the mixture was further kneaded to obtain an epoxy resin composition. (8) Preparation of hardened epoxy resin The epoxy resin composition prepared according to (7) above was degassed in a vacuum, and then heated from 30°C to 180°C at a rate of 1.7°C / min in a mold set to a thickness of 2 mm using a 2 mm Teflon (registered trademark) spacer, and cured at 180°C for 2 hours to obtain a 2 mm-thick plate-shaped cured resin. (9) Measurement of flexural modulus of cured resin under room temperature / dry conditions From the cured resin product prepared according to (8) above, rectangular test pieces 10 mm wide and 60 mm long were cut out and subjected to three-point bending in accordance with JIS K7171 (1994) using an Instron universal testing machine (manufactured by Instron Corp.) with a span of 32 mm, a crosshead speed of 2.5 mm / min, sample number n=6, and a load range for obtaining elastic modulus of 5-30 N. The average value of the elastic modulus was regarded as the bending modulus of the cured resin product under room temperature / dry conditions. (10) Measurement of flexural modulus of cured resin under high temperature / humid conditions From the cured resin produced according to (8) above, rectangular test pieces 10 mm wide and 60 mm long were cut out and immersed in boiling water at 98°C for 24 hours, after which they were subjected to three-point bending using an Instron universal testing machine (manufactured by Instron Corp.) under the same conditions as in (9) except that the measurement temperature was changed to 82°C, and the average value of the modulus of elasticity was taken as the flexural modulus of the cured resin under high temperature / humid conditions. A flexural modulus of 2.8 GPa or more, which is considered to be effective enough to improve the compressive strength of fiber-reinforced composite materials under high temperature / humid conditions, was deemed to pass. (11) Measurement of rubber-state elastic modulus of cured resin From the cured resin prepared according to (8) above, a rectangular specimen having a width of 10 mm and a length of 35 mm was cut out to obtain a test piece. Using a bending DMA (Q800: manufactured by TA Instruments), the storage modulus G' was measured by heating from 30°C to 320°C under the conditions of a measurement frequency of 1.0 Hz, a heating rate of 5°C / min, a strain of 0.1%, and a single cantilever mode, with the distance between the chucks set to 17.8 mm. In the storage modulus change curve with logG' on the vertical axis and temperature on the horizontal axis, the temperature at the intersection of the straight line portions of two regions that can be regarded as straight lines before and after the logG' suddenly drops with the temperature increase was determined as the glass transition temperature, and G' at a temperature 50°C or more above the glass transition temperature and at which the change curve of logG' can be regarded as a flat portion was determined as the rubber state modulus. The linear portions of the two regions are the region before the storage modulus drops sharply with the temperature rise, and the linear or nearly linear region shown in the region during the process of the storage modulus dropping sharply. A rubber-state modulus of 24 MPa or less, which is sufficient to improve the fiber strength utilization rate, was deemed to be acceptable. (12) Water absorption measurement of cured resin Three rectangular pieces, each 10 mm wide and 35 mm long, were cut out from the cured resin product prepared according to (8) above to obtain test pieces. The mass of the test piece before immersion in boiling water at 98°C and after immersion in boiling water at 98°C for 48 hours was measured, and the water absorption of the cured resin product was calculated using the following formula. The average value of the three test pieces was taken as the water absorption of the cured resin product.
[0062] Water absorption rate (%) = (mass of test piece after immersion - mass of test piece before immersion) / (mass of test piece before immersion) x 100 <Examples 1 to 27 and Comparative Examples 1 to 19> Epoxy resin compositions were prepared according to the above procedure (7) in accordance with the compounding ratios in Tables 1 to 4, and cured resins were obtained according to the above procedure (8). The cured resins were subjected to the measurements described in (9) to (12).
[0063] The various measurement results are shown in Tables 1 to 4.
[0064] [Table 1]
[0065] [Table 2]
[0066] [Table 3]
[0067] [Table 4]
[0068] <Examples 1 to 27> It is understood that the epoxy resin composition of the present invention contains all of the components [A] to [D] necessary for the composition, and contains 60 parts by mass or more of the component [A] and 13 to 45 parts by mass or less of the component [B] when the total epoxy resin is taken as 100 parts by mass, so that the resin cured product has both an excellent flexural modulus of 2.8 GPa or more under high temperature / humid conditions and an excellent rubber-state modulus of 24 MPa or less. Moreover, as can be seen from Example 7, it is understood that the flexural modulus under room temperature / dry conditions is excellent, especially when a compound containing a naphthalene ring is used as the component [B]. <Comparative Examples 1 to 4> This composition contains sufficient amounts of component [A], as well as [C] and [D], and does not contain component [B]. Compared with Comparative Examples 1 and 2, Comparative Examples 3 and 4 have improved flexural modulus and rubber state modulus under high temperature / humid conditions, but both are still insufficient. <Comparative Example 5> It contains a sufficient amount of component [A] as well as [C] and [D], and contains 60 parts by mass or more of component [A] when the total epoxy resin is 100 parts by mass, but does not contain component [B]. As an epoxy resin other than component [A], "Denacol" (registered trademark) EX-142 (a monofunctional epoxy resin having one epoxy group in the molecule) is used in combination with component [A] to reduce the free volume in the cured product. However, this resin composition has a very large amount of volatile matter during the curing process, and it was determined that it is not worthy of resin property evaluation. It can be understood that the monofunctional epoxy resin volatilized during the curing process because the reaction between the epoxy group of EX-142 and the active hydrogen in the amine contained in component [C] is slow. It is suggested that component [B] is important as a monofunctional component that fills the free volume in the cured product. <Comparative Examples 6 and 7> This composition contains sufficient amounts of component [A] as well as [C] and [D], does not contain component [B], and contains bisphenol F (a phenolic compound with two phenolic hydroxyl groups in one molecule) as a phenol other than component [B]. Both the improvement of the flexural modulus under high temperature / humid conditions and the reduction of the rubber-state modulus are insufficient. When the phenol is bisphenol F, it is found that even if it is incorporated into the epoxy resin crosslinking structure, it does not have the function of filling the free volume and increases the crosslinking density. <Comparative Example 8> This composition contains components [A], [B], [C], and [D], and contains 13 to 45 parts by mass of component [B] when the total epoxy resin is 100 parts by mass, but contains less than 60 parts by mass of component [A]. The cured product of this resin composition was very brittle and was determined to be unworthy of evaluation of resin properties. It can be assumed that the amount of component [A] blended was so small that a sufficient crosslinking structure could not be formed in the cured product. <Comparative Examples 9, 10, 12, 14, 15, 17 to 19> The composition contains a sufficient amount of component [A] as well as [B], [C] and [D], and the component [B] is less than 13 parts by mass when the total epoxy resin is 100 parts by mass. In Comparative Examples 9, 10, 18 and 19, the flexural modulus under high temperature / humid conditions is improved, but the amount of component [B] is small, so the reduction in the rubber state modulus is insufficient. In Comparative Examples 12, 14, 15 and 17, both the improvement in the flexural modulus under high temperature / humid conditions and the reduction in the rubber state modulus are insufficient. <Comparative Examples 11, 13, and 16> This composition contains sufficient amounts of component [A] as well as [B], [C], and [D], and the component [B] is more than 45 parts by mass when the total epoxy resin is 100 parts by mass. Because the amount of component [B] is large, the rubber-state elastic modulus is very low and excellent, but because a crosslinked structure with sufficient strength could not be formed, the cured product was brittle and the flexural modulus, especially under high temperature / humid conditions, was very low.
Claims
1. An epoxy resin composition comprising at least the following components [A] to [D]: Contains 60 to 100 parts by mass of component [A] relative to 100 parts by mass of the total epoxy resin; An epoxy resin composition comprising 13 parts by mass or more and 45 parts by mass or less of component [B]. [A]: an epoxy resin having four or more epoxy groups in one molecule [B]: Monofunctional phenols [C]: Hardener [D]: Curing accelerator
2. 2. The epoxy resin composition according to claim 1, wherein the component [A] is represented by general formula (I). 【Chemistry 1】 (In the above general formula (I), R 1 , R 2 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 1 , m 2 Each is an integer from 0 to 4. 1 Or m 2 When R is 2 or more, multiple R 1 , R 2 may be the same or different. X is -O-, -S-, -CO-, -C(=O)O-, -SO 2 --, --CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -N=N-, or any of the structures represented by the formula:
3. 3. The epoxy resin composition according to claim 1 or 2, wherein the component [B] is any one of a hydroxyphenyl compound, a naphthol compound, and a hydroxybiphenyl compound.
4. 2. The epoxy resin composition according to claim 1, wherein the component [B] is represented by general formula (II), general formula (III), general formula (IV) or general formula (V). 【Chemistry 2】 (In the above general formula (II), R 3 , R 4 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 3 is an integer from 0 to 4, m 4 is an integer from 0 to 5. 3 Or m 4 When R is 2 or more, multiple R 3 , R 4 may be the same or different. A is -O-, -S-, -CO-, -C(=O)O-, -SO 2 --, --CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -N=N-, or any of the structures represented by the formula: 【Chemistry 3】 (In the above general formula (III), R 5 represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 5 is an integer from 0 to 7. 5 When R is 2 or more, multiple R 5 may be the same or different.) 【Chemistry 4】 (In the above general formula (IV), R 6 , R 7 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 6 is an integer from 0 to 4, m 7 is an integer from 0 to 5. 6 Or m 7 When R is 2 or more, multiple R 6 , R 7 may be the same or different.) 【Chemistry 5】 (In the above general formula (V), R 8 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 8 is an integer from 0 to 5. 8 When R is 2 or more, multiple R 8 may be the same or different.)
5. 2. The epoxy resin composition according to claim 1, wherein component [C] is an aromatic polyamine.
6. 2. The epoxy resin composition according to claim 1, wherein the epoxy equivalent of the component [A] is 90 g / eq or more and 300 g / eq or less, and the active hydrogen equivalent derived from the phenolic hydroxyl group of the component [B] is 100 g / eq or more and 400 g / eq or less.
7. A prepreg obtained by impregnating reinforcing fibers with the epoxy resin composition according to any one of claims 1 to 6.
8. A fiber-reinforced composite material comprising a cured epoxy resin obtained by curing the epoxy resin composition according to any one of claims 1 to 6, and reinforcing fibers.
Citation Information
Patent Citations
Epoxy resin composition for fiber-reinforced composite material, prepreg, and fiber-reinforced composite material
WO2010109929A1
Epoxy resin composition, prepreg and fiber-reinforced composite material
WO2018159574A1
Epoxy resin composition, prepreg, and fiber reinforced composite material